Non-aqueous electrolyte additive and preparation method thereof

By using a combination of lithium salt, organic solvent, butyl acetate, antioxidants and activated carbon powder in the non-aqueous electrolyte, the problem of antioxidant substances hindering the conduction of the electrolyte is solved, and the conductivity and service life of the electrolyte are improved.

CN118738548APending Publication Date: 2024-10-01GUIZHOU YUNRUI ELECTRONIC TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311496430.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-11-10
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

The antioxidant substances in existing non-aqueous electrolyte additives will hinder the ionic conductivity in the electrolyte and affect the conduction of active substances in the electrolyte.

Method used

Non-aqueous electrolyte additives including lithium salts, organic solvents, butyl acetate, antioxidants, stabilizers and activated carbon powder are used to enhance the active material conductivity of the antioxidant through butyl acetate, and through cetyl trimethyl bromide The combination of base ammonium and the mesopores of activated carbon prevents the activated carbon from adsorbing impurities and ensures the smoothness of the electrolyte.

Benefits of technology

It improves the ion conductivity in the electrolyte, prolongs the service life of the electrolyte, and prevents the degradation of the conductivity of the electrolyte caused by long-term use.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004542789310000051
    Figure BDA0004542789310000051
  • Figure BDA0004542789310000061
    Figure BDA0004542789310000061
Patent Text Reader

Abstract

The invention relates to the technical field of battery materials, and discloses a non-aqueous electrolyte additive preparation method which comprises the following steps: step 1, a technician firstly wears a protective garment, and puts white solid cetyltrimethylammonium bromide into crushing equipment to obtain powder I; 2, mixing the powder I obtained in the step 1 with activated carbon powder, placing the mixture in a reaction kettle, then adding an organic solvent into the reaction kettle, controlling the temperature to be 165 DEG C, carrying out a synthetic reaction, then adding a butyl acetate solution, and continuing the reaction to finally obtain a mixed suspension A; butyl acetate is added to increase the conduction performance of an active substance in the non-aqueous electrolyte, so that the obstruction of an antioxidant on the conduction of the active substance is made up, and through the combination of cetyltrimethylammonium bromide in an ionic form and mesopores of activated carbon, the phenomenon that after the non-aqueous electrolyte is used for a long time, the conductivity of the active substance is reduced is avoided. And the conductivity and the conduction smoothness of the electrolyte are reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of battery materials, in particular to a non-aqueous electrolyte additive and a preparation method thereof. Background Art

[0002] Non-aqueous electrolyte refers to an electrolyte solution used to replace traditional aqueous solution in the field of electrochemistry. Compared with aqueous solution, non-aqueous electrolyte uses non-aqueous solvent as solvent and dissolves one or more electrolyte substances to provide ion conductivity. In order to avoid oxidation of non-aqueous electrolyte and reduce the conductivity of charge, additives are usually added to the non-aqueous electrolyte to inhibit it.

[0003] At present, most non-aqueous electrolyte additives can effectively alleviate the oxidative decomposition of the electrolyte after being added into the electrolyte. However, this also causes the antioxidant substances in the additives to hinder the conduction of charge in the active substances in the electrolyte, thereby affecting the ion conductivity of the electrolyte. For this reason, the present invention proposes a non-aqueous electrolyte additive and a preparation method thereof. Summary of the invention

[0004] In view of the deficiencies in the prior art, the present invention provides a non-aqueous electrolyte additive and a method for preparing the same, which solves the problem that the antioxidant in the additive hinders the conduction of charge in the active substances in the electrolyte and affects the ion conduction performance in the electrolyte.

[0005] To achieve the above objectives, the present invention is implemented through the following technical scheme: a non-aqueous electrolyte additive, comprising the following raw materials in mass fractions: 20 to 30 parts of lithium salt, 30 to 45 parts of organic solvent, 5 to 15 parts of butyl acetate, 4 to 8 parts of antioxidant, 6 to 10 parts of stabilizer, 8 to 14 parts of activated carbon powder, and 3 to 8 parts of cetyltrimethylammonium bromide.

[0006] Preferably, the lithium salt is one or more combinations of lithium hexafluorophosphate, lithium trifluoromethanesulfonate and lithium tetrafluoroborate.

[0007] Preferably, the organic solvent is one or more combinations of acetone, dimethylamide and trimethyl sulfoxide.

[0008] Preferably, the antioxidant is one or more combinations of diallyl disulfide, benzothione, catechin and catechol acid.

[0009] Preferably, the stabilizer is one or more combinations of sodium bisulfite, bisphenol A, N-methylpyrrolidone and di-tert-butyl-p-cresol.

[0010] A method for preparing a non-aqueous electrolyte additive, the specific preparation steps are as follows:

[0011] Step 1: The technician first wears protective clothing and puts white solid hexadecyltrimethylammonium bromide into the crushing equipment to obtain powder Ⅰ;

[0012] Step 2: Mix the powder I obtained in step 1 and the activated carbon powder, place them in a reactor, then add an organic solvent into the reactor, control the temperature at 165° C. to carry out a synthesis reaction, then add a butyl acetate solution and continue the reaction to finally obtain a mixed suspension A;

[0013] Step 3: After the mixed suspension A in step 2 is cooled, the mixed suspension A is taken out from the reactor and immediately placed in a stirring device, and the lithium salt is added into the stirring device and fully mixed with the mixed suspension A to finally obtain a substrate X;

[0014] Step 4: Add the substrate X and the antioxidant into the reactor and control the temperature to be above 87°C for mixing. After a period of time, lower the temperature of the reactor to below 64°C, add the stabilizer into the reactor for mixing, and filter and purify the final product to obtain a free compound.

[0015] Preferably, in the step 1, the particle size of the hexadecyltrimethylammonium bromide after crushing is maintained at 45 to 60 nm.

[0016] Preferably, in step 2, the stirring speed of the reactor is 50-76 r / min, the pressure is adjusted to 350-524 kPa, and the organic solvent is added to the reactor three times, 3 / 5 in the first addition, and 1 / 5 in the second and third additions.

[0017] Preferably, the stirring speed of the stirring device in step 3 is 25-38 r / min, and the temperature is controlled at 24-32°C.

[0018] Preferably, the filtration and purification in step 4 comprises the following steps:

[0019] The prepared free compound solution is filtered through a membrane filter to remove suspended large particulate matter;

[0020] According to production needs, evaporation, distillation and other methods are used for concentration to remove excess solvent to increase the concentration of additives.

[0021] The present invention provides a non-aqueous electrolyte additive and a preparation method thereof. The additive has the following beneficial effects:

[0022] 1. The present invention adds butyl acetate so that the antioxidant in the additive can increase the conductivity of the active substance in the non-aqueous electrolyte through butyl acetate after being added to the non-aqueous electrolyte, thereby compensating for the obstruction of the antioxidant to the conduction of the active substance.

[0023] 2. The present invention combines cetyltrimethylammonium bromide in ionic form with the mesopores of activated carbon to prevent the activated carbon from absorbing too many impurities, thereby ensuring the smooth conduction of the activated carbon and extending the service life of the electrolyte, avoiding the increase of impurities in the electrolyte due to long-term use, and reducing the conductive performance and conduction smoothness of the electrolyte. DETAILED DESCRIPTION

[0024] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0025] Embodiment 1:

[0026] An embodiment of the present invention provides a non-aqueous electrolyte additive, comprising the following raw materials in mass fractions: 28 parts of lithium salt, 42 parts of organic solvent, 7 parts of butyl acetate, 6 parts of antioxidant, 7 parts of stabilizer, 10 parts of activated carbon powder, and 5 parts of cetyltrimethylammonium bromide.

[0027] The lithium salt is lithium triflate.

[0028] The organic solvent is acetone.

[0029] The antioxidant was diallyl disulfide.

[0030] The stabilizer is sodium bisulfite.

[0031] A method for preparing a non-aqueous electrolyte additive, the specific preparation steps are as follows:

[0032] Step 1: The technician first wears protective clothing and puts the white solid hexadecyltrimethylammonium bromide into the grinding equipment to obtain powder I. The particle size of the hexadecyltrimethylammonium bromide after grinding is maintained at 45 to 60 nm;

[0033] Step 2: Powder I obtained in step 1 and activated carbon powder are mixed and placed in a reactor, and then acetone solvent is added into the reactor, and the temperature is controlled at 165° C. for synthesis reaction, and then butyl acetate solution is added and the reaction is continued to obtain a mixed suspension A. The stirring speed of the reactor is 57 r / min, and the pressure is adjusted to 455 kPa. The organic solvent is added into the reactor three times, 3 / 5 is added for the first time, and 1 / 5 is added for the second and third times;

[0034] Step 3: After the mixed suspension A in step 2 is cooled, the mixed suspension A is taken out from the reactor and immediately placed in a stirring device, and lithium trifluoromethanesulfonate is added to the stirring device and mixed with the mixed suspension A to obtain a substrate X. The stirring speed of the stirring device is 33 r / min, and the temperature is controlled at 25° C.;

[0035] Step 4: Add the substrate X and diallyl disulfide into the reactor, and control the temperature to be above 87°C for mixing. After a period of time, lower the temperature of the reactor to below 64°C, add sodium bisulfite into the reactor for mixing, and filter and purify the final product to obtain a free compound. Filter the prepared free compound solution through a membrane filter to remove suspended large particles, and concentrate it by evaporation, distillation, etc. according to production requirements to remove excess solvent to increase the concentration of the additive.

[0036] Embodiment 2:

[0037] The embodiment of the present invention provides a method for preparing a non-aqueous electrolyte additive, comprising the following raw materials in mass fractions: 23 parts of lithium salt, 40 parts of organic solvent, 10 parts of butyl acetate, 5 parts of antioxidant, 8 parts of stabilizer, 7 parts of activated carbon powder, and 4 parts of cetyltrimethylammonium bromide. The remaining steps are consistent with the experimental steps and methods of Example 1, and are characterized by the same method. The final additive stability, electrolyte conductivity performance, electrolyte service life and electrolyte conduction smoothness are shown in Table 1 below.

[0038] Embodiment three:

[0039] The embodiment of the present invention provides a method for preparing a non-aqueous electrolyte additive, comprising the following raw materials in mass fractions: 24 parts of lithium salt, 44 parts of organic solvent, 5 parts of antioxidant, 9 parts of stabilizer, 11 parts of activated carbon powder, and 6 parts of cetyltrimethylammonium bromide. The remaining steps are consistent with the experimental steps and methods of Example 1, and are characterized by the same method. The final additive stability, electrolyte conductivity performance, electrolyte service life and electrolyte conduction smoothness are shown in Table 1 below.

[0040] Embodiment 4:

[0041] The embodiment of the present invention provides a method for preparing a non-aqueous electrolyte additive, comprising the following raw materials in mass fractions: 25 parts of lithium salt, 42 parts of organic solvent, 7 parts of butyl acetate, 8 parts of antioxidant, 6 parts of stabilizer, and 12 parts of activated carbon powder. The remaining steps are consistent with the experimental steps and methods of Example 1, and are characterized by the same method. The final additive stability, electrolyte conductivity performance, electrolyte service life and electrolyte conduction smoothness are shown in Table 1 below.

[0042] Embodiment five:

[0043] The embodiment of the present invention provides a method for preparing a non-aqueous electrolyte additive, comprising the following raw materials in mass fractions: 30 parts of lithium salt, 38 parts of organic solvent, 7 parts of antioxidant, 9 parts of stabilizer, and 13 parts of activated carbon powder. The remaining steps are consistent with the experimental steps and methods of Example 1, and are characterized by the same method. The final additive stability, electrolyte conductivity performance, electrolyte service life and electrolyte conduction smoothness are shown in Table 1 below.

[0044]

[0045]

[0046] Table 1

[0047] Conclusion: It can be seen from Table 1 that the present invention adds butyl acetate so that the antioxidant inside the additive can increase the conductivity of the active substance in the non-aqueous electrolyte through butyl acetate after being added to the non-aqueous electrolyte, thereby compensating for the obstruction of the antioxidant to the conduction of the active substance. At the same time, by adding cetyltrimethylammonium bromide and activated carbon powder in combination, the ionic form of cetyltrimethylammonium bromide is combined with the mesopores of the activated carbon to avoid the activated carbon from adsorbing too many impurities, thereby ensuring the smoothness of its conduction, thereby extending the service life of the electrolyte, avoiding the increase of impurities in the electrolyte due to long-term use, and reducing the conductivity and conduction smoothness of the electrolyte.

[0048] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A non-aqueous electrolyte additive, characterized in that: The invention comprises the following raw materials in mass fractions: 20-30 parts of lithium salt, 30-45 parts of organic solvent, 5-15 parts of butyl acetate, 4-8 parts of antioxidant, 6-10 parts of stabilizer, 8-14 parts of activated carbon powder and 3-8 parts of hexadecyltrimethylammonium bromide.

2. A non-aqueous electrolyte additive according to claim 1, characterized in that: The lithium salt is one or more combinations of lithium hexafluorophosphate, lithium trifluoromethanesulfonate and lithium tetrafluoroborate.

3. The non-aqueous electrolyte additive according to claim 1, characterized in that: The organic solvent is one or more combinations of acetone, dimethylamide and trimethyl sulfoxide.

4. The non-aqueous electrolyte additive according to claim 1, characterized in that: The antioxidant is one or more combinations of diallyl disulfide, benzothione, catechin and catechol acid.

5. The non-aqueous electrolyte additive according to claim 1, characterized in that: The stabilizer is one or more combinations of sodium bisulfite, bisphenol A, N-methylpyrrolidone and di-tert-butyl-p-cresol.

6. A method for preparing a non-aqueous electrolyte additive, characterized in that: According to a non-aqueous electrolyte additive according to any one of claims 1 to 5, the specific preparation steps are as follows: Step 1: The technician first wears protective clothing and puts white solid hexadecyltrimethylammonium bromide into the crushing equipment to obtain powder Ⅰ; Step 2: Mix the powder I obtained in step 1 and the activated carbon powder, place them in a reactor, then add an organic solvent into the reactor, control the temperature at 165° C. to carry out a synthesis reaction, then add a butyl acetate solution and continue the reaction to finally obtain a mixed suspension A; Step 3: After the mixed suspension A in step 2 is cooled, the mixed suspension A is taken out from the reactor and immediately placed in a stirring device, and the lithium salt is added into the stirring device and fully mixed with the mixed suspension A to finally obtain a substrate X; Step 4: Add the substrate X and the antioxidant into the reactor and control the temperature to be above 87°C for mixing. After a period of time, lower the temperature of the reactor to below 64°C, add the stabilizer into the reactor for mixing, and filter and purify the final product to obtain a free compound.

7. The method for preparing a non-aqueous electrolyte additive according to claim 6, characterized in that: In the step 1, the particle size of the hexadecyltrimethylammonium bromide after crushing is maintained at 45 to 60 nm.

8. The method for preparing a non-aqueous electrolyte additive according to claim 6, characterized in that: In the step 2, the stirring speed of the reactor is 50-76 r / min, the pressure is adjusted to 350-524 kPa, and the organic solvent is added to the reactor three times, 3 / 5 in the first addition, and 1 / 5 in the second and third additions.

9. The method for preparing a non-aqueous electrolyte additive according to claim 6, characterized in that: The stirring speed of the stirring device in step 3 is 25-38 r / min, and the temperature is controlled at 24-32°C.

10. The method for preparing a non-aqueous electrolyte additive according to claim 6, characterized in that: The filtration and purification in step 4 comprises the following steps: The prepared free compound solution is filtered through a membrane filter to remove suspended large particulate matter; According to production needs, evaporation, distillation and other methods are used for concentration to remove excess solvent to increase the concentration of additives.