Polypropylene porous membrane and preparation method thereof, battery diaphragm and battery assembly

By using a polypropylene porous film in a lithium-ion battery separator, combined with a combination of homopolymer polypropylene and elastic modifiers, the problem of excessive tensile strength in the longitudinal direction of the separator is solved, the tear resistance is improved, and the electrical conductivity is reduced. core short circuit and cost, expanding the application scenarios.

CN118738760APending Publication Date: 2024-10-01SHENZHEN ZHONGXING NEW MATERIAL TECH CO LTD
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202410840990.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-26
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

The tensile strength of existing lithium-ion battery separators is too high in the longitudinal direction and low in the transverse direction. It is easy to tear under the action of external force in the thickness direction, resulting in short circuit of the battery cells and increased cost.

Method used

Using polypropylene porous membranes, the elasticity and tear resistance of the polypropylene porous membranes are improved by adding elastic modifiers, such as polyolefin elastomers, polyolefin plastomers, polyethylene oxide and polyethylene glycol, to homopolymer polypropylene. Properties, the preparation method includes blending, casting, annealing and stretching steps.

Benefits of technology

It significantly improves the tear resistance of the polypropylene porous film, reduces the rate of defective products in the battery cell manufacturing process, improves the battery cell manufacturing yield, and expands the application scenarios of lithium battery dry separators.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118738760A_ABST
    Figure CN118738760A_ABST
Patent Text Reader

Abstract

The invention discloses a polypropylene porous membrane and a preparation method thereof, a diaphragm for a battery and a battery component, the polypropylene porous membrane comprises homo-polypropylene and an elastic modifier, and the elastic modifier comprises one or more of a polyolefin elastomer, a polyolefin plastomer, polyoxyethylene, polyethylene glycol and co-polypropylene. By adding the elastic modifier, the elastic property and the strength property of the polypropylene porous membrane can be further enhanced on the basis of the original physical and chemical properties of the polypropylene porous membrane, and the external force tearing resistance of the diaphragm in the manufacturing process is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of lithium ion battery separators, and in particular to a polypropylene porous membrane and a preparation method thereof, a separator for a battery, and a battery assembly. Background Art

[0002] At present, lithium-ion power batteries widely use PP diaphragms prepared by dry single-drawing. However, since such diaphragms are made of highly isotactic homopolymer PP and are prepared by cast extrusion and longitudinal single-drawing, the tensile strength of the PP diaphragm in the MD direction (longitudinal) is too high and the TD (transverse) direction is relatively low. Therefore, when subjected to external forces in the thickness direction, it is easy to tear in the MD (longitudinal) direction. During the preparation of the battery cell, the PP diaphragm may tear, resulting in a high short-circuit rate of the lithium battery. Summary of the invention

[0003] The main purpose of the present invention is to provide a polypropylene porous membrane, aiming to improve the problem of membrane tearing.

[0004] To achieve the above objectives, the present invention provides a polypropylene porous membrane, wherein the material of the polypropylene porous membrane includes homopolymer polypropylene and an elastic modifier, wherein the elastic modifier includes one or more of polyolefin elastomers, polyolefin plastomers, polyethylene oxide, polyethylene glycol, and copolymer polypropylene.

[0005] In some embodiments, the weight average molecular weight of the elastic modifier is 1.5×10 3 ~8×10 4 .

[0006] In some embodiments, the homopolypropylene satisfies at least one of the following conditions:

[0007] (1) The isotacticity of the homopolypropylene is greater than or equal to 97;

[0008] (2) The melt index of the homopolymer polypropylene is 0.5 to 3 g / 10 min;

[0009] (3) The weight average molecular weight of the homopolymer polypropylene is 2×10 5 ~5×10 5 .

[0010] In some embodiments, the polypropylene porous membrane is a single-layer or double-layer structure;

[0011] Optionally, each of the layers independently comprises 80 to 95 parts of the homopolypropylene and 5 to 20 parts of the elastic modifier, based on weight percentage.

[0012] In some embodiments, the polypropylene porous membrane is a multilayer structure, including two surface layers and an intermediate layer sandwiched between the two surface layers;

[0013] Optionally, in terms of weight percentage, each of the surface layers independently comprises 80-95 parts of the homopolypropylene and 5-20 parts of the elastic modifier; the middle layer comprises 80-100 parts of the homopolypropylene and 0-20 parts of the elastic modifier.

[0014] The present invention also provides a battery separator, comprising the polypropylene porous membrane as described above.

[0015] The present invention further provides a battery assembly, comprising a positive electrode sheet, a negative electrode sheet and the battery separator as described above, wherein the battery separator is arranged between the positive electrode sheet and the negative electrode sheet.

[0016] The present invention also provides a method for preparing the polypropylene porous membrane as described above, comprising the following steps:

[0017] Blending: mixing the elastic modifier and the homopolypropylene to obtain a mixture;

[0018] Casting: the mixed material is melted and plasticized and then extruded, and the melt is cast to form a cast film;

[0019] Annealing: annealing the cast film to make the lamellae on the cast film regular;

[0020] Stretching: the annealed cast film is stretched to obtain the polypropylene porous film.

[0021] In some embodiments, the method for preparing the polypropylene porous membrane satisfies at least one of the conditions (1) to (4):

[0022] (1) The mixing time is 30 min to 60 min, and the mixing speed is 100 rpm to 600 rpm;

[0023] (2) The extrusion temperature is 180 to 250° C.;

[0024] (3) The casting temperature is 65 to 95° C.

[0025] (4) The annealing temperature is 135-148° C., and the annealing time is 10-15 hours.

[0026] In some embodiments, the stretching step includes cold drawing, hot drawing and heat setting, and the preparation method of the polypropylene porous membrane satisfies at least one of the conditions (1) to (3):

[0027] (1) In the cold drawing step, the stretching ratio is 1.2 to 1.8 and the temperature is 50 to 100° C.;

[0028] (2) in the step of heat drawing, the stretching ratio is 1.4 to 2.6 and the temperature is 145 to 155° C.;

[0029] (3) The temperature in the heat setting step is 150-160°C.

[0030] The technical solution of the present invention enhances the elasticity and strength properties of the polypropylene porous membrane and improves the external force tearing resistance of the polypropylene porous membrane in the manufacturing process by adding an elastic modifier to the raw materials for preparing the polypropylene porous membrane.

[0031] Since homopolymer polypropylene has a highly regular and symmetrical molecular structure, this regularity allows the molecular chains to be closely arranged and stacked to form a crystalline region. In the crystalline region, polymer molecules or chain segments are arranged in an orderly manner. This orderly arrangement increases the interaction forces between molecules, such as van der Waals forces, hydrogen bonds or dipole forces, thereby increasing the rigidity of the polypropylene porous membrane, causing the polypropylene porous membrane to easily break when subjected to force in the thickness direction. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the structures shown in these drawings without paying creative work.

[0033] Figure 1 is a schematic diagram of the pore morphology after the diaphragm is punctured in Example 1 of the present invention;

[0034] Figure 2 is a schematic diagram of the pore morphology after the diaphragm is punctured in Example 2 of the present invention;

[0035] Figure 3 is a schematic diagram of the pore morphology after the diaphragm is punctured in Example 3 of the present invention;

[0036] Figure 4 is a schematic diagram of the pore morphology after the diaphragm is punctured in Example 4 of the present invention;

[0037] Figure 5 is a schematic diagram of the pore morphology after the diaphragm is punctured in Example 5 of the present invention;

[0038] Figure 6 is a schematic diagram of the pore morphology after the diaphragm is punctured in Comparative Example 1 of the present invention;

[0039] Figure 7 is a schematic diagram of the pore morphology after the diaphragm is punctured in Comparative Example 2 of the present invention;

[0040] Figure 8 The present invention is a flow chart of the method for preparing the battery separator.

[0041] The realization of the purpose, functional features and advantages of the present invention will be further explained in conjunction with embodiments and with reference to the accompanying drawings. DETAILED DESCRIPTION

[0042] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0043] It should be noted that if the meaning of "and / or" appears in the full text is to include three parallel solutions, taking "A and / or B" as an example, it includes solution A, solution B, or a solution that satisfies both A and B. In addition, the technical solutions between the various embodiments can be combined with each other, but it must be based on the ability of ordinary technicians in the field to implement. When the combination of technical solutions is contradictory or cannot be implemented, it should be considered that such a combination of technical solutions does not exist and is not within the protection scope required by the present invention.

[0044] "Include", "comprising", "containing", "containing", "having" or other variations herein are intended to cover non-closed inclusions, and no distinction is made between these terms. The term "comprising" means that other steps and ingredients that do not affect the final result may be added. The term "comprising" also includes the terms "mainly consisting of..." and "essentially consisting of..." The compositions and methods / processes of the present invention include, consist of, and are essentially composed of the necessary elements and restrictions described herein and any additional or optional ingredients, components, steps or restrictions described herein. All numerical values ​​or expressions used in the specification and claims involving component amounts, process conditions, etc. should be understood to be modified by "about" in all cases. All ranges involving the same component or property include endpoints, which can be independently combined. Since these ranges are continuous, they include every numerical value between the minimum and maximum values. It should also be understood that any numerical range cited in this application is intended to include all sub-ranges within the range. As used herein, "parts by weight", "parts by weight", "parts by mass" or "parts by mass" are used interchangeably, and the parts by weight may be any fixed weight expressed in milligrams, grams or kilograms (such as 1 mg, 1 g, 2 g, 5 g, or 1 kg, etc.). For example, a composition consisting of 1 part by weight of component a and 9 parts by weight of component b may be a composition consisting of 1 gram of component a + 9 grams of component b, or 10 grams of component a + 90 grams of component b, etc.

[0045] The raw materials and equipment used in the present invention, unless otherwise specified, are all commonly used raw materials and equipment in the art; the methods used in the present invention, unless otherwise specified, are all conventional methods in the art. Unless otherwise specified, the meanings of the terms in this specification are the same as those generally understood by those skilled in the art, but in case of conflict, the definitions in this specification shall prevail.

[0046] In the related technology, high-specification homopolymer PP is used and prepared through cast extrusion and longitudinal single-drawing processes, which makes the tensile strength of the PP separator in the MD direction (longitudinal) too high and the TD direction (transverse) low. Therefore, when subjected to external force in the thickness direction, it is easy to tear in the MD direction (longitudinal). This phenomenon may cause the PP separator to tear during the preparation of the battery cell, which in turn causes problems such as battery cell short circuit failure and battery cell scrapping, increases the cost of the battery cell, and affects the promotion of dry-process separators in more application scenarios.

[0047] In this regard, one embodiment of the present invention provides a polypropylene porous membrane.

[0048] In an embodiment of the present invention, the polypropylene porous membrane comprises homopolypropylene and an elastic modifier, wherein the elastic modifier can increase the elasticity of the polypropylene porous membrane and improve the tear resistance of the polypropylene porous membrane.

[0049] Specifically, the elastic modifier includes one or more of polyolefin elastomer (POE), polyolefin plastomer (POP), polyethylene oxide or polyethylene oxide (PEO), polyethylene glycol (PEG), and copolymer polypropylene (copolymer PP).

[0050] Preferably, the elasticity modifier includes at least one of a polyolefin elastomer and a polyolefin plastomer.

[0051] More preferably, the elasticity modifier includes a mixture of at least one of a polyolefin elastomer and a polyolefin plastomer, and at least one of polyethylene oxide, polyethylene glycol, and copolymerized polypropylene.

[0052] Polyolefin elastomer (POE) and polyolefin plastomer (POP) are thermoplastic elastomers. In the embodiments of the present invention, by introducing POE or POP into the raw materials for preparing the diaphragm, the elasticity of the diaphragm can be significantly enhanced while maintaining a certain strength and modulus. POE and POP are equivalent to a flexible matrix, which can improve the elongation and tear resistance of the diaphragm.

[0053] The addition of polyethylene oxide (PEO), polyethylene glycol (PEG), etc. can weaken the crystallization effect of polypropylene film, reduce the overall crystallinity, and thus enhance toughness.

[0054] Copolymer polypropylene (Copolymer PP, Polypropylene Copolymer), copolymer PP is modified by copolymerization, such as copolymerization with rubber monomers for toughening, and then added to the raw materials for preparing polypropylene porous membranes to give PP better flexibility and impact resistance.

[0055] In order to improve the tear resistance of the polypropylene porous membrane in the process, reduce the defects caused by the tearing of the polypropylene porous membrane in the battery process, and improve the yield of the battery process, in some embodiments, the weight average molecular weight of the elastic modifier is 1.5×10 3 ~8×10 4 Preferably, the weight average molecular weight of the elastic modifier is 1.5×10 3 ~4×10 4. In this embodiment, since the molecular weight of the elastic modifier is relatively small and it is a small molecule substance, during the extrusion film forming process, it mainly forms an amorphous region in an amorphous state. The polymer chain segments in the amorphous region are relatively loose and disordered, which makes the polypropylene porous membrane have better elasticity. In the process of being subjected to external stress, elastic deformation is prone to occur, and the stress exerted on the polypropylene porous membrane is relieved and buffered, so that the polypropylene porous membrane is not easy to rupture. When the external load is removed, the elastic deformation of the polypropylene porous membrane can be restored. It can reduce defective products caused by the tearing of the polypropylene porous membrane in the battery cell manufacturing process and improve the yield rate of the battery cell manufacturing process.

[0056] In some embodiments, in order to ensure processability, the isotacticity of the homopolypropylene used in the polypropylene porous membrane of the present invention is greater than or equal to 97. Preferably, the isotacticity of the homopolypropylene is equal to 98. In the present invention, homopolypropylene with high isotacticity is used as the raw material for preparing the polypropylene porous membrane. The isotacticity affects the crystallinity of polypropylene. The higher the isotacticity, the higher the crystallinity of the polypropylene porous membrane. Within a certain range, the higher the crystallinity, the greater the tensile strength, hardness and rigidity of the polypropylene porous membrane. In addition, the height of the isotacticity of polypropylene will affect its melt rheological properties.

[0057] In some embodiments, the melt index of the homopolypropylene used in the polypropylene porous membrane is 0.5 to 3 g / 10 min. Homopolypropylene with a melt index within the above range has good processing performance. Preferably, the melt index of the homopolypropylene is 1.5 to 2.5 g / 10 min. More preferably, the melt index of the homopolypropylene is 2.0 g / 10 min.

[0058] In some embodiments, the weight average molecular weight of the homopolymer polypropylene used in the polypropylene porous membrane is 2×10 5 ~5×10 5 Preferably, the weight average molecular weight of the homopolymer polypropylene is 3×10 5 ~4×10 5 More preferably, the weight average molecular weight of the homopolymer polypropylene is 3.5×10 5 .

[0059] In some embodiments, the polypropylene porous membrane is a single-layer or double-layer structure. It can be understood that the composition of each layer in the polypropylene porous membrane can be the same or different.

[0060] Further, in terms of weight percentage, each of the layers independently comprises 80-95 parts of the homopolypropylene and 5-20 parts of the elastic modifier. Preferably, each of the layers independently comprises 80-90 parts of the homopolypropylene and 10-20 parts of the elastic modifier. Further, in terms of weight percentage, each of the layers independently comprises 80%-95% of the homopolypropylene and 5%-20% of the elastic modifier. Preferably, in each of the layers, the weight percentage of the homopolypropylene is 80%-90%; the weight percentage of the elastic modifier is 10%-20%.

[0061] In other embodiments, the polypropylene porous membrane is a multilayer structure, including two surface layers and an intermediate layer sandwiched between the two surface layers. It is understandable that the composition of each layer in the polypropylene porous membrane can be the same or different. The number of intermediate layers can be 1 layer, 2 layers or more.

[0062] Furthermore, in terms of weight, each of the surface layers independently comprises 80-95 parts of the homopolypropylene and 5-20 parts of the elastic modifier; the middle layer comprises 80-100 parts of the homopolypropylene and 0-20 parts of the elastic modifier. It can be understood that the inclusion of 5-20 parts of the elastic modifier in the surface layer can improve the tearing problem of the diaphragm, and the middle layer may or may not contain the elastic modifier, and the inclusion of the elastic modifier in the middle layer has a better effect on improving the tearing problem.

[0063] In some embodiments, the tensile strength of the polypropylene porous membrane in the MD direction (Machine Direction) is ≥ 1600 kgf / cm 2 Furthermore, the tensile strength of the polypropylene porous membrane in the MD direction (Machine Direction) is 1795-1890 kgf / cm 2 .

[0064] In some embodiments, the porosity of the polypropylene porous membrane is 30% to 50%. Optionally, the porosity of the polypropylene porous membrane is 30%, 35%, 40%, 45%, 50% or any range of the above values.

[0065] In some embodiments, the thickness of the polypropylene porous membrane is 10 μm to 25 μm. Optionally, the thickness of the polypropylene porous membrane is 10 μm, 12 μm, 15 μm, 20 μm, 25 μm or any range thereof.

[0066] In some embodiments, the puncture strength of the polypropylene porous membrane is ≥250 g. Further, the puncture strength of the polypropylene porous membrane is 331-352 g.

[0067] Another embodiment of the present invention further provides a battery separator, comprising the polypropylene porous membrane as described above.

[0068] In some embodiments, the battery separator includes the above-mentioned polypropylene porous film and a coating disposed on at least one surface of the polypropylene porous film. According to the battery requirements, the coating can achieve high heat resistance, high bonding strength, low heat shrinkage, thermal closure, high film rupture temperature and other effects through reasonable design of components.

[0069] Another embodiment of the present invention further provides a battery assembly, comprising a positive electrode sheet, a negative electrode sheet, and the battery separator as described above, wherein the battery separator is disposed between the positive electrode sheet and the negative electrode sheet.

[0070] Another embodiment of the present invention further provides a method for preparing a polypropylene porous membrane, comprising the following steps:

[0071] S1. Blending: mixing the elastic modifier and the homopolypropylene to obtain a mixture;

[0072] S2, casting: extruding the mixed material after melting and plasticizing, and forming a cast film after the melt is cast;

[0073] S3, annealing: annealing the cast film to make the lamellae on the cast film regular;

[0074] S4, stretching: stretching the annealed cast film to obtain the polypropylene porous film.

[0075] The method and apparatus for melt-mixing the elastic modifier and the homopolypropylene are not particularly limited as long as they can be melt-mixed uniformly. In the preparation of a high-concentration homopolyolefin mixture, an extruder can be selected, and the extruder can be a single-screw extruder or a twin-screw extruder, preferably implemented in a twin-screw extruder. Various additives such as antioxidants can be added as needed within the scope of not impairing the effect of the present invention.

[0076] In some embodiments, the extruder directly extrude the homopolymerized polypropylene melt after melt kneading from the extrusion die head, and molds it in a manner that the thickness of the microporous membrane of the final product is 10 μm to 25 μm, thereby obtaining an extrudate. In order to easily control the thickness of the microporous membrane of the final product, the slit gap of the extrusion die head is preferably 0.1 to 5 mm, and during extrusion, it is preferably heated to 180 to 250° C.

[0077] It should be noted that, in the embodiment of the present invention, the melting temperature and the extrusion temperature of the homopolypropylene are relatively close, and the melting temperature and the extrusion temperature can both be 180-250°C.

[0078] In some embodiments, the obtained extrudate is cooled to obtain a gel-like sheet, ie, a cast film. In the cooling process, the cooling temperature is preferably below the crystallization temperature.

[0079] In some embodiments, the extrudate may be cooled by directly contacting it with cold air, cooling water, other cooling media, contacting it with a roller cooled with a refrigerant, using a casting drum, etc. Specifically, in the embodiment of the present invention, the method of cooling with a casting cooling roller is preferred, wherein the temperature of the casting cooling roller is 65 to 95°C.

[0080] So far, the case where the polypropylene porous membrane is a single layer has been described, but the polypropylene porous membrane of the present invention is not limited to a single layer. For a porous membrane with a double-layer or multi-layer structure, the raw materials of each layer are melt-kneaded to form a melt that is extruded through a co-extrusion die.

[0081] In some embodiments, the cast film is rolled into a roll after being extruded and cooled, wherein the roll length of the cast film is 1000-6000 m and the roll width is 1-2 m.

[0082] In some embodiments, the cast film is also annealed after winding. For the process of producing polypropylene porous film by dry unidirectional stretching, the annealing process is of great significance. The cast base film formed by extrusion casting of polypropylene raw materials has a low degree of crystallinity and many defects in the lamella structure. The lamella thickness is small. If it is directly stretched, its lamella strength is small. During the stretching process, there will be problems such as lamella displacement and collapse. The porous film microporous structure and various properties are poor and cannot meet production needs. In addition, during the stretching process, due to its low degree of crystallinity and low melting point, in actual production, the layers of the porous film after stretching will adhere to each other and the stratification process cannot be completed.

[0083] During the high temperature annealing process, the temperature increase can increase the activity of the polypropylene molecular chain, thereby eliminating the defects in the crystal area, increasing the crystallinity and the thickness of the lamellae, making the lamellae regular, and finally leading to an increase in the elastic recovery rate. A hard elastic film with a high elastic recovery rate is an important prerequisite for preparing a microporous film with a regular porous structure, which can form a uniform porous structure after stretching.

[0084] In some embodiments of the present invention, the cast film is annealed in an oven, wherein the annealing temperature is 135-148° C., and the annealing time is 10-15 h.

[0085] In some embodiments, the cast film after annealing is only stretched longitudinally, or the cast film is stretched longitudinally and transversely. That is, the present invention is applicable to a dry single-stretching process and a dry double-stretching process. The hard elastic film is subjected to uniaxial stretching, and micropores are first induced by low-temperature cold drawing, and then the micropores are expanded by high-temperature hot drawing, so that the oriented lamellae are bent and deformed and separated from each other, thereby forming micropores.

[0086] In some embodiments, the longitudinal stretching step includes cold stretching, hot stretching and shaping. Cold stretching can stretch the parallel lamellae structure of the hard elastic film to produce micropores, while hot stretching can improve crystallization and eliminate internal stress.

[0087] The stretching ratio in the cold drawing step is 1.2-1.8, and the temperature in the cold drawing step is 50-100° C. The stretching ratio in the hot drawing step is 1.4-2.6, and the temperature in the hot drawing step is 145-155° C. The temperature in the heat setting step is 150-160° C., and the setting shrinkage rate is 0.7-0.9.

[0088] The technical solution of the present invention is to add an elastic modifier to the raw material for preparing the polypropylene porous membrane. During processing, the elastic modifier is melted and plasticized with the homopolymerized polypropylene raw material, and is extruded and cast into a part of the membrane structure. Since the molecular weight of the elastic modifier is relatively small and it is a small molecule substance, during the extrusion film forming process, it mainly forms an amorphous region in an amorphous state. The amorphous region has good toughness and is prone to elastic deformation during the process of being subjected to external stress. The stress on the diaphragm is relieved and buffered, so that the diaphragm is not easy to rupture. When the external load is removed, the elastic deformation of the diaphragm can be restored.

[0089] The addition of the elastic modifier can further enhance the elastic properties and strength properties of the polypropylene porous membrane on the basis of the original physical and chemical properties of the polypropylene porous membrane, improve the resistance of the polypropylene porous membrane to external force tearing during the manufacturing process, reduce the defects caused by diaphragm tearing during the battery cell manufacturing process, improve the battery cell process yield, and expand the application scenarios of dry-process diaphragms for lithium batteries.

[0090] The embodiments of the present invention will be described in detail below in conjunction with specific examples, but it will be appreciated by those skilled in the art that the following examples are only used to illustrate the present invention and should not be considered to limit the scope of the present invention. If specific conditions are not specified in the examples, they are carried out according to normal conditions or conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.

[0091] The following examples and comparative examples were all prepared using the above-mentioned method for preparing a battery separator.

[0092] Example 1

[0093] By weight, homopolymer polypropylene material (isotacticity is 98, melt index is 2.0g / 10min, weight average molecular weight is 3.5×10 5 ), 90 parts. The elastic modifier is POE (weight average molecular weight is 1.5×10 3 ), 10 parts. The mixing speed was 400 rpm and the mixing time was 40 minutes. After mixing, the casting extrusion temperature was 220°C, the casting roller was 80°C, and the 2000m cast film was rolled up and annealed at 140°C for 13 hours; then longitudinally stretched, the cold drawing temperature was 70°C, the ratio was 1.3; the hot drawing temperature was 148°C, the ratio was 2.4; the setting temperature was 154°C. A 14μm thick, 41% porosity sample was prepared.

[0094] Example 2

[0095] By weight, homopolymer polypropylene material (isotacticity is 98, melt index is 2.0g / 10min, weight average molecular weight is 3.5×10 5 ), 80 parts. The elastic modifier is POE (weight average molecular weight is 1.5×10 3 ), 20 parts. The mixing speed was 600 rpm and the mixing was carried out for 60 minutes. After mixing, the casting extrusion temperature was 210°C, the casting roller was 80°C, and the 2000m cast film was rolled up and annealed at 135°C for 13h; then longitudinally stretched, the cold drawing temperature was 70°C, the ratio was 1.3; the hot drawing temperature was 148°C, the ratio was 2.4; the setting temperature was 154°C. A sample with a thickness of 14μm and a porosity of 41% was prepared.

[0096] Example 3

[0097] By weight, homopolymer polypropylene material (isotacticity is 98, melt index is 2.0g / 10min, weight average molecular weight is 3.5×10 5 ), 95 parts. The elastic modifier is POE (weight average molecular weight is 4×10 4 ), 10 parts. The mixing speed was 400 rpm and the mixing time was 30 minutes. After mixing, the casting extrusion temperature was 210°C, the casting roller was 80°C, and the 2000m casting film was rolled up and annealed at 145°C for 13 hours; then longitudinally stretched, the cold drawing temperature was 70°C, the ratio was 1.3; the hot drawing temperature was 148°C, the ratio was 2.4; the setting temperature was 154°C. A 14μm thick, 41% porosity sample was prepared.

[0098] Example 4

[0099] By weight, homopolymer polypropylene material (isotacticity is 98, melt index is 2.0g / 10min, weight average molecular weight is 3.5×10 5 ), 90 parts. The elastic modifier is POP (weight average molecular weight is 4×104 ), 10 parts. The mixing speed was 400 rpm and the mixing time was 40 minutes. After mixing, the casting extrusion temperature was 220°C, the casting roller was 80°C, and the 2000m cast film was rolled up and annealed at 140°C for 13 hours; then longitudinally stretched, the cold drawing temperature was 70°C, the ratio was 1.3; the hot drawing temperature was 148°C, the ratio was 2.4; the setting temperature was 154°C. A 14μm thick, 41% porosity sample was prepared.

[0100] Example 5

[0101] By weight, homopolymer polypropylene material (isotacticity is 98, melt index is 2.0g / 10min, weight average molecular weight is 3.5×10 5 ), 90 parts. The elastic modifier is POP (weight average molecular weight is 2×10 4 ) and copolymerized polypropylene (weight average molecular weight 4×10 4 ), of which POP5 parts, copolymerized polypropylene 5 parts. The speed of mixing was 500rpm, and the mixing time was 60min. After mixing, the casting extrusion temperature was 230℃, the casting roller was 80℃, and the 2000m cast film was rolled up, and then annealed at 140℃ for 13h; then longitudinally stretched, the cold drawing temperature was 70℃, the ratio was 1.3; the hot drawing temperature was 148℃, the ratio was 2.4; the setting temperature was 154℃. A 14μm thick, 41% porosity sample was prepared.

[0102] Example 6

[0103] By weight, homopolymer polypropylene material (isotacticity is 98, melt index is 2.0g / 10min, weight average molecular weight is 3.5×10 5 ), 90 parts. The elastic modifier is POP (weight average molecular weight is 2×10 4 ) and PEO (weight average molecular weight is 3×10 3 ), of which POP5 parts, PEO 5 parts. The mixing speed was 500rpm, and the mixing time was 60min. After mixing, the casting extrusion temperature was 230℃, the casting roller was 80℃, and the 2000m cast film was rolled up, and then annealed at 140℃ for 13h; then longitudinally stretched, the cold drawing temperature was 70℃, the ratio was 1.3; the hot drawing temperature was 148℃, the ratio was 2.4; the setting temperature was 154℃. Prepare a 14μm thick, 41% porosity sample.

[0104] Example 7

[0105] By weight, homopolymer polypropylene material (isotacticity is 98, melt index is 2.0g / 10min, weight average molecular weight is 3.5×10 5 ), 90 parts. The elastic modifier is POP (weight average molecular weight is 2×10 4) and PEG (weight average molecular weight of 8×10 4 ), of which POP 5 parts, PEG 5 parts. The mixing speed was 500rpm, and the mixing time was 60min. After mixing, the casting extrusion temperature was 230℃, the casting roller was 80℃, and the 2000m cast film was rolled up, and then annealed at 140℃ for 13h; then longitudinally stretched, the cold drawing temperature was 70℃, the ratio was 1.3; the hot drawing temperature was 148℃, the ratio was 2.4; the setting temperature was 154℃. Prepare a 14μm thick, 41% porosity sample.

[0106] Example 8

[0107] Homopolymer polypropylene material (isotacticity is 98, melt index is 2.0g / 10min, weight average molecular weight is 3.5×10 3 ), elastic modifier is POP (weight average molecular weight is 2×10 4 ). A three-layer co-extruded A / B / A structure is prepared, which adopts a 3:4:3 structure. The surface layer A is a raw material mixed with homopolymer polypropylene and POP, with 90 parts of homopolymer polypropylene and 10 parts of POP by weight; the middle layer B is a pure homopolymer polypropylene layer.

[0108] When the surface material, homopolymer polypropylene and POP are mixed, the speed is 500rpm and the mixing time is 60min. After mixing, the A / B / A structure raw materials are melt cast and co-extruded at an extrusion temperature of 230℃. The casting roll is 80℃, and 2000m of three-layer cast film is rolled up, and then annealed at 140℃ for 13h; then longitudinally stretched, the cold drawing temperature is 70℃, the ratio is 1.3; the hot drawing temperature is 148℃, the ratio is 2.4; the setting temperature is 154℃. A 14μm thick, 41% porosity sample is prepared.

[0109] Comparative Example 1

[0110] By weight, the homopolymer polypropylene material has an isotacticity of 98, a melt index of 2.0 g / 10 min, a proportion of 100%, and a weight average molecular weight of 3.5×10 5 The extrusion processing temperature was 220℃, the casting roll temperature was 80℃, 2000m of cast film was rolled up, and then annealed at 140℃ for 13h; then longitudinally stretched, the cold drawing temperature was 70℃, the ratio was 1.3; the hot drawing temperature was 148℃, the ratio was 2.4; the setting temperature was 154℃. A sample with a thickness of 14μm and a porosity of 41% was prepared.

[0111] Comparative Example 2

[0112] The homopolymer polypropylene material has an isotacticity of 98, a melt index of 2.0 g / 10 min, and a weight average molecular weight of 3.5×10 5 A three-layer co-extruded A / A / A ​​structure was prepared, which adopted a 3:4:3 structure, and its raw materials were all pure homopolymer polypropylene.

[0113] The casting extrusion temperature was 230°C, the casting roll was 80°C, 2000m of cast film was rolled up, and then annealed at 140°C for 13h; then longitudinally stretched, the cold drawing temperature was 70°C, the ratio was 1.3; the hot drawing temperature was 148°C, the ratio was 2.4; the setting temperature was 154°C. A sample with a thickness of 14μm and a porosity of 41% was prepared.

[0114] Table 1: Composition of Examples 1-7 and Comparative Examples 1-2

[0115]

[0116]

[0117] The samples in the comparative examples and embodiments were tested for thickness, porosity, puncture, puncture tear morphology, and tensile strength, and the corresponding test methods are as follows.

[0118] The thickness is measured by a Mahr thickness gauge, the air permeability is tested by a Gurley air permeability instrument, the porosity is calculated by a mass method, the thermal shrinkage is tested by baking in an oven, and the tensile strength is tested by a universal electronic testing machine.

[0119] The tear resistance is evaluated by the pore morphology of the diaphragm after puncture. Under certain puncture load conditions, the diaphragm will be punctured and ruptured. Since the dry film is only stretched longitudinally but not transversely, it is prone to tearing when punctured.

[0120] See also Figure 1-7 When tearing occurs, the puncture hole of the diaphragm is in the shape of a narrow and long tear hole. When the tear resistance of the diaphragm is relatively good, no tearing occurs during the puncture process, and the corresponding puncture hole is a round hole without tearing. Figure 6 , Figure 7 The picture shows the morphology of the through holes formed during the puncture process of the polypropylene porous membrane of Comparative Example 1-2, which are tear holes. Figures 1 to 5 The morphological pictures of the through holes formed during the puncture of the polypropylene porous membrane of Examples 1-5 are circular holes. The test process specifically collects puncture data of 100 points, and respectively counts the proportion of slit holes and circular holes in the diaphragm after puncture and rupture, and compares and analyzes the tear resistance of the diaphragm in the corresponding embodiments and comparative examples. The proportion of puncture and tear holes represents the proportion of the number of slit holes counted in 100 puncture data.

[0121] Table 2: Property measurement data of Examples 1-8 and Comparative Examples

[0122]

[0123] As can be seen from Table 1 and Table 2, in the present invention, at the same thickness, the porosity and air permeability of the samples prepared in Examples 1 to 8 are not much different from those in Comparative Examples 1 and 2, indicating that the diaphragm prepared by the present invention meets the basic requirements of battery diaphragms. However, the puncture strength and tensile strength of the samples prepared in Examples 1 to 8 are higher than the puncture strength and tensile strength of the comparative example. At the same time, the data on the proportion of puncture tear holes show that the proportion of the number of tear holes in Examples 1 to 8 is significantly less than that in the comparative example, indicating that by adding an elastic modifier, the tearing phenomenon of the diaphragm when encountering an external force in the thickness direction can be significantly improved. By adding the elastic modifier of the present invention to the raw materials of the lithium battery polypropylene diaphragm, the strength and tear resistance of the diaphragm prepared by the dry single-pulling process can be effectively improved. In Example 1 and Example 2, when the amount of POE added is changed from 10 parts to 20 parts, the porosity of the sample does not change much, the air permeability, puncture strength and MD tensile strength are slightly increased, and the proportion of puncture tear holes is significantly reduced, indicating that POE can significantly improve the tearing phenomenon of the diaphragm when encountering an external force in the thickness direction.

[0124] In Example 3 and Example 4, the porosity, air permeability and puncture strength of the sample prepared by using POP as the elastic modifier in Example 4 are not much different from those of the sample prepared by using POE as the elastic modifier in Example 3. However, the puncture tear hole ratio and MD tensile strength in Example 4 are better than those in Example 3, especially the puncture tear hole ratio, indicating that at the same weight average molecular weight, POP as an elastic modifier is better than POE in improving the tearing phenomenon of the diaphragm when encountering external force in the thickness direction.

[0125] The foregoing examples are merely illustrative and are used to explain some features of the method of the present invention. The appended claims are intended to claim the widest possible range that can be conceived, and the embodiments presented herein are only illustrations of selected implementations according to the combination of all possible embodiments. Therefore, it is the applicant's intention that the appended claims are not limited by the selection of examples that illustrate the features of the present invention. Some numerical ranges used in the claims also include sub-ranges within them, and changes in these ranges should also be interpreted as being covered by the appended claims where possible.

Claims

1. A polypropylene porous membrane, characterized in that: The material of the polypropylene porous membrane includes homopolymer polypropylene and an elastic modifier, and the elastic modifier includes one or more of polyolefin elastomer, polyolefin plastomer, polyethylene oxide, polyethylene glycol, and copolymer polypropylene.

2. The polypropylene porous membrane according to claim 1, characterized in that The weight average molecular weight of the elastic modifier is 1.5×10 3 ~8×10 4 .

3. The polypropylene porous membrane according to claim 1, characterized in that The homopolypropylene satisfies at least one of the following conditions (1) to (3): (1) The isotacticity of the homopolypropylene is greater than or equal to 97; (2) The melt index of the homopolymer polypropylene is 0.5 to 3 g / 10 min; (3) The weight average molecular weight of the homopolymer polypropylene is 2×10 5 ~5×10 5 .

4. The polypropylene porous membrane according to claim 1, characterized in that The polypropylene porous membrane is a single-layer or double-layer structure; Optionally, each of the layers independently comprises 80 to 95 parts of the homopolypropylene and 5 to 20 parts of the elastic modifier, based on weight percentage.

5. The polypropylene porous membrane according to claim 1, characterized in that The polypropylene porous membrane is a multi-layer structure, including two surface layers and an intermediate layer sandwiched between the two surface layers; Optionally, in terms of weight percentage, each of the surface layers independently comprises 80-95 parts of the homopolypropylene and 5-20 parts of the elastic modifier; the middle layer comprises 80-100 parts of the homopolypropylene and 0-20 parts of the elastic modifier.

6. A battery separator, characterized in that: The invention comprises the polypropylene porous membrane as claimed in any one of claims 1 to 5.

7. A battery assembly, characterized in that: It comprises a positive electrode sheet, a negative electrode sheet and a battery separator as claimed in claim 6, wherein the battery separator is arranged between the positive electrode sheet and the negative electrode sheet.

8. The method for preparing a polypropylene porous membrane according to any one of claims 1 to 5, characterized in that: The following steps are involved: Blending: mixing the elastic modifier and the homopolypropylene to obtain a mixture; Casting: the mixed material is melted and plasticized and then extruded, and the melt is cast to form a cast film; Annealing: annealing the cast film to make the lamellae on the cast film regular; Stretching: the annealed cast film is stretched to obtain the polypropylene porous film.

9. The method for preparing a polypropylene porous membrane according to claim 8, characterized in that: The method for preparing the polypropylene porous membrane satisfies at least one of the conditions (1) to (4): (1) The mixing time is 30 min to 60 min, and the mixing speed is 100 rpm to 600 rpm; (2) The extrusion temperature is 180 to 250° C.; (3) The casting temperature is 65 to 95° C. (4) The annealing temperature is 135-148° C., and the annealing time is 10-15 hours.

10. The method for preparing a polypropylene porous membrane according to claim 8 or 9, characterized in that: The stretching step includes cold drawing, hot drawing and heat setting. The preparation method of the polypropylene porous membrane meets at least one of the conditions (1) to (3): (1) In the cold drawing step, the stretching ratio is 1.2 to 1.8 and the temperature is 50 to 100° C.; (2) in the step of heat drawing, the stretching ratio is 1.4 to 2.6 and the temperature is 145 to 155° C.; (3) The temperature in the heat setting step is 150-160°C.

Citation Information

Cited By

  • Multilayer microporous membranes and uses thereof

    CN119518234A

  • Multilayer microporous membranes and uses thereof

    CN119518234B