High-voltage lithium ion battery electrolyte, preparation method and lithium ion energy storage battery
By using high-voltage lithium-ion electrolyte in lithium-ion batteries, which contains electrolyte lithium salt, organic solvent and silyl sulfate, a protective film is formed, which solves the problem of rapid capacity fading of high-nickel ternary cathode materials at high voltage and improves efficiency. Cycle life and rate performance of lithium-ion energy storage batteries.
Patent Information
- Application Number
- CN202410815273.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-24
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-06-24
AI Technical Summary
High-nickel ternary cathode materials in lithium-ion batteries cause rapid capacity fading and shortened cycle life due to material surface decomposition and transition metal ion dissolution, especially when the voltage is higher than 4.3V.
Use high-voltage lithium ion battery electrolyte, including electrolyte lithium salt, organic solvent and silyl sulfate. The dosage of silyl sulfate is 0.1-0.3% of the total mass of electrolyte lithium salt and organic solvent to form a protective film and inhibit the electrolyte. Decomposition and material transformation.
Significantly improves the cycle life of lithium-ion energy storage batteries at 4.5V voltage, extends the service life of the battery, and improves rate performance and safety.
Smart Images

Figure CN118738554A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of lithium-ion batteries, and in particular to a high-voltage lithium-ion battery electrolyte, a preparation method, and a lithium-ion energy storage battery. Background Art
[0002] Lithium-ion batteries (LIBs) have the advantages of high energy density, long cycle life and environmental friendliness, and they dominate the portable energy storage technology in today's electronic devices and electric vehicle markets. In order to achieve the goal of high-energy lithium-ion batteries, researchers have made many efforts, such as expanding the electrochemical window and improving the specific capacity of electrode materials. Among many advanced cathode materials, high-nickel ternary cathode materials are considered to be one of the most attractive and promising cathode materials due to their high reversible capacity and low cost.
[0003] However, commercial carbonate-based electrolytes decompose severely on the surface of highly lithium-ionized materials, and the accumulation of products increases the interfacial impedance. At the same time, during the charge and discharge process, the layered high-nickel ternary material is accompanied by the dissolution of transition metal ions, resulting in an irreversible phase transition from a layered structure to a spinel structure. As a result, when the voltage is higher than 4.3 V, the high-nickel ternary material will be used as a positive electrode material in lithium-ion energy storage batteries, accompanied by rapid capacity decay, resulting in a shortened cycle life. Summary of the invention
[0004] In view of the above-mentioned deficiencies in the related art, the present application provides a high-voltage lithium-ion battery electrolyte, a preparation method and a lithium-ion energy storage battery. The high-voltage lithium-ion battery electrolyte used in the present application can increase the cycle life of the lithium-ion energy storage battery at a voltage of 4.5V.
[0005] In the first aspect, the present application provides a high-voltage lithium-ion battery electrolyte using the following technical solution: A high-voltage lithium-ion battery electrolyte comprises an electrolyte lithium salt, an organic solvent and a silane sulfate, wherein the amount of the silane sulfate is 0.1-0.3% of the total mass of the electrolyte lithium salt and the organic solvent.
[0006] Preferably, the silane sulfate is bis(trimethylsilyl) sulfate.
[0007] Preferably, the organic solvent comprises cyclic carbonate and linear carbonate in a weight ratio of 1:1-3.
[0008] Preferably, the organic solvent comprises cyclic carbonate and linear carbonate in a weight ratio of 3:7.
[0009] Preferably, the cyclic carbonate includes: one or more of ethylene carbonate, propylene carbonate, butylene carbonate, butyrolactone and valerolactone; the linear carbonate includes: one or more of dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, ethyl acetate, butyl acetate, methyl propionate, ethyl propionate and propyl propionate.
[0010] Preferably, the linear carbonate comprises ethyl methyl carbonate and diethyl carbonate in a weight ratio of 5:1-3.
[0011] Preferably, the linear carbonate comprises ethyl methyl carbonate and diethyl carbonate in a weight ratio of 5:2.
[0012] Preferably, the electrolyte lithium salt includes one or more of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium perchlorate, lithium bis(trifluoromethylsulfonyl)imide, lithium trifluoromethylsulfonate, lithium difluorooxalatoborate, lithium dioxalatoborate and lithium difluorooxalatoborate.
[0013] Preferably, the concentration of the electrolyte lithium salt is 0.5-1.5 mol / L.
[0014] Preferably, the concentration of the electrolyte lithium salt is 1 mol / L.
[0015] In a second aspect, the present application provides a method for preparing a high-voltage lithium-ion battery electrolyte using the following technical solution: A method for preparing a high-voltage lithium-ion battery electrolyte comprises the following steps: adding electrolyte lithium salt into an organic solvent to dissolve it to obtain a raw electrolyte, and adding silyl sulfate into the raw electrolyte to dissolve it to obtain the high-voltage lithium-ion battery electrolyte.
[0016] Preferably, the organic solvent is prepared by mixing cyclic carbonate and linear carbonate in proportion and purifying by removing impurities and water.
[0017] In a third aspect, the present application provides a lithium-ion energy storage battery adopting the following technical solution: A lithium-ion energy storage battery comprises a positive electrode, a negative electrode, a separator and a high-voltage lithium-ion battery electrolyte.
[0018] Preferably, the positive electrode comprises one or more positive electrode active materials selected from the group consisting of NCM811, NCM622, LCO and LNMO.
[0019] Preferably, the positive electrode includes one of NCM622, NCM811 and LCO as a positive electrode active material.
[0020] Preferably, the positive electrode comprises NCM622 or NCM811 as the positive electrode active material.
[0021] Preferably, the positive electrode includes NCM622 as the positive electrode active material.
[0022] Preferably, the positive electrode further comprises graphite particles, acetylene black, Ketjen black and carbon nanofibers as conductive materials.
[0023] Preferably, the negative electrode comprises one or more of natural graphite, artificial graphite, silicon, silicon-carbon composite and lithium metal.
[0024] Preferably, the diaphragm comprises a polyethylene diaphragm or a polypropylene diaphragm.
[0025] In summary, the present application includes at least one of the following beneficial technical effects: 1. By adding 0.1-0.3 parts of silane sulfate, the voltage that the high-voltage lithium-ion battery electrolyte of the present application can act on is increased to 4.5V, thereby increasing the cycle life of the lithium-ion energy storage battery when the voltage is above 4.3V; 2. When NCM622 is used as the positive electrode active material, silyl sulfate can be preferentially enriched on the surface of NCM622 before other basic components in the system are oxidized, occupy active sites, and form a protective film before NCM622 deintercalates lithium ions, inhibiting the decomposition of other basic components in the electrolyte, protecting other basic components in the electrolyte, and improving the cycle life and rate performance of lithium-ion energy storage batteries; 3. By adding 0.1-0.3 parts of silyl sulfate, it is helpful to suppress the polarization of Li metal as the negative electrode, which is beneficial to improve the cycle life and safety of lithium-ion energy storage batteries. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 A comparison chart of the cycle tests of the lithium-ion energy storage batteries of Example 2 and Comparative Example 1; Figure 2 This is a comparison chart of the results of cyclic voltammetry tests of the lithium-ion energy storage batteries of Example 2 and Comparative Example 1; Figure 3 The results of theoretical calculation of HOMO and LUMO for EC, EMC and DEC in the lithium-ion energy storage battery of Example 2; Figure 4 A comparison chart of rate performance tests of lithium-ion energy storage batteries of Example 2 and Comparative Example 1; Figure 5 This is a comparison chart of impedance tests of lithium-ion energy storage batteries of Example 2 and Comparative Example 1 after 3 cycles of cycle testing; Figure 6 Impedance test comparison chart of the lithium-ion energy storage batteries of Example 2 and Comparative Example 1 after 200 cycles of cycle testing; Figure 7A comparison chart of TEM and SEM characterization results of the pole pieces of the lithium-ion energy storage batteries of Example 2 and Comparative Example 1 after 200 cycles; Figure 8 This is a comparison chart of ICP test results of the negative electrode surface of the lithium-ion energy storage battery of Example 2 and Comparative Example 1 after 200 cycles.
[0027] Fig. 9 This is a cycle performance diagram of a cycle test of a lithium-lithium symmetric battery made from the high-voltage lithium-ion battery electrolyte obtained in the preparation process of Example 2 and Comparative Example 1. DETAILED DESCRIPTION
[0028] The present application is further described in detail below in conjunction with examples. The following examples are only used to illustrate the present invention and should not be construed as limiting the scope of the present invention. In the following examples, if specific conditions are not specified, they are carried out according to normal conditions or conditions recommended by the manufacturer. The methods used are conventional methods known in the art unless otherwise specified, and the consumables and reagents used are commercially available unless otherwise specified. Unless otherwise specified, the professional and scientific terms used herein have the same meaning as those familiar to those skilled in the art. In addition, any method or material similar or equivalent to the recorded content may also be applied to the present invention.
[0029] The raw materials used in the examples and comparative examples can be obtained from commercial sources, among which bis(trimethylsilyl) sulfate, English name: Bis(trimethylsilyl)Sulfate, CAS number: 18306-29-1, molecular formula: C6H18O4SSi2, molecular weight: 242.4400, is also known as BTTS.
[0030] Example 1 Embodiment 1 of the present application provides a lithium-ion energy storage battery, which is prepared by the following method: Preparation of positive electrode: LiNi 0.6 Co 0.2 Mn 0.2 (NCM622), polytetrafluoroethylene (PVDF) and acetylene black are dissolved in N-methylpyrrolidone (NMP) in a mass ratio of 8:1:1. The slurry is evenly coated on the current collector aluminum foil, first dried in an oven at 80 °C for 1 h, then transferred to 120 °C for vacuum drying for 12 h, and cut to obtain a positive electrode sheet with a diameter of 12 mm.
[0031] Preparation of high-voltage lithium-ion battery electrolyte: Ethylene carbonate (EC), ethyl methyl carbonate (EMC) and diethyl carbonate are mixed in a mass ratio of 3:5:2, and an organic solvent is obtained by purification and removal of impurities and water (water content is less than 10 ppm) using molecular sieves, calcium hydride and lithium hydride; at room temperature, the conductive lithium salt LiPF6 is dissolved in the organic solvent and stirred evenly, and the final concentration of LiPF6 is 1.0 mol / L to obtain a basic electrolyte; bis(trimethylsilyl) sulfate is added to the basic electrolyte, and the addition amount of bis(trimethylsilyl) sulfate is 0.1 wt.% of the basic electrolyte, and stirred evenly to obtain a high-voltage lithium-ion battery electrolyte.
[0032] The positive electrode plate, high-voltage lithium-ion battery electrolyte, separator and Li as the negative electrode plate are assembled to obtain a lithium-ion energy storage battery.
[0033] In this embodiment, the type of the separator is Celgard 2400, LiNi 0.6 Co 0.2 Mn 0.2 (NCM622) is the positive electrode active material, polytetrafluoroethylene (PVDF) is the binder, and acetylene black is the conductive material.
[0034] Example 2 Example 2 of the present application provides a lithium-ion energy storage battery. The difference between Example 2 and Example 1 is that in the process of preparing the high-voltage lithium-ion battery electrolyte in Example 2, the amount of bis(trimethylsilyl) sulfate added is 0.2wt.% of the basic electrolyte.
[0035] Example 3 Example 3 of the present application provides a lithium-ion energy storage battery. The difference between Example 3 and Example 1 is that in the process of preparing the high-voltage lithium-ion battery electrolyte in Example 3, the amount of bis(trimethylsilyl) sulfate added is 0.3wt.% of the basic electrolyte.
[0036] Example 4 Example 4 provides a lithium-ion energy storage battery. The difference between Example 4 and Example 2 is that in the process of preparing the positive electrode sheet, NCM811 (LiNi 0.8 Co 0.1 Mn 0.1 ) replaced NCM622 as the positive electrode active material.
[0037] Example 5 Example 5 provides a lithium-ion energy storage battery. The difference between Example 5 and Example 2 is that in the process of preparing the positive electrode plate in Example 5, LCO (lithium cobalt oxide) is used to replace NCM622 as the positive electrode active material.
[0038] Comparative Example 1 Comparative Example 1 provides a lithium-ion energy storage battery. The difference between Comparative Example 1 and Example 2 is that in the process of preparing the high-voltage lithium-ion battery electrolyte in Comparative Example 1, no bis(trimethylsilyl) sulfate is added.
[0039] Comparative Example 2 Comparative Example 2 provides a lithium-ion energy storage battery. The difference between Comparative Example 2 and Example 2 is that in the process of preparing the high-voltage lithium-ion battery electrolyte in Comparative Example 2, tri-thiophene boric acid is used to replace bis(trimethylsilyl) sulfate and added to the basic electrolyte.
[0040] Comparative Example 3 Comparative Example 3 provides a lithium-ion energy storage battery. The difference between Comparative Example 3 and Comparative Example 1 is that in the process of preparing the positive electrode sheet, NCM811 (LiNi 0.8 Co 0.1 Mn 0.1 ) replaced NCM622 as the positive electrode active material.
[0041] Comparative Example 4 Comparative Example 4 provides a lithium-ion energy storage battery. The difference between Comparative Example 4 and Example 2 is that in the process of preparing the positive electrode plate, Comparative Example 4 uses LCO (lithium cobalt oxide) instead of NCM622 as the positive electrode active material.
[0042] Test and Inspection (1) The lithium ion energy storage batteries prepared in Examples 1-5 and Comparative Examples 1-4 were subjected to cycle tests, and the capacity retention rates after 200 cycles were as shown in Table 1. The comparison of the number of cycles-capacity retention rates of the lithium ion energy storage batteries in Example 2 and Comparative Example 1 is shown in Table 1. Figure 1 shown.
[0043] Table 1: Capacity retention rate of lithium-ion energy storage batteries of Examples 1-5 and Comparative Examples 1-4
[0044] (2) The lithium-ion energy storage batteries prepared in Example 2 and Comparative Example 1 were subjected to cyclic voltammetry (CV) testing. The results are as follows: Figure 2 shown.
[0045] (3) Theoretical calculations were performed on the HOMO and LOMO of the high-voltage lithium-ion battery electrolyte prepared in Example 2. The results are as follows: Figure 3 shown.
[0046] (4) The lithium-ion energy storage batteries prepared in Example 2 and Comparative Example 1 were subjected to cycle performance tests at different rates (0.3C, 1.0C, 3.0C, 7.0C, 0.3C, 10C, 15C). The test results are as follows: Figure 4 shown.
[0047] (5) The lithium ion energy storage batteries prepared in Example 2 and Comparative Example 1 were subjected to a cycle performance test and then subjected to a battery impedance test after three cycles. Figure 5 As shown, the battery impedance test was performed after 200 cycles. Figure 6 Shown (6) The positive electrode sheets of the lithium-ion energy storage batteries prepared in Example 2 and Comparative Example 1 after 200 cycles of the cycle performance test were imaged using transmission electron microscopy (TEM) and scanning electron microscopy (SEM). Figure 7 shown.
[0048] (7) ICP (inductively coupled plasma mass spectrometry) test was performed on the negative electrode surface of the lithium-ion energy storage battery of Example 2 and Comparative Example 1 after 200 cycles. The test results are as follows: Figure 8 shown.
[0049] (8) The high-voltage lithium-ion battery electrolytes obtained in the preparation process of Example 2 and Comparative Example 1 were made into lithium-lithium symmetrical batteries, and then -2 Cycling under current density of Fig. 9 shown.
[0050] (9) Using DFT to analyze the Ni 2+ 、Ni 4+ , Mn 4+ The binding energy of each component in the electrolyte is calculated, and the calculation results are shown in Table 2.
[0051] Table 2: DFT binding energy calculation results
[0052] Results Analysis The following is a combination of Table 1-2 and Figure 1-9 The experimental data provided are used to explain this application in detail.
[0053] From the capacity retention rate of the lithium-ion energy storage battery in Examples 1-5 after 200 cycles, it can be seen that the lithium-ion energy storage battery with 0.2 wt.% BTTS exhibits the best capacity retention rate under the condition of charge and discharge cut-off voltage of 3.0-4.5 V, reaching 81.3%, that is, the service life of the lithium-ion energy storage battery when the working voltage is above 4.3 V is improved. When the BTTS concentration is 0.1wt.%, the capacity retention rate is lower than that of the lithium-ion energy storage battery containing 0.2 wt.% BTTS, which is only 76.3%. The analysis is that the interface film formed by BTTS is not enough to completely cover the surface of the material; and when the BTTS concentration is 0.3 wt.%, the capacity retention rate after long cycles is 80.7%, which is slightly less than the capacity retention rate of the lithium-ion energy storage battery with 0.2 wt.% BTTS. The analysis is that the increase in BTTS concentration will slightly increase the impedance of the battery and reduce the first cycle efficiency.
[0054] It can be seen from Example 2 and Comparative Example 1, Example 4 and Comparative Example 3, and Example 5 and Comparative Example 4 that the high-voltage lithium-ion battery electrolyte with the addition of BTTS increases the capacity retention rate of the lithium-ion energy storage battery prepared using NCM622 as the positive electrode active material from 52.5% to 81.3%, the high-voltage lithium-ion battery electrolyte with the addition of BTTS increases the capacity retention rate of the lithium-ion energy storage battery prepared using NCM811 as the positive electrode active material from 57.6% to 71.0%, and the high-voltage lithium-ion battery electrolyte with the addition of BTTS increases the capacity retention rate of the lithium-ion energy storage battery prepared using LCO as the positive electrode active material from 44.5% to 53.3%. Therefore, the high-voltage lithium-ion battery electrolyte with the addition of BTTS has a synergistic effect in improving the capacity retention rate of the lithium-ion energy storage battery prepared using NCM622 as the positive electrode active material.
[0055] Referring to Comparative Examples 1-2 and Example 2, it can be seen that the capacity retention rate of the lithium-ion energy storage battery prepared by combining the high-voltage lithium-ion battery electrolyte with tri-thiophene boronic acid with NCM622 as the positive electrode active material is not only much lower than the capacity retention rate of the high-voltage lithium-ion battery electrolyte with BTTS added and the lithium-ion energy storage battery prepared by using NCM622 as the positive electrode active material, but even lower than the capacity retention rate of the basic electrolyte and the lithium-ion energy storage battery prepared by using NCM622 as the positive electrode active material. It further illustrates that the high-voltage lithium-ion battery electrolyte with BTTS added has a synergistic effect in improving the capacity retention rate of the lithium-ion energy storage battery prepared by using NCM622 as the positive electrode active material.
[0056] And if Figure 1As shown, it can be seen that the lithium-ion energy storage battery in Comparative Example 1 has obvious capacity decay, and the capacity retention rate after 200 cycles is only 52.5% of the initial capacity. However, the lithium-ion energy storage battery in Example 2 still has a capacity retention rate of 81.3% after 200 cycles, indicating that the use of high-voltage lithium-ion battery electrolyte with added bis(trimethylsilyl) sulfate can significantly improve the cycle stability of lithium-ion energy storage batteries.
[0057] Referring to Example 2 and Comparative Example 1, Figure 2-Figure 7 , of which Figure 2 and Figure 3 Compared with the lithium ion energy storage battery of comparative example 1, when the lithium ion energy storage battery of embodiment 2 is subjected to cyclic voltammetry scanning, it can be clearly observed that the battery has an oxidation current in advance between 3.4 V and 3.65 V. Figure 3 The results in also confirm this point. The theoretical calculation results of HOMO and LUMO show that BTTS undergoes oxidation reaction preferentially over other components in high-voltage lithium-ion battery electrolyte. Figure 4 It can be seen that at a high rate of 7.0 C and above, the battery capacity of Example 2 with BTTS added as the high-voltage lithium-ion battery electrolyte component is better than that of the lithium-ion energy storage battery in Comparative Example 1. This phenomenon is particularly obvious at a high rate of 15 C. The battery capacity of the lithium-ion energy storage battery in Comparative Example 1 can only exert 53.5% of the initial capacity, while the lithium-ion energy storage battery in Example 2 can exert 75.1% of the initial capacity. Figure 5 and Figure 6 , the impedance of the lithium-ion energy storage battery in Example 2 is significantly smaller than that of the lithium-ion energy storage battery in Comparative Example 1, which proves that the addition of BTTS in the electrolyte of the high-voltage lithium-ion battery is beneficial to the capacity of the lithium-ion energy storage battery at a high rate. The analysis shows that this is due to the participation of BTTS in the construction of the interface film. After 200 cycles, the impedance of the lithium-ion energy storage battery in Example 2 increased slightly. This is due to the fact that the interface film formed by BTTS during the initial activation process is more uniform, which better inhibits the decomposition of other components in the electrolyte of the high-voltage lithium-ion battery. In contrast, in Comparative Example 1, as the number of cycles increases, the membrane impedance and charge transfer impedance of the lithium-ion energy storage battery increase sharply, resulting in a significant reduction in the cycle performance of the battery. Refer to Figure 7, through the results of TEM, it was found that the thickness of the interface film formed by the lithium-ion energy storage battery of Comparative Example 1 after cycling was distributed in the range of 5 to 26 nm, with low uniformity. However, the thickness of the interface film formed by the lithium-ion energy storage battery of Example 2 after cycling was around 6.5 nm, indicating that the interface film formed with the participation of BTTS was thinner and more uniform, reducing the impedance of the battery. The test results of SEM were consistent with the results of TEM, and after the lithium-ion energy storage battery of Comparative Example 1 was cycled 200 times, cracks appeared on the surface of the bulk particles of the positive electrode sheet, indicating that the positive electrode sheet was severely damaged during the long cycle. In contrast, after the lithium-ion energy storage battery of Example 2 was cycled 200 times, the appearance of the positive electrode sheet remained intact, and there was no obvious change compared to the fresh electrode sheet (the positive electrode sheet of the lithium-ion energy storage battery of Example 2 before 200 cycles). Figure 8 The ICP results further verified the stability of the interfacial film formed by the additive. By comparison, it was found that 0.2 wt.% BTTS can significantly inhibit the dissolution of transition metals in the positive electrode active material, thereby improving the capacity retention rate of lithium-ion energy storage batteries after long cycles.
[0058] Reference Fig. 9 The high-voltage lithium-ion battery electrolytes obtained in the preparation processes of Example 2 and Comparative Example 1 were made into lithium-lithium symmetrical batteries, and then cycled at a current density of 1 mAcm-2 respectively. The lithium-ion energy storage battery of Example 2 using the high-voltage lithium-ion battery electrolyte added with 0.2 wt.% BTTS, compared with the lithium-ion energy storage battery of Comparative Example 1 using the basic electrolyte without adding BTTS, the cycle time of the lithium-lithium symmetrical battery was increased from 120 h to 325 h, indicating that the high-voltage lithium-ion battery electrolyte added with 0.2 wt.% BTTS can improve the cycle stability of the lithium-ion energy storage battery using lithium metal as the negative electrode. Analysis shows that the high-voltage lithium-ion battery electrolyte added with 0.2 wt.% BTTS reduces the polarization of lithium metal and inhibits the formation of lithium dendrites.
[0059] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.
Claims
1. A high voltage lithium ion battery electrolyte, characterized in that: The invention comprises an electrolyte lithium salt, an organic solvent and a silane sulfate, wherein the amount of the silane sulfate is 0.1-0.3% of the total mass of the electrolyte lithium salt and the organic solvent.
2. The high voltage lithium ion battery electrolyte according to claim 1, characterized in that: The silane sulfate is bis(trimethylsilyl) sulfate.
3. The high voltage lithium ion battery electrolyte according to claim 1, characterized in that: The organic solvent comprises cyclic carbonate and linear carbonate in a weight ratio of 1:1-3.
4. The high-voltage lithium-ion battery electrolyte according to claim 3, characterized in that: The cyclic carbonates include one or more of ethylene carbonate, propylene carbonate, butylene carbonate, butyrolactone and valerolactone; the linear carbonates include one or more of dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, ethyl acetate, butyl acetate, methyl propionate, ethyl propionate and propyl propionate.
5. The high-voltage lithium-ion battery electrolyte according to claim 4, characterized in that: The linear carbonate comprises ethyl methyl carbonate and diethyl carbonate in a weight ratio of 5:1-3.
6. The high voltage lithium ion battery electrolyte according to claim 1, characterized in that: The electrolyte lithium salt includes one or more of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium perchlorate, lithium bis(trifluoromethylsulfonyl)imide, lithium trifluoromethylsulfonate, lithium difluorooxalatoborate, lithium dioxalatoborate and lithium difluorooxalatoborate.
7. A method for preparing a high voltage lithium ion battery electrolyte according to any one of claims 1 to 6, characterized in that: The following steps are involved: The electrolyte lithium salt is added into an organic solvent to be dissolved to obtain a raw electrolyte solution, and the silyl sulfate is added into the raw electrolyte solution to be dissolved to obtain the high-voltage lithium-ion battery electrolyte solution.
8. The method for preparing a high-voltage lithium-ion battery electrolyte according to claim 7, characterized in that: The organic solvent is prepared by mixing cyclic carbonate and linear carbonate in proportion and purifying the mixture by removing impurities and water.
9. A lithium-ion energy storage battery, characterized in that: The invention comprises a positive electrode, a negative electrode, a separator and a high-voltage lithium-ion battery electrolyte as claimed in any one of claims 1 to 6.
10. A lithium-ion energy storage battery according to claim 9, characterized in that: The positive electrode includes one or more of NCM811, NCM622, LCO and LNMO as positive electrode active materials.
Citation Information
Patent Citations
Electrolyte and lithium ion battery
CN107293776A
Electrolyte and lithium ion battery
CN107293783A
Ternary lithium ion battery electrolyte and lithium ion battery containing same
CN109873204A
Non-aqueous electrolyte solution and secondary battery
CN117321824A
Cited By
Electrolyte and lithium ion battery
CN119725752A
Electrolyte and lithium ion battery
CN119725752B
Electrolyte and silicon carbon battery
CN119764339A