Safe composite current collector
By arranging a high-density first metal coating and a low thermal shrinkage support layer on the support layer of the composite current collector, a point resistance is formed, which solves the problem of poor flame retardant effect of the composite current collector in the battery and significantly improves the performance of the battery. security.
Patent Information
- Application Number
- CN202410768110.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-14
- Publication Date
- 2024-10-01
AI Technical Summary
Existing composite current collectors have poor flame retardant effects in battery puncture experiments, leading to safety issues.
A combination of the support layer and the first metal coating is used. The density of the first metal coating is 50%-80%, and the thermal shrinkage rate of the support layer is less than or equal to 3%, forming a point resistance to isolate short-circuit current and improve the flame retardant effect.
It effectively improves the flame retardant effect of the composite current collector, enhances the safety of the battery, and prevents short circuits and fires when punctured by sharp objects.
Smart Images

Figure CN118738401A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of lithium batteries, and in particular to a safe composite current collector. Background Art
[0002] The composite current collector is a new type of current collector material composed of polymer materials and metals. It is used to gather current in batteries. Its structure is a "sandwich" structure with a plastic film layer in the middle and two surfaces in the thickness direction of the plastic film layer. There are metals on the two surfaces. Compared with traditional pure metal current collectors, composite current collectors have advantages in safety and potential cost-effectiveness.
[0003] However, after the composite current collectors currently produced by manufacturers were used in puncture tests in batteries, it was found that their flame retardant effect was still poor, which caused battery safety issues. Summary of the invention
[0004] In view of the above-mentioned deficiencies in the prior art, an object of the present invention is to provide a safe composite current collector, aiming to improve the flame retardant effect of the composite current collector and improve the safety of the product.
[0005] In order to achieve the above object, the present invention adopts the following technical solutions:
[0006] The invention provides a safe composite current collector, which comprises a support layer, wherein a first metal coating is arranged in the thickness direction of the support layer, the density of the first metal coating is 50%-80%, and the heat shrinkage rate of the support layer in the length direction is less than or equal to 3%.
[0007] In one embodiment, the thermal shrinkage rate of the support layer in the width direction is less than or equal to 1%.
[0008] In one embodiment, the thermal shrinkage rate of the first metal coating layer is smaller than the thermal shrinkage rate of the support layer.
[0009] In one embodiment, an insulating coating is further included, wherein the insulating coating is disposed between the first metal coating and the support layer.
[0010] In one embodiment, the thermal shrinkage rate of the insulating coating layer is greater than or equal to the thermal shrinkage rate of the supporting layer, and greater than the thermal shrinkage rate of the first metal coating layer.
[0011] In one embodiment, it further includes a second metal coating layer, wherein the second metal coating layer is disposed on the surface of the first metal coating layer;
[0012] The first metal coating is a metal coating made of nickel alloy, copper alloy, aluminum alloy, titanium alloy, aluminum metal, copper metal, or titanium metal;
[0013] The second metal coating is a metal coating made of copper, aluminum, titanium, nickel or chromium.
[0014] In one embodiment, the sum of the thicknesses of the first metal coating and the second metal coating is 1 um.
[0015] In one embodiment, the first metal coating is a magnetron sputtering coating or a vacuum evaporation coating, and the second metal coating is a magnetron sputtering coating or a vacuum evaporation coating or an acid plating coating.
[0016] In one embodiment, the heat shrinkage rate of the support layer is obtained by:
[0017] The support layer was placed in an oven at 150° for 30 minutes, and the heat shrinkage rate of the support layer was obtained after measuring the dimensional changes of the support layer in the width and length directions.
[0018] In one embodiment, the support layer is a heat shrinkable film made of at least one material selected from the group consisting of polyamide, polyterephthalate, polyimide, polyethylene, polypropylene, polystyrene, polyvinyl chloride, acrylonitrile-butadiene-styrene copolymer, polybutylene terephthalate, poly(p-phenylene terephthalamide), polypropylene, polyoxymethylene, epoxy resin, phenolic resin, polytetrafluoroethylene, polyvinylidene fluoride, silicone rubber, and polycarbonate.
[0019] Compared with the prior art, the present invention provides a safe composite current collector, including a support layer, a first metal coating is provided in the thickness direction of the support layer, the density of the first metal coating is 50%-80%, and the thermal shrinkage rate of the support layer in the length direction is less than or equal to 3%. When the composite current collector of the present invention encounters a sharp object piercing the first metal coating on the surface of the support layer, based on the density characteristics of the first metal coating and the thermal shrinkage characteristics of the support layer, the current collector part short-circuits, causing the battery temperature to rise and then causing the support layer to shrink thermally. After the support layer shrinks thermally, the first coating metal will not gather at the point where the sharp object pierces, thereby forming a point resistance, isolating the short-circuit current, and can effectively improve the flame retardant effect of the composite current collector, making the battery using the composite current collector safer. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the prior art descriptions are briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those of ordinary skill in the art, other drawings can be obtained according to the structures shown in these drawings without creative work. In the drawings:
[0021] Figure 1Schematic diagram of the structure of the safety composite current collector in an embodiment of the present invention. DETAILED DESCRIPTION
[0022] In order to make the technical problems, technical solutions and beneficial effects to be solved by the embodiments of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.
[0023] It should be noted that when a component is referred to as being "fixed to" or "disposed on" another component, it can be directly on the other component or indirectly on the other component. When an element is referred to as being "connected to" another element, it can be directly connected to the other element or indirectly connected to the other element. In addition, connection can be used for fixing or for circuit connection.
[0024] It should be understood that the terms "length", "width", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", etc., indicating the orientation or position relationship, are based on the orientation or position relationship shown in the accompanying drawings, and are only for the convenience of describing the embodiments of the present invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present invention.
[0025] In addition, the terms "first" and "second" are used for descriptive purposes only and cannot be understood as indicating or implying relative importance or implicitly indicating the number of indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features. In the description of the embodiments of the present invention, the meaning of "multiple" is two or more, unless otherwise clearly and specifically defined. In addition, the technical solutions between the various embodiments can be combined with each other, but it must be based on the ability of ordinary technicians in the field to implement. When the combination of technical solutions is contradictory or cannot be implemented, it should be deemed that such combination of technical solutions does not exist and is not within the scope of protection required by the present invention.
[0026] The present invention provides a safe composite current collector, such as Figure 1 As shown, the safety composite current collector includes a support layer 100, and a first metal coating 201 is provided in the thickness direction of the support layer 100. The support layer 100 is used as the supporting body of the safety composite current collector. The support layer 100 has an upper and lower surface, and the first metal coating 201 is provided on both the upper and lower surfaces, wherein the density of the first metal coating 201 is 50%-80%, and the thermal shrinkage rate of the support layer 100 in the length direction is less than or equal to 3%.
[0027] When a conventional composite current collector is used in a battery for a puncture test, a short circuit occurs due to the contact between the metal coatings on the upper and lower surfaces of the composite current collector, causing excessive internal heat accumulation, causing the battery to explode and burn, and affecting the safety of the battery. When the safety composite current collector of the present invention is used in a battery, if a sharp object pierces the first metal coating 201 on the surface of the support layer 100, based on the density characteristics of the first metal coating 201 and the thermal shrinkage characteristics of the support layer 100, the current collector part short-circuits, causing the battery temperature to rise and then causing the support layer 100 to shrink. After the support layer 100 shrinks, the first coating metal will not gather at the point where the sharp object penetrates, thereby forming a point resistance, isolating the short-circuit current, and effectively improving the flame retardant effect of the composite current collector, making the battery using the composite current collector of the present invention safer.
[0028] Specifically, the support layer 100 is a heat shrinkable film made of at least one material selected from polyamide, polyterephthalate, polyimide, polyethylene, polypropylene, polystyrene, polyvinyl chloride, acrylonitrile-butadiene-styrene copolymer, polybutylene terephthalate, poly(p-phenylene terephthalamide), polypropylene, polyoxymethylene, epoxy resin, phenolic resin, polytetrafluoroethylene, polyvinylidene fluoride, silicone rubber, and polycarbonate. By using a film made of a polymer material with corresponding heat shrinkage properties as the support layer 100, when a battery using a composite current collector encounters a sharp object, the current collector part short-circuits to increase the battery temperature, and the support layer 100 undergoes heat shrinkage so that the metal does not gather at the point where the sharp object penetrates, thereby forming a point resistance and improving the flame retardant effect.
[0029] Preferably, the heat shrinkage rate of the support layer 100 in the width direction is less than or equal to 1%. In this embodiment, the support layer 100 of the safety composite current collector has a heat shrinkage rate of less than or equal to 3% in the length direction and a heat shrinkage rate of less than or equal to 1% in the width direction. In this way, the bonding force between the first metal coating 201 and the support layer 100 in the transverse and longitudinal directions of the support layer 100 can be improved. This is because the first metal coating 201 is usually formed by magnetron sputtering or vacuum coating, and the temperature of the above preparation method is relatively high. If the heat shrinkage rate is high, the surface of the support layer 100 will be wrinkled, which will cause the crystal nucleus of the first metal coating 201 to be unable to be well combined with the surface of the support layer 100, so that the first metal coating 201 is easy to fall off. Therefore, the safety composite current collector of the present invention adopts a support layer 100 with corresponding heat shrinkage characteristics in the length direction and width direction, so that while improving the flame retardant effect of the composite current collector, the bonding force between the support layer 100 and the first metal coating 201 is also improved, ensuring that the appearance and performance of the battery are not affected.
[0030] Preferably, the thermal shrinkage rate of the first metal coating 201 is less than the thermal shrinkage rate of the support layer 100. In the safety composite current collector of this embodiment, on the basis that the support layer 100 has corresponding thermal shrinkage characteristics, the thermal shrinkage rate of the first metal coating 201 is also less than the thermal shrinkage rate of the support layer 100, so that when the composite current collector is punctured, since the thermal shrinkage rate of the support layer 100 is higher, more support layers 100 will cover the punctured place, and the support layer 100 is not conductive, so that resistance is formed in this place. Therefore, the thermal shrinkage rate of the first metal coating 201 in the composite current collector is less than the thermal shrinkage rate of the support layer 100, which can make the composite current collector more easily form point resistance when punctured, making the battery safer.
[0031] Specifically, the heat shrinkage rate of the support layer 100 is obtained by the following method: the support layer 100 is placed in a 150° oven for 30 minutes, and the heat shrinkage rate is obtained after the dimensional changes of the support layer 100 in the width and length directions are detected. The heat shrinkage rate mainly refers to the volume change of thermoplastic materials due to the thermal expansion rate. The memory property of the heat shrinkage material enables it to shrink and wrap around the outer surface of the object when heated, playing the role of insulation, moisture-proof, sealing, protection and connection. In this embodiment, the detection of the heat shrinkage rate is carried out by measuring the shrinkage change of the material within a certain temperature range. Specifically, the test sample of the support layer 100 is placed in a 150° oven for 30 minutes, and the heat shrinkage rate is calculated after recording the dimensional changes of the test sample in the width and length directions. By using the support layer 100 with corresponding heat shrinkage characteristics in the length direction and the width direction, when a partial short circuit occurs and the battery heats up, the support layer 100 can shrink and wrap the pierced position to form a point resistance to improve the flame retardant effect.
[0032] Preferably, the safety composite current collector of the present invention further includes an insulating coating 200, and the insulating coating 200 is disposed between the first metal coating 201 and the support layer 100. The insulating coating 200 can be a metal oxide coating such as aluminum oxide, silicon oxide, titanium oxide, etc. In this embodiment, the insulating coating 200 is disposed on the upper and lower surfaces of the support layer 100, and the first metal coating 201 is disposed on the surface of the insulating coating 200. The insulating coating 200 between the first metal coating 201 and the support layer 100 can effectively prevent the metal connection between the upper and lower surfaces of the current collector, prevent the occurrence of danger, and improve the safety of the product.
[0033] Furthermore, the thermal shrinkage rate of the insulating coating 200 is greater than or equal to the thermal shrinkage rate of the supporting layer 100, and greater than the thermal shrinkage rate of the first metal coating 201. In the safety composite current collector of this embodiment, an insulating coating 200 with a higher thermal shrinkage rate is arranged between the supporting layer 100 and the first metal coating 201, and the thermal shrinkage rate of the insulating coating 200 is greater than or equal to the thermal shrinkage rate of the supporting layer 100, and greater than the thermal shrinkage rate of the first metal coating 201. In this way, when the safety composite current collector of the present invention is pierced by a sharp object and a short circuit occurs, and the local heat is high, the supporting layer 100 shrinks, and the insulating coating 200 also shrinks together. At this time, the thermal shrinkage rate of the first metal coating 201 is smaller, so it shrinks slowly, and the thermal shrinkage rate of the insulating coating 200 is higher. In this way, the insulating coating 200 will wrap up the pierced position to prevent the metal connection between the upper and lower surfaces of the current collector, and can effectively form a point resistance to prevent danger, further improve the flame retardant effect of the composite current collector, and make the battery using the composite current collector safer.
[0034] Preferably, the safety composite current collector of the present invention also includes a second metal coating 202, which is arranged on the surface of the first metal coating 201, wherein the first metal coating 201 is a magnetron sputtering coating or a vacuum evaporation coating, and the second metal coating 202 is a magnetron sputtering coating or a vacuum evaporation coating or an acid plating coating.
[0035] Specifically, the metal coating group formed by the first metal coating 201 and the second metal coating 202 is arranged on the upper surface and the lower surface of the support layer 100. Taking the upper surface as an example, when the safety composite current collector is formed, the first metal coating 201 can be first formed on the support layer 100 by vapor deposition. Of course, when there is an insulating coating 200, the insulating coating 200 is first formed on the support layer 100 before the first metal coating 201 is formed, and then the first metal coating 201 is formed on the insulating coating 200, and then the second metal coating 202 is formed on the first metal coating 201 by vapor deposition or other methods. Among them, the first metal coating 201 is a metal coating made of nickel alloy, copper alloy, aluminum alloy, titanium alloy, aluminum metal, copper metal, and titanium metal. The first metal coating 201 mainly plays the role of improving the adhesion between the second metal coating 202 and the support layer 100 material. The second metal coating 202 is a metal coating made of copper metal, aluminum metal, titanium metal, nickel metal, and chromium metal. The second metal coating 202 mainly plays the role of converging current. After the second metal coating 202 is formed on the support layer 100, a composite current collector with good flame retardant effect and greater safety can be obtained.
[0036] Preferably, the sum of the thicknesses of the first metal coating 201 and the second metal coating 202 is 1 um. In this embodiment, by controlling the sum of the thicknesses of the first metal coating 201 and the second metal coating 202 to 1 um, the mass of the composite current collector can be greatly reduced. The more lightweight the composite current collector is, the more beneficial it is, which helps to improve the mass energy density of the battery, which is crucial for manufacturing lightweight and energy-efficient battery products, and can significantly improve the volume energy density of the battery, which has a positive impact on improving the overall performance of the battery.
[0037] In a preparation process, the first metal coating 201 of the safety composite current collector of the present invention can be sprayed, rolled or bonded to the support layer 100 with an adhesive, or can be formed on the support layer 100 by magnetron sputtering, vacuum evaporation, etc. Magnetron sputtering and vacuum evaporation are both physical vapor deposition methods, wherein magnetron sputtering refers to: using plasma generated by rare gas to bombard the surface of the cathode target under the action of electric field and magnetic field, and then sputtering out molecules, atoms, ions and electrons on the surface of the target, and the sputtered particles are ejected toward the surface of the base film in a certain direction, and then a coating is formed on the surface of the base film. The advantages of using this method are: 1) the sputtering atom energy is high, and the adhesion between the film and the substrate is strong; 2) the film thickness is controlled by controlling the target current, and the controllability and repeatability are good; 3) the material components of the crucible heater will not be mixed, and the metal film layer has high purity and high quality. Vacuum evaporation means: melting the metal into liquid, forming metal vapor and starting to volatilize, and then condensing the atoms in the vapor to deposit and grow on the surface of the polymer material. The deposition rate of vacuum evaporation is 3-4 times that of magnetron sputtering, which can quickly make up the thickness of the metal coating. Its advantages are: 1) heating and melting, fast film formation rate and high efficiency; 2) evaporation and adhesion do not require a high voltage electric field, the equipment is relatively simple and easy to operate; 3) vacuum heating evaporation atoms have low momentum and the film thickness is uniform.
[0038] The first metal coating 201 in this embodiment is preferably formed on the support layer 100 by magnetron sputtering. Specifically, the insulating coating 200 of the composite current collector is prepared on the support layer 100 by magnetron sputtering, and the thickness of the insulating coating 200 is 10nm-30nm; then the first metal coating 201 is formed on the insulating coating 200 by the same method, and the thickness of the first metal coating 201 is 50nm-100nm; and then one or more vacuum evaporation or magnetron sputtering is used to form a second metal coating 202 of 800nm-950nm on the first metal coating 201, so that a coating with a thickness of 900nm-1500nm is formed on one of the surfaces in the thickness direction of the support layer 100. In the preparation process adopted in this embodiment, the above-mentioned multiple steps and a single process (magnetron sputtering or evaporation) can greatly reduce costs and reduce holes when forming the coating.
[0039] Alternatively, in another preparation process, the composite current collector of the present invention can be formed in the following manner: the first metal coating 201 can be sprayed, rolled or bonded to the support layer 100 with an adhesive, or can be formed on the support layer 100 by magnetron sputtering, vacuum evaporation, etc. Preferably, magnetron sputtering is used to form the support layer 100, and the plasma generated by the rare gas is used to bombard the surface of the cathode target under the action of the electric field and the magnetic field, thereby sputtering out the molecules, atoms, ions and electrons on the surface of the target, and the sputtered particles are ejected toward the surface of the base film in a certain direction, thereby forming a coating on the surface of the base film, and obtaining the insulating coating 200 of the present application. At this time, the thickness of the insulating coating 200 is 10nm-30nm. The same method is used to form a first metal coating 201 on the insulating coating 200. At this time, the thickness of the first metal coating 201 is 50nm-100nm, and then an acid plating method is used to form a second metal coating 202 of 800nm-950nm on the surface of the first metal coating 201, so that a coating of 900nm-1500nm is formed on one of the surfaces in the thickness direction of the support layer 100. Among them, acid plating refers to using phosphor copper balls as anodes in an electroplating tank, placing the phosphor copper balls in an anode bag made of titanium blue, and then immersing the entire anode bag in an acidic agent (acidic sulfuric acid solution: sulfuric acid 90-170g / L, copper ions 50-160g / L, chloride ions 30-60ppm), with the metal layer on the membrane surface as the cathode, and the membrane surface passes between the rollers under the agent tank liquid. The membrane surface is immersed in the agent to perform ion migration replacement. After obtaining electrons on the membrane surface, a copper layer will be formed. The copper accumulation layer thickness is 800-950nm, and the membrane passes at a speed of 3-5m / min.
[0040] In the first preparation process mentioned above, after obtaining the finished film, it is also necessary to cut, pack and ship it. In the second preparation process mentioned above, after acid plating, it is also necessary to perform anti-oxidation treatment, which specifically refers to letting the above-mentioned current collector after acid plating pass through an antioxidant tank, in which an antioxidant liquid is placed. After the current collector passes through the antioxidant liquid, antioxidant liquid will remain on the surface, and then the antioxidant liquid is dried to retain the possible components of the antioxidant liquid on the finished film, and then such a film is cut to achieve the width required by the customer. Preferably, it is also necessary to wash with water after acid plating to wash off the acid plating solution on the surface of the current collector to prevent the plating solution from contaminating the antioxidant liquid.
[0041] In the above two processes, an optical density tester can be added to the vacuum evaporation or magnetron sputtering. The optical density tester directly senses the light transmittance or optical density of the film through optical contact, and uses a certain proportional relationship between the optical density and the coating thickness to detect the uniformity of the coating thickness. By adding an optical density tester to the vacuum evaporation or magnetron sputtering, the thickness of the coating formed on the support layer 100 can be detected online at any time. In this way, there is no need to open the cavity and then use a square resistance tester to detect the coating thickness, so that the coating thickness is accurately controllable, which effectively improves the preparation efficiency and performance reliability of the safety composite current collector.
[0042] In particular, if the first metal coating 201 is directly provided on the support layer 100, the preparation method of the first metal coating 201 can be formed on the support layer 100 by vacuum evaporation or magnetron sputtering to form a first metal coating 201 with a thickness of 10nm-500nm, and then the second metal coating 202 can be formed on the first metal coating 201 by magnetron sputtering, vacuum evaporation or acid plating. The thickness of the second metal coating 202 can be 100nm-500nm. The second metal coating 202 can be formed by multiple coatings or formed once, wherein the once-formed film has better bonding with the support layer 100, because the multiple-formed film is easy to fall off between the coatings, and the one-time forming method completes the coating in a vacuum chamber, without frequently opening and closing the vacuum chamber, which is more energy-saving and more efficient. At the same time, because there is no need to open and close the vacuum chamber, there is no process of transporting to the next workspace after production in multiple forming, so the coating can be avoided from being oxidized and the yield rate can be improved. When the second metal coating 202 is formed by acid plating, the thickness of the first metal coating 201 needs to be 300-500 nm to meet the requirements of subsequent acid plating, so as to avoid the difficulty of metallization of the second metal coating 202 and ensure the coating quality of the composite current collector.
[0043] The present application also provides experimental data, including comparative examples and embodiments. The current collector of the embodiment adopts the safety composite current collector of the present application, and the current collector includes a heat shrinkable film made of PP film with a thickness of 6um, and a first metal coating of 1um is formed on the upper and lower surfaces of the heat shrinkable film, and the first metal coating is aluminum; the current collector of the comparative example is also a heat shrinkable film made of PP film with a thickness of 6um, and a first metal coating is formed on the heat shrinkable film, and the first metal coating is also aluminum; the difference between the comparative example and the embodiment is that the first metal coating The density and thermal shrinkage of the supporting layer are measured, and then the above current collectors are assembled into batteries. Then, a puncture test is carried out using the test method of CATL. At room temperature, the battery is charged to 4.2V at a constant current of 0.5C (i.e., the current value that completely discharges the theoretical capacity within 2 hours), and then charged to 0.05C at a constant voltage, and then discharged to 3.0V at a constant current of 0.5C; the battery is left for 24 hours, charged to 4.2V at a constant current of 0.5C, and then charged to 0.05C at a constant voltage, and then the battery with 100% SOC is subjected to a nail penetration test. The nailing speed is controlled at 80mm / s, the nailing direction is perpendicular to the surface of the battery pole piece, and the nailing diameter is 6mm. The experimental results are divided into three levels according to the experimental phenomena, namely HL3, HL4 and HL5. Among them, the failure level HL5 means that a large spark first appears at the battery explosion-proof valve and then catches fire, the failure level HL4 means that a spark appears at the battery explosion-proof valve but no fire occurs, and the failure level HL3 means that there is no obvious spark at the battery explosion-proof valve and the battery has no leakage. The experimental data are as follows:
[0044] sample Density Thermal shrinkage grade Example 1 50% 3% HL3 Example 2 80% 1% HL3 Comparative Example 1 81% 3.5% HL4 Comparative Example 2 90% 4% HL5
[0045] It can be seen from the above experimental data that: by comparing Example 1-2 with Comparative Example 1-2, the failure level of Example 1-2 is higher than the failure level of Comparative Example 1-2. The safety composite current collector of the present application effectively improves the flame retardant effect of the composite current collector, making the battery based on the composite current collector safer.
[0046] In summary, the present invention provides a safe composite current collector, including a support layer, a first metal coating is provided in the thickness direction of the support layer, the density of the first metal coating is 50%-80%, and the thermal shrinkage rate of the support layer in the length direction is less than or equal to 3%. When the composite current collector of the present invention encounters a sharp object piercing the first metal coating on the surface of the support layer, based on the density characteristics of the first metal coating and the thermal shrinkage characteristics of the support layer, the current collector part short-circuits, causing the battery temperature to rise and then causing the support layer to shrink thermally. After the support layer shrinks thermally, the first coating metal will not gather at the place where the sharp object penetrates, thereby forming a point resistance, isolating the short-circuit current, and can effectively improve the flame retardant effect of the composite current collector, making the battery using the composite current collector safer.
[0047] The above contents are further detailed descriptions of the present invention in combination with specific preferred embodiments, and it cannot be determined that the specific implementation of the present invention is limited to these descriptions. For those skilled in the art of the present invention, several equivalent substitutions or obvious variations can be made without departing from the concept of the present invention, and the performance or use is the same, which should be regarded as belonging to the protection scope of the present invention.
Claims
1. A safe composite current collector, characterized in that: It comprises a supporting layer, wherein a first metal coating is arranged in the thickness direction of the supporting layer, the density of the first metal coating is 50%-80%, and the heat shrinkage rate of the supporting layer in the length direction is less than or equal to 3%.
2. The safety composite current collector according to claim 1, characterized in that: The heat shrinkage rate of the support layer in the width direction is less than or equal to 1%.
3. The safety composite current collector according to claim 1, characterized in that: The thermal shrinkage rate of the first metal coating layer is smaller than the thermal shrinkage rate of the support layer.
4. The safety composite current collector according to claim 1, characterized in that: Also included is an insulating coating layer disposed between the first metal coating layer and the support layer.
5. The safety composite current collector according to claim 4, characterized in that: The thermal shrinkage rate of the insulating coating layer is greater than or equal to the thermal shrinkage rate of the supporting layer, and is greater than the thermal shrinkage rate of the first metal coating layer.
6. The safety composite current collector according to claim 1 or 4, characterized in that: Also comprising a second metal coating, the second metal coating being disposed on a surface of the first metal coating; The first metal coating is a metal coating made of nickel alloy, copper alloy, aluminum alloy, titanium alloy, aluminum metal, copper metal, or titanium metal; The second metal coating is a metal coating made of copper, aluminum, titanium, nickel or chromium.
7. The safety composite current collector according to claim 6, characterized in that: The sum of the thickness of the first metal coating and the second metal coating is 1 um.
8. The safety composite current collector according to claim 6, characterized in that: The first metal coating is a magnetron sputtering coating or a vacuum evaporation coating, and the second metal coating is a magnetron sputtering coating or a vacuum evaporation coating or an acid plating coating.
9. The safety composite current collector according to claim 1, characterized in that: The thermal shrinkage of the support layer is obtained by: The support layer was placed in an oven at 150° for 30 minutes, and the heat shrinkage rate of the support layer was obtained after measuring the dimensional changes of the support layer in the width and length directions.
10. The safety composite current collector according to claim 1, characterized in that: The support layer is a heat shrinkable film made of at least one material selected from the group consisting of polyamide, polyterephthalate, polyimide, polyethylene, polypropylene, polystyrene, polyvinyl chloride, acrylonitrile-butadiene-styrene copolymer, polybutylene terephthalate, poly(p-phenylene terephthalamide), polypropylene, polyoxymethylene, epoxy resin, phenolic resin, polytetrafluoroethylene, polyvinylidene fluoride, silicone rubber, and polycarbonate.