Diaphragm and preparation method thereof, secondary battery and electric equipment
By coating the surface of the non-woven fabric base membrane with inorganic materials and binders to form a coating, the problem of low lithium ion transmission speed and electrochemical stability caused by the pore size distribution of the non-woven fabric separator is solved, and more uniform lithium ion transmission is achieved. and battery performance improvements.
Patent Information
- Application Number
- CN202411042033.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-30
- Publication Date
- 2024-10-01
AI Technical Summary
The existing non-woven separators have a wide pore size distribution, causing ceramic particles to enter the pores and block them, reducing the lithium ion transmission speed and battery electrochemical stability.
Inorganic materials and binders are coated on the surface of the non-woven fabric base film to form a coating to ensure that the inorganic materials cannot easily penetrate into the pores and improve electrochemical stability through the fibrous structure.
It improves the consistency of lithium-ion transmission speed and the overall performance of the battery, reduces short circuits in separator leaks, and enhances electrochemical stability.
Smart Images

Figure CN118738764A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of batteries, and in particular to a diaphragm and a preparation method thereof, a secondary battery and electrical equipment. Background Art
[0002] The patent with publication number CN111584797A discloses a method for preparing a non-woven fabric coated diaphragm, which first involves dipping the non-woven fabric with a water-based ceramic slurry, which penetrates into the holes of the non-woven fabric to plug the holes, and then coating the surface with an oil-based aramid slurry to form a protective film with high mechanical strength. The patent with publication number CN110459724A discloses a high-strength PET ceramic diaphragm and a method for preparing the same, which first involves adding ceramic powder and a binder to acetone to obtain a ceramic slurry, and then using a coating technique to coat the ceramic slurry on both surfaces of the PET non-woven fabric base film to form a ceramic coating.
[0003] Although these patents improve the mechanical strength of non-woven membranes, they also reduce the pore size of non-woven membranes by dipping in ceramic slurry, coating with ceramic slurry, etc., thereby avoiding leakage and short circuit. However, because the pore size distribution of non-woven membranes is relatively wide and has some large pores, during the process of dipping and coating ceramic slurry in the non-woven membrane, ceramic particles will enter the pores of the membrane, causing the pores inside the membrane to be partially blocked, reducing the lithium ion transmission rate inside the membrane. Uneven pore blockage will also affect the consistency of lithium ion transmission rate in the membrane and affect the overall performance of the battery. In addition, during the assembly and operation of the battery, inorganic particles are easily detached from the surface of the non-woven base membrane, thereby reducing the electrochemical stability of the battery; therefore, how to overcome the above-mentioned technical problems and defects has become a key issue that needs to be solved. Summary of the invention
[0004] In view of the problems that the existing diaphragm has low ion transmission speed, inorganic particles are easy to fall off from the surface of the base membrane, and the electrochemical stability of the battery is reduced, the present invention provides a diaphragm and a preparation method thereof, a secondary battery and an electrical device.
[0005] The technical solution adopted by the present invention to solve the above technical problems is as follows:
[0006] The first aspect of the present invention provides a diaphragm, including a base film and a coating, wherein the coating is arranged on at least one surface of the base film, the coating includes an inorganic material and a binder, the aspect ratio of the inorganic material is 50 to 1000, and the length of the inorganic material is greater than 1 μm.
[0007] Optionally, the diameter of the inorganic material is 10 nm to 1000 nm, and the length of the inorganic material is 1 μm to 100 μm.
[0008] Optionally, the inorganic material includes a fibrous inorganic material.
[0009] Optionally, the inorganic material includes Al2O3, AlOOH, Al2(SiO3)3, SiO2, ZnO, ZrO2, TiO2, CeO2, CaCO3, SiC, BN, Ca 10 One or more of (PO4)6(OH)2.
[0010] Optionally, the binder comprises a fibrous polymer.
[0011] Optionally, the aspect ratio of the binder is 50-1000.
[0012] Optionally, the diameter of the binder is 2 nm to 100 nm, and the length of the binder is 1 μm to 100 μm.
[0013] Optionally, the binder includes one or more of cellulose, chitin, polyimide, polyacrylonitrile, poly(p-phenylene benzobisoxazole), para-aramid, and meta-aramid.
[0014] Optionally, the mass ratio of the inorganic material to the binder is 100:1 to 100:50.
[0015] Optionally, the coating has a thickness of 0.2 μm to 5 μm.
[0016] Optionally, the base membrane comprises a non-woven fabric base membrane.
[0017] Optionally, the non-woven fabric base membrane includes a main material, and the main material includes polyimide, polyamide, aromatic polyamide, polyethylene terephthalate, poly(p-phenylene benzobisoxazole), poly(2,5-dihydroxy-1,4-phenylene pyridine diimidazole), cellulose, and polyphenylene sulfide, wherein the aromatic polyamide is selected from one or more of para-aramid, meta-aramid, poly(4,4'-diphenylene terephthalamide), poly(4,4'-diphenylene isophthalamide), poly(2,6-naphthalene terephthalamide) and poly(2,6-naphthalene isophthalamide).
[0018] Optionally, the nonwoven fabric base film further comprises a low melting point polymer.
[0019] Optionally, the low melting point polymer is selected from one or more of polyethylene, polypropylene, ethylene-vinyl acetate copolymer, ethylene-acrylic acid copolymer, ethylene-ethyl acrylate copolymer, ethylene-methyl acrylate copolymer, ethylene-butyl acrylate copolymer, polyethylene oxide, cellulose acetate, nylon 6, nylon 66, polyurethane, polyether sulfone, polyvinylidene fluoride and polymethyl methacrylate.
[0020] Optionally, the melting point of the low melting point polymer is 60°C to 150°C.
[0021] Optionally, the main material is fibrous, the diameter of the main material is 0.5μm to 100μm, and the length of the main material is 10μm to 10000μm; and / or, the low-melting point polymer is fibrous, the diameter of the low-melting point polymer is 0.5μm to 100μm, and the length of the low-melting point polymer is 10μm to 10000μm.
[0022] Optionally, the ratio of the main material to the low melting point polymer is 10:0.05 to 10:1.
[0023] Optionally, the base film has a thickness of 10 μm to 100 μm.
[0024] A second aspect of the present invention provides a method for preparing a diaphragm, comprising the following steps:
[0025] Step 1: preparing a coating slurry: dispersing the inorganic material and the binder in a solvent to obtain a coating slurry;
[0026] Step 2: Apply the coating slurry to the surface of the base film and form a separator after drying.
[0027] The third aspect of the present invention provides a secondary battery, comprising a positive electrode, a negative electrode, and a separator located between the positive electrode and the negative electrode, wherein the separator comprises the separator as described in the first aspect above or a separator prepared by the method for preparing the separator described in the second aspect above.
[0028] A fourth aspect of the present application provides an electrical device, comprising the secondary battery described in the third aspect.
[0029] According to the diaphragm provided by the present invention, a coating is coated on at least one surface of the base membrane, the coating includes an inorganic material and a binder, the aspect ratio of the inorganic material is 50 to 1000, and the length of the inorganic material is greater than 1 μm. Compared with granular ceramic materials, the inorganic material of the present invention is not easy to penetrate into the pores inside the non-woven base membrane, and will not cause the pores inside the base membrane to be blocked by the inorganic material, will not reduce the lithium ion transmission speed inside the diaphragm, and will not affect the overall performance of the battery; at the same time, during the assembly and operation of the battery, the inorganic material of the present invention is not easy to fall off from the surface of the non-woven base membrane, thereby improving the electrochemical stability of the battery. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the description of the embodiments of the present invention will be briefly introduced below. Obviously, the drawings in the following description are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.
[0031] Figure 1 is a SEM image of the inorganic / organic fiber coating in Example 16 of the present invention; DETAILED DESCRIPTION
[0032] In order to make the technical problems, technical solutions and beneficial effects solved by the present invention clearer, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0033] Unless otherwise specified, the experimental methods used in the following examples are all conventional methods; the materials and reagents used are reagents and materials that can be obtained from commercial channels unless otherwise specified.
[0034] In one embodiment, the present invention provides a diaphragm including a base film and a coating, wherein the coating is disposed on at least one surface of the base film, the coating includes an inorganic material and a binder, the aspect ratio of the inorganic material is 50 to 1000, and the length of the inorganic material is greater than 1 μm.
[0035] Specifically, the aspect ratio of the inorganic material can be any point value or a range of any two points of 50, 100, 200, 300, 400, 500, 600, 700, 800, 900, 1000. In a preferred embodiment, the aspect ratio of the inorganic material is 100-500.
[0036] In the prior art, ceramic particles are mostly used as the main coating material, and non-morphological polyvinylidene fluoride, sodium carboxymethyl cellulose, etc. are used as binders. The ceramic particles are easy to fall off from the surface of the non-woven base film, thereby reducing the electrochemical stability of the battery.
[0037] Specifically, the aspect ratio of the inorganic material is controlled within the range of 50 to 1000, and the length of the inorganic material is greater than 1 μm, so that the inorganic material has a better ability to form a mesh coating. Compared with granular ceramic materials, the inorganic material of the present invention is not easy to penetrate into the pores inside the non-woven fabric base film, and will not cause the pores inside the base film to be blocked by the inorganic material, will not reduce the lithium ion transmission speed inside the diaphragm, and will not affect the overall performance of the battery; at the same time, during the assembly and operation of the battery, the inorganic material of the present invention is not easy to fall off from the surface of the non-woven fabric base film, thereby improving the electrochemical stability of the battery.
[0038] In one embodiment, the inorganic material has a diameter of 10 nm to 1000 nm and a length of 1 μm to 100 μm.
[0039] Specifically, the diameter of the inorganic material is any point value of 10nm, 20nm, 50nm, 100nm, 200nm, 300nm, 400nm, 500nm, 600nm, 700nm, 800nm, 900nm or 1000nm, or a range of any two point values. In a preferred embodiment, the diameter of the inorganic material is 100nm to 500nm.
[0040] Specifically, the length of the inorganic material is any point value of 1 μm, 2 μm, 5 μm, 10 μm, 20 μm, 30 μm, 40 μm, 50 μm, 60 μm, 70 μm, 80 μm, 90 μm or 100 μm, or a range of any two point values. In a preferred embodiment, the length of the inorganic material is 10 μm to 50 μm.
[0041] The inorganic material of the present application has a diameter of 10 nm to 1000 nm and a length of 1 μm to 100 μm, and has a high aspect ratio. Compared with granular ceramic materials, the inorganic material of the present invention is not easy to penetrate into the pores inside the non-woven fabric base film.
[0042] In one embodiment, the inorganic material comprises a fibrous inorganic material.
[0043] Specifically, the inorganic material may be a fibrous inorganic material, or may be one or more of a linear inorganic material and a rod-shaped inorganic material.
[0044] The inorganic material is one or more of linear inorganic material, fibrous inorganic material or rod-shaped inorganic material, which has the following advantages:
[0045] First, the linear inorganic material, the fibrous inorganic material or the rod-shaped inorganic material all have a high aspect ratio and a length greater than 1 μm. Compared with the granular ceramic material, the inorganic material of the present invention is not easy to penetrate into the pores inside the non-woven fabric base film.
[0046] Second, the linear inorganic material, fibrous inorganic material or rod-shaped inorganic material are cross-linked to form a small-pore fiber mesh coating, which can reduce the leakage and short circuit of the diaphragm, and at the same time, has almost no effect on the migration of ions between the positive and negative electrodes.
[0047] In one embodiment, the inorganic material includes Al2O3, AlOOH, Al2(SiO3)3, SiO2, ZnO, ZrO2, TiO2, CeO2, CaCO3, SiC, BN, Ca 10 One or more of (PO4)6(OH)2.
[0048] Specifically, Al2O3, AlOOH, Al2(SiO3)3, SiO2, ZnO, ZrO2, TiO2, CeO2, CaCO3, SiC, BN, Ca 10 (PO4)6(OH)2 all have excellent ability to form a mesh coating; it is not easy to penetrate into the pores inside the non-woven base membrane, will not cause the pores inside the base membrane to be blocked by inorganic materials, will not reduce the lithium ion transmission speed inside the diaphragm, and will not affect the overall performance of the battery; at the same time, during the assembly and operation of the battery, the inorganic material of the present invention is not easy to fall off from the surface of the non-woven base membrane, thereby improving the electrochemical stability of the battery.
[0049] In one embodiment, the binder comprises a fibrous polymer.
[0050] The binder may be a fibrous polymer, or may be one or more of a linear binder or a rod-shaped binder, which has the following advantages:
[0051] First, the fibrous binder, the linear binder or the rod-shaped binder all have a high aspect ratio and a length greater than 1 μm. Compared with the common soluble binder, the binder of the present invention is not easy to penetrate into the pores inside the non-woven fabric base film.
[0052] Second, the binder polymer of the fibrous binder, linear binder or rod-shaped binder can tightly fix the mesh coating on the fibers on the surface of the base film through the fiber entanglement effect, preventing the inorganic material in the mesh coating from falling off from the surface of the non-woven base film.
[0053] Third, the fibrous binder, linear binder or rod-shaped binder are cross-linked to form a small-pore fiber mesh coating, which can reduce the leakage and short circuit of the diaphragm, and at the same time, has almost no effect on the migration of ions between the positive and negative electrodes.
[0054] In one embodiment, the aspect ratio of the binder is 50-1000.
[0055] Specifically, the aspect ratio of the binder is any value or a range of any two values among 50, 100, 200, 300, 400, 500, 600, 700, 800, 900 and 1000. In a preferred embodiment, the aspect ratio of the binder is 100-500.
[0056] The aspect ratio of the binder is in the range of 100 to 500, and the binder has excellent entanglement ability and ability to form a fiber network.
[0057] In one embodiment, the diameter of the binder is 2 nm to 100 nm, and the length of the binder is 1 μm to 100 μm.
[0058] Specifically, the diameter of the binder is any point value of 2nm, 5nm, 10nm, 20nm, 30nm, 40nm, 50nm, 60nm, 70nm, 80nm, 90nm or 100nm, or a range of any two point values. In a preferred embodiment, the diameter of the binder is 10nm to 50nm.
[0059] Specifically, the length of the adhesive is any point value of 1 μm, 2 μm, 5 μm, 10 μm, 20 μm, 30 μm, 40 μm, 50 μm, 60 μm, 70 μm, 80 μm, 90 μm or 100 μm, or a range of any two point values. In a preferred embodiment, the length of the adhesive is 10 μm to 50 μm.
[0060] The diameter of the binder is 2nm-100nm, the length is 1μm-100μm, and the binder has a high aspect ratio. The binder of the invention has excellent entanglement ability and the ability to form a fiber network.
[0061] In one embodiment, the binder includes one or more of cellulose, chitin, polyimide, polyacrylonitrile, poly(p-phenylene benzobisoxazole), para-aramid, and meta-aramid.
[0062] Specifically, cellulose includes, but is not limited to, commonly used commercial cellulose, various grouped celluloses, celluloses of various fiber sizes, cellulose extracted from various cellulose raw materials, and the like.
[0063] Cellulose, chitin, polyimide, polyacrylonitrile, poly(p-phenylene benzobisoxazole), para-aramid and meta-aramid all have excellent entanglement ability and the ability to form fiber networks. When used in combination with inorganic materials, the coating has both toughness and rigidity, is not easy to break, and has a certain hardness.
[0064] In one embodiment, the mass ratio of the inorganic material to the binder is 100:1 to 100:50.
[0065] Specifically, the mass ratio of the inorganic material to the binder is any one of 100:1, 100:2, 100:5, 100:8, 100:10, 100:12, 100:15, 100:18, 100:20, 100:22, 100:25, 100:28, 100:30, 100:32, 100:35, 100:38, 100:40, 100:42, 100:45, 100:48 or 100:50, or a range of any two values. In a preferred embodiment, the mass ratio of the inorganic material to the binder is 100:10 to 100:30.
[0066] When the mass ratio of inorganic material to binder is between 100:1 and 100:50, the coating has both toughness and rigidity, is not easy to break, and has a certain hardness; when the mass ratio of inorganic material to binder is less than 100:1, the coating has poor toughness and is easy to break; when the mass ratio of inorganic material to binder is greater than 100:50, the porosity of the coating is low, the battery impedance increases, and is not conducive to the migration of lithium ions between the positive and negative electrodes.
[0067] In one embodiment, the coating thickness is 0.2 μm to 5 μm.
[0068] Specifically, the coating thickness is 0.2μm, 0.3μm, 0.4μm, 0.5μm, 0.6μm, 0.7μm, 0.8μm, 0.9μm, 1μm, 1.1μm, 1.2μm, 1.3μm, 1.4μm, 1.5μm, 1.6μm, 1.7μm, 1.8μm, 1.9μm, 2μm, 2.1μm, 2.2μm, 2.3μm, 2.4μm, 2.5μm, 2.6μm, 2.7μm, 2.8μm, 2.9μm, 3μm, 3.1μm, 3.2μm, 3.3μm, 3.4μm, 3.5μm, 3.6μm, 3.7μm, 3.8μm, 3.9μm, 4μm, 4.1μm, 4.2μm, 4.3μm, 4.4μm, 4.5μm, 4.6μm, 4.7μm, 4.8μm, 4.9μm or 5μm, or a range of any two values. In a preferred embodiment, the coating thickness is 1μm to 4μm.
[0069] When the coating thickness is 0.2μm to 5μm, the coating can reduce the leakage and short circuit of the diaphragm, and at the same time, has almost no effect on the migration of ions between the positive and negative electrodes; when the coating thickness is less than 0.2μm, the coating thickness is uneven, and the reduction of leakage and short circuit of the diaphragm is not obvious; when the coating thickness is greater than 5μm, the diaphragm cost is relatively high.
[0070] In one embodiment, the base film comprises a nonwoven base film.
[0071] Specifically, the base film includes, but is not limited to, one or more of a non-woven base film, a polyethylene film, a polypropylene film, a polypropylene-polyethylene-polypropylene three-layer composite film, or a polyimide film.
[0072] The non-woven fabric base membrane is used as the base membrane, which has the characteristics of high membrane porosity, high liquid absorption rate and high safety.
[0073] In one embodiment, the non-woven fabric base film includes a main material, and the main material includes polyimide, polyamide, aromatic polyamide, polyethylene terephthalate, poly(p-phenylene benzobisoxazole), poly(2,5-dihydroxy-1,4-phenylene pyridine diimidazole), cellulose, and polyphenylene sulfide, wherein the aromatic polyamide is selected from one or more of para-aramid, meta-aramid, poly(4,4'-diphenyl terephthalamide), poly(4,4'-diphenyl isophthalamide), poly(2,6-naphthalenediamine) and poly(2,6-naphthalenediamine) isophthalamide.
[0074] Specifically, the main material has the characteristics of high melting point, excellent heat resistance, flame retardancy and rich polar groups, excellent wettability with electrolyte and low swelling.
[0075] In one embodiment, the nonwoven base film further comprises a low melting point polymer.
[0076] The low melting point polymer plays a bonding role. By adding the low melting point polymer to the non-woven base membrane, the tensile strength and hardness of the non-woven membrane can be improved.
[0077] In one embodiment, the low melting point polymer is selected from one or more of polyethylene, polypropylene, ethylene-vinyl acetate copolymer, ethylene-acrylic acid copolymer, ethylene-ethyl acrylate copolymer, ethylene-methyl acrylate copolymer, ethylene-butyl acrylate copolymer, polyethylene oxide, cellulose acetate, nylon 6, nylon 66, polyurethane, polyethersulfone, polyvinylidene fluoride and polymethyl methacrylate.
[0078] Specifically, the low melting point polymer has the characteristics of low swelling, low melting point, excellent processing performance and low cost in the electrolyte, and can improve the tensile strength and hardness of the non-woven fabric separator.
[0079] In one embodiment, the melting point of the low melting point polymer is 60°C to 150°C.
[0080] Specifically, the melting point of the low melting point polymer is 60°C, 62°C, 65°C, 68°C, 70°C, 72°C, 75°C, 78°C, 80°C, 82°C, 85°C, 88°C, 90°C, 92°C, 95°C, 98°C, 100°C, 102°C, 105°C, 108°C, 110°C, 112°C, 115°C, 118°C, 120°C, 122°C, 125°C, 128°C, 130°C, 132°C, 135°C, 138°C, 140°C, 142°C, 145°C, 148°C or 150°C, any point value or a range value composed of any two point values. In a preferred embodiment, the melting point of the low melting point polymer is 80°C to 120°C.
[0081] When the melting point of the low-melting-point polymer is between 60°C and 150°C, it has a suitable processing temperature and will not affect the operation of the battery at normal temperature. When the melting point of the low-melting-point polymer is less than 60°C, the diaphragm structure is easily damaged, resulting in reduced performance of the battery at normal temperature; when the melting point of the low-melting-point polymer is greater than 150°C, the processing temperature is too high and may damage the structure of the main material.
[0082] In one embodiment, the main material is fibrous, the diameter of the main material is 0.5μm~100μm, and the length of the main material is 10μm~10000μm; and / or, the low melting point polymer is fibrous, the diameter of the low melting point polymer is 0.5μm~100μm, and the length of the low melting point polymer is 10μm~10000μm.
[0083] Specifically, the diameter of the main body material is any point value of 0.5μm, 1μm, 2μm, 5μm, 10μm, 20μm, 30μm, 40μm, 50μm, 60μm, 70μm, 80μm, 90μm or 100μm, or a range of any two point values. In a preferred embodiment, the diameter of the main body material is 5μm to 50μm.
[0084] When the diameter of the main material is 0.5μm to 100μm, a diaphragm with porosity and thickness that meet the requirements can be prepared; when the diameter of the main material is less than 0.5μm, the porosity of the diaphragm is low; when the diameter of the main material is greater than 100μm, the thickness of the diaphragm is large and the processing performance is poor.
[0085] Specifically, the length of the main body material is any point value of 10μm, 20μm, 50μm, 100μm, 500μm, 1000μm, 2000μm, 3000μm, 4000μm, 5000μm, 6000μm, 7000μm, 8000μm, 9000μm or 10000μm, or a range of any two point values. In a preferred embodiment, the length of the main body material is 100μm to 1000μm.
[0086] When the length of the main material is 10μm to 10000μm, the mechanical properties and processing properties are better; when the length of the main material is less than 10μm, the tensile strength of the diaphragm is poor; when the length of the main material is greater than 10000μm, the processing properties are poor.
[0087] Specifically, the diameter of the low melting point polymer is any point value of 0.5 μm, 1 μm, 2 μm, 5 μm, 10 μm, 20 μm, 30 μm, 40 μm, 50 μm, 60 μm, 70 μm, 80 μm, 90 μm or 100 μm, or a range of any two point values. In a preferred embodiment, the diameter of the low melting point polymer is 5 μm to 50 μm.
[0088] When the diameter of the low melting point polymer is 0.5 μm to 100 μm, the processing performance is better; when the diameter of the low melting point polymer is less than 0.5 μm, it is difficult to disperse and easy to agglomerate; when the diameter of the low melting point polymer is greater than 100 μm, the bonding effect is poor.
[0089] Specifically, the length of the low melting point polymer is any point value of 10 μm, 20 μm, 50 μm, 100 μm, 500 μm, 1000 μm, 2000 μm, 3000 μm, 4000 μm, 5000 μm, 6000 μm, 7000 μm, 8000 μm, 9000 μm or 10000 μm, or a range of any two point values. In a preferred embodiment, the length of the low melting point polymer is 100 μm to 1000 μm.
[0090] When the length of the low melting point polymer is 10 μm to 10000 μm, the processing performance is better; when the length of the low melting point polymer is less than 10 μm, the bonding effect is poor and the dispersion is uneven; when the length of the low melting point polymer is greater than 10000 μm, processing is difficult.
[0091] In one embodiment, the ratio of the main material to the low melting point polymer is 10:0.05 to 10:1.
[0092] Specifically, the mass ratio of the inorganic material to the binder is any point value among 100:0.05, 100:0.1, 100:0.2, 100:0.3, 100:0.4, 100:0.5, 100:0.6, 100:0.7, 100:0.8, 100:0.9 or 100:1, or a range value consisting of any two point values; in a preferred embodiment, the mass ratio of the inorganic material to the binder is 100:0.3 to 100:0.8.
[0093] When the ratio of the main material to the low-melting-point polymer is 10:0.05 to 10:1, the porosity and tensile strength of the non-woven base membrane meet the requirements of the diaphragm; when the ratio of the main material to the low-melting-point polymer is less than 10:0.05, the tensile strength of the non-woven base membrane is low; when the ratio of the main material to the low-melting-point polymer is greater than 10:1, the porosity of the non-woven base membrane is low.
[0094] In one embodiment, the base film has a thickness of 10 μm to 100 μm.
[0095] Specifically, the thickness of the base film is any value of 10 μm, 20 μm, 30 μm, 40 μm, 50 μm, 60 μm, 70 μm, 80 μm, 90 μm or 100 μm, or a range of any two values. In a preferred embodiment, the thickness of the base film is 20 to 80 μm.
[0096] When the thickness of the base film is 10μm to 100μm, it meets the separator standard; when the thickness of the base film is less than 10μm, the base film has poor tensile strength and is easy to break; when the thickness of the base film is greater than 100μm, it will cause the battery impedance to increase.
[0097] A second aspect of the present invention provides a method for preparing a diaphragm, comprising the following steps:
[0098] Step 1: preparing coating slurry: dispersing inorganic materials and binders in a solvent to obtain coating slurry; Step 2: applying the coating slurry to the surface of the base film and forming a diaphragm after drying.
[0099] In one embodiment of the present application, the base film may be a finished base film, which has undergone a drying and rolling preparation process; therefore, the coating slurry may be directly applied to the surface of the finished base film and formed into a diaphragm after drying.
[0100] In another embodiment of the present application, the base film may be a semi-finished base film, and the semi-finished base film may be a base film semi-finished product prepared by a papermaking process or a wet yarn making process. The coating slurry is applied to the surface of the base film semi-finished product and dried to form a diaphragm.
[0101] In this embodiment, a base film semi-finished product is prepared by a papermaking process or a wet yarn copying process. The base film semi-finished product does not require a drying or rolling process. The coating slurry can be directly coated on the surface of the base film semi-finished product. Then, the base film semi-finished product and the coating are rolled and dried together to form a diaphragm.
[0102] In the method, one rolling and drying process is reduced, and the semi-finished product of the base film and the coating are dried and rolled together, so that the interaction force between the base film and the coating is stronger.
[0103] The third aspect of the present invention provides a secondary battery, comprising a positive electrode, a negative electrode, and a separator located between the positive electrode and the negative electrode, wherein the separator comprises the separator as described in the first aspect or a separator prepared by the method for preparing the separator as described in the second aspect.
[0104] The battery containing the above-mentioned battery separator not only has good safety, but also has excellent electrochemical properties. Specifically, the secondary battery includes a battery housing and a battery cell and an electrolyte contained in the battery housing, wherein the battery cell includes a positive electrode sheet, a negative electrode sheet and a separator located between the positive electrode sheet and the negative electrode sheet, and the separator includes the battery separator of the present application. In the embodiment of the present application, the secondary battery can be any one of a lithium secondary battery, a potassium secondary battery, a sodium secondary battery, a magnesium secondary battery, a zinc secondary battery, and an aluminum secondary battery.
[0105] In the present application, the negative electrode of the secondary battery may be any negative electrode known in the art. In the embodiment of the present application, the negative electrode may include one or more of a carbon-based negative electrode, a silicon-based negative electrode, a tin-based negative electrode, a lithium negative electrode, a sodium negative electrode, a potassium negative electrode, a magnesium negative electrode, a zinc negative electrode and an aluminum negative electrode. Among them, the carbon-based negative electrode may include graphite, hard carbon, soft carbon, graphene, etc.; the silicon-based negative electrode may include silicon, silicon carbon, silicon oxygen, silicon metal compounds, etc.; the tin-based negative electrode may include tin, tin carbon, tin oxygen, tin metal compounds; the lithium negative electrode may include metallic lithium or a lithium alloy. The lithium alloy may specifically be at least one of a lithium silicon alloy, a lithium sodium alloy, a lithium potassium alloy, a lithium aluminum alloy, a lithium tin alloy and a lithium indium alloy. In some embodiments of the present application, the current collector of the negative electrode is copper foil, and the negative electrode active material includes one or more of natural graphite, artificial graphite, hard carbon, soft carbon, lithium titanate, iron oxide, lithium titanium phosphate, titanium dioxide, silicon, silicon oxide, aluminum, tin and antimony; the binder includes one or more of polyacrylic acid (PAA), polyvinylidene fluoride (PVDF), carboxymethyl cellulose (CMC) and styrene butadiene latex (SBR); the conductive agent includes one or more of acetylene black, Ketjen black, Super-P, carbon nanotubes, carbon nanofibers, activated carbon and graphene. In the present application, the preparation method of the negative electrode can adopt any method known in the art.
[0106] In the embodiment of the present application, the positive electrode of the secondary battery includes a positive electrode active material that can reversibly embed / de-embed metal ions (lithium ions, sodium ions, potassium ions, magnesium ions, zinc ions, aluminum ions, etc.). The positive electrode of the secondary battery in the present application can be any positive electrode known in the art.
[0107] Taking lithium secondary batteries as an example, the positive electrode active material can be but is not limited to lithium cobalt oxide (LiCoO2), lithium iron phosphate (LiFePO4), LiNi 0.33 Co 0.33 Mn 0.33 O2(NCM111)LiNi 0.4 Co0.2 Mn 0.4 O2(NCM424),LiNi 0.5 Co 0.2 Mn 0.3 O2(NCM523),LiNi 0.6 Co 0.2 Mn 0.2 O2(NCM622),LiNi 0.8 Co 0.1 Mn 0.1 O2 (NCM811) or more.
[0108] The preparation method of the secondary battery comprises: stacking a positive electrode sheet, a separator and a negative electrode sheet in sequence to form a battery core, accommodating the battery core in a battery shell, injecting an electrolyte, and then sealing the battery shell to obtain the secondary battery.
[0109] A fourth aspect of the present invention provides an electrical device, comprising the secondary battery described in the third aspect.
[0110] By applying secondary batteries to electrical equipment, such as vehicles, etc., the safety performance of the electrical equipment can be improved, and the service life of the electrical equipment can be increased, thereby improving the user experience and enhancing the product competitiveness of the electrical equipment.
[0111] The beneficial effects of the present invention are further illustrated below in conjunction with embodiments.
[0112] In order to make the invention purpose, technical scheme and beneficial technical effect of the present invention clearer, the present invention is further described in detail below in conjunction with examples. However, it should be understood that the examples of the present invention are only for explaining the present invention, not for limiting the present invention, and the examples of the present invention are not limited to the examples given in the specification. The specific experimental conditions or operating conditions not specified in the examples are made under conventional conditions, or are made under the conditions recommended by the material supplier.
[0113] In addition, it should be understood that one or more method steps mentioned in the present invention do not exclude the existence of other method steps before or after the combination step or the insertion of other method steps between these explicitly mentioned steps, unless otherwise specified; it should also be understood that the combination connection relationship between one or more devices / apparatuses mentioned in the present invention does not exclude the existence of other devices / apparatuses before or after the combination device / apparatus or the insertion of other devices / apparatuses between these explicitly mentioned two devices / apparatuses, unless otherwise specified. Moreover, unless otherwise specified, the numbering of each method step is only a convenient tool for identifying each method step, and is not intended to limit the order of arrangement of each method step or the scope of the present invention. Changes or adjustments in their relative relationships should also be regarded as the scope of the present invention without substantially changing the technical content.
[0114] In the following examples, the reagents, materials and instruments used, unless otherwise specified, can be purchased commercially or obtained by synthetic methods known in the art.
[0115] Table 1 Design of coatings in Examples 1-16 and Comparative Examples 1-3
[0116]
[0117]
[0118] Example 1
[0119] A diaphragm comprises a base film and a coating applied on one side of the base film, wherein the inorganic material of the coating is AlOOH fiber with a diameter of 10 nm and a length of 1 μm, and the aspect ratio of the inorganic material is 100; the binder of the coating is para-aramid fiber with a fibrous diameter of 2 nm and a length of 1 μm, and the aspect ratio of the coating is 500; the thickness of the coating is 0.2 μm; the mass ratio of the inorganic material to the binder is 100:1;
[0120] The main material of the base film is fibrous para-aramid with a diameter of 0.5 μm and a length of 10 μm. The low-melting-point polymer of the base film is polyethylene with a diameter of 0.5 μm and a length of 10 μm. The base film thickness is 10 μm. The mass ratio of the main material to the low-melting-point polymer is 10:1.
[0121] Example 2-16
[0122] Examples 2-16 are used to illustrate the coating and base film disclosed in the present invention, and include most of the operating steps in Example 1, except that:
[0123] The composition, length, diameter and aspect ratio of the inorganic material shown in Table 1; the mass of the inorganic material and the binder and the thickness of the coating were used.
[0124] Comparative Examples 1-3
[0125] Comparative Examples 1-3 are used to illustrate the coating and base film disclosed in the present invention, and include most of the operating steps in Example 1, except that:
[0126] The composition, length, diameter and aspect ratio of the inorganic material shown in Table 1; the mass of the inorganic material and the binder and the thickness of the coating were used.
[0127] Test methods and results of Examples 1-16 and Comparative Examples 1-3
[0128] Fiber diameter test
[0129] Optical microscope, scanning electron microscope and transmission electron microscope were selected for the diaphragms prepared in Examples 1-16 and Comparative Examples 1-3 according to the fiber diameter to take microscopic morphology pictures of the fibers, and then fiber diameter analysis software such as imagej, Simpleware, UV-TXW and other image analysis software were used to calculate the fiber diameter and length.
[0130] Diaphragm thickness test
[0131] The diaphragms prepared in Examples 1-16 and Comparative Examples 1-3 were tested for thickness with reference to the national standard GB / T36363-2018.
[0132] Battery capacity test at 0.5C, 1C, 2C, 4C
[0133] The batteries prepared in Examples 1-16 and Comparative Examples 1-3 were placed in a room temperature environment, first charged at a constant current of 0.1C, charged to 3.65V, then charged at a constant voltage, then discharged at a constant current of 0.1C, discharged to 2.0V, and cycled 3 times; the charge and discharge currents were adjusted to 0.5C, cycled 5 times, and the average value of the 5 discharge capacities was recorded as the capacity of the battery at 0.5C; the charge and discharge currents were adjusted to 1C, cycled 5 times, and the average value of the 5 discharge capacities was recorded as the capacity of the battery at 1C; the charge and discharge currents were adjusted to 2C, cycled 5 times, and the average value of the 5 discharge capacities was recorded as the capacity of the battery at 2C; the charge and discharge currents were adjusted to 4C, cycled 5 times, and the average value of the 5 discharge capacities was recorded as the capacity of the battery at 4C.
[0134] The test results of the above experiment are shown in Table 2:
[0135] Table 2 Thickness of diaphragm and capacity of assembled LFP battery in Examples 1-16 and Comparative Examples 1-3
[0136]
[0137]
[0138] Figure 1 is a SEM image of the inorganic / organic fiber coating in Example 16 of the present invention;
[0139] In Examples 1-4, the aspect ratio of the inorganic material is between 50 and 1000, the length of the inorganic material is 1 μm-100 μm, and the length of the inorganic material is greater than 1 μm, the diameter of the inorganic material is 10 nm to 1000 nm, and the battery has a high capacity at 0.5C, 1C, 2C, and 4C. At the same time, the thickness of the diaphragm is relatively thin.
[0140] In Comparative Example 2, the inorganic material has an aspect ratio of 1 and is granular; in Comparative Example 3, the inorganic material has an aspect ratio of 10000; in Example 5, the diameter of the inorganic material is 2nm; in Example 6, the diameter of the inorganic material is 2000nm; in Example 7, the length of the inorganic material is 200μm; in Comparative Example 1, the length of the inorganic material is 0.5μm; when the aspect ratio of the inorganic material is less than 50 or greater than 1000, the length of the inorganic material is less than 1μm or greater than 100μm, and when the diameter of the inorganic material is less than 10nm or greater than 1000nm, the battery has a relatively low capacity at 0.5C, 1C, 2C, and 4C, and the thickness of the diaphragm is relatively thick.
[0141] In Example 2 and Examples 8-9, the mass ratio of the inorganic material to the binder is 100:1 to 100:50, and the battery has a high capacity at 0.5C, 1C, 2C, and 4C, and the thickness of the separator is thin.
[0142] In Example 10, the mass ratio of the inorganic material to the binder is 100:0.1; in Example 11, the mass ratio of the inorganic material to the binder is 100:55; the battery has a relatively low capacity at 0.5C, 1C, 2C, and 4C, and the thickness of the diaphragm is relatively thick.
[0143] In summary, when the mass ratio of the inorganic material to the binder is 100:1 to 100:50, the battery has a high capacity at 0.5C, 1C, 2C, and 4C, indicating that the use of inorganic materials and binders with a higher aspect ratio is not easy to penetrate into the pores inside the non-woven fabric base film, and will not cause the pores inside the base film to be blocked by inorganic materials and binders, will not reduce the lithium ion transmission speed inside the diaphragm, and will not affect the overall performance of the battery;
[0144] In Example 2 and Examples 12-13, the thickness of the coating is 0.2 μm to 5 μm, and the battery has a high capacity at 0.5C, 1C, 2C, and 4C, and the thickness of the separator is thin;
[0145] In Example 14, the thickness of the coating is 0.1 μm; in Example 15, the thickness of the coating is 5.5 μm; the battery has a relatively low capacity at 0.5C, 1C, 2C, and 4C, and the thickness of the separator is relatively thick.
[0146] In summary, when the thickness of the coating is 0.2μm to 5μm, the battery has a high capacity at 0.5C, 1C, 2C, and 4C, indicating that the coating can reduce the leakage and short circuit of the diaphragm, and at the same time, it has almost no effect on the migration of ions between the positive and negative electrodes;
[0147] In Example 16, the length of the inorganic material is 50 μm, and the diameter of the inorganic material is 100 nm; the aspect ratio of the inorganic material is 500; the mass ratio of the inorganic material to the binder is 100:20, and when the thickness of the coating is 3 μm, the battery has a higher capacity at 0.5C, 1C, 2C, and 4C, indicating that the use of inorganic materials and binders with a higher aspect ratio is not easy to penetrate into the pores inside the non-woven base membrane, will not cause the pores inside the base membrane to be blocked by the inorganic material and the binder, will not reduce the lithium ion transmission speed inside the diaphragm, and will not affect the overall performance of the battery; at the same time, during the assembly and operation of the battery, the inorganic material of the present invention is not easy to fall off from the surface of the non-woven base membrane, thereby improving the electrochemical stability of the battery.
[0148] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A diaphragm, characterized in that: The invention comprises a base film and a coating, wherein the coating is arranged on at least one surface of the base film, the coating comprises an inorganic material and a binder, the aspect ratio of the inorganic material is 50 to 1000, and the length of the inorganic material is greater than 1 μm.
2. The diaphragm according to claim 1, characterized in that: The diameter of the inorganic material is 10 nm to 1000 nm, and the length of the inorganic material is 1 μm to 100 μm.
3. The diaphragm according to claim 1, characterized in that: The inorganic material includes a fibrous inorganic material.
4. The diaphragm according to claim 1, characterized in that: The inorganic materials include Al2O3, AlOOH, Al2(SiO3)3, SiO2, ZnO, ZrO2, TiO2, CeO2, CaCO3, SiC, BN, Ca 10 One or more of (PO4)6(OH)2.
5. The diaphragm according to claim 1, characterized in that: The binder includes a fibrous polymer.
6. The diaphragm according to claim 1 or 5, characterized in that: The aspect ratio of the binder is 50-1000.
7. The diaphragm according to claim 6, characterized in that: The diameter of the binder is 2 nm to 100 nm, and the length of the binder is 1 μm to 100 μm.
8. The diaphragm according to claim 1, characterized in that: The binder includes one or more of cellulose, chitin, polyimide, polyacrylonitrile, poly(p-phenylene benzobisoxazole), para-aramid, and meta-aramid.
9. The diaphragm according to claim 1, characterized in that: The mass ratio of the inorganic material to the binder is 100:1 to 100:
50.
10. The diaphragm according to claim 1, characterized in that: The coating has a thickness of 0.2 μm to 5 μm.
11. The diaphragm according to claim 1, characterized in that: The base film includes a nonwoven fabric base film.
12. The diaphragm according to claim 11, characterized in that: The non-woven fabric base film includes a main material, which includes polyimide, polyamide, aromatic polyamide, polyethylene terephthalate, poly(p-phenylene benzobisoxazole), poly(2,5-dihydroxy-1,4-phenylene pyridine diimidazole), cellulose, and polyphenylene sulfide, wherein the aromatic polyamide is selected from one or more of para-aramid, meta-aramid, poly(4,4'-diphenylene terephthalamide), poly(4,4'-diphenylene isophthalamide), poly(2,6-naphthalenediamine) and poly(2,6-naphthalenediamine) .
13. The diaphragm according to claim 12, characterized in that: The nonwoven base film further includes a low melting point polymer.
14. The diaphragm according to claim 13, characterized in that: The low melting point polymer is selected from one or more of polyethylene, polypropylene, ethylene-vinyl acetate copolymer, ethylene-acrylic acid copolymer, ethylene-ethyl acrylate copolymer, ethylene-methyl acrylate copolymer, ethylene-butyl acrylate copolymer, polyethylene oxide, cellulose acetate, nylon 6, nylon 66, polyurethane, polyether sulfone, polyvinylidene fluoride and polymethyl methacrylate.
15. The diaphragm according to claim 13, characterized in that: The melting point of the low melting point polymer is 60°C to 150°C.
16. The diaphragm according to claim 13, characterized in that: The main material is fibrous, the diameter of the main material is 0.5μm to 100μm, and the length of the main material is 10μm to 10000μm; and / or the low-melting point polymer is fibrous, the diameter of the low-melting point polymer is 0.5μm to 100μm, and the length of the low-melting point polymer is 10μm to 10000μm.
17. The diaphragm according to any one of claims 13 to 16, characterized in that: The mass ratio of the main material to the low melting point polymer is 10:0.05 to 10:
1.
18. The diaphragm according to claim 1, characterized in that: The base film has a thickness of 10 μm to 100 μm.
19. The method for preparing a diaphragm according to any one of claims 1 to 18, characterized in that: The steps include: Step 1: preparing a coating slurry: dispersing the inorganic material and the binder in a solvent to obtain a coating slurry; Step 2: Apply the coating slurry to the surface of the base film and form a separator after drying.
20. A secondary battery, characterized in that: It comprises a positive electrode, a negative electrode, and a separator located between the positive electrode and the negative electrode, wherein the separator comprises the separator according to any one of claims 1 to 18 or a separator prepared by the method for preparing the separator according to claim 19.
21. An electric device comprising the secondary battery according to claim 20.
Citation Information
Cited By
Separator, and electrochemical device and electronic device including same
CN121367026A