A sodium ion battery positive electrode material and preparation method thereof

By preparing a composite structure of sodium-rich oxide with graphene nanosheets and carbon nanotubes, the problems of chemical stability and electrical conductivity of sodium-ion battery cathode materials were solved, realizing the preparation of high-performance battery materials and improving the overall performance of the battery.

CN118738359BActive Publication Date: 2024-11-19ZMARTEC TECH(SHENZHEN) LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411234294.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-09-04
Publication Date
2024-11-19
Estimated Expiration
2044-09-04

AI Technical Summary

Technical Problem

Existing sodium-ion battery cathode materials have poor overall performance in terms of chemical stability and conductivity, making it difficult to meet the requirements of high energy density and high conductivity, thus limiting their use in high-performance application scenarios.

Method used

Sodium-rich oxide powder is mixed with graphene nanosheets and carbon nanotubes, and through steps such as humidification, pre-pressing, drying, primary sintering and secondary sintering, a composite structure of sodium-rich composite oxide core, carbon-based conductive network and interface optimization layer is formed, thereby optimizing the electrochemical performance of the material.

Benefits of technology

It improves the conductivity and structural stability of the cathode material in sodium-ion batteries, enhances the overall performance of the battery, and strengthens the chemical stability and electron transport capability of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118738359B_ABST
    Figure CN118738359B_ABST
Patent Text Reader

Abstract

The invention discloses a method for preparing a positive electrode material for a sodium ion battery. The method comprises the following steps: mixing sodium-rich oxide powder with graphene nanosheets and carbon nanotubes to form a primary mixed powder, adding an appropriate amount of a polyol solution, and stirring to form a wetted material; placing the wetted material in a preset mold, pre-pressing it at room temperature to form a green body, drying it at a low temperature and then heating it to a medium temperature for primary sintering to solidify the shape of the green body and preliminarily form a microstructure; heating the green body subjected to the primary sintering to a high temperature and performing a secondary sintering to completely form a sodium-rich composite oxide inner core and an outer carbon-based conductive network, and cooling it to room temperature to obtain the positive electrode material for the sodium ion battery; the double-layer structure design of the sodium-rich composite oxide inner core and the carbon-based conductive network outer layer enables the electrode material to have excellent electrical conductivity and structural stability, is beneficial to improving the electrical conductivity and electrochemical stability of the electrode material, and improves the overall performance of the battery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of sodium ion batteries, and in particular to a sodium ion battery positive electrode material and a preparation method thereof. Background Art

[0002] As an important energy storage technology, sodium-ion batteries have gradually become the focus of market attention due to their low cost and high resource availability. Compared with lithium-ion batteries, sodium-ion batteries use more abundant materials and are environmentally friendly, making them have great application potential in electric vehicles, large-scale energy storage systems and portable electronic products. However, despite their obvious environmental and cost advantages, sodium-ion batteries still have a gap with lithium-ion batteries in energy density and cycle stability, which is mainly limited by the electrochemical properties of existing battery materials.

[0003] Existing sodium-ion battery cathode materials mostly use traditional single-phase structures, such as layered oxides or phosphates. Although these materials perform well in initial performance, they often face problems of poor structural stability and low conductivity during high-rate charge and discharge and long-term cyclic use. In addition, single-phase materials often find it difficult to simultaneously meet the requirements of high energy density and high conductivity, which limits the widespread use of sodium-ion batteries in high-performance application scenarios. For example, some materials may sacrifice the battery's cycle stability and charge and discharge efficiency when increasing energy density, making it difficult to meet the comprehensive performance requirements of chemical stability and conductivity, limiting their scope of application.

[0004] In view of this, it is necessary to improve the positive electrode materials of sodium ion batteries in the prior art to solve the technical problem of poor comprehensive performance of chemical stability and electrical conductivity. Summary of the invention

[0005] The object of the present invention is to provide a sodium ion battery positive electrode material and a preparation method thereof to solve the above technical problems.

[0006] To achieve this object, the present invention adopts the following technical solutions:

[0007] A method for preparing a positive electrode material for a sodium ion battery, comprising:

[0008] mixing sodium-rich oxide powder with graphene nanosheets and carbon nanotubes to form a primary mixed powder;

[0009] Add an appropriate amount of polyol solution to the obtained primary mixed powder, and stir to ensure uniform wetting to form a wetted material;

[0010] The wetted material is placed in a preset mold and pre-pressed at room temperature to form a green body;

[0011] The pre-pressed green body is dried at low temperature and then raised to medium temperature for primary sintering to solidify the shape of the green body and initially form a microstructure;

[0012] The primary sintered green body is heated to a high temperature and subjected to secondary sintering to form a sodium-rich composite oxide core, a carbon-based conductive network covering the surface of the sodium-rich composite oxide core, and an interface optimization layer formed between the carbon-based conductive network and the sodium-rich composite oxide core; wherein the sodium-rich composite oxide core is used for the storage and release of sodium ions, the carbon-based conductive network is a three-dimensional network structure composed of graphene nanosheets and carbon nanotubes, and is used to provide an electron transmission path and enhance the structural stability of the material; the interface optimization layer is used to improve interface adhesion and electrochemical stability;

[0013] After sintering, the mixture is naturally cooled to room temperature to obtain the positive electrode material for sodium ion batteries.

[0014] Optionally, the polyol solution is any one of glycerol, propylene glycol or ethylene glycol, or a combination of several of them.

[0015] Optionally, in the primary mixed powder, the mass ratio of sodium-rich oxide powder, graphene nanosheets and carbon nanotubes is 50% of sodium-rich oxide powder, 20% to 30% of graphene nanosheets, and 10% to 20% of carbon nanotubes.

[0016] Optionally, the step of adding a proper amount of polyol solution to the obtained primary mixed powder and stirring to ensure uniform wetting to form a wetted material specifically includes:

[0017] Mixing the selected polyols according to a preset ratio to prepare a polyol solution having a first concentration; the first concentration ranges from 15% to 20%;

[0018] The polyol solution is heated to 35°C to 40°C for temperature adjustment;

[0019] The primary mixed powder is mixed with the temperature-adjusted polyol solution using a stirrer; wherein the stirring speed of the stirrer is controlled at 300 rpm for 20 minutes;

[0020] The stirred mixture was subjected to ultrasonic treatment with the frequency set to 40 kHz and the treatment time set to 10 min;

[0021] The ultrasonically treated mixture was allowed to stand for 1 hour to allow the primary mixed powder to fully absorb the polyol solution and be reorganized to form a wet material.

[0022] Optionally, the pre-pressed green body is dried at a low temperature and then raised to a medium temperature for primary sintering to solidify the shape of the green body and preliminarily form a microstructure, specifically comprising:

[0023] The pre-pressed green body was left to stand at room temperature for 2 hours, and then dried in a constant temperature oven at 50°C for 4 hours;

[0024] The dried green body was placed in a resistance furnace, heated from room temperature to 200°C at a rate of 10°C per hour, and maintained at 200°C for 1 hour;

[0025] The temperature of the resistance furnace was increased from 200°C to 500°C at a rate of 50°C per hour and maintained at 500°C for 2 hours;

[0026] During the heating process, gas flow control technology is introduced to control the microscopic particle size and crystal structure of the microscopic particles by injecting a preset proportion of oxygen and nitrogen mixed gas into the resistance furnace.

[0027] Optionally, during the heating process, a gas flow control technology is introduced to control the microscopic particle size and crystal structure of the microscopic particles by injecting a preset ratio of oxygen and nitrogen mixed gas into the resistance furnace, specifically including:

[0028] Set the mixing ratio of oxygen and nitrogen; the ratio of oxygen is set between 10% and 20%;

[0029] Use a flow meter to control the gas injection rate at 1~5L / min to ensure uniform distribution of gas in the resistance furnace;

[0030] As the temperature rises from 200°C to 500°C, the mixed gas is continuously injected to form a slight oxidation reaction to control the growth rate and direction of the material crystals;

[0031] The image information of crystal growth is obtained in real time by an infrared imaging system installed in the resistance furnace. According to the obtained image information of crystal growth, the gas flow rate or temperature setting is adjusted to control the microscopic particle size and crystal structure of the microscopic particles.

[0032] Optionally, the primary sintered green body is heated to a high temperature and subjected to secondary sintering to form a sodium-rich composite oxide core, a carbon-based conductive network covering the surface of the sodium-rich composite oxide core, and an interface optimization layer formed between the carbon-based conductive network and the sodium-rich composite oxide core, specifically comprising:

[0033] The primary sintered green body is placed in a high temperature furnace, the temperature is increased from 500°C to 800°C at a rate of 100°C per hour, and maintained at 800°C for 3 hours;

[0034] Introducing a carbon source gas into the high temperature furnace, and fine-tuning the flow control to 5 ml per hour, so that the carbon source gas is decomposed at high temperature to form nano-scale carbon particles, and the nano-scale carbon particles are deposited on the microscopic particle surface of the green body to form a carbon-based conductive network;

[0035] The speed and direction of crystal growth are controlled by temperature gradient control and gas flow rate regulation, thereby optimizing the interface between the sodium-rich composite oxide core and the carbon-based conductive network to form an interface optimization layer between the carbon-based conductive network and the sodium-rich composite oxide core.

[0036] Optionally, after the sintering is completed, the sintering is naturally cooled to room temperature to obtain a positive electrode material for a sodium ion battery, and then the following steps are further included:

[0037] The cooled sodium-ion battery positive electrode material is mechanically polished and chemically surface treated to remove surface impurities.

[0038] The present invention also provides a sodium ion battery positive electrode material, which is prepared by the method for preparing the sodium ion battery positive electrode material as described above, and the sodium ion battery positive electrode material comprises:

[0039] A sodium-rich composite oxide core for storage and release of sodium ions;

[0040] A carbon-based conductive network, a three-dimensional network structure composed of graphene nanosheets and carbon nanotubes, covers the surface of the sodium-rich composite oxide core to provide an electron transfer path and enhance the structural stability of the material;

[0041] The interface optimization layer is formed between the carbon-based conductive network and the sodium-rich composite oxide core to improve interface adhesion and electrochemical stability.

[0042] Compared with the prior art, the present invention has the following beneficial effects: during processing, the primary mixed powder formed by mixing sodium-rich oxide powder with graphene nanosheets and carbon nanotubes ensures the uniform distribution of various materials at the microscopic level, and then through wetting, molding, drying and sintering treatment, not only the macroscopic morphology of the material is solidified, but more importantly, the chemical and physical interactions between the sodium-rich composite oxide and the carbon-based material are promoted at high temperature through the sintering process to form a stable composite structure. The double-layer structure of the sodium-rich composite oxide inner core and the carbon-based conductive network outer layer, as well as the interface optimization layer design, make the electrode material have excellent electrical conductivity and structural stability, which is beneficial to improve the electrical conductivity and electrochemical stability of the electrode material, and improve the overall performance of the battery. BRIEF DESCRIPTION OF THE DRAWINGS

[0043] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.

[0044] The structures, proportions, sizes, etc. illustrated in the drawings of this specification are only used to match the contents disclosed in the specification so as to facilitate understanding and reading by persons familiar with this technology. They are not used to limit the conditions under which the present invention can be implemented, and therefore have no substantive technical significance. Any structural modification, change in proportion or adjustment of size, without affecting the effects and purposes that can be achieved by the present invention, should still fall within the scope of the technical contents disclosed by the present invention.

[0045] Figure 1 This is a schematic diagram of a process for preparing a positive electrode material for a sodium ion battery according to Example 1;

[0046] Figure 2 The second schematic diagram is a process flow diagram of the method for preparing the positive electrode material for a sodium ion battery of Example 1;

[0047] Figure 3 The third schematic diagram is a process flow diagram of the method for preparing the positive electrode material of a sodium ion battery of Example 1. DETAILED DESCRIPTION

[0048] In order to make the purpose, features and advantages of the present invention more obvious and easy to understand, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the embodiments described below are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0049] In the description of the present invention, it should be understood that the terms "upper", "lower", "top", "bottom", "inside", "outside" and the like indicate positions or positional relationships based on the positions or positional relationships shown in the drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation of the present invention. It should be noted that when a component is considered to be "connected" to another component, it may be directly connected to the other component or there may be a centrally arranged component at the same time.

[0050] The technical solution of the present invention is further described below with reference to the accompanying drawings and through specific implementation methods.

[0051] Embodiment 1:

[0052] Combination Figures 1 to 3 As shown, an embodiment of the present invention provides a method for preparing a positive electrode material for a sodium ion battery, comprising:

[0053] S1, mixing sodium-rich oxide powder with graphene nanosheets and carbon nanotubes to form a primary mixed powder; wherein the sodium-rich oxide powder is composed of sodium ion active compounds, such as sodium cobalt oxide (NCO) or sodium nickel manganese oxide (NNMO).

[0054] In this step, sodium-rich oxide powder is mixed with graphene nanosheets and carbon nanotubes to form a primary mixed powder. This step is the basis of the preparation process and ensures the uniform distribution of the different materials, providing a uniform starting point for the subsequent composite material structure. Sodium-rich oxide provides the necessary lithium ions for the battery, while the addition of graphene and carbon nanotubes is intended to enhance the conductivity and mechanical stability of the final product.

[0055] S2, adding an appropriate amount of polyol solution to the obtained primary mixed powder, and stirring to ensure uniform wetting to form a wetted material;

[0056] In this step, the polyol solution is added to the primary mixed powder and stirred thoroughly to ensure that each particle is evenly wetted by the solution. This process is critical to improving the fluidity and uniformity of the powder during the subsequent pressing process, which helps to improve the density and microstructure of the final material.

[0057] S3, placing the wetted material into a preset mold and pre-pressing it at room temperature to form a green body;

[0058] This step is mainly to transform the loose powder into a green body with a certain shape and strength, preparing for the subsequent sintering process. The control of pressure and time during the pre-pressing process is crucial to maintaining the shape of the green body and reducing the generation of cracks.

[0059] S4, drying the pre-pressed green body at low temperature, and then raising the temperature to medium temperature for primary sintering to solidify the shape of the green body and preliminarily form a microstructure;

[0060] The shape of the solid body is solidified and the microstructure begins to form through heat treatment. Primary sintering is a key step in adjusting the microstructure of the material and enhancing the physical properties. The appropriate sintering temperature and time can effectively enhance the structural integrity of the material.

[0061] S5, heating the primary sintered green body to a high temperature and performing secondary sintering to form a sodium-rich composite oxide core, a carbon-based conductive network covering the surface of the sodium-rich composite oxide core, and an interface optimization layer formed between the carbon-based conductive network and the sodium-rich composite oxide core; wherein the sodium-rich composite oxide core is used for the storage and release of sodium ions, the carbon-based conductive network is a three-dimensional network structure composed of graphene nanosheets and carbon nanotubes, and is used to provide an electron transmission path and enhance the structural stability of the material; and the interface optimization layer is used to improve interface adhesion and electrochemical stability;

[0062] High-temperature sintering not only further enhances the structural stability of the material, but also optimizes the conductivity network through chemical reactions and physical changes at high temperatures, ultimately forming a high-performance positive electrode material.

[0063] S6, after sintering, naturally cool to room temperature to obtain the positive electrode material for sodium ion batteries. After sintering, the green body needs to be naturally cooled to room temperature. During this process, the microstructure and chemical properties of the material will stabilize. Gradual cooling helps to avoid internal stress and micro cracks that may be caused by rapid cooling, ensuring a high-quality final product.

[0064] The working principle of the present invention is as follows: during operation, the primary mixed powder formed by mixing sodium-rich oxide powder with graphene nanosheets and carbon nanotubes ensures the uniform distribution of various materials at the microscopic level. Subsequently, through wetting, molding, drying and sintering treatments, not only the macroscopic morphology of the material is solidified, but more importantly, the chemical and physical interactions between the sodium-rich composite oxide and the carbon-based material are promoted at high temperature through the sintering process to form a stable composite structure. The double-layer structure of the sodium-rich composite oxide inner core and the carbon-based conductive network outer layer, as well as the interface optimization layer design, enable the electrode material to have excellent electrical conductivity and structural stability, which is beneficial to improving the electrical conductivity and electrochemical stability of the electrode material and improving the overall performance of the battery.

[0065] In this embodiment, the polyol solution is any one of glycerol, propylene glycol or ethylene glycol or a combination of several of them.

[0066] It should be noted that different polyols have different solubility, viscosity and volatilization speed, which makes it possible to accurately control the wetting degree of the mixed powder according to specific material requirements and processing conditions, thereby optimizing the subsequent molding and sintering processes and improving the uniformity and performance of the final material.

[0067] In this embodiment, in the primary mixed powder, the mass ratio of sodium-rich oxide powder, graphene nanosheets and carbon nanotubes is 50% for sodium-rich oxide powder, 20% to 30% for graphene nanosheets and 10% to 20% for carbon nanotubes.

[0068] It should be noted that the mass ratio of sodium-rich oxide powder, graphene nanosheets and carbon nanotubes is 50% sodium-rich oxide, while the ratio of graphene nanosheets and carbon nanotubes is adjustable within a set range. This ratio ensures that the composite material optimizes the electron conduction path and structural strength by adding graphene and carbon nanotubes while maintaining high-capacity sodium-rich oxide, thereby improving the overall electrochemical performance and mechanical stability of the battery. This design also provides the possibility of adjusting the proportion of each component according to performance requirements during the preparation process, further enhancing the flexibility and practicality of material design.

[0069] In this embodiment, it is specifically described that step S2 specifically includes:

[0070] S21, mixing the selected polyols (glycerol, propylene glycol or ethylene glycol) according to a preset ratio to prepare a polyol solution with a first concentration; the first concentration ranges from 15% to 20%; to ensure sufficient wetting ability while avoiding excessive moisture introduction.

[0071] S22, heating the polyol solution to 35°C to 40°C for temperature adjustment; this temperature range helps to improve the penetration ability of the solvent while reducing the risk of material damage caused by excessive temperature.

[0072] S23, using a stirrer to mix the primary mixed powder with the temperature-adjusted polyol solution; wherein the stirring speed of the stirrer is controlled at 300 rpm for 20 minutes; ensuring that all the powders are evenly wetted by the solution while avoiding agglomeration of the powders.

[0073] S24, subjecting the stirred mixture to ultrasonic treatment, with the frequency set to 40 kHz and the treatment time being 10 minutes; this step helps to break up microaggregates that may exist in the material and enhance the uniformity of the material.

[0074] S25, the ultrasonically treated mixture is allowed to stand for 1 hour to allow the primary mixed powder to fully absorb the polyol solution and be reorganized to form a wetted material, so as to optimize the interaction between particles and the structural arrangement.

[0075] In this embodiment, it is specifically described that step S4 specifically includes:

[0076] S41, leaving the pre-pressed green body at room temperature for 2 hours, and then drying it in a constant temperature oven at 50°C for 4 hours; this step ensures that moisture inside the green body is fully removed to avoid structural damage caused by steam pressure during sintering.

[0077] S42, placing the dried green body into a resistance furnace, heating it from room temperature to 200°C at a rate of 10°C per hour, and maintaining it at 200°C for 1 hour; this temperature stage is mainly used to eliminate residual organic matter and promote the bonding of powders.

[0078] S43, raising the temperature of the resistance furnace from 200°C to 500°C at a rate of 50°C per hour, and maintaining the temperature at 500°C for 2 hours; this stage is mainly used to promote the initial sintering between powder particles to form a microstructure framework.

[0079] S44, during the heating process, introduces gas flow control technology to control the microscopic particle size and crystal structure of the microscopic particles by injecting a preset ratio of oxygen and nitrogen mixed gas into the resistance furnace.

[0080] Introduce a mixed gas of oxygen and nitrogen to adjust the furnace atmosphere, optimize the redox reaction, and control the particle growth rate and morphology. This step helps to accurately control the microscopic particle size and crystal structure of the material. The oxygen content is 10%.

[0081] In this embodiment, it is specifically explained that step S44 specifically includes:

[0082] S441, sets the mixing ratio of oxygen and nitrogen; the proportion of oxygen is set at 10% to 20%; nitrogen accounts for the remaining proportion, which helps to create a slightly oxidizing environment, thereby controlling the degree of oxidation of the material and the formation of the crystal structure.

[0083] S442, use a flow meter to control the gas injection rate of 1~5L / min to ensure uniform distribution of gas in the resistance furnace; the flow rate is usually controlled between 1 and 5 liters per minute, which is set according to the volume of the furnace and the required gas replacement rate.

[0084] S443, in the process of increasing the temperature from 200°C to 500°C, continuously injecting the mixed gas to form a slight oxidation reaction to control the growth speed and direction of the material crystal;

[0085] The gas flow at this stage not only helps to maintain the gas pressure balance in the furnace, but also controls the growth rate and direction of the material crystals through a slight oxidation reaction, which is achieved by affecting the grain boundary migration and particle growth mechanism.

[0086] S444, by acquiring image information of crystal growth in real time through an infrared imaging system installed in the resistance furnace, and adjusting the gas flow rate or temperature setting according to the acquired image information of crystal growth to control the microscopic particle size and crystal structure of the microscopic particles.

[0087] According to the image information of the crystal growth obtained, the gas flow rate or temperature setting is adjusted to control the microscopic particle size and crystal structure of the microscopic particles, specifically including:

[0088] Use image analysis software to process the acquired image information of crystal growth, measure the size, shape and growth rate of the crystal, and analyze the interface roughness of the crystal and the clarity of the crystal boundary;

[0089] According to the changes in the measured crystal size, shape and growth rate, a corresponding control strategy is formulated; the control strategy includes:

[0090] 1. If the crystal grows too fast or has an irregular shape, reduce the flow of reducing gas (such as hydrogen) and increase the proportion of oxygen to stabilize crystal growth and reduce defects.

[0091] 2. If the crystal growth is too slow or the crystal size is smaller than expected, increase the flow rate of reducing gas to promote crystal growth.

[0092] 3. According to the real-time feedback of crystal growth, appropriately increase or decrease the temperature in the furnace. If the crystal is too large or the growth rate is too fast, appropriately reduce the temperature; if the crystal is too small or the growth rate is too slow, appropriately increase the temperature.

[0093] In this embodiment, it is specifically described that step S5 specifically includes:

[0094] S51, placing the primary sintered green body in a high temperature furnace, heating from 500°C to 800°C at a rate of 100°C per hour, and maintaining the temperature at 800°C for 3 hours; this rate and temperature setting help to slowly release any residual organic components and avoid the material from becoming unstable too quickly. After reaching 800°C, maintain this temperature for 3 hours. This high temperature maintenance is to ensure the full formation of the sodium-rich composite oxide core, at which point the composite oxide crystals will further grow through lattice rearrangement and grain boundary diffusion, enhancing the structural integrity of the material.

[0095] S52, introducing a carbon source gas into the high temperature furnace, and fine-tuning the flow control to set it to 5 ml per hour, so that the carbon source gas is decomposed at high temperature to form nano-scale carbon particles, and the nano-scale carbon particles are deposited on the microscopic particle surface of the green body to form a carbon-based conductive network;

[0096] The carbon source decomposes at high temperature to form nano-scale carbon particles, which are deposited on the surface of the microscopic particles (sodium-rich oxide particles) of the green body to form a carbon-based conductive network. This technology helps to control the uniform distribution and structural morphology of carbon-based materials at high temperatures to ensure maximum conductivity. The carbon source gas can be methane.

[0097] S53, controlling the speed and direction of crystal growth by temperature gradient control and gas flow rate regulation, thereby optimizing the interface between the sodium-rich composite oxide core and the carbon-based conductive network to form an interface optimization layer between the carbon-based conductive network and the sodium-rich composite oxide core. This operation ensures that the material has optimized electrochemical properties and mechanical stability.

[0098] In this embodiment, it is further explained that after step S6, the following steps are further included:

[0099] S7, mechanically grinding and chemically surface treating the cooled sodium ion battery positive electrode material to remove surface impurities.

[0100] Embodiment 2:

[0101] The present invention also provides a sodium ion battery positive electrode material, which is prepared by the above method for preparing the sodium ion battery positive electrode material, and the sodium ion battery positive electrode material comprises:

[0102] The sodium-rich composite oxide core is used for the storage and release of sodium ions; the sodium-rich composite oxide core is the core of the positive electrode material, an active substance based on sodium ions, responsible for the storage and release of sodium ions, which generally exhibits higher energy density and chemical stability, providing basic electrochemical functions for the battery.

[0103] The carbon-based conductive network, a three-dimensional network structure composed of graphene nanosheets and carbon nanotubes, covers the surface of the sodium-rich composite oxide core, and is used to provide an electron transmission path and enhance the structural stability of the material; the carbon-based conductive network is tightly combined with the sodium-rich composite oxide core through physical methods, ensuring efficient exchange of electrons and ions.

[0104] The interface optimization layer is formed between the carbon-based conductive network and the sodium-rich composite oxide core to improve interface adhesion and electrochemical stability; the interface optimization layer includes slight carbon doping or oxide coating to reduce interface impedance and prevent material degradation in long-term cycles.

[0105] In addition, a protective outer shell layer can be provided, and a nano-carbon coating layer is formed on the outermost layer through coating technology to protect the internal structure from environmental factors and maintain good contact between the electrolyte and the active material.

[0106] As described above, the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features thereof may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A method for preparing a positive electrode material for a sodium ion battery, It is characterized in that include: mixing sodium-rich oxide powder with graphene nanosheets and carbon nanotubes to form a primary mixed powder; Add an appropriate amount of polyol solution to the obtained primary mixed powder, and stir to ensure uniform wetting to form a wetted material; The wetted material is placed in a preset mold and pre-pressed at room temperature to form a green body; The pre-pressed green body is dried at low temperature and then raised to medium temperature for primary sintering to solidify the shape of the green body and initially form a microstructure; The primary sintered green body is heated to a high temperature and subjected to secondary sintering to form a sodium-rich composite oxide core, a carbon-based conductive network covering the surface of the sodium-rich composite oxide core, and an interface optimization layer formed between the carbon-based conductive network and the sodium-rich composite oxide core; wherein the sodium-rich composite oxide core is used for the storage and release of sodium ions, the carbon-based conductive network is a three-dimensional network structure composed of graphene nanosheets and carbon nanotubes, and is used to provide an electron transmission path and enhance the structural stability of the material; the interface optimization layer is used to improve interface adhesion and electrochemical stability; After sintering, the mixture is naturally cooled to room temperature to obtain a positive electrode material for a sodium ion battery; The process of heating the primary sintered green body to a high temperature and performing secondary sintering to form a sodium-rich composite oxide core, a carbon-based conductive network covering the surface of the sodium-rich composite oxide core, and an interface optimization layer formed between the carbon-based conductive network and the sodium-rich composite oxide core specifically includes: The primary sintered green body is placed in a high temperature furnace, the temperature is increased from 500°C to 800°C at a rate of 100°C per hour, and maintained at 800°C for 3 hours; Introducing a carbon source gas into the high temperature furnace, and fine-tuning the flow control to 5 ml per hour, so that the carbon source gas is decomposed at high temperature to form nano-scale carbon particles, and the nano-scale carbon particles are deposited on the microscopic particle surface of the green body to form a carbon-based conductive network; The speed and direction of crystal growth are controlled by temperature gradient control and gas flow rate regulation, thereby optimizing the interface between the sodium-rich composite oxide core and the carbon-based conductive network to form an interface optimization layer between the carbon-based conductive network and the sodium-rich composite oxide core.

2. The method for preparing the positive electrode material for a sodium ion battery according to claim 1, It is characterized in that The polyol solution is any one of glycerol, propylene glycol or ethylene glycol or a combination of several of them.

3. The method for preparing the positive electrode material for a sodium ion battery according to claim 1, It is characterized in that In the primary mixed powder, the mass ratio of sodium-rich oxide powder, graphene nanosheets and carbon nanotubes is 50% of sodium-rich oxide powder, 20% to 30% of graphene nanosheets and 10% to 20% of carbon nanotubes.

4. The method for preparing the positive electrode material for a sodium ion battery according to claim 1, It is characterized in that The method further comprises adding a proper amount of polyol solution to the obtained primary mixed powder, and stirring to ensure uniform wetting to form a wetted material, which specifically comprises: Mixing the selected polyols according to a preset ratio to prepare a polyol solution having a first concentration; the first concentration ranges from 15% to 20%; The polyol solution is heated to 35°C to 40°C for temperature adjustment; The primary mixed powder is mixed with the temperature-adjusted polyol solution using a stirrer; wherein the stirring speed of the stirrer is controlled at 300 rpm for 20 minutes; The stirred mixture was subjected to ultrasonic treatment with the frequency set to 40 kHz and the treatment time set to 10 min; The ultrasonically treated mixture was allowed to stand for 1 hour to allow the primary mixed powder to fully absorb the polyol solution and be reorganized to form a wet material.

5. The method for preparing the positive electrode material for a sodium ion battery according to claim 1, It is characterized in that The pre-pressed green body is dried at a low temperature and then raised to a medium temperature for primary sintering to solidify the shape of the green body and preliminarily form a microstructure, specifically comprising: The pre-pressed green body was left to stand at room temperature for 2 hours, and then dried in a constant temperature oven at 50°C for 4 hours; The dried green body was placed in a resistance furnace, heated from room temperature to 200°C at a rate of 10°C per hour, and maintained at 200°C for 1 hour; The temperature of the resistance furnace was increased from 200°C to 500°C at a rate of 50°C per hour and maintained at 500°C for 2 hours; During the heating process, gas flow control technology is introduced to control the microscopic particle size and crystal structure of the microscopic particles by injecting a preset proportion of oxygen and nitrogen mixed gas into the resistance furnace.

6. The method for preparing the positive electrode material for a sodium ion battery according to claim 5, It is characterized in that During the heating process, gas flow control technology is introduced to control the microscopic particle size and crystal structure of the microscopic particles by injecting a preset ratio of oxygen and nitrogen mixed gas into the resistance furnace, including: Set the mixing ratio of oxygen and nitrogen; the ratio of oxygen is set between 10% and 20%; Use a flow meter to control the gas injection rate at 1~5L / min to ensure uniform distribution of gas in the resistance furnace; As the temperature rises from 200°C to 500°C, the mixed gas is continuously injected to form a slight oxidation reaction to control the growth rate and direction of the material crystals; The image information of crystal growth is obtained in real time by an infrared imaging system installed in the resistance furnace. According to the obtained image information of crystal growth, the gas flow rate or temperature setting is adjusted to control the microscopic particle size and crystal structure of the microscopic particles.

7. The method for preparing the positive electrode material for a sodium ion battery according to claim 1, It is characterized in that After the sintering is completed, the mixture is naturally cooled to room temperature to obtain a positive electrode material for a sodium ion battery, and then the following steps are further included: The cooled sodium-ion battery positive electrode material is mechanically polished and chemically surface treated to remove surface impurities.

8. A sodium ion battery cathode material, It is characterized in that The method for preparing a positive electrode material for a sodium ion battery according to any one of claims 1 to 7 is adopted, wherein the positive electrode material for a sodium ion battery comprises: A sodium-rich composite oxide core for storage and release of sodium ions; A carbon-based conductive network, a three-dimensional network structure composed of graphene nanosheets and carbon nanotubes, covers the surface of the sodium-rich composite oxide core to provide an electron transfer path and enhance the structural stability of the material; The interface optimization layer is formed between the carbon-based conductive network and the sodium-rich composite oxide core to improve interface adhesion and electrochemical stability.