Electrolyte of local high-concentration ionic liquid, preparation method of electrolyte and assembled high-voltage zinc tellurium battery

By using local high-concentration ionic liquid electrolyte in zinc-tellurium batteries and utilizing ZnBr42-activated positive valence conversion of tellurium, the problems of shuttle effect and slow conversion reaction kinetics of zinc-ion batteries in aqueous systems are solved, significantly improving the performance of the battery. The rate performance and energy output achieve an increase in the discharge capacity of the high-voltage platform.

CN118738599AActive Publication Date: 2024-10-01GUANGDONG UNIV OF TECH

Patent Information

Application Number
CN202411063672.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-05
Publication Date
2024-10-01
Estimated Expiration
2044-08-05

AI Technical Summary

Technical Problem

Existing zinc-ion batteries have shuttle effect, hydrogen evolution, corrosion and dendrite growth problems in the water system, resulting in shortened cycle life. The conversion reaction kinetics of the tellurium cathode is slow, low energy efficiency, and cannot meet the demand for high energy density energy storage.

Method used

Using a local high-concentration ionic liquid electrolyte, ZnBr42- species activates the positive valence conversion of tellurium, combines zinc bromide and zinc fluoride, and adds organic co-solvents to form an electrolyte with high ionic conductivity and stimulate the Te0/Te4+ redox couple. , improve the high voltage platform and energy output of zinc tellurium batteries.

Benefits of technology

It significantly improves the rate performance and energy efficiency of zinc tellurium batteries, extends the cycle life, improves the energy output and electrochemical performance of the tellurium cathode, and achieves a significant increase in the discharge capacity of the high-voltage platform.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118738599A_ABST
    Figure CN118738599A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of batteries, and discloses an electrolyte of local high-concentration ionic liquid, a preparation method of the electrolyte and an assembled high-voltage zinc tellurium battery. The electrolyte comprises an ionic liquid, zinc bromide, zinc fluoride and an organic cosolvent, the ionic liquid is one or more of 1-vinyl-3-butylimidazolium bromide, 1-ethyl-3-methylimidazolium bromide, 1-propyl-3-methylimidazolium bromide, and 1-butyl-3-methylimidazolium bromide, and the ionic liquid is one or more of 1-vinyl-3-butylimidazolium bromide, 1-ethyl-3-methylimidazolium bromide, 1-propyl-3-methylimidazolium bromide and 1-butyl-3-methylimidazolium bromide. The local high-concentration ionic liquid electrolyte contains an active species ZnBr4 < 2->, so that positive valence conversion of tellurium can be activated, and the effect of exciting and stabilizing Te0 / Te4 < + > redox pairs is achieved. The zinc-tellurium battery assembled by the zinc-tellurium battery material can realize Te < 4 + > / Te and Te / Te < 2-> two-step conversion reaction of a tellurium positive electrode, the energy output of the battery is improved, the high-voltage discharge platform capacity ratio of the zinc-tellurium battery is improved to 80.6%, and meanwhile, the rate capability of the zinc-tellurium battery is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of electrolytes, and more specifically, relates to an electrolyte with a locally high concentration of ionic liquid, a preparation method thereof, and an assembled high-voltage zinc-tellurium battery. Background Art

[0002] Rechargeable batteries, as highly efficient devices with high power and energy density, play an indispensable role in a variety of applications, including renewable energy, uninterruptible power supply systems, electric transportation, and smart grids. Zinc-ion batteries, a newly emerging class of rechargeable energy storage devices, offer advantages such as low cost, high safety, and high performance, and hold great potential for large-scale energy storage.

[0003] At present, the development of high-energy-density conversion-type cathode materials with multiple electron transfer is an important idea to make up for the energy density shortcomings of zinc-ion batteries. However, the current aqueous zinc batteries based on chalcogenide (sulfur, selenium, tellurium and their compounds) conversion-type cathode materials generally have a serious "shuttle effect", which leads to a rapid loss of effective active materials in the cathode and rapid performance degradation, which cannot meet the energy storage needs. In addition, in conventional aqueous electrolytes, the zinc anode has serious problems such as hydrogen evolution, corrosion, and dendrite growth, which greatly shortens the cycle life of the conversion-type zinc-ion battery. These problems further limit the development of zinc-ion batteries.

[0004] As a conversion cathode, tellurium has rich variable valence states and high specific capacity, and has good application prospects in high energy density zinc batteries. Because tellurium has a large atomic radius (140pm), the chain structure presented by tellurium has a relatively low surface negative charge density, which enables tellurium to achieve positive valence reversible conversion under specific electrochemical conditions. However, in traditional Te 0 / Te 4+ The reaction kinetics are slow and the positive conversion is incomplete, resulting in low voltage and specific capacity for the tellurium multi-step reaction, further reducing the energy efficiency of the tellurium conversion. Therefore, the development of electrolytes that can increase the tellurium positive reaction voltage and have high ionic conductivity is particularly critical. Summary of the Invention

[0005] In order to solve the above-mentioned deficiencies and shortcomings of the prior art, the primary purpose of the present invention is to provide an electrolyte with a local high concentration of ionic liquid, which is obtained by ZnBr4 2- Species activation of tellurium positive conversion, ZnBr4 2- To stimulate and stabilize Te 0 / Te 4+ The effect of the redox pair enables the zinc-telluride battery to have a higher high-voltage platform discharge capacity, greatly improving the energy output of the tellurium battery positive electrode, thereby improving the rate performance of the zinc-telluride battery.

[0006] Another object of the present invention is to provide a method for preparing the above-mentioned locally high-concentration ionic liquid electrolyte.

[0007] Another object of the present invention is to provide a high voltage zinc-telluride battery assembled with the electrolyte of the local high concentration ionic liquid, wherein the positive electrode generates Te 2- / Te / Te 4+ reversible electrochemical reaction.

[0008] The purpose of the present invention is achieved through the following technical solutions:

[0009] A locally high-concentration ionic liquid electrolyte comprises an ionic liquid, zinc bromide, zinc fluoride, and an organic cosolvent; the ionic liquid is one or more of 1-vinyl-3-butylimidazolium bromide, 1-ethyl-3-methylimidazolium bromide, 1-propyl-3-methylimidazolium bromide, or 1-butyl-3-methylimidazolium bromide.

[0010] Preferably, the organic co-solvent is one or more of dichloromethane, dichloroethane, dichloropropane, chloroform, fluorobenzene, toluene or p-xylene.

[0011] Preferably, the molar ratio of the ionic liquid, zinc bromide, zinc fluoride and organic co-solvent is 1:(1-1.8):(0.05-0.1):(0.1-0.5).

[0012] The method for preparing the electrolyte of the locally high-concentration ionic liquid comprises the following specific steps:

[0013] S1. Under protective gas, the ionic liquid and zinc bromide were mixed and stirred at 80 to 120 ° C to obtain an ionic liquid precursor;

[0014] S2. Under protective gas, zinc fluoride was added to the ionic liquid precursor, and stirred at 90 to 120 ° C to obtain an ionic liquid electrolyte;

[0015] S3. Under protective gas, an organic co-solvent is added to the ionic liquid electrolyte and stirred at room temperature to prepare an electrolyte with a locally high concentration of ionic liquid.

[0016] Preferably, the protective gases in steps S1-S3 are nitrogen, argon or helium.

[0017] Preferably, the stirring time in step S1 is 8 to 12 hours, the stirring time in step S2 is 10 to 12 hours, and the stirring time in step S3 is 1 to 5 hours.

[0018] A zinc-tellurium battery for high voltage comprises a positive electrode, a negative electrode, a separator and an electrolyte of the locally high-concentration ionic liquid.

[0019] Preferably, the positive electrode is an ordered mesoporous carbon-encapsulated tellurium composite material, the negative electrode is a zinc sheet, and the separator is glass fiber.

[0020] More preferably, the ordered mesoporous carbon-encapsulated tellurium composite material comprises mesoporous carbon and a single tellurium element supported thereon.

[0021] Compared with the existing technology, the above technical solution has the following beneficial effects:

[0022] 1. The local high concentration ionic liquid electrolyte of the present invention is formed by adding an organic co-solvent to the ionic liquid electrolyte, which contains ionic liquid, Zn 2+ 、F-、Br - and organic co-solvents, compared with conventional ionic liquid electrolytes (<1mS cm -1 ) has a high ionic conductivity (2.14 mS cm -1 ), which helps to further improve Te 0 / Te 4+ The reaction activity of zinc-telluride batteries can be increased, and the rate performance of zinc-telluride batteries can be improved significantly, thereby improving their electrochemical performance.

[0023] 2. Active species ZnBr4 in the electrolyte of the present invention 2- It can activate the positive conversion of tellurium, stimulate and stabilize Te 0 / Te 4+ The effect of redox couple enables zinc-telluride batteries to have a higher voltage platform (greater than (1.2V) and discharge capacity, greatly improving the energy output of the tellurium positive electrode.

[0024] 3. By optimizing the ratio of ionic liquid, zinc bromide, zinc fluoride and organic co-solvent in the electrolyte, the present invention increases the high-voltage discharge platform capacity of the zinc-telluride battery to 80.6%, thereby improving the energy efficiency and rate performance of the zinc-telluride battery. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 Raman spectra of the electrolytes prepared in Example 1 and Comparative Examples 1-3;

[0026] Figure 2 Graphs showing ionic conductivity and viscosity of the electrolytes prepared in Example 1 and Comparative Examples 1-3;

[0027] Figure 3 Cyclic voltammetry curves of zinc-telluride batteries assembled in Application Example 1 and Comparative Example 1;

[0028] Figure 4 The constant current charge and discharge curves of the zinc-telluride batteries assembled in Application Example 1 and Comparative Example 1 are shown;

[0029] Figure 5The charge and discharge curves and corresponding in-situ Raman spectra of the in-situ zinc-telluride battery assembled for Application Example 1;

[0030] Figure 6 This is a constant current charge and discharge curve of the zinc-telluride battery assembled in Application Example 2;

[0031] Figure 7 This is a constant current charge and discharge curve of the zinc-telluride battery assembled in Application Example 3;

[0032] Figure 8 Cyclic voltammograms of zinc-telluride batteries assembled in Comparative Examples 2 and 3;

[0033] Figure 9 The constant current charge and discharge curves of the zinc-telluride batteries assembled in Application Example 1 and Comparative Example 3 are shown;

[0034] Figure 10 This is a rate performance diagram of the zinc-telluride battery assembled in Application Example 1 and Comparative Example 3. DETAILED DESCRIPTION

[0035] The following will be combined with the accompanying drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. The embodiments described herein are only used to illustrate and explain the present invention and should not be understood as limiting the present invention. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative efforts are within the scope of protection of the present invention.

[0036] Example 1

[0037] 1. Under argon protection, 1-vinyl-3-butylimidazolium bromide (VBIMBr) and zinc bromide with a molar ratio of 1:1.2, which had been pre-treated by vacuum drying, were placed in a slurry bottle and slowly stirred at 100°C for 12 hours to prepare an ionic liquid precursor.

[0038] 2. Under argon protection, zinc fluoride at a molar ratio of 0.05:1 was added to the ionic liquid precursor and slowly stirred at 110°C for 12 hours to prepare an ionic liquid electrolyte;

[0039] 3. Under argon protection, dichloroethane with a molar ratio of 0.35:1 was added to the ionic liquid electrolyte and slowly stirred at room temperature for 4 hours to prepare a locally high-concentration ionic liquid electrolyte.

[0040] Example 2

[0041] 1. Under helium protection, 1-vinyl-3-butylimidazolium bromide (VBIMBr) and zinc bromide with a molar ratio of 1:1 and pre-treated by vacuum drying were placed in a slurry bottle and slowly stirred at 110°C for 12 hours to prepare an ionic liquid precursor.

[0042] 2. Under helium protection, zinc fluoride at a molar ratio of 0.1:1 was added to the ionic liquid precursor and slowly stirred at 110°C for 12 hours to prepare an ionic liquid electrolyte;

[0043] 3. Under helium protection, dichloromethane with a molar ratio of 0.1:1 was added to the ionic liquid electrolyte and slowly stirred at room temperature for 4 hours to prepare a locally high-concentration ionic liquid electrolyte.

[0044] Example 3

[0045] 1. Under nitrogen protection, 1-vinyl-3-butylimidazolium bromide (VBIMBr) and zinc bromide with a molar ratio of 1:1.5, which had been pre-treated by vacuum drying, were placed in a slurry bottle and slowly stirred at 120°C for 12 hours to prepare an ionic liquid precursor.

[0046] 2. Under nitrogen protection, zinc fluoride at a molar ratio of 0.05:1 was added to the ionic liquid precursor and slowly stirred at 110°C for 12 hours to prepare an ionic liquid electrolyte;

[0047] 3. Under nitrogen protection, dichloropropane with a molar ratio of 0.5:1 was added to the ionic liquid electrolyte and slowly stirred at room temperature for 4 hours to prepare a locally high-concentration ionic liquid electrolyte.

[0048] Comparative Example 1

[0049] 1. Under argon protection, 1-vinyl-3-butylimidazolium bromide (VBIMBr) and zinc bromide with a molar ratio of 1:1.2, which had been pre-treated by vacuum drying, were placed in a slurry bottle and slowly stirred at 100°C for 12 hours to prepare an ionic liquid precursor.

[0050] 2. Under argon protection, zinc fluoride with a molar ratio of 0.05:1 was added to the ionic liquid precursor and slowly stirred at 110°C for 12 hours to prepare an ionic liquid electrolyte.

[0051] Under argon protection, Te@CMK-3, SuperP and PVDF with a mass ratio of 8:1:1 were coated on a titanium mesh to produce a Te@CMK-3 electrode. Under helium protection, the ionic liquid electrolyte obtained in Comparative Example 1 was used as the electrolyte, the Te@CMK-3 electrode was used as the cathode, and a zinc sheet was used as the anode to assemble a zinc tellurium battery, abbreviated as VB-Br / F.

[0052] Comparative Example 2

[0053] The difference from Comparative Example 1 is that the zinc salt in step 1 is zinc chloride, and the remaining steps are the same to assemble a zinc tellurium battery, abbreviated as VB-Cl / F.

[0054] Comparative Example 3

[0055] The difference from Example 1 is that the zinc salt in step 1 is zinc chloride, and the remaining steps are the same, and a zinc tellurium battery is assembled, which is abbreviated as VB-Cl / F-EDC.

[0056] Figure 1 The Raman spectra of the electrolytes prepared in Example 1 and Comparative Examples 1-3 are shown. Figure 1 It can be seen that Example 1 and Comparative Example 1 provide active species ZnBr4 2- , while Comparative Examples 2-3 provide ZnCl4 2- , due to the active species ZnBr4 2- Activate Te 0 / Te 4+ The redox couple is more effective than ZnCl4 2- Therefore, the high voltage discharge capacity ratios of Example 1 and Comparative Example 1 are higher than those of Comparative Examples 2-3. Figure 2 The ionic conductivity and viscosity of the electrolytes prepared in Example 1 and Comparative Examples 1-3 are shown in FIG. Figure 2 It can be seen that Example 1 has the highest ionic conductivity and the lowest viscosity, indicating that the addition of organic co-solvents ethylene dichloride (EDC), zinc bromide and zinc fluoride improves the ionic conductivity of the electrolyte and reduces its viscosity.

[0057] Application Example 1

[0058] 1. CMK-3 and Te powder in a mass ratio of 1:2 were mixed in isopropanol by wet ball milling at 400 r / min for 10 h. After the isopropanol was evaporated in air at 60°C, the tube was vacuum sealed at a pressure of 10 MPa and then heat-treated in a sealed quartz tube at 600°C for 10 h with argon filling to obtain Te@CMK-3 composite material.

[0059] 2. Under argon protection, ordered mesoporous carbon encapsulated tellurium composite (Te@CMK-3), SuperP and PVDF with a mass ratio of 8:1:1 were coated on a titanium mesh to produce a Te@CMK-3 electrode;

[0060] 3. Under argon protection, a zinc-tellurium battery (VB-Br / F-EDC) was assembled using the locally high-concentration ionic liquid obtained in Example 1 as the electrolyte, a Te@CMK-3 electrode as the cathode, and a zinc sheet as the anode.

[0061] Figure 3 The cyclic voltammetry curves of the zinc-telluride battery assembled in Application Example 1 and Comparative Example 1 are shown. Figure 3 It can be seen that at 0.2mVs -1 The zinc-telluride battery of Application Example 1 below exhibits a larger response current. Figure 4 The constant current charge and discharge curves of the zinc-telluride battery assembled in Application Example 1 and Comparative Example 1 are shown. Figure 4 It can be seen that at 0.1Ag -1The discharge capacity of the zinc-telluride battery in Application Example 1 can reach 667 mAh g -1 , the proportion of high-voltage platform discharge increased to 80.6%. Figure 5 The charge and discharge curves and corresponding in-situ Raman spectra of the in-situ zinc-telluride battery assembled in Application Example 1. Figure 5 It can be seen that when the zinc-tellurium battery assembled in Application Example 1 is charged and discharged, Te 4+ / Te and Te / Te 2- Two-step transformation reaction.

[0062] Application Example 2

[0063] 1. Under helium protection, Te@CMK-3, SuperP and PVDF with a mass ratio of 8:1:1 were coated on a titanium mesh to produce a Te@CMK-3 electrode;

[0064] 2. Under helium protection, a zinc-tellurium battery was assembled using the locally high-concentration ionic liquid electrolyte obtained in Example 2 as the electrolyte, a Te@CMK-3 electrode as the cathode, and a zinc sheet as the anode.

[0065] Figure 6 This is the constant current charge and discharge curve of the zinc-telluride battery assembled in Application Example 2. Figure 6 It can be seen that at 0.2mV s -1 The zinc-telluride battery in Application Example 2 below has a capacity of 358 mAh g -1 Of the discharge capacity, high voltage platform discharge accounts for 70.9%.

[0066] Application Example 3

[0067] 1. Under nitrogen protection, Te@CMK-3, SuperP and PVDF with a mass ratio of 8:1:1 were coated on a titanium mesh to produce a Te@CMK-3 electrode;

[0068] 2. Under nitrogen protection, a zinc-tellurium battery was assembled using the locally high-concentration ionic liquid electrolyte obtained in Example 3 as the electrolyte, a Te@CMK-3 electrode as the cathode, and a zinc sheet as the anode.

[0069] Figure 7 This is the constant current charge and discharge curve of the zinc-telluride battery assembled in Application Example 3. Figure 7 It can be seen that at 0.2mV s -1 The zinc-telluride battery in Application Example 3 below has a capacity of 562 mAh g -1 Of the discharge capacity, high voltage platform discharge accounts for 80.3%. Figure 8 The cyclic voltammetry curves of the zinc-telluride batteries assembled in Comparative Examples 2 and 3 are shown. Figure 8 It can be seen that at 0.2mV s -1 The zinc-tellurium battery of Comparative Example 3 shows a larger response current. Figure 9 The constant current charge and discharge curves of the zinc-telluride battery assembled in Application Example 1 and Comparative Example 3 are shown. Figure 9 It can be seen that at 0.1Ag -1 Application Example 1 exhibits a higher discharge capacity at a current density of , and the high voltage discharge platform of Application Example 1 accounts for as high as 80.6%, which is much higher than 56.4% of Comparative Example 3. Figure 10 The figure shows the rate performance of the zinc-telluride battery assembled in Application Example 1 and Comparative Example 3. Figure 10 It can be seen that the rate performance of application example 1 is better than that of comparative example 3, and the rate performance of application example 1 is better than that of comparative example 3 at 0.2, 0.5, 0.7, 1.0, 2.0 and 5.0Ag. -1 At current densities of 1, 2, 3, 4, 5, 7, 10, and 10 mAh g, respectively. -1 The excellent rate performance of the zinc-telluride battery assembled in Application Example 1 reflects its faster kinetic performance.

[0070] The above embodiments are preferred implementations of the present invention, but the implementations of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations and simplifications that do not deviate from the spirit and principles of the present invention should be considered as equivalent replacement methods and are included in the scope of protection of the present invention.

Claims

1. An electrolyte with a local high concentration of ionic liquid, It is characterized in that The electrolyte comprises an ionic liquid, zinc bromide, zinc fluoride and an organic co-solvent; the ionic liquid is one or more of 1-vinyl-3-butylimidazolium bromide, 1-ethyl-3-methylimidazolium bromide, 1-propyl-3-methylimidazolium bromide or 1-butyl-3-methylimidazolium bromide.

2. The electrolyte of the locally high-concentration ionic liquid according to claim 1, It is characterized in that The organic co-solvent is one or more of dichloromethane, dichloroethane, dichloropropane, chloroform, fluorobenzene, toluene or p-xylene.

3. The electrolyte of the locally high-concentration ionic liquid according to claim 1, It is characterized in that The molar ratio of the ionic liquid, zinc bromide, zinc fluoride and organic co-solvent is 1:(1-1.8):(0.05-0.1):(0.1-0.5).

4. A method for preparing a locally high-concentration ionic liquid electrolyte according to any one of claims 1 to 3, It is characterized in that The specific steps include: S1. Under a protective gas, the ionic liquid and zinc bromide are mixed and stirred at 80 to 120 ° C to obtain an ionic liquid precursor; S2. Under protective gas, zinc fluoride is added to the ionic liquid precursor and stirred at 90 to 120 ° C to obtain an ionic liquid electrolyte; S3. Under protective gas, an organic co-solvent is added to the ionic liquid electrolyte, and stirred at room temperature to prepare a locally high-concentration ionic liquid electrolyte.

5. The method for preparing the electrolyte of the local high concentration ionic liquid according to claim 4, It is characterized in that The protective gas in steps S1-S3 is nitrogen, argon or helium.

6. The method for preparing the electrolyte of the local high concentration ionic liquid according to claim 4, It is characterized in that The stirring time in step S1 is 8 to 12 hours, the stirring time in step S2 is 10 to 12 hours, and the stirring time in step S3 is 1 to 5 hours.

7. A zinc-tellurium battery with high voltage, It is characterized in that The zinc-tellurium battery comprises a positive electrode, a negative electrode, a separator and an electrolyte of the locally high-concentration ionic liquid according to any one of claims 1 to 3.

8. The zinc-tellurium battery with high voltage according to claim 7, It is characterized in that The positive electrode is an ordered mesoporous carbon encapsulated tellurium composite material, the negative electrode is a zinc sheet, and the separator is glass fiber.

9. The zinc-tellurium battery with high voltage according to claim 7, It is characterized in that The ordered mesoporous carbon encapsulated tellurium composite material comprises mesoporous carbon and a single tellurium substance supported thereon.

Citation Information

Patent Citations

  • Zinc-based dual-ion battery and preparation method thereof

    CN108242560A

  • Zinc negative electrode with zinc ion conductivity interface modification layer, battery and preparation method

    CN111933912A

  • Shuttle-effect-free zinc-silicon battery based on conversion type positive electrode and preparation method thereof

    CN116936939A

  • Electrolyte for metal zinc secondary battery

    JP2023127391A

Cited By

  • Supramolecular ionic liquid gel electrolyte of solid-state zinc-iodine battery for high-voltage platform

    CN119400978A

  • Nanowire structure squaric acid tellurium zinc ion battery positive electrode material and preparation method and application thereof

    CN120757445A

  • A nanowire structured square tellurium-zinc ion battery positive electrode material, a preparation method and application thereof

    CN120757445B

  • Aqueous tellurium battery and preparation method thereof

    CN121790543A