Modification method of perfluorosulfonic acid proton exchange membrane, modified perfluorosulfonic acid proton exchange membrane and application of modified perfluorosulfonic acid proton exchange membrane
By mixing perfluorosulfonic acid resin with polyvinylpyrrolidone to optimize the proton transmission channel, the problem of vanadium ion permeability in all-vanadium redox flow batteries is solved, and the Coulombic efficiency and capacity retention performance of the battery are significantly improved.
Patent Information
- Application Number
- CN202410409185.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-07
- Publication Date
- 2024-10-01
AI Technical Summary
In all-vanadium redox flow batteries, the high permeability of vanadium ions leads to capacity fading and self-discharge phenomena. It is difficult for existing technology to effectively solve the capacity fading problem caused by membrane ion selectivity defects.
By mixing perfluorosulfonic acid resin and polyvinylpyrrolidone, the proton transmission channel is optimized, the penetration of vanadium ions is reduced, the barrier properties of the membrane are improved, and drying and annealing are used to form a modified perfluorosulfonic acid proton exchange membrane.
Significantly reduces the permeability of vanadium ions and improves proton selectivity, extending the Coulombic efficiency and storage capacity retention performance of the battery.
Smart Images

Figure CN118738481A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of energy technology, and in particular to a modification method of a perfluorosulfonic acid proton exchange membrane, a modified perfluorosulfonic acid proton exchange membrane and applications thereof. Background Art
[0002] The material basis for the prosperity and development of modern society mainly comes from the acquisition of energy, such as fossil energy, nuclear energy, solar energy and wind energy. In recent years, the large-scale consumption of fossil energy has caused serious environmental pollution problems, which has promoted the development of renewable energy such as solar energy and wind energy. However, renewable energy has the disadvantages of randomness and intermittency. Large-scale grid connection will lead to the output quality of the power grid and endanger the safe operation of the power grid. Energy storage technology is an important way to solve the steady-state output of renewable energy power. Among them, redox flow battery is a large-scale energy storage system with broad development prospects, which can store energy up to several megawatts for a long time. Represented by all-vanadium redox flow battery (VRFBs), VRFBs have many advantages due to the multiple oxidation states of vanadium, such as large storage capacity, fast response speed, and long cycle life. Despite the many advantages of VRFBs system, its full commercialization is still restricted by many obstacles.
[0003] The working principle of VRFBs is that the positive electrode V is separated by a proton conducting membrane in the battery. 4+ / V 5+ and negative electrode V 2+ / V 3+ Redox occurs. As one of the core components of flow batteries, the characteristics of the proton conducting membrane will have a significant impact on battery performance. The main function of the diaphragm is to separate the positive and negative electrolytes to prevent short circuits and inhibit the crossover of active species (such as V 2+ / V 3+ and VO2 + / VO 2+ ). At the same time, the separator should be able to effectively conduct charge carriers (H + ) and have good proton selectivity to maintain the necessary charge balance in the system.
[0004] In practical applications, proton conducting membranes are exposed to harsh environments, including strong acids (2-4M H2SO4) and strong oxidizing VO2 + . Nafion membrane is widely regarded as the standard for VRFBs research and development due to its high proton conductivity, chemical and mechanical stability. However, Nafion membrane has inherent deficiencies. The size of its proton conduction channel (1.5-5nm) is much larger than the size of hydrated multivalent vanadium ions (~0.6nm), resulting in high permeability of vanadium ions. Therefore, there are serious capacity decay and self-discharge phenomena in large-scale long-term operation.
[0005] In short, the vanadium permeation problem is an important challenge facing all-vanadium flow batteries. To address the vanadium permeation problem, we can start from two aspects: the proton conductive membrane and the electrolyte. By optimizing the formula of the electrolyte, such as changing the acidity and alkalinity of the electrolyte, adding additives, etc., the kinetic behavior of vanadium ions at the electrolyte / proton conductive membrane interface can be regulated, thereby reducing the capacity decay caused by vanadium permeation. However, this method can only inhibit the transmembrane permeation of vanadium ions by adjusting the properties of the electrolyte, and it is difficult to effectively solve problems such as capacity decay caused by membrane ion selectivity defects. Summary of the invention
[0006] The purpose of the present invention is to provide a modification method of a perfluorosulfonic acid proton exchange membrane, a modified perfluorosulfonic acid proton exchange membrane and applications thereof. The present invention can effectively reduce vanadium permeation and improve the performance of an all-vanadium liquid flow battery by optimizing the proton transmission channel in the perfluorosulfonic acid proton exchange membrane. The present invention can fundamentally improve the barrier property of vanadium ions from the source of the membrane structure.
[0007] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0008] The present invention provides a method for modifying a perfluorosulfonic acid proton exchange membrane, comprising the following steps:
[0009] Mixing perfluorosulfonic acid resin, polyvinyl pyrrolidone and an organic solvent to obtain a casting solution;
[0010] The casting solution is subjected to membrane formation to obtain a modified perfluorosulfonic acid proton exchange membrane.
[0011] Preferably, the perfluorosulfonic acid resin comprises Nafion.
[0012] Preferably, the weight average molecular weight of the polyvinyl pyrrolidone is 3500 to 13000000 Da.
[0013] Preferably, based on the total mass of the polyvinyl pyrrolidone and the perfluorosulfonic acid resin being 100%, the mass fraction of the polyvinyl pyrrolidone is 1 to 30%, and the mass fraction of the perfluorosulfonic acid resin is 70 to 99%.
[0014] Preferably, the organic solvent includes one or more of N,N-dimethylformamide, N,N-dimethylacetamide, N-methyl-2-pyrrolidone and dimethyl sulfoxide.
[0015] Preferably, the film forming comprises: placing the film casting liquid on a substrate, and performing drying and annealing treatments in sequence.
[0016] Preferably, the drying temperature is 40° C. to 80° C.; and the drying time is 24 h to 48 h.
[0017] Preferably, the temperature of the annealing treatment is 120° C. to 160° C.; and the time of the annealing treatment is 24 h to 72 h.
[0018] The present invention provides a modified perfluorosulfonic acid proton exchange membrane prepared by the modification method described in the above technical solution, comprising perfluorosulfonic acid resin and polyvinyl pyrrolidone.
[0019] The present invention provides application of the modified perfluorosulfonic acid proton exchange membrane described in the above technical solution in a battery.
[0020] The present invention provides a method for modifying a perfluorosulfonic acid proton exchange membrane, comprising the following steps: mixing a perfluorosulfonic acid resin, polyvinyl pyrrolidone (PVP) and an organic solvent to obtain a casting solution; forming the casting solution into a film to obtain a modified perfluorosulfonic acid proton exchange membrane. In the present invention, unlike other nitrogen heterocyclic polymers, the electrostatic interaction between the pyrrolidone in the PVP monomer and the sulfonic acid in the perfluorosulfonic acid resin after being protonated is weak, and no coagulation phenomenon occurs, thereby obtaining a membrane with good mechanical properties. The present invention utilizes the weak interaction characteristics between PVP and the perfluorosulfonic acid resin, and the hydrophilic PVP can selectively aggregate in the proton conduction channel of the perfluorosulfonic acid resin. While reducing the channel size, the influence on the proton conductivity of the perfluorosulfonic acid proton exchange membrane is reduced to a certain extent, thereby improving the vanadium resistance of the proton exchange membrane under the condition of reducing the proton conductivity as little as possible. When the perfluorosulfonic acid proton exchange membrane is in a dry state, the linear PVP can penetrate the isolated ion clusters to a certain extent, making the ion clusters interconnected. This method is beneficial for the perfluorosulfonic acid proton exchange membrane to establish a more connected proton transmission channel after wetting.
[0021] Taking the all-vanadium liquid flow battery as an example, the present invention can effectively improve the ion selectivity of the proton exchange membrane of the liquid flow battery through the modification method, greatly reduce the cross-contamination of vanadium ions with different valence states in the electrolyte on both sides of the positive and negative electrodes, and improve the coulombic efficiency and storage capacity retention performance of the liquid flow battery. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 The vanadium ion permeability of Nafion-PVP-6w-5%;
[0023] Figure 2 The vanadium ion permeability of Nafion-PVP-6w-15%;
[0024] Figure 3 The vanadium ion permeability of Nafion-PVP-6w-30%;
[0025] Figure 4 The vanadium ion permeability of Nafion-PVP-130w-5%;
[0026] Figure 5 This is a comparison chart of the vanadium ion permeability of Nafion-PVP-130w-5% and Nafion-212;
[0027] Figure 6 This is a comparison chart of the charge and discharge capacity retention rates of commercial Nafion-212 membrane and modified Nafion membrane;
[0028] Figure 7 This is a comparison chart of the coulombic efficiency of commercial Nafion-212 membrane and modified Nafion membrane. DETAILED DESCRIPTION
[0029] The present invention provides a method for modifying a perfluorosulfonic acid proton exchange membrane, comprising the following steps:
[0030] Mixing perfluorosulfonic acid resin, polyvinyl pyrrolidone and an organic solvent to obtain a casting solution;
[0031] The casting solution is subjected to membrane formation to obtain a modified perfluorosulfonic acid proton exchange membrane.
[0032] The present invention mixes perfluorosulfonic acid resin, polyvinyl pyrrolidone and organic solvent to obtain a casting solution. In the present invention, the perfluorosulfonic acid resin preferably includes Nafion. In the present invention, the perfluorosulfonic acid resin (taking Nafion as an example) has a perfluoro main chain, a fluoroether side chain and a hydrophilic sulfonic acid end group, and the main chain, the side chain and the sulfonic acid end group in Nafion undergo self-assembled microphase separation, so that the hydrated ion phase region in the membrane forms a three-dimensional interwoven network structure.
[0033] In a specific embodiment of the present invention, when the perfluorosulfonic acid resin is Nafion, dry Nafion is preferably used. In the present invention, the preparation method of the dry Nafion preferably includes: drying the Nafion solution at 60°C for 48 hours; then placing it in water to elute the solid Nafion; drying the obtained solid Nafion at 60°C for 48 hours to obtain dry Nafion.
[0034] In the present invention, the weight average molecular weight of the polyvinyl pyrrolidone is preferably 3500-13000000 Da, more preferably 60,000-1.3 million Da, and further preferably 60,000-500,000 Da. In the present invention, the polyvinyl pyrrolidone is a linear polymer that can penetrate the ion clusters, gradually connect the isolated ion clusters, and improve the connectivity of the proton transport channel.
[0035] In the present invention, based on the total mass of the polyvinyl pyrrolidone and the perfluorosulfonic acid resin as 100%, the mass fraction of the polyvinyl pyrrolidone is preferably 1-30%, more preferably 5-15%, and the mass fraction of the perfluorosulfonic acid resin is preferably 70-99%, more preferably 85-95%.
[0036] In the present invention, the organic solvent preferably includes one or more of N,N-dimethylformamide (DMF), N,N-dimethylacetamide, N-methyl-2-pyrrolidone and dimethyl sulfoxide.
[0037] In the present invention, the mixing of the perfluorosulfonic acid resin, polyvinyl pyrrolidone and the organic solvent is preferably carried out under stirring; the stirring time is preferably 48 to 72 hours, more preferably 72 hours.
[0038] In the present invention, the total mass concentration of the perfluorosulfonic acid resin and polyvinyl pyrrolidone in the casting solution is preferably 0.1 g / mL.
[0039] After obtaining the casting solution, the present invention forms a membrane with the casting solution to obtain a modified perfluorosulfonic acid proton exchange membrane. In the present invention, the membrane forming preferably includes: placing the casting solution on a substrate, and sequentially performing drying and annealing treatments. In the present invention, the casting solution is preferably dripped onto a substrate; the substrate is preferably a glass plate.
[0040] In the present invention, the drying temperature is preferably 40° C. to 80° C., more preferably 60° C.; the drying time is preferably 24 to 48 hours, more preferably 48 hours.
[0041] In the present invention, the temperature of the annealing treatment is preferably 120°C to 160°C, more preferably 150°C; the time of the annealing treatment is preferably 24 to 72 hours, more preferably 72 hours. In the present invention, the atmosphere of the annealing treatment is preferably a nitrogen atmosphere. In the present invention, the annealing treatment can enhance the mechanical strength of the proton exchange membrane and reduce the size of the proton transport channel.
[0042] The present invention provides a modified perfluorosulfonic acid proton exchange membrane prepared by the modification method of the above technical solution, comprising perfluorosulfonic acid resin and polyvinyl pyrrolidone. In the present invention, the thickness of the modified perfluorosulfonic acid proton exchange membrane is preferably 50 to 70 μm, more preferably 60 μm.
[0043] The present invention provides the application of the modified perfluorosulfonic acid proton exchange membrane in energy technology; the application in energy technology is specifically application in batteries. In the present invention, the battery is preferably a liquid flow battery, more preferably an all-vanadium liquid flow battery.
[0044] The technical solutions in the present invention will be described clearly and completely below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only a part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0045] Types and sources of raw materials: perfluorosulfonic acid resin (Nafion, Kemu D520) polyvinyl pyrrolidone (PVP, CAS No.: 9003-39-8).
[0046] Example 1
[0047] In this embodiment, the weight average molecular weight of PVP is 60,000 Da, the mass fraction of PVP is 5%, and the specific preparation method is:
[0048] Place Nafion solution (manufacturer: Kemu. Model: D520) in a culture dish, put it in an oven, and dry it at 60°C for 48 hours; then place the culture dish in water to elute the solid Nafion; place the obtained solid Nafion in an oven for drying (drying temperature is 60°C, time is 48 hours) to obtain dry Nafion;
[0049] 0.95 g of the dry Nafion and 0.05 g of PVP were mixed and dissolved in 10 mL of DMF and stirred for 48 hours to obtain a casting solution;
[0050] The casting solution was dropped onto a glass plate, placed in an oven, dried at 60° C. for 48 h, and then placed in an oven in a nitrogen environment and annealed at 150° C. for 72 h to obtain a modified Nafion membrane with a thickness of 60 μm, recorded as Nafion-PVP-6w-5%.
[0051] Example 2
[0052] In this embodiment, the weight average molecular weight of PVP is 60,000 Da, the mass fraction of PVP is 15%, and the specific preparation method is:
[0053] Place Nafion solution (manufacturer: Kemu. Model: D520) in a culture dish, put it in an oven, and dry it at 60°C for 48 hours; then place the culture dish in water to elute the solid Nafion; place the obtained solid Nafion in an oven for drying (drying temperature is 60°C, time is 48 hours) to obtain dry Nafion;
[0054] 0.85 g of the dry Nafion and 0.15 g of PVP were mixed and dissolved in 10 mL of DMF and stirred for 48 h to obtain a casting solution;
[0055] The casting solution was dropped onto a glass plate, placed in an oven, dried at 60° C. for 48 h, and then placed in an oven in a nitrogen environment and annealed at 150° C. for 72 h to obtain a modified Nafion membrane with a thickness of 60 μm, recorded as Nafion-PVP-6w-15%.
[0056] Example 3
[0057] In this embodiment, the weight average molecular weight of PVP is 60,000 Da, and the mass fraction of PVP is 30%. The specific preparation method is:
[0058] Place Nafion solution (manufacturer: Kemu. Model: D520) in a culture dish, put it in an oven, and dry it at 60°C for 48 hours; then place the culture dish in water to elute the solid Nafion; place the obtained solid Nafion in an oven for drying (drying temperature is 60°C, time is 48 hours) to obtain dry Nafion;
[0059] 0.7 g of the dry Nafion and 0.3 g of PVP were mixed and dissolved in 10 mL of DMF and stirred for 48 h to obtain a casting solution;
[0060] The casting solution was dropped onto a glass plate, placed in an oven, dried at 60° C. for 48 h, and then placed in an oven in a nitrogen environment and annealed at 150° C. for 72 h to obtain a modified Nafion membrane with a thickness of 60 μm, recorded as Nafion-PVP-6w-30%.
[0061] Example 4
[0062] In this embodiment, the weight average molecular weight of PVP is 1.3 million Da, and the mass fraction of PVP is 5%. The specific preparation method is:
[0063] Place Nafion solution (manufacturer: Kemu. Model: D520) in a culture dish, put it in an oven, and dry it at 60°C for 48 hours; then place the culture dish in water to elute the solid Nafion; place the obtained solid Nafion in an oven for drying (drying temperature is 60°C, time is 48 hours) to obtain dry Nafion;
[0064] 0.95 g of the dry Nafion and 0.05 g of PVP were mixed and dissolved in 10 mL of DMF and stirred for 48 hours to obtain a casting solution;
[0065] The casting solution was dropped onto a glass plate, placed in an oven, dried at 60° C. for 48 h, and then placed in an oven in a nitrogen environment and annealed at 150° C. for 72 h to obtain a modified Nafion membrane with a thickness of 60 μm, recorded as Nafion-PVP-130w-5%.
[0066] Example 5
[0067] In this embodiment, the weight average molecular weight of PVP is 360,000 Da, and the mass fraction of PVP is 1%. The specific preparation method is:
[0068] Place Nafion solution (manufacturer: Kemu. Model: D520) in a culture dish, put it in an oven, and dry it at 60°C for 48 hours; then place the culture dish in water to elute the solid Nafion; place the obtained solid Nafion in an oven for drying (drying temperature is 60°C, time is 48 hours) to obtain dry Nafion;
[0069] 0.99 g of the dry Nafion and 0.01 g of PVP were mixed and dissolved in 10 mL of DMF and stirred for 48 h to obtain a casting solution;
[0070] The casting solution was dropped onto a glass plate, placed in an oven, dried at 60° C. for 48 h, and then placed in an oven in a nitrogen environment and annealed at 150° C. for 72 h to obtain a modified Nafion membrane with a thickness of 60 μm, recorded as Nafion-PVP-36w-1%.
[0071] Example 6
[0072] In this embodiment, the weight average molecular weight of PVP is 360,000 Da, and the mass fraction of PVP is 5%. The specific preparation method is:
[0073] Place Nafion solution (manufacturer: Kemu. Model: D520) in a culture dish, put it in an oven, and dry it at 60°C for 48 hours; then place the culture dish in water to elute the solid Nafion; place the obtained solid Nafion in an oven for drying (drying temperature is 60°C, time is 48 hours) to obtain dry Nafion;
[0074] 0.95 g of the dry Nafion and 0.05 g of PVP were mixed and dissolved in 10 mL of DMF and stirred for 48 hours to obtain a casting solution;
[0075] The casting solution was dropped onto a glass plate, placed in an oven, dried at 60° C. for 48 h, and then placed in an oven in a nitrogen environment and annealed at 150° C. for 72 h to obtain a modified Nafion membrane with a thickness of 60 μm, recorded as Nafion-PVP-36w-5%.
[0076] Test Example 1
[0077] The vanadium resistance and ion selectivity of the flow battery can be tested by vanadium ion permeation experiments. The membrane sample (3×3 cm 2) was soaked in 3M (mol / L) H2SO4 solution for 12 hours in advance and then clamped in the middle of the diffusion cell; the left diffusion half cell was filled with 40mL 1.5M VOSO4 3M H2SO4 solution, and the right diffusion half cell was filled with 40mL 1.5M MgSO4 3M H2SO4 solution to balance the osmotic pressure. During the test (60 hours), magnetic stirring was always maintained to eliminate concentration polarization. Every other day, 3mL of solution was taken out from the right diffusion half cell for ultraviolet absorption spectrum (UV-visible spectrophotometer) detection to determine the absorption peak intensity of the solution at 762nm. After the test, the solution was recovered to the right diffusion half cell. Vanadium ion permeability P (cm 2 ·min -1 ) and proton selectivity S (S·min·cm -3 ) is calculated by the following formula:
[0078]
[0079]
[0080] Where L (cm) is the thickness of the film sample, A (cm 2 ) is the effective area of the membrane sample sandwiched in the middle of the diffusion cell in contact with the solution; V R is the volume of the solution in the right diffusion half cell; C0 and C t (mol L -1 ) are the VO of the left and right hemi-pools at time t, respectively. 2+ The concentration of C0 is set to 1.5M by default, and C t According to different concentrations of VO in 3M H2SO4 solution 2+ The absorbance intensity of the standard curve is plotted. -1 ) is the proton conductivity in the membrane permeation direction.
[0081] The results of vanadium ion permeability P and proton selectivity S are as follows:
[0082] Figure 1 is the vanadium ion permeability of Nafion-PVP-6w-5%. After calculation, the vanadium ion permeability P = 2.64×10 - 7 cm 2 ·min -1 , proton selectivity S = 3.07S·min·cm -3 .
[0083] Figure 2 is the vanadium ion permeability of Nafion-PVP-6w-15%. After calculation, the vanadium ion permeability P = 1.40 × 10 - 7 cm2 ·min -1 , proton selectivity S = 6.36S·min·cm -3 .
[0084] Figure 3 is the vanadium ion permeability of Nafion-PVP-6w-30%. After calculation, the vanadium ion permeability P = 0.98 × 10 - 7 cm 2 ·min -1 , proton selectivity S = 9.25S·min·cm -3 .
[0085] Figure 4 is the vanadium ion permeability of Nafion-PVP-130w-5%. After calculation, the vanadium ion permeability P = 0.32×10 -7 cm 2 ·min -1 , proton selectivity S = 18.93S·min·cm -3 .
[0086] Comparing Nafion-PVP-130w-5% with commercial Nafion-212 membrane, Figure 5 The vanadium ion permeability of the two is compared. Figure 5 As shown in the figure, the modified Nafion membrane prepared by the present invention has a greatly improved vanadium ion barrier property. The lower the permeability value, the better the vanadium ion barrier property. The vanadium ion permeability of Nafion-PVP-130w-5% is calculated to be P=0.32×10 -7 cm 2 ·min -1 , the vanadium ion permeability of Nafion-212 is P = 6.46 × 10 -7 cm 2 ·min -1 The higher the proton selectivity value, the better the vanadium ion barrier. The proton selectivity of Nafion-PVP-130w-5% is S = 18.93S·min·cm -3 , the proton selectivity of Nafion-212 is S = 3.93S·min·cm -3 By comparing the proton selectivity values of the two, it can be concluded that the modified Nafion-PVP-130w-5% has better proton selectivity.
[0087] Test Example 2
[0088] Taking Nafion, the most representative perfluorosulfonic acid membrane, as an example, Figure 6The figure shows the performance of the commercial Nafion-212 membrane and the Nafion-PVP modified membrane (Nafion-PVP-36w-5%, denoted as Nafion-PVP) prepared in Example 6 in terms of battery capacity retention. The capacity of the commercial Nafion-212 membrane decays to 20% after about 65 cycles, while the modified Nafion membrane prepared in the present invention needs 125 cycles before the capacity decays to 20%. This result fully reflects the excellent performance of the modified Nafion membrane in blocking the penetration of vanadium ions.
[0089] Figure 7 The coulombic efficiency of the commercial Nafion-212 membrane is compared with that of the Nafion-PVP modified membrane (Nafion-PVP-36w-5%, denoted as Nafion-PVP) prepared in Example 6. The coulombic efficiency of the commercial Nafion-212 membrane is 92% on average, while the modified Nafion membrane has an average coulombic efficiency of 98% due to the suppression of vanadium ion cross contamination.
[0090] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for modifying a perfluorosulfonic acid proton exchange membrane, The following steps are involved: Mixing perfluorosulfonic acid resin, polyvinyl pyrrolidone and an organic solvent to obtain a casting solution; The casting solution is subjected to membrane formation to obtain a modified perfluorosulfonic acid proton exchange membrane.
2. The modification method according to claim 1, It is characterized in that The perfluorosulfonic acid resin includes Nafion.
3. The modification method according to claim 1, It is characterized in that The weight average molecular weight of the polyvinyl pyrrolidone is 3500 to 13000000 Da.
4. The modification method according to any one of claims 1 to 3, It is characterized in that Based on the total mass of the polyvinyl pyrrolidone and the perfluorosulfonic acid resin as 100%, the mass fraction of the polyvinyl pyrrolidone is 1 to 30%. , The mass fraction of the perfluorosulfonic acid resin is 70-99%.
5. The modification method according to claim 1, It is characterized in that The organic solvent includes one or more of N,N-dimethylformamide, N,N-dimethylacetamide, N-methyl-2-pyrrolidone and dimethyl sulfoxide.
6. The modification method according to claim 1, It is characterized in that The film forming comprises: placing the film casting liquid on a substrate, and performing drying and annealing treatments in sequence.
7. The modification method according to claim 6, It is characterized in that The drying temperature is 40° C. to 80° C.; the drying time is 24 h to 48 h.
8. The modification method according to claim 6, It is characterized in that The temperature of the annealing treatment is 120° C. to 160° C.; the time of the annealing treatment is 24 h to 72 h.
9. The modified perfluorosulfonic acid proton exchange membrane prepared by the modification method according to any one of claims 1 to 8, comprising perfluorosulfonic acid resin and polyvinyl pyrrolidone.
10. Application of the modified perfluorosulfonic acid proton exchange membrane according to claim 9 in energy technology.
Citation Information
Cited By
Cross-linked polymer doped and modified perfluorosulfonic acid membrane and preparation method thereof
CN118909287A
Preparation method of cross-linked polyvinylpyrrolidone surface modified perfluorosulfonic acid membrane
CN118909288A