Porous composite current collector and preparation method thereof and negative electrode-free alkali metal battery
By using a vertical pore structure with porous composite fluid-collection in an anode-free alkali metal battery, the dendrites growth problem is solved, and the cycle stability and safety performance of the battery are improved.
Patent Information
- Application Number
- CN202411231577.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-04
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-09-04
AI Technical Summary
The disorderly distribution of alkali metal ions in the negative electrode-free alkali metal batteries leads to dendrite growth during charging and discharging, which damages electrochemical performance and safety performance.
Using porous composite fluid collection, including toughened polymer layer, functional metal layer and porous conductive layer, is prepared by magnetron sputtering and electron beam lithography to form a vertical pore structure to induce directional deposition of alkali metal ions and inhibit branches. Crystal growth.
It improves the cycle stability and mechanical properties of the battery, reduces the shedding and damage during the preparation of the pole sheet, and significantly improves the energy density and safety performance of the battery.
Smart Images

Figure CN118738406B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of electrochemical devices, and in particular to a porous composite current collector and a preparation method thereof, and a negative electrode-free alkali metal battery. Background Art
[0002] Alkali metal batteries are electrochemical devices that use alkali metal ions as charge carriers, which are reversibly embedded and released between the positive and negative electrodes to achieve the storage and release of electrical energy. They mainly include lithium batteries, sodium batteries, and potassium batteries. Among alkali metal batteries, negative electrode-free batteries refer to battery systems that only use current collectors as active ion deposition carriers. They do not add negative electrode active materials such as graphite and hard carbon to serve as hosts for alkali metal ions, which can save negative electrode active materials, battery cell mass, and battery space, and maximize the energy density of the battery.
[0003] However, during the charge and discharge process of the negative electrode-free battery, the alkali metal ions will be directly deposited on the current collector. The uneven electric field distribution and the large nucleation barrier will cause the disordered distribution of the alkali metal ions, leading to the formation of alkali metal dendrites. The tip effect caused by the alkali metal dendrites will further promote the growth of alkali metals in the direction away from the current collector, seriously damaging the electrochemical performance and safety performance of the negative electrode-free alkali metal battery. Summary of the invention
[0004] Based on this, it is necessary to provide a porous composite current collector and a preparation method thereof and a negative electrode-free alkali metal battery to solve the serious problem of dendrite growth in the negative electrode-free alkali metal battery during the charge and discharge process.
[0005] The above-mentioned purpose of the present application is achieved through the following technical solutions:
[0006] In a first aspect of the present application, a porous composite current collector is provided, comprising a toughening polymer layer, a functional metal layer and a porous conductive layer stacked in sequence;
[0007] The toughened polymer layer includes a polymer and an inorganic nanofiller dispersed in the polymer;
[0008] The functional metal layer includes one or more of gold, silver, platinum, zinc, tin, antimony, bismuth and magnesium;
[0009] The porous conductive layer has a plurality of pores perpendicular to the functional metal layer.
[0010] In one embodiment, the porous conductive layer comprises one or more of copper and nickel; and / or,
[0011] The shape of the holes in the porous conductive layer includes one or more of a circle, a square, a rhombus, an equilateral triangle, an hourglass and an irregular shape;
[0012] The pores in the porous conductive layer have a pore size of 0.5 μm to 5 μm; and / or,
[0013] The distance between the holes in the porous conductive layer is 200 nm to 800 nm; and / or,
[0014] The porosity of the porous conductive layer is 40% to 75%.
[0015] In one embodiment, the mass ratio of the polymer to the inorganic nanofiller is 100:(5-50); and / or,
[0016] The polymer includes one or more of polyethylene, polypropylene, polyimide, polyvinyl chloride, polystyrene, polyvinyl alcohol, polyethylene terephthalate and polybutylene terephthalate; and / or,
[0017] The inorganic nanofiller comprises one or more of layered double hydroxide, silicon dioxide, calcium carbonate, montmorillonite, graphene and carbon nanotubes; and / or,
[0018] The particle size of the inorganic nanofiller is 40nm~500nm.
[0019] In one embodiment, the thickness of the toughened polymer layer is 2 μm to 10 μm; and / or,
[0020] The thickness of the functional metal layer is 10 nm to 200 nm; and / or,
[0021] The thickness of the porous conductive layer is 0.5 μm to 6 μm.
[0022] In a second aspect of the present application, a method for preparing the porous composite current collector as described above is provided, comprising the following steps:
[0023] The polymer and the inorganic nanofiller are melt-blended and molded to form a toughened polymer layer;
[0024] forming a functional metal layer on the toughened polymer layer by magnetron sputtering;
[0025] A porous conductive layer is formed on the functional metal layer by electron beam lithography.
[0026] In one embodiment, the melt blending treatment conditions include: a temperature of 160° C. to 350° C. and a time of 0.5 h to 4 h; and / or,
[0027] The molding method includes one or more of compression molding, hot pressing molding, autoclave molding and calendering molding; and / or,
[0028] The conditions of the magnetron sputtering method include: the sputtering atmosphere is an inert gas, the sputtering gas pressure is 0.2Pa~10Pa, and the sputtering power is 40W~80W.
[0029] In one embodiment, the electron beam lithography method comprises the following steps:
[0030] forming a photoresist layer and a first conductive layer in sequence on the functional metal layer;
[0031] The photoresist layer is formed into photosensitive areas and non-photosensitive areas through electron beam photosensitive treatment;
[0032] removing the first conductive layer, and removing the photosensitive area by developing treatment to expose the functional metal layer under the photosensitive area;
[0033] forming a second conductive layer on the functional metal layer and on the non-photosensitive area;
[0034] The non-photosensitive area and the second conductive layer on the non-photosensitive area are removed so that the second conductive layer on the functional metal layer forms the porous conductive layer.
[0035] In one embodiment, the method for forming the photoresist layer comprises a spin coating method; and / or,
[0036] The method for forming the first conductive layer comprises an evaporation method; and / or,
[0037] The second conductive layer is formed by magnetron sputtering.
[0038] In one embodiment, the first conductive layer comprises chromium, and the method for removing the first conductive layer comprises the following steps:
[0039] The first conductive layer is etched using a mixed solution containing ammonium cerium nitrate and perchloric acid.
[0040] In a third aspect of the present application, there is provided a negative electrode-free alkali metal battery, comprising a positive electrode plate, a separator, the porous composite current collector as described above, and an electrolyte.
[0041] This application has at least the following beneficial effects:
[0042] In the porous composite current collector provided by the present application, the toughening polymer layer is a composite of a polymer and an inorganic nanofiller, which can enhance the tensile strength, elongation at break and toughness of the material, and effectively avoid the degradation of the mechanical properties of the current collector. The functional metal layer is selected from one or more of gold, silver, zinc, tin, antimony, bismuth and magnesium. These metals have alkali metal affinity, which can induce alkali metal ions to be oriented and deposited. At the same time, they also have a bonding effect, which can enhance the bonding force between the toughening polymer layer and the porous conductive layer, and reduce the phenomenon of falling off or damage during the preparation process of the pole piece and the electrochemical cycle. The porous conductive layer has a plurality of holes perpendicular to the functional metal layer. This vertical pore structure can guide the deposition of alkali metal ions from bottom to top in the pore structure, promote the in-plane growth of alkali metals, and thus inhibit the growth of alkali metal dendrites. The porous composite current collector provided by the present application is applied to a negative electrode-free alkali metal battery, which can greatly improve its cycle stability. BRIEF DESCRIPTION OF THE DRAWINGS
[0043] In order to more clearly illustrate the technical solutions in the embodiments of the present application and to more completely understand the present application and its beneficial effects, the following is a brief introduction to the drawings required for the description of the embodiments. Obviously, the drawings described below are only some embodiments of the present application, and those skilled in the art can obtain other drawings based on these drawings without creative work.
[0044] Figure 1 is a schematic structural diagram of a porous composite current collector in one embodiment;
[0045] Figure 2 is a top view of a porous conductive layer in one embodiment;
[0046] Figure 3 is a schematic flow chart of a method for preparing a porous composite current collector in one embodiment;
[0047] Figure 4 is a schematic flow chart of a method for preparing a porous conductive layer in one embodiment;
[0048] Figure 5 is a schematic diagram of the structure of the current collector after step S200;
[0049] Figure 6 is a schematic diagram of the structure of the current collector after step S310;
[0050] Figure 7 is a schematic diagram of the structure of the current collector after step S320;
[0051] Figure 8 is a schematic diagram of the structure of the current collector after step S330;
[0052] Fig. 9Schematic diagram of the structure of the current collector after step S340.
[0053] Reference numerals: toughened polymer layer 10 , functional metal layer 20 , photoresist layer 30 , photosensitive area 31 , non-photosensitive area 32 , first conductive layer 40 , second conductive layer 50 , porous conductive layer 61 , pores 62 . DETAILED DESCRIPTION
[0054] In order to facilitate the understanding of the present application, the present application is further described in detail below in conjunction with specific embodiments. However, the present application can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the understanding of the disclosure of the present application more thorough and comprehensive.
[0055] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which this application belongs. The terms used herein in the specification of this application are only for the purpose of describing specific embodiments and are not intended to limit this application.
[0056] In the present application, the meaning of "and / or" includes any and all combinations of one or more related listed items. "At least one" means more than one, such as one, two and more than two. "Multiple" or "several" means at least two, such as two, three, etc., and "multi-layer" means at least two layers, such as two layers, three layers, etc., unless otherwise clearly and specifically defined. In the description of the present application, "several" means at least one, such as one, two, etc., unless otherwise clearly and specifically defined.
[0057] When a numerical range is disclosed in this application, the above range is considered to be continuous and includes the minimum and maximum values of the range, as well as every value between such minimum and maximum values. Further, when a range refers to an integer, every integer between the minimum and maximum values of the range is included. In addition, when multiple ranges are provided to describe features or characteristics, the ranges can be combined. In other words, unless otherwise indicated, all ranges disclosed in this application should be understood to include any and all subranges included therein.
[0058] Unless otherwise specified, all steps of the present application may be performed sequentially or randomly. For example, the method includes steps (a) and (b), which means that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may also include step (c), which means that step (c) may be added to the method in any order. For example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.
[0059] In this application, "above" or "below" includes the number itself. For example, "1 below" includes 1.
[0060] The temperature parameters in this application, unless otherwise specified, are allowed to be either constant temperature treatment or to vary within a certain temperature range. It should be understood that the constant temperature treatment allows the temperature to fluctuate within the accuracy range controlled by the instrument. Fluctuations within the range of ±5°C, ±4°C, ±3°C, ±2°C, and ±1°C are allowed.
[0061] In the present application, room temperature refers to indoor temperature, normal temperature or general temperature. Generally speaking, the range of room temperature can be any one of the following temperature intervals: 23°C ± 2°C, 25°C ± 5°C or 20°C ± 5°C.
[0062] Current collectors can be divided into two categories: metal current collectors and composite current collectors. Composite current collectors, also known as metallized plastic current collectors, are usually composed of a polymer layer and a conductive metal layer covering at least one side of the polymer layer. Compared with metal current collectors, composite current collectors are lighter, thinner and have better safety performance. Applying them to negative electrode-free batteries can further improve the battery's mass energy density and volume energy density. However, the tensile strength and elongation at break of the composite current collector deteriorate, resulting in poor structural stability of the battery. At the same time, the growth of alkali metal dendrites in the negative electrode-free battery during the charge and discharge process is severe, further damaging the battery's electrochemical performance and safety performance.
[0063] Based on this, in the first aspect of the present application, a porous composite current collector is provided to solve the problems of poor mechanical properties of traditional composite current collectors and severe lithium dendrite growth in negative electrode-free batteries.
[0064] See also Figure 1 , which is a schematic diagram of the structure of a porous composite current collector in one embodiment.
[0065] like Figure 1As shown, the porous composite current collector includes a toughened polymer layer 10, a functional metal layer 20 and a porous conductive layer 61 stacked in sequence;
[0066] The toughened polymer layer 10 includes a polymer and an inorganic nanofiller dispersed in the polymer;
[0067] The functional metal layer 20 includes one or more of gold, silver, zinc, tin, antimony, bismuth and magnesium;
[0068] The porous conductive layer 61 has a plurality of pores 62 perpendicular to the functional metal layer 20 .
[0069] In the porous composite current collector provided by the present application, the toughening polymer layer 10 is a composite of a polymer and an inorganic nanofiller, which can enhance the tensile strength, elongation at break and toughness of the material, and effectively avoid the degradation of the mechanical properties of the current collector. The functional metal layer 20 is selected from one or more of gold, silver, zinc, tin, antimony, bismuth and magnesium. These metals have alkali metal affinity, which can induce alkali metal ions to be oriented and deposited. At the same time, they also have a bonding effect, which can enhance the bonding force between the toughening polymer layer 10 and the porous conductive layer 61, and reduce the phenomenon of falling off or damage during the preparation process of the pole piece and the electrochemical cycle. The porous conductive layer 61 has a plurality of holes 62 perpendicular to the functional metal layer 20. This vertical pore structure can guide the deposition of alkali metal ions from bottom to top in the pore structure, promote the in-plane growth of alkali metals, and thus inhibit the growth of alkali metal dendrites. The porous composite current collector provided by the present application is applied to a negative electrode-free alkali metal battery, which can greatly improve its cycle stability.
[0070] Optionally, in the toughened polymer layer 10, the mass ratio of the polymer to the inorganic nanofiller is 100:(5~50), including but not limited to 100:5, 100:10, 100:15, 100:20, 100:25, 100:30, 100:35, 100:40, 100:45 or 100:50, and can further be 100:(15~25).
[0071] Adding an appropriate amount of inorganic nanofiller to the toughening polymer layer 10 can give full play to its toughening effect, and improve the mechanical strength of the porous composite current collector without affecting its processing performance, so that it can play a role in buffering stress and maintaining structural stability during the preparation and operation of the battery core, thereby providing a guarantee for the performance of the battery. If the amount of inorganic nanofiller added is too little, an effective network structure cannot be formed or sufficient stress concentration points cannot be generated, so the effect of improving the toughness and strength of the material is not obvious. If the amount of inorganic nanofiller added is too much, the polymer is not enough to fully wrap the inorganic nanofiller, and cracks or defects are easily formed, thereby reducing the toughness and strength of the material.
[0072] Optionally, it includes one or more of polyethylene (PE), polypropylene (PP), polyimide (PI), polyvinyl chloride (PVC), polystyrene (PS), polyvinyl alcohol (PVA), polyethylene terephthalate (PET) and polybutylene terephthalate (PBT), and can further be selected from one or more of polypropylene (PP) and polyimide (PI).
[0073] Optionally, the inorganic nanofiller includes one or more of layered double hydroxide, silicon dioxide, calcium carbonate, montmorillonite, graphene and carbon nanotubes, and may further be layered double hydroxide.
[0074] Among them, layered double hydroxides (LDH) are anionic layered materials, which contain two or more metal hydroxide skeleton layers and have the advantages of being environmentally friendly, having strong adsorption, good flame retardancy and low cost. At the same time, LDH materials have significant surface and interface effects and rich hydroxyl functional groups, which can form stronger interface interactions with the polymer matrix, thereby effectively enhancing the mechanical properties of the toughened polymer layer.
[0075] Optionally, the layered double hydroxide includes one or more of brucite-type layered double hydroxide, magnesia-magnesium-iron-gold-type layered double hydroxide, magnesia-magnesium-copper-aluminum-vanadium-type layered double hydroxide and carbon-magnesium-aluminum-sodium-vanadium layered double hydroxide, and magnesia-magnesium-aluminum-vanadium-type layered double hydroxide may be further selected.
[0076] Optionally, the particle size of the inorganic nanofiller is 40 nm to 500 nm, including but not limited to 40 nm, 50 nm, 100 nm, 150 nm, 200 nm, 250 nm, 300 nm, 350 nm, 400 nm, 450 nm or 500 nm, and can further be 200 nm to 400 nm.
[0077] Optionally, the thickness of the toughened polymer layer is 2μm~10μm, including but not limited to: 2μm, 2.5μm, 3μm, 3.5μm, 4μm, 4.5μm, 5μm, 5.5μm, 6μm, 6.5μm, 7μm, 7.5μm, 8μm, 8.5μm, 9μm, 9.5μm or 10μm.
[0078] In the present application, the functional metal layer 20 can serve as an adhesive layer on the one hand to improve the bonding ability between the toughened polymer layer 10 and the porous conductive layer 61 to prevent the porous composite current collector from falling off or being damaged. On the other hand, the metal element selected for the functional metal layer 20 has affinity for alkali metal ions, such as lithium affinity, sodium affinity or potassium affinity, and can provide active sites for the deposition of alkali metal ions to induce and regulate the in-plane deposition behavior of alkali metal ions.
[0079] It can be understood that the functional metal layer 20 can be any metal single substance of gold (Au), silver (Ag), platinum (Pt), zinc (Zn), tin (Sn), antimony (Sb), bismuth (Bi) and magnesium (Mg), or an alloy composed of at least two metals of Au, Ag, Pt, Zn, Sn, Sb, Bi and Mg, including but not limited to gold-silver alloy, gold-zinc alloy, gold-tin alloy, gold-antimony alloy, gold-bismuth alloy, gold-magnesium alloy, silver-zinc alloy, silver-tin alloy, silver-antimony alloy, silver-bismuth alloy, silver-magnesium alloy, zinc-tin alloy, zinc-antimony alloy, zinc-bismuth alloy, zinc-magnesium alloy, tin-antimony alloy, tin-bismuth alloy, tin-magnesium alloy, antimony-bismuth alloy, antimony-magnesium alloy, bismuth-magnesium alloy or gold-silver-zinc alloy. Further optionally, the functional metal layer 20 includes one or more of Au, Ag, Pt, Zn and Sn. Further optionally, the functional metal layer 20 is Au.
[0080] Optionally, the thickness of the functional metal layer 20 is 10 nm to 200 nm, including but not limited to 10 nm, 20 nm, 40 nm, 60 nm, 80 nm, 100 nm, 120 nm, 140 nm, 160 nm, 180 nm or 200 nm, and can further be 50 nm to 100 nm.
[0081] Optionally, the porous conductive layer 61 includes one or more of copper (Cu) and nickel (Ni), which may be copper alone, nickel alone, or a copper-nickel alloy, and may further be Cu.
[0082] See also Figure 2 , which is a top view of the porous conductive layer 61 in one embodiment. Figure 2 As shown in Figures (a) to (h), the shape of the holes 62 in the porous conductive layer 61 includes one or more of a circle, a square, a rhombus, a regular triangle, an hourglass shape and an irregular shape, and can further be selected to be one or more of a circle, a square and a rhombus.
[0083] It can be understood that if the hole 62 in the porous conductive layer 61 is circular, the aperture of the hole 62 is the diameter of the circular hole; if the hole 62 in the porous conductive layer 61 is square, rhombus or regular triangle, the aperture of the hole 62 is the side length of the square hole, rhombus hole or regular triangle hole; if the hole 62 in the porous conductive layer 61 is hourglass-shaped or irregular, the aperture of the hole 62 refers to the equivalent circle diameter, that is, the diameter of the circle equivalent to the plane projection area of the hole is used as the aperture of the hole 62. The distance between the holes 62 in the porous conductive layer 61 refers to the shortest distance between the edges of two adjacent holes 62.
[0084] Optionally, the pores 62 in the porous conductive layer 61 have a pore size of 0.5 μm to 5 μm, including but not limited to 0.5 μm, 1 μm, 1.5 μm, 2 μm, 2.5 μm, 3 μm, 3.5 μm, 4 μm, 4.5 μm or 5 μm, and can further be 2 μm to 4 μm.
[0085] Optionally, the distance between the holes 62 in the porous conductive layer 61 is 200 nm to 800 nm, including but not limited to 200 nm, 300 nm, 400 nm, 500 nm, 600 nm, 700 nm or 800 nm, and may further be 400 nm to 600 nm.
[0086] Optionally, the porosity of the porous conductive layer 61 is 40% to 75%, including but not limited to 40%, 45%, 50%, 55%, 60%, 65%, 70% or 75%, and may further be 50% to 60%.
[0087] Optionally, the thickness of the porous conductive layer 61 is 0.5 μm to 6 μm, including but not limited to 0.5 μm, 1 μm, 1.5 μm, 2 μm, 2.5 μm, 3 μm, 3.5 μm, 4 μm, 4.5 μm, 5 μm, 5.5 μm or 6 μm, and can be further optionally 1 μm to 3 μm.
[0088] In a second aspect of the present application, a method for preparing the porous composite current collector as described above is provided.
[0089] See also Figure 3 , which is a schematic diagram of a process for preparing a porous composite current collector in one embodiment. Figure 3 As shown, the method for preparing the porous composite current collector comprises the following steps:
[0090] S100: melt-blending and molding the polymer and the inorganic nanofiller to form a toughened polymer layer 10;
[0091] S200: forming a functional metal layer 20 on the toughened polymer layer 10 by magnetron sputtering;
[0092] S300 : forming a porous conductive layer 61 on the functional metal layer 20 by electron beam lithography.
[0093] The following is a detailed description of the preparation method of the porous composite current collector in a step-by-step manner.
[0094] S100: melt-blending and molding the polymer and the inorganic nanofiller to form a toughened polymer layer 10 .
[0095] Optionally, the conditions of the melt blending process include: a temperature of 160°C to 350°C and a time of 0.5h to 4h. The temperature of the melt blending process may be 160°C, 180°C, 200°C, 220°C, 240°C, 260°C, 280°C, 300°C, 320°C, 340°C or 350°C; and the time of the melt blending process may be 0.5h, 1h, 2h, 3h or 4h.
[0096] Optionally, the molding process includes one or more of compression molding, hot press molding, autoclave molding and calendering molding.
[0097] S200 : forming a functional metal layer 20 on the toughened polymer layer 10 by magnetron sputtering.
[0098] Optionally, the conditions of the magnetron sputtering method include: the sputtering atmosphere is an inert gas, the sputtering pressure is 0.2Pa~10Pa, and the sputtering power is 40W~80W. The sputtering atmosphere includes one or more of helium, neon, argon, krypton and xenon; the sputtering pressure can be 0.2Pa, 1Pa, 2Pa, 3Pa, 4Pa, 5Pa, 6Pa, 7Pa, 8Pa, 9Pa or 10Pa; the sputtering power can be 40W, 45W, 50W, 55W, 60W, 65W, 70W, 75W or 80W, and can further be 60W.
[0099] Optionally, the functional metal layer 20 is prepared by magnetron sputtering, comprising the following steps: placing the toughened polymer layer 10 in a cavity, evacuating the cavity to a vacuum of ≤1×10 -4 Pa, argon gas is introduced at a flow rate of 60 sccm-100 sccm, and DC magnetron sputtering coating is performed under the conditions of sputtering gas pressure of 0.2 Pa-10 Pa and sputtering power of 40 W-80 W to form a functional metal layer 20.
[0100] S300 : forming a porous conductive layer 61 on the functional metal layer 20 by electron beam lithography.
[0101] Electron Beam Lithography (EBL) is a lithography technology that uses a high-energy electron beam to replace a light source to engrave patterns on a substrate coated with a photoresist (electronic resist). It has the advantages of high resolution, high precision and high flexibility. It can realize the production of fine patterns at the nanometer level and does not require the preparation of a mask, which allows for rapid modification and optimization of pattern design.
[0102] See also Figure 4 , which is a schematic flow chart of a method for preparing a porous conductive layer 61 in one embodiment. Figure 4 As shown, electron beam lithography includes the following steps:
[0103] S310: forming a photoresist layer 30 and a first conductive layer 40 in sequence on the functional metal layer 20;
[0104] S320: forming a photosensitive area 31 and a non-photosensitive area 32 on the photoresist layer 30 through electron beam photosensitive treatment;
[0105] S330: removing the first conductive layer 40 and removing the photosensitive area 31 by developing treatment to expose the functional metal layer 20 under the photosensitive area 31;
[0106] S340: forming a second conductive layer 50 on the functional metal layer 20 and on the non-photosensitive area 32;
[0107] S350 : removing the non-photosensitive area 32 and the second conductive layer 50 on the non-photosensitive area 32 , so that the second conductive layer 50 on the functional metal layer 20 forms a porous conductive layer 61 .
[0108] The following is a detailed description of the method for preparing the porous conductive layer 61 through a step-by-step method.
[0109] S310 : forming a photoresist layer 30 and a first conductive layer 40 in sequence on the functional metal layer 20 .
[0110] See also Figure 5 and Figure 6 , Figure 5 is a schematic diagram of the structure of the current collector after step S200, Figure 6 Schematic diagram of the structure of the current collector after step S310.
[0111] Optionally, the photoresist layer 30 is formed by a spin coating method to ensure that the thickness of the photoresist layer 30 is uniform.
[0112] Optionally, the method for forming the photoresist layer 30 includes the following steps: spin coating the photoresist on the functional metal layer 20 , and performing a baking process to form the photoresist layer 30 .
[0113] The photoresist may be a positive photoresist commonly used in electron beam lithography technology such as polymethyl methacrylate (PMMA) or poly (1-butene-sulfone) (PBS). In some specific examples, the photoresist is PMMA-950K positive photoresist. The photoresist spin coating speed is 2000rpm~6000rpm, such as 2000rpm, 3000rpm, 4000rpm, 5000rpm or 6000rpm; the photoresist spin coating time is 60s~120s, such as 60s, 70s, 80s, 90s, 100s, 110s or 120s; by controlling the spin coating speed and spin coating time, it is ensured that the photoresist layer 30 covers the surface and side of the functional metal layer 20 to prevent the functional metal layer 20 from being corroded when the first conductive layer 40 is etched. The baking temperature is 100°C to 150°C, for example, 100°C, 110°C, 120°C, 130°C, 140°C or 150°C.
[0114] Optionally, a method for forming the first conductive layer 40 includes an evaporation method.
[0115] Optionally, the first conductive layer 40 includes chromium (Cr).
[0116] Metallic chromium has good conductivity and stability. It can be used as a conductive layer in electron beam lithography to enhance the conductivity of electron beam photosensitive processing, providing a stable grounding path for the entire photosensitive process. At the same time, it can prevent the accumulation of charge on the surface of the photoresist layer 30 and produce a charging effect, thereby improving the stability and accuracy of electron beam photosensitive processing.
[0117] Optionally, the thickness of the first conductive layer 40 is 10 nm to 50 nm, for example, 10 nm, 20 nm, 30 nm, 40 nm or 50 nm, and may further be 20 nm.
[0118] S320 : forming a photosensitive area 31 and a non-photosensitive area 32 on the photoresist layer 30 through electron beam exposure treatment.
[0119] See also Figure 7 , which is a schematic diagram of the structure of the current collector after step S320.
[0120] According to the preset pattern, the photoresist layer 30 is accurately exposed by electron beam, so that the photoresist layer 30 is divided into a photosensitive area 31 and a non-photosensitive area 32. If the photoresist layer 30 uses a positive photoresist, the photosensitive area 31 of the focused electron reaction is easily soluble in a developer, and the photosensitive area 31 can be dissolved and removed by the developer, leaving the non-photosensitive area 32 as a mask; if the photoresist layer 30 uses a negative photoresist, the photosensitive area 31 of the focused electron reaction is difficult to dissolve in a developer, and the non-photosensitive area 32 can be dissolved and removed by the developer, leaving the photosensitive area 31 as a mask.
[0121] S330 : removing the first conductive layer 40 , and removing the photosensitive region 31 by developing treatment to expose the functional metal layer 20 under the photosensitive region 31 .
[0122] See also Figure 8 , which is a schematic diagram of the structure of the current collector after step S330.
[0123] Optionally, the first conductive layer 40 includes chromium (Cr), and the method for removing the first conductive layer 40 includes the following steps: etching the first conductive layer 40 using a mixed solution containing cerium ammonium nitrate (Ce(NH4)2(NO3)6) and perchloric acid (HClO4).
[0124] Ammonium cerium nitrate is oxidizing under acidic conditions and can oxidize metallic chromium into high-valent chromium ions, while perchloric acid provides an acidic environment to promote oxidation. The two can synergistically etch the chromium layer effectively.
[0125] Optionally, the mass ratio of ammonium cerium nitrate, perchloric acid and water in the mixed solution is (10-12):(3-5):(84-86), and can further be 10.9:4.25:84.85. The water in the mixed solution can be one or more of tap water, deionized water, pure water, ultrapure water, reverse osmosis water and distilled water.
[0126] Optionally, etching the first conductive layer 40 with the mixed solution includes the following steps: soaking the first conductive layer 40 in the mixed solution for 10s to 20s, ultrasonically cleaning it with deionized water for 5min to 15min, and drying it with an N2 gun.
[0127] Optionally, the photosensitive area 31 is removed by development treatment, including the following steps: dissolving the photosensitive area 31 with a developer, and performing ultrasonic cleaning with isopropyl alcohol for 5 minutes to 15 minutes to remove the residual developer. If the photoresist layer 30 uses PMMA positive photoresist, the developer for dissolving the photosensitive area 31 includes one or more of methyl isobutyl ketone (MIBK), ethyl lactate (EL) and propylene glycol methyl ether acetate (PGMEA), and methyl isobutyl ketone (MIBK) can be further selected.
[0128] S340 : forming a second conductive layer 50 on the functional metal layer 20 and on the non-photosensitive area 32 .
[0129] See also Fig. 9 , which is a schematic diagram of the structure of the current collector after step S340.
[0130] Optionally, the second conductive layer 50 is formed by a magnetron sputtering method.
[0131] Optionally, the second conductive layer 50 is formed by magnetron sputtering, comprising the following steps: placing the device obtained in step 330 in a cavity, and evacuating the cavity to a vacuum of <1×10 -4 Pa, argon gas is introduced at a flow rate of 60 sccm-100 sccm, and DC magnetron sputtering is performed under the conditions of sputtering gas pressure of 0.2 Pa-10 Pa and sputtering power of 100 W-200 W to form the second conductive layer 50.
[0132] S350 : removing the non-photosensitive area 32 and the second conductive layer 50 on the non-photosensitive area 32 , so that the second conductive layer 50 on the functional metal layer 20 forms a porous conductive layer 61 .
[0133] See also Figure 1 , which is a schematic diagram of the structure of the porous composite current collector obtained after step S350.
[0134] Optionally, removing the non-photosensitive area 32 and the second conductive layer 50 on the non-photosensitive area 32 includes the following steps: using an organic solvent to dissolve the non-photosensitive area 32, and the second conductive layer 50 on the non-photosensitive area 32 falls off, while the second conductive layer 50 on the functional metal layer 20 is retained as the porous conductive layer 61. If the photoresist layer 30 uses PMMA positive photoresist, the organic solvent for dissolving the non-photosensitive area 32 includes one or more of acetone, chlorobenzene, anisole, ethyl acetate and tetrahydrofuran (THF), and acetone can be further selected.
[0135] In a third aspect of the present application, there is provided a negative electrode-free alkali metal battery, comprising a positive electrode plate, a separator, the porous composite current collector as described above, and an electrolyte.
[0136] Understandably, in a negative electrode-free alkali metal battery, the porous composite current collector serves as a substrate for the deposition of alkali metal ions, and there is no need to load a negative electrode active layer containing negative electrode active materials on the porous composite current collector. During the charge and discharge cycle, active alkali metal ions repeatedly travel between the positive electrode plate and the porous composite current collector; the electrolyte conducts lithium ions between the positive electrode plate and the negative electrode plate; the separator is located between the positive electrode plate and the negative electrode plate to prevent short circuits and allow active alkali metal ions to pass through.
[0137] Optionally, the positive electrode plate includes a positive electrode current collector and a positive electrode active layer covering at least one surface of the positive electrode current collector.
[0138] Optionally, the positive electrode current collector includes a metal current collector or a composite current collector. The metal current collector may be aluminum foil; the composite current collector includes a polymer layer and a metal layer supported on at least one surface of the polymer layer; the polymer substrate may be made of one or more of polyethylene (PE), polypropylene (PP), polyimide (PI), polyvinyl chloride (PVC), polystyrene (PS), polyvinyl alcohol (PVA), polyethylene terephthalate (PET) and polybutylene terephthalate (PBT); the metal layer may be made of one or more of aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy.
[0139] Optionally, the positive electrode active layer comprises a positive electrode active material, a conductive agent and a binder, wherein the mass ratio of the positive electrode active material, the conductive agent and the binder is (80-95):(2.5-10):(2.5-10), and further optionally 84:8:8.
[0140] Optionally, when the negative electrode-free alkali metal battery is a lithium battery, the positive electrode active material includes one or more of a lithium transition metal oxide and an olivine structured lithium phosphate. Among them, the lithium transition metal oxide includes but is not limited to: lithium cobalt oxide, such as LiCoO2; lithium nickel oxide, such as LiNiO2; lithium manganese oxide, such as LiMnO2 or LiMn2O4; lithium nickel cobalt oxide; lithium manganese cobalt oxide; lithium nickel manganese oxide; lithium nickel cobalt manganese oxide, such as LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2 (NCM333), LiNi 0.5 Co 0.2 Mn 0.3 O2 (NCM523), LiNi 0.6 Co 0.1 Mn 0.3 O2 (NCM613), LiNi 0.6 Co 0.2 Mn 0.2 O2 (NCM622), LiNi 0.8 Co 0.1 Mn 0.1 O2 (NCM811); lithium nickel cobalt aluminum oxide, such as LiNi 0.8 Co 0.15 Al 0.05 O2; and modified compounds of the above lithium transition metal oxides. Lithium phosphates with olivine structure include but are not limited to: lithium iron phosphate, such as LiFePO4 (LFP); composite materials of lithium iron phosphate and carbon; lithium manganese phosphate, such as LiMnPO4; composite materials of lithium manganese phosphate and carbon; lithium manganese iron phosphate, such as LiFe 0.5 Mn 0.5PO4; a composite material of lithium manganese iron phosphate and carbon; and a modified compound of the above-mentioned olivine structured lithium-containing phosphate. The modified compound of each material can be one or more of doping modification and surface coating modification.
[0141] Optionally, when the negative electrode-free alkali metal battery is a sodium battery, the positive electrode active material includes one or more of a transition metal oxide material, a polyanion compound material, a Prussian blue compound, and an organic positive electrode material. Among them, the transition metal oxide mainly includes a layered structure and a tunnel structure, and the structural formula can be expressed as Na x TMO2 (TM = Co, Cu, Ni, Fe, Mn, etc.), such as NaMnO2, NaNiO2, NaCrO2 or NaCu 1 / 9 Ni 2 / 9 Fe 1 / 3 Mn 1 / 3 O2; polyanion compound materials include Na3V2(PO4)3 (NVP), Na3V2(PO4)2F3 (NVPF) and Na2MP2O7 (M = Fe, Co, Mn or Cu); the molecular formula of Prussian blue compounds is KM II Fe III (CN)6 (M = Mn, Fe, Co, Ni, Zn, etc.); organic cathode materials include disodium rose palmitic acid (Na2C6O6), perylenetetracarboxylic dianhydride (PTCDA) and perylene diimide (PTCDI). And the modified compounds of the above transition metal oxide materials, polyanion compound materials, Prussian blue compounds and organic cathode materials, the modified compounds of each material can be one or more of doping modification and surface coating modification.
[0142] Optionally, when the negative electrode-free alkali metal battery is a potassium battery, the positive electrode active material includes one or more of a transition metal oxide material, a polyanion compound material, a Prussian blue compound, and an organic positive electrode material. Among them, the transition metal oxide mainly includes a layered structure, such as K x CrO2 (x=0.69, 0.8, 1), K x MnO2 (x=0.3, 0.5, 0.7), KxCoO2 (x=0.44, 0.6), K 0.48 Mn 0.4 Co 0.6 O2, KxFe0.5Mn 0.5 O2 (x=0.45, 0.65, 0.7), K 0.45 Mn 0.5 Co 0.5 O2, K 0.5 Mn 0.8 Co 0.1 Ni 0.1 O2, K0.67 Ni 0.17 Co 0.17 Mn 0.66 O2, K 1.39 Mn3O6, K2V3O8, K 0.72 Li 0.27 Ni 0.6 Co 0.2 Mn 0.2 O2, K 0.7 Fe 0.05 Co 0.1 Mn 0.75 Ni 0.05 V 0.05 O2; polyanion compound materials include KFeSO4F, KCuSO4F, KVPO4F, KVOPO4, K3V2(PO4)3, etc.; the molecular formula of Prussian blue compounds is K x M[M′(CN)6] 1-y (0≤x≤2, 0≤y<1,), M and M′ are transition metals such as Zn, Cu, Ni, Co, Fe, Cr, and Ti; organic cathode materials include 1,4-benzoquinone polymer (PAQS), polytriphenylamine (PTPAn), copper tetracyanoquinodimethane (CuTCNQ) and anthraquinone-2,6-disulfonate sodium (AQDs), etc. And the modified compounds of the above transition metal oxide materials, polyanion compound materials, Prussian blue compounds and organic cathode materials, the modified compounds of each material can be one or more of doping modification and surface coating modification.
[0143] Optionally, the binder in the positive electrode active layer includes one or more of polyvinylidene fluoride (PVDF), sodium alginate (SA), polyvinyl alcohol (PVA), polymethyl methacrylate (PMMA), hydrogenated nitrile rubber (HNBR), polytetrafluoroethylene (PTFE) and polyacrylic acid (PAA), and can further be polyvinylidene fluoride (PVDF).
[0144] Optionally, the conductive agent in the positive electrode active layer includes one or more of conductive carbon black, superconductive carbon black (SP), acetylene black, Ketjen black, carbon quantum dots, carbon nanotubes, graphene and carbon nanofibers, and may further be superconductive carbon black (SP).
[0145] Optionally, the preparation method of the positive electrode sheet includes the following steps: dispersing the positive electrode active material, the conductive agent and the binder in an organic solvent (such as N-methylpyrrolidone) to prepare a positive electrode slurry; covering the positive electrode slurry on at least one surface of the positive electrode collector, and obtaining the positive electrode sheet through drying, rolling and cutting.
[0146] It can be understood that the electrolyte in the negative electrode-free alkali metal battery can be liquid, gel or all-solid. Optionally, the electrolyte adopts an electrolyte solution, which includes an alkali metal salt and an organic solvent. Among them, the alkali metal salt includes lithium salt, sodium salt and potassium salt; lithium salt includes lithium hexafluorophosphate, lithium tetrafluoroborate, lithium perchlorate, lithium hexafluoroarsenate, lithium bisfluorosulfonyl imide, lithium bistrifluoromethanesulfonyl imide, lithium trifluoromethanesulfonate, lithium difluorophosphate, lithium difluorooxalate borate, lithium dioxalate borate, lithium difluorodioxalate phosphate and lithium tetrafluorooxalate phosphate. One or more; sodium salt includes sodium hexafluorophosphate, sodium bisfluorosulfonyl imide, sodium bistrifluoromethanesulfonyl imide; potassium salt includes potassium hexafluorophosphate, potassium bisfluorosulfonyl imide, bistrifluoromethanesulfonyl imide, Potassium imide; the organic solvent includes one or more of ethylene carbonate, propylene carbonate, ethyl methyl carbonate, diethyl carbonate, dimethyl carbonate, dipropyl carbonate, methyl propyl carbonate, ethyl propyl carbonate, butylene carbonate, fluoroethylene carbonate, methyl formate, methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate, methyl butyrate, ethyl butyrate, 1,4-butyrolactone, trimethyl phosphate, triethyl phosphate, cyclopentane, dimethyl sulfone, methyl ethyl sulfone, diethyl sulfone and diethylene glycol dimethyl ether.
[0147] It is understandable that the separator can be a porous separator with good chemical stability and mechanical stability; at the same time, the separator can be a single-layer film or a multi-layer composite film. When the separator is a multi-layer composite film, the materials of each layer can be the same or different, without special restrictions. Optionally, the material of the separator includes one or more of glass fiber, non-woven fabric, polyethylene (PE) and polypropylene (PP).
[0148] Optionally, the positive electrode sheet, the negative electrode sheet and the separator can be made into an electrode assembly through a winding process or a lamination process, and then injected with an electrolyte to form a battery.
[0149] Optionally, the negative electrode-free alkali metal battery may include an outer package for encapsulating the electrode assembly and the electrolyte. The outer package of the negative electrode-free alkali metal battery may be a hard shell, such as a hard plastic shell, an aluminum shell, a steel shell, etc. The outer package of the negative electrode-free alkali metal battery may also be a soft package, such as a bag-type soft package, and the material of the soft package may be an aluminum-plastic film, etc.
[0150] The following is further described in conjunction with specific embodiments and comparative examples. The raw materials involved in the following specific embodiments and comparative examples, unless otherwise specified, can all be commercially available, the instruments used, unless otherwise specified, can all be commercially available, and the processes involved, unless otherwise specified, are all routinely selected by those skilled in the art.
[0151] Example 1
[0152] Please refer to Table 1, the preparation method of the negative electrode-free lithium battery in this embodiment is as follows:
[0153] 1. Preparation of toughened polymer layer 10:
[0154] The polymer and the inorganic filler are mixed and melt-treated at 200° C., uniformly dispersed at a rotation speed of 1000 rpm for 1 hour, and molded to form a toughened polymer layer 10 .
[0155] Wherein, the polymer is polypropylene (PP);
[0156] The inorganic nanofiller is a yellow aluminum manganese vanadium ore type LDH material with a particle size of 300nm;
[0157] The mass ratio of polymer to inorganic nanofiller is 100:20;
[0158] The thickness of the toughened polymer layer 10 is 4 μm.
[0159] 2. Preparation of functional metal layer 20:
[0160] The toughened polymer layer 10 is placed in the chamber of a magnetron sputtering device and evacuated to a vacuum of ≤1×10 -4 Pa, Ar is introduced at a flow rate of 80 sccm, and DC magnetron sputtering coating is performed under the conditions of a sputtering gas pressure of 0.2 Pa and a sputtering power of 60 W, thereby forming a functional metal layer 20 on the toughened polymer layer 10.
[0161] The functional metal layer 20 is an Au layer with a thickness of 50 nm.
[0162] 3. Prepare the porous conductive layer 61 using electron beam lithography technology:
[0163] (1) Spin-coat PMMA-950K positive photoresist onto the functional metal layer 20 at a spin-coating speed of 4000 rpm to ensure that the photoresist covers the surface and side surfaces of the functional metal layer 20. The spin-coating time is 1 min. Then, bake on a hot plate at 120° C. for 30 min to form a photoresist layer 30. Plate a first conductive layer 40 on the photoresist layer 30 by vacuum evaporation.
[0164] The thickness of the photoresist layer 30 is 10 μm, and the first conductive layer 40 is a Cr layer with a thickness of 20 nm.
[0165] (2) The photoresist layer 30 is exposed to electron beams according to a preset pattern, so that the photoresist layer 30 forms a photosensitive area 31 and a non-photosensitive area 32.
[0166] (3) preparing a mixed solution of ammonium cerium nitrate, perchloric acid and deionized water in a mass ratio of 10.9:4.25:84.85, soaking the device obtained in step (2) in the mixed solution for 15 seconds to etch the first conductive layer 40, quickly ultrasonically cleaning it with deionized water for 10 minutes, and drying it with an N2 gun; developing it with methyl isobutyl ketone as a developer to dissolve the photosensitive area 31, and after development, ultrasonically cleaning it with isopropyl alcohol for 2 minutes to remove the residual developer, thereby exposing the functional metal layer 20 below the photosensitive area 31.
[0167] (4) Place the device obtained in step (3) in the chamber of a magnetron sputtering device and evacuate the chamber to a vacuum of ≤1×10 -4 Pa, Ar is introduced at a flow rate of 80 sccm, and DC magnetron sputtering coating is performed under the conditions of a sputtering gas pressure of 5 Pa and a sputtering power of 150 W, thereby forming a second conductive layer 50 on the functional metal layer 20 and on the non-photosensitive area 32.
[0168] The second conductive layer 50 is a Cu layer with a thickness of 2 μm.
[0169] (5) Acetone is used to dissolve the non-photosensitive area 32 of the device obtained in step (4), and the second conductive layer 50 on the non-photosensitive area 32 is then removed, while the second conductive layer 50 on the functional metal layer 20 is retained as a porous conductive layer 61, thereby obtaining a porous composite current collector.
[0170] The top view of the porous conductive layer 61 is as follows Figure 2 As shown in Figure (a), the hole 62 is circular, the pore diameter is 3µm, the distance between the edges of two adjacent holes is 0.5µm, and the porosity is 54%.
[0171] 4. Preparation of negative electrode-free lithium battery:
[0172] (1) The positive electrode active material LiNi 0.8 Co 0.1 Mn 0.1 O2, superconductive carbon black SP, and binder PVDF are dispersed in N-methylpyrrolidone, mixed and homogenized to obtain positive electrode slurry; the positive electrode slurry is coated on aluminum foil, dried, rolled and cut to obtain positive electrode sheets.
[0173] (2) In a glove box (Ar atmosphere, water and O2 content <0.1ppm), the positive electrode plate, glass fiber separator and composite porous current collector were encapsulated with aluminum-plastic film and injected with electrolyte to make a laminated soft-pack battery cell; wherein the electrolyte includes 1 mol / L lithium salt LiFSI, an organic solvent (DOL and DME with a volume ratio of 1:1) and an additive LiNO3 with a mass fraction of 2%.
[0174] Embodiments 2 to 9
[0175] Embodiments 2 to 9 are substantially the same as Embodiment 1, except that:
[0176] Example 2: The top view of the porous conductive layer 61 is as follows Figure 2 As shown in FIG. 5( b ), the hole 62 is square, the hole diameter is 3 μm, the distance between the edges of two adjacent holes is 0.5 μm, and the porosity is 68%.
[0177] Example 3: The top view of the porous conductive layer 61 is as follows Figure 2 As shown in Figure (c), the hole 62 is diamond-shaped, the pore diameter is 3µm, the distance between the edges of two adjacent holes is 0.5µm, and the porosity is 68%.
[0178] Example 4: The top view of the porous conductive layer 61 is as follows Figure 2 As shown in Figure (d), the holes 62 are alternately distributed in the shape of squares and diamonds, the pore diameter of the holes 62 is 3µm, the distance between the edges of two adjacent holes is 0.5µm, and the porosity is 68%.
[0179] Embodiment 5: The porous conductive layer 61 is a porous Ni layer.
[0180] Embodiment 6: The functional metal layer 20 is a Zn layer with a thickness of 50 nm.
[0181] Example 7: In the toughened polymer layer 10, the mass ratio of the polymer to the inorganic nanofiller is 100:10.
[0182] Embodiment 8: The polymer in the toughened polymer layer 10 is polyimide (PI).
[0183] Example 9: The inorganic nanofiller in the toughened polymer layer 10 is silicon dioxide, and the particle size is 300 nm.
[0184] Example 10
[0185] The preparation method of the negative electrode-free sodium battery in this embodiment is as follows:
[0186] 1. Preparation of toughened polymer layer 10: the same as step 1 of Example 1.
[0187] 2. Preparation of the functional metal layer 20: Same as step 2 of Example 1, the functional metal layer 20 is an Au layer with a thickness of 100 nm.
[0188] 3. Prepare the porous conductive layer 61 by electron beam lithography technology: the same as step 3 of embodiment 1.
[0189] 4. Preparation of negative electrode-free sodium battery:
[0190] (1) According to the mass ratio of 84:8:8, the positive electrode active material Na3V2(PO4)3, superconducting carbon black SP, and binder PVDF are dispersed in N-methylpyrrolidone, mixed and homogenized to obtain positive electrode slurry; the positive electrode slurry is coated on aluminum foil, dried, rolled and cut to obtain positive electrode sheets.
[0191] (2) In a glove box (Ar atmosphere, water and O2 content <0.1ppm), the positive electrode plate, glass fiber separator and composite porous current collector are encapsulated with aluminum-plastic film and injected with electrolyte to make a laminated soft-pack battery cell; wherein the electrolyte includes 1 mol / L sodium salt NaPF6 and an organic solvent (diethylene glycol dimethyl ether, G2).
[0192] Comparative Examples 1 to 6
[0193] Comparative Examples 1 to 5 are substantially the same as Example 1, except that:
[0194] Comparative Example 1: The toughened polymer layer was replaced with a polypropylene layer of the same thickness.
[0195] Comparative Example 2: No functional metal layer 20 was prepared.
[0196] Comparative Example 3: The functional metal layer 20 is replaced by a Cu layer with the same thickness.
[0197] Comparative Example 4: The porous conductive layer 61 is replaced by a Cu layer.
[0198] Comparative Example 5: The porous conductive layer 61 is replaced by a porous Cu layer without a vertical channel structure. The preparation method is as follows: a Cu50-Zn50 alloy layer is deposited on the surface of the functional metal layer using magnetron sputtering, and then the alloy layer is etched for 2 hours using 1M hydrochloric acid to dissolve the Zn component in the alloy to obtain a porous copper layer without a vertical channel structure.
[0199] Comparative Example 6 is substantially the same as Example 10, except that the functional metal layer 20 is not prepared.
[0200] Test Case
[0201] The following tests were performed on each embodiment and each comparative example:
[0202] (1) The prepared battery cells were subjected to room temperature cycle tests at 0.5C / 0.5C, and the first discharge specific capacity of the battery cells at 0.5C and the number of cycles until the capacity decayed to 80% were recorded. The results are shown in Table 2.
[0203] (2) Peel strength of porous composite current collector: Attach the tape flatly to the steel plate, fix the sample (i.e., porous composite current collector) on the tape, attach the auxiliary tape to the surface of the sample, fix the steel plate and the auxiliary tape on a constant speed tensile machine and start the test. Record the peel strength of each sample. The results are shown in Table 2.
[0204] (3) Mechanical strength of porous composite current collector: Cut three sample strips with a length and width of 150 mm × 15 mm, ensure that the samples are placed vertically on the test clamp of the tensile testing machine, set the test parameters and start the test, record the tensile strength and elongation at break, and the results are shown in Table 2.
[0205] It can be seen from Table 2 that the peel strength of the porous composite current collector prepared in Examples 1 to 10 reaches 3.5N / 25mm~4.7N / 25mm, the adhesion between the layers is strong, and it is not easy to detach or peel off; the tensile strength of the porous composite current collector reaches 163MPa~189MPa, the elongation at break reaches 6%~11%, and the mechanical strength is high, which is conducive to maintaining the structural stability of the electrode during the preparation of the battery cell and the battery cycle; the porous composite current collector is applied to a negative electrode-free alkali metal battery, and the negative electrode-free lithium battery has an initial discharge capacity of 162.6mAh / g~168.1mAh / g, and the number of cycles when the capacity retention rate is reduced to 80% is 54 times~76 times; the negative electrode-free sodium battery has an initial discharge capacity of 103.7mAh / g, and the number of cycles when the capacity retention rate is reduced to 80% is 76 times, both of which have the advantages of high initial discharge capacity and good cycle stability.
[0206] Taking Example 1 as a reference, Comparative Example 1 uses a traditional polymer layer as a substrate, and its peel strength, tensile strength and elongation at break are reduced, resulting in poor cycle performance. Comparative Examples 2 and 6 do not have a functional metal layer, which leads to a significant reduction in peel strength, and it is easy to peel off or fall off during the charge and discharge cycle, so the battery cycle performance is very poor. Comparative Example 3 uses a Cu layer to replace the functional metal layer, which does not have a bonding effect, causing a decrease in peel strength, and cannot provide active sites for inducing alkali metal deposition, and it is difficult to inhibit the growth of alkali metal dendrites, so the battery cycle performance is also deteriorated. The porous conductive layer of Comparative Example 4 is replaced by a Cu layer that does not have a porous structure, so it is impossible to induce alkali metals to deposit in the vertical pore structure, dendrite growth is serious, and the battery cycle performance is very poor. Although the porous conductive layer of Comparative Example 5 has a porous structure, the pores are disorderly distributed, and the induced alkali metal deposition behavior is limited, so the battery cycle performance is deteriorated.
[0207] In summary, the porous composite current collector provided in the present application has the characteristics of high peeling strength and good mechanical properties. Its functional metal layer and the porous conductive layer with a vertical pore structure can induce the deposition of alkali metals from bottom to top in the pore structure, effectively inhibiting the growth of alkali metal dendrites, thereby greatly improving the cycle stability of the negative electrode-free alkali metal battery.
[0208] Table 1. Structure of porous composite current collectors
[0209]
[0210] Table 2. Performance of porous composite current collectors and negative electrode-free alkali metal batteries
[0211]
[0212] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0213] The above-described embodiments only express several implementation methods of the present application, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of protection of the present application. It should be pointed out that, for a person of ordinary skill in the art, several variations and improvements can be made without departing from the concept of the present application, and these all belong to the scope of protection of the present application. Therefore, the scope of protection of the present application shall be subject to the attached claims.
Claims
1. A porous composite current collector, characterized in that: It includes a toughened polymer layer, a functional metal layer and a porous conductive layer stacked in sequence; The toughened polymer layer comprises a polymer and an inorganic nanofiller dispersed in the polymer, the inorganic nanofiller comprises a layered double hydroxide, and the mass ratio of the polymer to the inorganic nanofiller is 100:(5-50); The functional metal layer includes one or more of gold, platinum, zinc, tin, antimony, bismuth and magnesium, and the thickness of the functional metal layer is 10nm to 200nm; The porous conductive layer has multiple holes perpendicular to the functional metal layer, the pore size of the holes in the porous conductive layer is 2μm~4μm, the distance between the holes in the porous conductive layer is 200nm~800nm, and the porosity of the porous conductive layer is 40%~75%.
2. The porous composite current collector according to claim 1, characterized in that: The porous conductive layer comprises one or more of copper and nickel; and / or, The shapes of the holes in the porous conductive layer include one or more of a circle, a square, a rhombus, a regular triangle, an hourglass shape and an irregular shape.
3. The porous composite current collector according to claim 1, characterized in that: The polymer includes one or more of polyethylene, polypropylene, polyimide, polyvinyl chloride, polystyrene, polyvinyl alcohol, polyethylene terephthalate and polybutylene terephthalate; and / or, The particle size of the inorganic nanofiller is 40nm~500nm.
4. The porous composite current collector according to any one of claims 1 to 3, characterized in that: The thickness of the toughened polymer layer is 2 μm to 10 μm; and / or, The thickness of the porous conductive layer is 0.5 μm to 6 μm.
5. A method for preparing a porous composite current collector according to any one of claims 1 to 4, characterized in that: The following steps are involved: The polymer and the inorganic nanofiller are melt-blended and molded to form a toughened polymer layer; forming a functional metal layer on the toughened polymer layer by magnetron sputtering; A porous conductive layer is formed on the functional metal layer by electron beam lithography.
6. The method for preparing the porous composite current collector according to claim 5, characterized in that: The melt blending treatment conditions include: a temperature of 160° C. to 350° C. and a time of 0.5 h to 4 h; and / or, The molding method includes one or more of compression molding, hot pressing molding, autoclave molding and calendering molding; and / or, The conditions of the magnetron sputtering method include: the sputtering atmosphere is an inert gas, the sputtering gas pressure is 0.2Pa~10Pa, and the sputtering power is 40W~80W.
7. The method for preparing the porous composite current collector according to claim 5, characterized in that: The electron beam lithography method comprises the following steps: forming a photoresist layer and a first conductive layer in sequence on the functional metal layer; The photoresist layer is formed into photosensitive areas and non-photosensitive areas through electron beam photosensitive treatment; removing the first conductive layer, and removing the photosensitive area by developing treatment to expose the functional metal layer under the photosensitive area; forming a second conductive layer on the functional metal layer and on the non-photosensitive area; The non-photosensitive area and the second conductive layer on the non-photosensitive area are removed so that the second conductive layer on the functional metal layer forms the porous conductive layer.
8. The method for preparing the porous composite current collector according to claim 7, characterized in that: The method for forming the photoresist layer comprises a spin coating method; and / or, The method for forming the first conductive layer comprises an evaporation method; and / or, The second conductive layer is formed by magnetron sputtering.
9. The method for preparing the porous composite current collector according to claim 7, characterized in that: The first conductive layer includes chromium, and the method for removing the first conductive layer includes the following steps: The first conductive layer is etched using a mixed solution containing ammonium cerium nitrate and perchloric acid.
10. A negative electrode-free alkali metal battery, characterized in that: The invention comprises a positive electrode sheet, a separator, a porous composite current collector as claimed in any one of claims 1 to 4, and an electrolyte.