Interface modifier, application thereof and electrochemical battery

By using a combination of interface modifiers of lithium salts and specific solvents in lithium-ion batteries, the interface impedance problem between the solid electrolyte and the electrode is solved, the lithium ion transport capacity and battery performance are improved, and the LGPS solid electrolyte and the metal are ensured The compatibility and stability of lithium anodes improve the performance of all-solid-state batteries.

CN118738601APending Publication Date: 2024-10-01ZHEJIANG GEELY HLDG GRP CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310311308.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-03-28
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

In existing lithium-ion batteries, the solid-solid interface impedance between the solid electrolyte and the electrode is high, resulting in limited transmission of lithium ions and limiting the performance of all-solid-state batteries, especially the gap between the LGPS solid electrolyte and the metallic lithium anode. The interface is incompatible and there are irreversible side reactions, which affects its large-scale application.

Method used

Use an interfacial modifier including lithium salts (such as lithium bistrifluoromethanesulfonimide and lithium bisfluorosulfonimide) and specific solvents (such as anisole, triethylene glycol dimethyl ether, cyclopentyl Methyl ether, etc.), the lithium salt is completely dissolved through magnetic stirring to form an interface modifier, and it is applied between the lithium metal anode and the solid sulfide electrolyte to improve the compatibility and stability of the interface.

Benefits of technology

Significantly improves the conductivity of lithium ions, reduces the contact resistance of the solid-solid interface, prevents side reactions, improves the performance and stability of all-solid-state batteries, makes the interface between the LGPS solid electrolyte and the metallic lithium anode more compatible, and extends the battery life service life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118738601A_ABST
    Figure CN118738601A_ABST
Patent Text Reader

Abstract

The invention provides an interface modifier and application thereof and an electrochemical battery, the interface modifier comprises a lithium salt and a solvent, the solvent is selected from any one or more of anisole (AN), triethylene glycol dimethyl ether (TGME), cyclopentyl methyl ether (CPME), tetrahydrofuran (THF), polyethylene glycol dimethyl methacrylate (PEGDMA) and 1, 3-dioxolane (DOL); the lithium salt is selected from any one or more of lithium bis (trifluoromethanesulfonyl) imide (LiTFSI) and lithium bis (fluorosulfonyl) imide (LiFSI). The interface modifier provided by the invention is simple in synthesis process and wide in application range, has relatively high lithium ion conductivity in the lithium ion battery, and can reduce the contact resistance of a solid-solid interface and prevent side reaction when a solid sulfide electrolyte is used, so that the performance of the all-solid-state battery is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to, but is not limited to, energy storage battery technology, and in particular to, but is not limited to, an interface modifier and its application and an electrochemical cell. Background Art

[0002] Among many energy storage systems, lithium-ion batteries are currently the most widely used secondary batteries, with many advantages such as high energy density, low self-discharge rate, high potential difference, and long cycle life. However, the energy density of lithium-ion batteries based on organic liquid electrolytes has reached its limit. In addition, traditional organic liquid electrolytes have safety hazards such as flammability and poor thermal stability, which seriously restrict the development of lithium-ion batteries.

[0003] All-solid-state lithium-ion batteries use highly safe and thermally stable solid electrolytes to replace traditional liquid electrolytes, effectively preventing safety issues such as thermal runaway. Moreover, the negative electrode can use metallic lithium with higher specific capacity, which effectively improves the energy density of the battery. Solid electrolytes are one of the most critical components in solid-state batteries. The most widely studied solid electrolytes are polymers, oxides, and sulfides. Sulfide electrolytes have high room temperature ionic conductivity. According to the crystal morphology, they can be divided into crystalline, glassy, ​​and glass-ceramic states. Li 10 GeP2S 12 (LGPS) is a new type of sulfide solid electrolyte with ionic conductivity comparable to that of liquid electrolytes, which has set off a new wave of research and development.

[0004] Although sulfide solid electrolytes with ionic conductivity close to or higher than that of liquid organic electrolytes have been developed, the solid-solid contact between the electrolyte and the electrode causes a high interfacial impedance, which seriously hinders the transmission of lithium ions and leads to the deterioration of the performance of all-solid-state batteries. Generally speaking, all-solid-state batteries mainly contain three types of solid / solid interfaces: (1) solid electrolyte / lithium negative electrode interface; (2) solid electrolyte / solid electrolyte interface; (3) positive electrode / solid electrolyte interface. In order to improve the interface problem, researchers have proposed many solutions. However, the existing interface modifier solutions still have limited effect on improving interface resistance and unsatisfactory results.

[0005] For the current LGPS solid electrolyte, it has high lithium ion conductivity, excellent thermal stability and electrochemical stability, and a simple synthesis process. However, its solid-solid interface problem is still one of the problems that hinder the large-scale application of LGPS solid electrolytes. Because LGPS is in direct contact with lithium metal, irreversible and continuous side reactions will occur at the interface, limiting its practical application. Adding a small amount of interface modifier between the lithium metal anode and the LGPS interface can enhance the lithium ion transmission capacity, reduce the interface impedance, and enhance the stability of the interface. However, the existing lithium metal interface modifiers have low conductivity and are incompatible with sulfide electrolytes. Therefore, it is necessary to develop interface modifiers between LGPS solid electrolyte materials and metal lithium anodes to improve the compatibility of the solid-solid interface. Summary of the invention

[0006] The following is a summary of the subject matter described in detail herein. This summary is not intended to limit the scope of the claims.

[0007] The present application provides an interface modifier, which includes a lithium salt and a solvent.

[0008] The solvent is selected from any one or more of anisole (AN), triethylene glycol dimethyl ether (TGME), cyclopentyl methyl ether (CPME), tetrahydrofuran (THF), polyethylene glycol dimethyl methacrylate (PEGDMA), and 1,3-dioxolane (DOL);

[0009] The lithium salt is selected from any one or more of lithium bis(trifluoromethanesulfonyl)imide (LiTFSI) and lithium bis(fluorosulfonyl)imide (LiFSI).

[0010] In one embodiment provided in the present application, the concentration of the lithium salt in the interface modifier is 1M to 4M.

[0011] On the other hand, the present application provides a method for preparing the above-mentioned interface modifier, the preparation method comprising: weighing a lithium salt in a glove box, adding the lithium salt to a certain amount of the solvent, and magnetically stirring until it is completely dissolved.

[0012] In yet another aspect, the present application provides an electrochemical cell, wherein the electrochemical cell comprises the above-mentioned interface modifier.

[0013] In one embodiment provided in the present application, the amount of the interface modifier between the negative electrode and the electrolyte of the electrochemical cell is 1 μL / cm 2 Up to 10 μL / cm 2 .

[0014] In one embodiment provided in the present application, the negative electrode of the electrochemical cell is a lithium metal negative electrode.

[0015] In one embodiment provided in the present application, the electrochemical cell is a lithium ion battery, and the positive electrode of the lithium ion battery is a ternary positive electrode material with a coating layer.

[0016] In one embodiment provided in the present application, the electrochemical cell is a solid-state lithium-ion battery.

[0017] In one embodiment provided in the present application, the electrolyte in the solid-state lithium-ion battery is a solid-state sulfide electrolyte; in one embodiment provided in the present application, the solid-state sulfide electrolyte is Li 10 GeP2S 12 (LGPS).

[0018] In another aspect, the present application provides the use of the above-mentioned interface modifier in a lithium-ion battery.

[0019] In one embodiment provided in the present application, the lithium ion battery is a solid-state lithium ion battery.

[0020] In one embodiment provided in the present application, the electrolyte in the solid-state lithium-ion battery is a solid-state sulfide electrolyte.

[0021] In one embodiment provided in the present application, the solid sulfide electrolyte is Li 10 GeP2S 12 (LGPS).

[0022] On the other hand, the present application provides a device, which includes a device housing, and a motor and / or a circuit board located inside the device housing. The device housing also includes a battery, which is electrically connected to the motor and / or the circuit board for powering the motor and / or the circuit board. The battery includes the above-mentioned secondary battery.

[0023] Beneficial effects of this application:

[0024] 1) The synthesis process is simple. The present application only requires weighing the lithium salt in a glove box, adding the lithium salt to a certain amount of solvent, and magnetically stirring until it is completely dissolved. When used, the interface modifier only needs to be added dropwise or applied to the interface between the solid sulfide electrolyte and the electrode by other acceptable methods in the art. The present application is quick and convenient to operate, without the need for additional complex steps and expensive instruments. The interface modifier provided in the present application directly acts on the interface between the solid-state battery electrolyte and the lithium-containing electrode, and the conductivity measured is significantly higher than similar interface modifier formulations in the prior art. The feasibility, efficiency and effect of the operation method of the present application are significantly improved.

[0025] 2) Higher lithium ion conductivity: The ion conductivity of the interface modifier at room temperature is higher than 1mS / cm.

[0026] 3) Wide application range: The interface modifier described in this application is applicable to LGPS solid electrolyte.

[0027] 4) Good effect. The interface modifier of the present application has high ionic conductivity, reduces the contact impedance of the solid-solid interface, and prevents the occurrence of side reactions, thereby improving the performance of the all-solid-state battery.

[0028] 5) The interface modifier of the present application has the advantages of being stable with LGPS and metallic lithium, and can improve the contact of the solid-solid interface on the negative electrode side, reduce the interface resistance, and improve the performance of the all-solid-state battery.

[0029] Other features and advantages of the present application will be described in the following description, and partly become apparent from the description, or be understood by implementing the present application. Other advantages of the present application can be invented and obtained by the schemes described in the description. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] The accompanying drawings are used to provide an understanding of the technical solution of the present application and constitute a part of the specification. Together with the embodiments of the present application, they are used to explain the technical solution of the present application and do not constitute a limitation on the technical solution of the present application.

[0031] Figure 1 It is the impedance statistics diagram of different interface modifiers.

[0032] Figure 2 The charge and discharge curves of the lithium symmetric mold battery of LGPS with an interface modifier (a) and without an interface modifier (b) in the application example. The interface modifier added is the 2M anisole solution of LiTFSI in Example 1.

[0033] Figure 3 It is a schematic diagram of LGPS mixed with an interfacial modifier (2M LiTFSI cyclopentyl methyl ether solution in Example 3) and immersed for 30 days. DETAILED DESCRIPTION

[0034] In order to make the purpose, technical solution and advantages of the present application more clear, the embodiments of the present application are described in detail below. It should be noted that the embodiments and features in the embodiments of the present application can be combined with each other arbitrarily without conflict.

[0035] Example 1

[0036] Prepare a lithium bis(trifluoromethanesulfonyl)imide (LiTFSI) anisole solution, weigh anisole, weigh LiTFSI in a glove box filled with argon (water <0.01ppm, oxygen <0.01ppm), then add anisole thereto, stir magnetically for 1h, so that the lithium salt LiTFSI is completely dissolved, and obtain the interface modifier, which is in liquid state and has good fluidity. Use an ion conductivity tester to measure the ionic conductivity of the interface modifier, as shown in Table 1.

[0037] Table 1: Electrical conductivity of the interfacial modifier of Example 1

[0038]

[0039] Example 2

[0040] Prepare LiTFSI triethylene glycol dimethyl ether solution, weigh triethylene glycol dimethyl ether, weigh LiTFSI in a glove box filled with argon (water <0.01ppm, oxygen <0.01ppm), then add triethylene glycol dimethyl ether, stir magnetically for 1h, so that the lithium salt LiTFSI is completely dissolved, and obtain the interface modifier, which is in liquid state and has good fluidity. Use an ion conductivity tester to measure the ionic conductivity of the interface modifier.

[0041] Table 2: Electrical conductivity of the interfacial modifier of Example 2

[0042]

[0043] Example 3

[0044] Prepare LiTFSI cyclopentyl methyl ether solution, weigh cyclopentyl methyl ether, weigh LiTFSI in a glove box filled with argon (water <0.01ppm, oxygen <0.01ppm), then add cyclopentyl methyl ether, stir magnetically for 1h, so that the lithium salt LiTFSI is completely dissolved, and obtain the interface modifier, which is in liquid state and has good fluidity. Use an ion conductivity tester to measure the ionic conductivity of the interface modifier.

[0045] Table 3: Electrical conductivity of the interfacial modifier of Example 3

[0046]

[0047] Example 4

[0048] Prepare a concentrated LiTFSI tetrahydrofuran solution, weigh tetrahydrofuran, weigh LiTFSI in a glove box filled with argon (water <0.01ppm, oxygen <0.01ppm), then add tetrahydrofuran, stir magnetically for 1h, so that the lithium salt LiTFSI is completely dissolved, and obtain the interface modifier, which is in liquid state and has good fluidity. Use an ion conductivity tester to measure the ionic conductivity of the interface modifier.

[0049] Table 4: Electrical conductivity of the interfacial modifier of Example 4

[0050]

[0051] Example 5

[0052] Prepare a 1,3-dioxolane solution with a concentration of LiTFSI, weigh 1,3-dioxolane, and weigh LiTFSI in a glove box filled with argon (water <0.01ppm, oxygen <0.01ppm), then add 1,3-dioxolane, and stir magnetically for 1h to dissolve all the lithium salt LiTFSI to obtain the interface modifier, which is in liquid state and has good fluidity. Use an ion conductivity tester to measure the ionic conductivity of the interface modifier.

[0053] Table 5: Conductivity of the interfacial modifier of Example 5

[0054]

[0055] Example 6

[0056] Prepare a polyethylene glycol dimethyl methacrylate (PEGDMA) solution with a concentration of LiTFSI, weigh polyethylene glycol dimethyl methacrylate (PEGDMA), weigh LiTFSI in a glove box filled with argon (water <0.01ppm, oxygen <0.01ppm), then add polyethylene glycol dimethyl methacrylate (PEGDMA) thereto, stir magnetically for 1h, and completely dissolve the lithium salt LiTFSI to obtain the interface modifier, which is in liquid state and has good fluidity. Use an ion conductivity tester to measure the ionic conductivity of the interface modifier.

[0057] Table 6: Conductivity of the interfacial modifier of Example 6

[0058]

[0059] Example 7

[0060] Prepare lithium bis(fluorosulfonyl)imide (LiFSI) anisole solution, weigh anisole, weigh LiFSI in a glove box filled with argon (water <0.01ppm, oxygen <0.01ppm), then add anisole, stir magnetically for 1h, so that the lithium salt LiFSI is completely dissolved, and obtain the interface modifier, which is in liquid state and has good fluidity. Use an ion conductivity tester to measure the ionic conductivity of the interface modifier, as shown in Table 7.

[0061] Table 7: Electrical conductivity of the interfacial modifier of Example 7

[0062]

[0063] Application Examples

[0064] Lithium symmetric batteries are usually used to evaluate the improvement of the battery interface after adding interface modifiers. Prepare lithium symmetric mold batteries. First, press the sulfide electrolyte sheet, with pure lithium sheets at both ends. The electrolyte is a solid electrolyte Li 10 GeP2S 12 (LGPS), the interface modifiers of Examples 1 to 7 were used between the solid electrolyte and the lithium sheet, and the dosage was 5 μL / cm 2 , and the corresponding lithium symmetric mold battery was prepared. High ionic conductivity was achieved, while reducing the contact impedance of the solid-solid interface and preventing the occurrence of side reactions.

[0065] Taking the 2M LiTFSI anisole solution in Example 1 as an example, Figure 2 As shown in Figure 2, the critical current density of the lithium symmetric battery without the addition of an interface modifier is 0.75 mA / cm 2 After adding the interface modifier, the critical current density of the lithium symmetric battery increased to 1 mA / cm 2 , the improvement effect is more obvious.

[0066] A lithium sheet immersion test was conducted. After 30 days of pure lithium sheet immersion test, the surface of the lithium sheet still maintained its metallic luster and was not dissolved.

[0067] Table 8: Weight comparison data of the interface modifier lithium sheets of Examples 1 to 7 before and after immersion

[0068] Example Before soaking (mg) After soaking (mg) Example 1: 2M LiTFSI in anisole solution 45.91 45.89 Example 2: 1M LiTFSI solution in triethylene glycol dimethyl ether 45.92 45.91 Example 3: 2M LiTFSI in cyclopentyl methyl ether solution 45.89 45.89 Example 4: 2M LiTFSI in tetrahydrofuran solution 45.94 45.93 Example 5: 2M LiTFSI in 1,3-dioxolane solution 45.90 45.90 Example 6: 3M LiTFSI in PEGDMA solution 45.91 45.90 Example 7: 2M LiFSI in anisole solution 45.89 45.88

[0069] from Figure 1 and Figure 2 It can be seen that the solid-state battery interface wetting agent stabilizes the interface with the sulfide solid electrolyte, improves the ionic conductivity between the solid-solid interface, reduces the solid-solid interface impedance, and thus improves the performance of the solid-state battery.

[0070] The interfacial modifier provided in the present application will not undergo significant changes in the solution after being mixed with the LGPS electrolyte. After the two are mixed, the chemical properties of the LGPS electrolyte are stable. Figure 3 This is a schematic diagram of LGPS mixed with the 2M LiTFSI cyclopentyl methyl ether solution in Example 3 and immersed for 30 days. From the figure, it can be seen that after the LGPS electrolyte and the interfacial modifier are mixed and left alone for 30 days, the supernatant of the mixed solution remains transparent and colorless, and no obvious color change is found. It can be seen that the LGPS electrolyte and the interfacial modifier have excellent chemical stability.

[0071] Comparative Example

[0072] The interface buffer layer contains an ester solvent formula such as polyvinyl carbonate, acrylate and its derivative oligomers, and the like, and is easily reacted with the chemically active sulfide solid electrolyte Li on the surface of the solid electrolyte and the lithium metal negative electrode in the same manner as in the embodiment application example. 10 GeP2S 12 (LGPS) will undergo interfacial reactions, affecting battery performance, stability and safety. In addition, other types of solvents such as water, ethers, alcohols and other polar solvents will also react with sulfide solid electrolytes to generate byproducts with low ionic conductivity, affecting ion transmission.

Claims

1. An interfacial modifier, characterized in that: The interface modifier is composed of a lithium salt and a solvent, and the solvent is selected from any one or more of anisole, triethylene glycol dimethyl ether, cyclopentyl methyl ether, tetrahydrofuran, polyethylene glycol dimethyl methacrylate and 1,3-dioxolane; The lithium salt is selected from lithium bis(trifluoromethanesulfonyl imide) or lithium bis(fluorosulfonyl imide).

2. The interface modifier according to claim 1, characterized in that The concentration of the lithium salt in the interface modifier is 1M to 4M.

3. An electrochemical cell, characterized in that: The electrochemical cell comprises the interface modifier according to claim 1 or 2.

4. The electrochemical cell according to claim 3, characterized in that The amount of the interfacial modifier between the negative electrode and the electrolyte of the electrochemical cell is 1 μL / cm 2 Up to 10 μL / cm 2 .

5. The electrochemical cell according to claim 3 or 4, characterized in that The negative electrode of the electrochemical cell is a negative electrode containing metallic lithium.

6. The electrochemical cell according to claim 3 or 4, characterized in that The electrochemical cell is a lithium ion battery, and the positive electrode of the lithium ion battery is a ternary positive electrode material with a coating layer.

7. The electrochemical cell according to claim 3 or 4, characterized in that The electrochemical cell is a solid-state lithium-ion battery.

8. The electrochemical cell according to claim 7, characterized in that The electrolyte in the solid-state lithium-ion battery is a solid-state sulfide electrolyte; optionally, the solid-state sulfide electrolyte is Li 10 GeP2S 12 (LGPS).

9. Use of the interface modifier according to claim 1 or 2 in a lithium ion battery, wherein the lithium ion battery is a solid-state lithium ion battery; wherein the electrolyte in the solid-state lithium ion battery is a solid-state sulfide electrolyte; wherein the solid-state sulfide electrolyte is Li 10 GeP2S 12 (LGPS).

10. A device, comprising a device housing, and a motor and / or a circuit board located inside the device housing, wherein the device housing also includes a battery, wherein the battery is electrically connected to the motor and / or the circuit board for supplying power to the motor and / or the circuit board, wherein: The battery comprises the electrochemical cell of any one of claims 3 to 8.