Heater member assembly

By using the honeycomb structure heater component with PTC characteristics and combining it with the clamping design of the resin frame, the problem of low energy efficiency and large space occupation of the heater component in winter is solved, achieving more efficient thermal management and space utilization. .

CN118741779APending Publication Date: 2024-10-01NGK INSULATORS LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410271717.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-03-30
Filing Date
2024-03-11
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Existing heater components have low energy efficiency in winter, especially in electric vehicles, resulting in reduced cruising distance, and traditional heater components tend to become large and occupy space in the vehicle.

Method used

A honeycomb structure heater component with PTC characteristics is used, and is clamped by a resin frame to protect and reduce heat loss and improve compactness.

Benefits of technology

The protective performance and heat loss reduction of the heater components are improved, the compactness is enhanced, and the energy efficiency under low temperature conditions is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118741779A_ABST
    Figure CN118741779A_ABST
Patent Text Reader

Abstract

Provided is a heater member assembly which is provided with a heater member having a honeycomb structure part having PTC characteristics, and a housing, and which has excellent protection performance against the heater member and contributes to the reduction of heat loss. This heater member assembly is provided with: a heater member that is provided with a honeycomb structure section that has an outer peripheral wall and partition walls that contain a material having PTC characteristics, are disposed on the inner peripheral side of the outer peripheral wall, and define a plurality of cells, and that is capable of generating heat by energization; the plurality of cells form a flow path extending from a first end surface to a second end surface, and the frame body has a first frame part made of resin and a second frame part made of resin for sandwiching the heater member from the first end surface side and the second end surface side.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a heater component assembly including a heater component and a frame. Background Art

[0002] In various vehicles such as automobiles, there is an increasing demand for improving the cabin environment. Specific requirements include: reducing CO 2 As an effective countermeasure to such requirements, ventilation can be cited, which is the main reason for the significant loss of heater energy in winter, resulting in the deterioration of energy efficiency in winter. In particular, in electric vehicles (BEVs), there is a problem of a significant reduction in cruising range due to energy loss.

[0003] Therefore, Patent Documents 1 and 2 disclose a vehicle cabin purification system in which water vapor and CO in the vehicle cabin air are removed. 2 The removal target components are captured by functional materials such as adsorbent materials, and then the removal target components are reacted or separated by heating and released outside the vehicle to regenerate the functional materials. In such a vehicle cabin purification system, in order to ensure the capture performance of the removal target components, the air and the functional materials are required to have as much contact as possible, and in order to promote the regeneration of the functional materials, the functional materials are required to be heated to a specified temperature. Regarding regeneration, for example, regeneration is performed by a method of removing substances adsorbed on the functional materials by an oxidation reaction and a method of separating and discharging substances adsorbed on the functional materials. However, these methods all require that the functional materials be heated to an appropriate temperature according to the adsorbed substances.

[0004] As a heating structure, a vapor compression heat pump is excellent from the viewpoint of thermal efficiency, but the vapor compression heat pump has the following problems, that is, it is difficult to work when the outside air is at an extremely low temperature, and it is difficult to quickly warm up the vehicle cabin when the vehicle is started. Therefore, it is considered to be more practical to use a vapor compression heat pump as a main heating device and to use a heater member that fully utilizes Joule heat as an auxiliary when rapid heating is required when the vehicle is started and when the outside air temperature is very low.

[0005] However, the heater component using Joule heat has the following problem: it is easy to be large-sized, which squeezes the space inside the vehicle. Therefore, it is desired to provide a more compact heater component. In this regard, it is known that a heater component having a honeycomb structure having PTC characteristics can increase the heat transfer area per unit volume and prevent excessive heat generation, which is advantageous (Patent Document 3).

[0006] Patent document 3 describes a heater component, which has a columnar honeycomb structure portion, the columnar honeycomb structure portion has an outer peripheral side wall and a partition wall, the partition wall has a PTC characteristic, and is arranged on the inner side of the outer peripheral side wall and partitions a plurality of compartments, and the plurality of compartments form a flow path from a first bottom surface to a second bottom surface. Patent document 3 also describes: after a pair of electrodes are joined to the heater component, heat is generated by applying a voltage between the pair of electrodes.

[0007] In addition, Patent Document 4 describes a heating device characterized by having the following mechanism, that is, a positive characteristic magnet having a large number of through holes is used to constitute all or part of the heating element, so that gas or liquid convects in the through holes. In addition, it is described that a positive characteristic magnet (PTCR) and a fan are placed opposite each other in a cylindrical frame, and the PTCR is fixed to the frame with a heat-resistant insulating support.

[0008] Prior art literature

[0009] Patent Literature

[0010] Patent Document 1: Japanese Patent Application Publication No. 2020-104774

[0011] Patent Document 2: Japanese Patent Application Publication No. 2020-111282

[0012] Patent Document 3: International Publication No. 2020 / 036067

[0013] Patent Document 4: Japanese Patent Application Laid-Open No. 49-114130 Summary of the invention

[0014] When a heater component having a honeycomb structure having PTC characteristics is arranged in a vehicle, it is assumed that the heater component is arranged in a ventilation path in the vehicle's air conditioning system, i.e., HVAC. In this case, it is considered that the heater component is preferably arranged in a state protected by a frame. In this regard, Patent Document 4 records that a PTCR is fixed to a frame with a heat-resistant insulating support, but from the perspective of protecting the PTCR and reducing heat loss, the discussion is not sufficient.

[0015] The present invention is created in view of the above situation. In one embodiment, the subject is to provide a heater component assembly, which includes a heater component and a frame, and the heater component includes a honeycomb structure portion with PTC characteristics. The heater component assembly has excellent protection performance for the heater component and also helps to reduce heat loss.

[0016] The inventors of the present invention have conducted intensive research to solve the above problems and have found that it is advantageous to sandwich a heater member having a honeycomb structure having PTC characteristics from the end surface side by a resin frame having a predetermined structure. The present invention completed based on this finding is exemplified below.

[0017] [1] A heater component assembly comprising a heater component and a frame,

[0018] The heater component assembly is characterized in that

[0019] The heater component comprises:

[0020] A honeycomb structure part, the honeycomb structure part has an outer peripheral wall and partition walls and can generate heat when powered, the partition walls contain a material having PTC characteristics and are arranged on the inner peripheral side of the outer peripheral wall to partition into a plurality of compartments, the plurality of compartments forming a flow path extending from the first end face to the second end face;

[0021] a first electrode layer covering a part or the whole of the surface of the partition wall forming the first end face;

[0022] a second electrode layer covering a part or the whole of the surface of the partition wall forming the second end face;

[0023] a first terminal connected to an outer surface of the first electrode layer; and

[0024] a second terminal connected to an outer surface of the second electrode layer,

[0025] The frame body includes a first frame portion and a second frame portion for clamping the heater member from the first end surface side and the second end surface side.

[0026] The first frame portion is a resin-made first frame portion arranged on the first end face side, and includes a flange portion arranged on the outer peripheral side of the outer peripheral contour of the first end face, and a retaining portion arranged on the inner peripheral side of the outer peripheral contour of the first end face and applying pressure to at least a portion of the outer peripheral portion of the first end face.

[0027] The second frame portion is a second frame portion made of resin and arranged on the side of the second end face, and has a flange portion arranged on the outer peripheral side of the outer peripheral contour of the second end face, and a retaining portion arranged on the inner peripheral side of the outer peripheral contour of the second end face and applying pressure relative to at least a portion of the outer peripheral portion of the second end face.

[0028] [2] The heater component assembly according to [1], characterized in that:

[0029] The Rockwell hardness of the resin constituting the first frame portion and / or the second frame portion measured in accordance with ASTM D785-2008R15 is 150 HRR or less and / or 120 HRM or less.

[0030] [3] The heater component assembly according to [1] or [2], characterized in that:

[0031] The deflection temperature under load of the resin constituting the first frame portion and / or the second frame portion measured in accordance with JIS K7191-1:2015 is 145° C. or higher.

[0032] [4] The heater component assembly according to any one of [1] to [3], characterized in that:

[0033] The melting point of the resin constituting the first frame portion and / or the second frame portion is 250° C. or higher.

[0034] [5] The heater component assembly according to any one of [1] to [4], characterized in that:

[0035] The resin constituting the first frame portion and / or the second frame portion has a thermal conductivity of 0.5 W / m / K or less at 25° C. as measured in accordance with JIS R1611:2010.

[0036] [6] The heater component assembly according to any one of [1] to [5], characterized in that:

[0037] The volume resistivity of the resin constituting the first frame portion and / or the second frame portion at 25° C. measured in accordance with JIS C2139:2008 is 1.0×10 16 Ω·cm or more.

[0038] [7] The heater component assembly according to any one of [1] to [6], characterized in that:

[0039] The resin constituting the first frame portion and / or the second frame portion includes one or two selected from polyetheretherketone and polybutylene terephthalate (PBT).

[0040] [8] The heater component assembly according to any one of [1] to [7], characterized in that:

[0041] The ratio of the area of ​​the first end surface to which the pressure is applied by the holding portion of the first frame portion relative to the area of ​​the first end surface is 10% or less, and / or

[0042] A ratio of an area of ​​the second end surface to which pressure is applied by the holding portion of the second frame portion relative to an area of ​​the second end surface is 10% or less.

[0043] [9] The heater component assembly according to any one of [1] to [7], characterized in that:

[0044] The ratio of the area of ​​the first end surface to which the pressure is applied by the holding portion of the first frame portion relative to the area of ​​the first end surface is 2% or less, and / or

[0045] A ratio of an area of ​​the second end surface to which pressure is applied by the holding portion of the second frame portion relative to an area of ​​the second end surface is 2% or less.

[0046]

[10] The heater component assembly according to any one of [1] to [9], characterized in that:

[0047] The holding portion of the first frame portion has a portion that presses the first terminal toward the first end surface, and / or

[0048] The holding portion of the second frame portion has a portion that presses the second terminal toward the second end surface.

[0049]

[11] The heater component assembly according to any one of [1] to

[10] , characterized in that:

[0050] A cushioning material is sandwiched between the holding portion of the first frame portion and the first end surface, and / or

[0051] A cushioning material is interposed between the holding portion of the second frame portion and the second end surface.

[0052]

[12] The heater component assembly according to any one of [1] to

[11] , characterized in that:

[0053] The frame body includes a third frame portion made of resin and surrounding an outer peripheral surface of the outer peripheral wall of the heater member.

[0054]

[13] The heater component assembly according to

[12] , characterized in that:

[0055] A cushioning material is interposed between the third frame portion and the outer peripheral wall.

[0056]

[14] The heater component assembly according to any one of [1] to

[13] , characterized in that:

[0057] The first frame portion and the second frame portion are divided from each other and connected by a fastener.

[0058]

[15] The heater component assembly according to any one of [1] to

[13] , characterized in that:

[0059] The first frame portion and the second frame portion are divided from each other and connected by a fitting structure.

[0060]

[16] The heater component assembly according to any one of [1] to

[13] , characterized in that:

[0061] The first frame portion and the second frame portion are divided from each other and connected with an adhesive.

[0062]

[17] The heater component assembly according to any one of [1] to

[16] , characterized in that:

[0063] The average value of the thickness of the first electrode layer at the outer peripheral portion of the first end surface and the connection portion with the first terminal is greater than the average value of the thickness of the first electrode layer at other portions, and / or

[0064] An average value of the thickness of the second electrode layer at an outer peripheral portion of the second end surface and a connection portion with the second terminal is larger than an average value of the thickness of the second electrode layer at other portions.

[0065]

[18] The heater component assembly according to any one of [1] to

[17] , characterized in that:

[0066] The average value of the thickness of the first electrode layer at the entire periphery of the first end surface is greater than the average value of the thickness of the first electrode layer at other portions, and / or the average value of the thickness of the second electrode layer at the entire periphery of the second end surface is greater than the average value of the thickness of the second electrode layer at other portions.

[0067] Effects of the Invention

[0068] According to a heater component assembly involved in one embodiment of the present invention, a resin frame protects a heater component having a honeycomb structure having PTC characteristics by clamping two end faces. Generally, resin is softer than metal, so by making the frame made of resin, the part of the heater component in contact with the frame is not easily damaged. In addition, resin generally has a lower thermal conductivity than metal, so it also helps to reduce heat loss. BRIEF DESCRIPTION OF THE DRAWINGS

[0069] Figure 1A This is a schematic diagram of the heater member according to one embodiment of the present invention as viewed from the first end surface side.

[0070] Figure 1B yes Figure 1A Schematic X-ray cross-section diagram of .

[0071] Figure 1CThis is a schematic diagram of a heater member according to another embodiment of the present invention as viewed from the first end surface side.

[0072] Figure 1D yes Figure 1C Schematic X-ray cross-section diagram of .

[0073] Figure 2A This is a schematic diagram of an example of a heater member assembly including a frame that sandwiches the heater member from the first end surface side and the second end surface side as viewed from the first end surface side.

[0074] Figure 2B yes Figure 2A Schematic X-ray cross-section diagram of .

[0075] Figure 3A This is a schematic diagram of another example of a heater member assembly including a frame that sandwiches the heater member from the first end surface side and the second end surface side, as viewed from the first end surface side.

[0076] Figure 3B yes Figure 3A Schematic X-ray cross-section diagram of .

[0077] Figure 4A This is a schematic diagram of another example of a heater member assembly including a frame that sandwiches the heater member from the first end surface side and the second end surface side, as viewed from the first end surface side.

[0078] Figure 4B yes Figure 4A Schematic X-ray cross-section diagram of .

[0079] Figure 5A This is a schematic diagram of another example of a heater member assembly including a frame that sandwiches the heater member from the first end surface side and the second end surface side, as viewed from the first end surface side.

[0080] Figure 5B yes Figure 5A Schematic X-ray cross-section diagram of .

[0081] Figure 6 It is a schematic diagram showing a configuration example of an air conditioning system according to one embodiment of the present invention.

[0082] Explanation of symbols

[0083] 100: heater member, 101a: first end surface, 101b: second end surface, 102a: first electrode layer, 102b: second electrode layer, 103: peripheral wall, 103a: passage, 103e: peripheral surface, 104: partition, 105a: power-carrying member, 105b: power-carrying member, 105c: end, 106: partition, 107a: first functional material-containing layer, 107b: second functional material-containing layer, 109a: first terminal, 109b: second terminal, 111a: third functional material-containing layer, 111b: fourth functional material-containing layer, 113: fifth functional material-containing layer, 120: frame, 121: first frame portion, 121a: holding portion, 121b: flange portion, 122: second frame portion, 122a: holding portion, 1 22b: flange portion, 123: third frame portion, 124: fastener, 125: recessed portion, 126a: portion partially protruding toward the inner circumference side, 126b: portion partially protruding toward the inner circumference side, 127: cushioning material, 131: cushioning material, 132: cushioning material, 150: connecting portion, 151: convex portion, 152: recessed portion, 154: dividing portion, 200: power supply, 300: switching valve, 310: rotating shaft, 312: opening and closing door, 314: actuator, 400: inflow piping, 500: outflow piping, 500a: first path, 500b: second path, 600: ventilator, 810: electric wire, 820: electric wire, 830: electric wire, 900: control unit, 910: power switch, 1000: first air conditioning system. DETAILED DESCRIPTION

[0084] The embodiments of the present invention are described in detail below with reference to the accompanying drawings. The present invention is not limited to the following embodiments, and it should be understood that within the scope of the present invention, the following embodiments can be appropriately modified, improved, etc. based on the common knowledge of those skilled in the art and also fall within the scope of the present invention.

[0085] (1. Heater component)

[0086] The heater component of the embodiment of the present invention can be preferably used for improving the indoor environment in various vehicles such as automobiles. As a vehicle, there is no particular limitation, and automobiles and electric cars can be mentioned. As a car, there is no particular limitation, and gas fuel vehicles using CNG (compressed natural gas), LNG (liquefied natural gas), etc., fuel cell vehicles, electric vehicles, and plug-in hybrid vehicles can be mentioned. The heater component of the embodiment of the present invention can be preferably used in vehicles that do not have an internal combustion engine, especially electric cars and electric cars.

[0087] Furthermore, the heater member according to the embodiment of the present invention can be used for improving the interior space of buildings such as houses, offices, factories, stores, warehouses, and cold storages, and vehicles such as ships and airplanes, in addition to vehicles.

[0088] The heater member of the embodiment of the present invention can be used for heating purposes, and can also be added with a function of removing the target components in the air, which can contribute to the improvement of the indoor environment. For example, by providing a functional material layer having a function of adsorbing the target components in the air such as water vapor, carbon dioxide, and odor components on the surface of the wall of the heater member forming the flow path inside the compartment, the function can be added.

[0089] Figure 1A Schematic diagram of the heater member 100 according to one embodiment of the present invention as viewed from the first end surface side is shown in FIG. Figure 1B Shown in Figure 1A Schematic X-ray cross-section diagram of . Figure 1C Schematic diagram of a heater member 100 according to another embodiment of the present invention as viewed from the first end surface side is shown in FIG. Figure 1D Shown in Figure 1C Schematic X-ray cross-section diagram of .

[0090] The heater member 100 includes a honeycomb structure having an outer peripheral wall 103 and partition walls 106 disposed on the inner peripheral side of the outer peripheral wall 103 to partition a plurality of cells 104 forming a flow path extending from a first end surface 101 a to a second end surface 101 b .

[0091] The heater member 100 includes a first electrode layer 102a covering part or all of the surface of the partition wall 106 forming the first end surface 101a and a second electrode layer 102b covering part or all of the surface of the partition wall 106 forming the second end surface 101b.

[0092] The heater component 100 includes: a first functional material-containing layer 107a covering a portion of the outer surface of the first electrode layer 102a (thereby indirectly covering the first end surface 101a), and a second functional material-containing layer 107b covering a portion of the outer surface of the second electrode layer 102b (thereby indirectly covering the second end surface 101b).

[0093] The heater component 100 comprises: a first terminal 109a connected to the outer surface of the first electrode layer 102a (when a first functional material-containing layer 107a is provided, preferably a portion of the outer surface of the first electrode layer 102a not covered by the first functional material-containing layer 107a), and a second terminal 109b connected to the outer surface of the second electrode layer 102b (when a second functional material-containing layer 107b is provided, preferably a portion of the outer surface of the second electrode layer 102b not covered by the second functional material-containing layer 107b).

[0094] The heater member 100 includes a third function-material-containing layer 111 a covering a portion of the outer surface of the first terminal 109 a , and a fourth function-material-containing layer 111 b covering a portion of the outer surface of the second terminal 109 b .

[0095] The heater member 100 includes a fifth functional material-containing layer 113 that covers a part or the entirety of the surface of the partition wall 106 that forms the flow path inside the partition 104 .

[0096] Hereinafter, the structure of the heater member 100 will be described in detail.

[0097] (1-1. Honeycomb structure)

[0098] The shape of the honeycomb structure portion is not particularly limited. For example, the outer shape of the cross section of the honeycomb structure portion that is orthogonal to the direction in which the flow path extends (the direction in which the compartment 104 extends) is a polygon (a quadrilateral (rectangle, square), pentagon, hexagon, heptagon, octagon, etc.), a rounded shape (circular, elliptical, approximately oval, oval, oblong, a quadrilateral with roundness (a quadrilateral in which each side and each corner is composed of a curve and the radius of curvature of each side is greater than the radius of curvature of each corner, and the whole is composed of curves)), etc. In addition, when the outer shape of the cross section is a polygon, the corners can be chamfered. For the reason of preventing damage to the honeycomb structure portion and making it easy to wind the buffer material on the outer peripheral surface, the corners are particularly preferably in a shape with R chamfering, more preferably without a corner having a radius of curvature of less than 5 mm, further preferably with a radius of curvature of more than 10 mm, and further preferably with more than 20 mm. The upper limit of the radius of curvature of the corner is not limited, and can be less than 40 mm, typically less than 30 mm. It should be noted that the end faces (the first end face 101 a and the second end face 101 b ) have the same shape as the cross section. Figure 1A and Figure 1B In the heater member 100 shown, the outer shape of the cross section of the honeycomb structure part is circular, and the outer shape of the honeycomb structure part is cylindrical as a whole. Figure 1C and Figure 1DIn the heater member 100 shown, the outer shape of the cross section of the honeycomb structure part is a rectangular shape with rounded corners, and the outer shape of the honeycomb structure part as a whole is a quadrangular prism shape with rounded corners.

[0099] The opening shape of the compartment 104 is not particularly limited, and in the cross section of the honeycomb structure portion that is orthogonal to the direction in which the flow path extends, it can be a polygon (a quadrilateral (rectangle, square), a pentagon, a hexagon, a heptagon, an octagon, etc.), a shape with a rounded arc (a circle, an ellipse, a nearly oval, an oval, an oblong, etc.), etc. These shapes can be single, or two or more can be combined. In addition, among these shapes, a quadrilateral or a hexagon is preferred. By providing the compartment 104 of the above-mentioned shape, the pressure loss during air circulation can be reduced. In the case where the opening shape of the compartment 104 is a polygon, the corners can be R-chamfered. It should be noted that in the illustrated heater component 100, the opening shape of the compartment 104 is a square.

[0100] The honeycomb structure portion can be a honeycomb joint body, which has a plurality of honeycomb units and a joint layer for joining the peripheral surfaces of the plurality of honeycomb units to each other. By using a honeycomb joint body, the generation of cracks can be suppressed, and the total cross-sectional area of ​​the compartment 104, which is very important for ensuring the flow rate of air, can be increased. The joint layer can be formed using a joint material. As a joint material, there is no particular limitation, and a material made into a paste by adding solvents such as water to a ceramic material can be used. The joint material can contain a material having PTC properties, and can also contain the same material as the peripheral wall 103 and the next door 106. In addition to having the effect of joining the honeycomb units to each other, the joint material can also be used as a peripheral coating material after the honeycomb units are joined.

[0101] From the viewpoints of ensuring the strength of the honeycomb structure, reducing the pressure loss when air passes through the cell 104, ensuring the loading amount of functional materials, ensuring the contact area with the air flowing in the cell 104, the resistance between the end faces, etc., it is desired to well combine the thickness of the partition wall 106, the cell density, and the cell spacing (or the opening ratio of the cell).

[0102] In this specification, the thickness of the partition wall 106 refers to the length of a line segment that connects the centers of gravity of adjacent cells 104 in a cross section perpendicular to the direction in which the flow path extends and that crosses the partition wall 106. The thickness of the partition wall 106 refers to the average thickness of all the partition walls 106.

[0103] In this specification, the cell density is a value obtained by dividing the number of cells by the area of ​​one end surface of the honeycomb structure part (the total area of ​​the partition walls 106 and the cells 104 excluding the external peripheral wall 103 ).

[0104] In this specification, the cell spacing refers to a value obtained by the following calculation. First, the area of ​​one end surface of the honeycomb structure part (the total area of ​​the partition wall 106 and the cell 104 excluding the peripheral wall 103) is divided by the number of cells to calculate the area of ​​each cell. Next, the square root of the area of ​​each cell is calculated and set as the cell spacing.

[0105] In this specification, the opening ratio of the cell 104 is a value obtained by dividing the total area of ​​the cells 104 partitioned by the partition walls 106 in the cross section of the honeycomb structure part orthogonal to the direction in which the flow path extends by the area of ​​one end face (the total area of ​​the partition walls 106 and the cells 104 excluding the peripheral wall 103). It should be noted that when calculating the opening ratio of the cell 104, layers such as the electrode layer and the functional material-containing layer provided on the partition walls 106 are not considered.

[0106] In an advantageous embodiment from the viewpoint of supporting a sufficient amount of functional material, the thickness of the partition wall is 0.180 mm or less, and the cell density is 100 cells / cm 2 In a preferred embodiment, the thickness of the partition wall is 0.130 mm or less, and the cell density is 70 cells / cm 2 In a more preferred embodiment, the thickness of the partition wall is 0.100 mm or less, and the cell density is 65 cells / cm 2 Below, and the compartment spacing is above 1.3 mm.

[0107] In each of the above-mentioned embodiments, from the viewpoint of ensuring the strength of the honeycomb structure and keeping the electrical resistance low, the lower limit of the thickness of the partition walls is preferably 0.010 mm or more, more preferably 0.020 mm or more, and even more preferably 0.030 mm or more.

[0108] In each of the above-mentioned embodiments, from the viewpoints of ensuring the strength of the honeycomb structure, keeping the resistance at a low level, and increasing the surface area to promote the reaction, adsorption, and separation of the functional material, the lower limit of the cell density is preferably 30 cells / cm 2 More than 35 cells / cm 2 More preferably, 40 cells / cm 2 above.

[0109] In each of the above-mentioned embodiments, from the viewpoint of ensuring the strength of the honeycomb structure, maintaining the electrical resistance at a low level, and increasing the surface area to promote the reaction, adsorption, and detachment of functional materials, the upper limit of the cell spacing is preferably less than 2.0 mm, more preferably less than 1.8 mm, and further preferably less than 1.6 mm.

[0110] In an embodiment advantageous from the viewpoint of simultaneously achieving reduced pressure loss and maintained strength, the thickness of the cell walls is 0.08 mm or more and 0.36 mm or less, and the cell density is 2.54 cells / cm 2 Above and 140 compartments / cm 2 In a preferred embodiment, the thickness of the partition wall is 0.09 mm to 0.35 mm, and the cell density is 15 cells / cm 2 More than 100 cells / cm 2 In a more preferred embodiment, the thickness of the partition wall is 0.10 mm to 0.30 mm, and the cell density is 20 cells / cm 2 More than 90 compartments / cm 2 Below, the opening ratio of the cell is 0.77 or more.

[0111] In each of the above-mentioned embodiments, from the viewpoint of ensuring the strength of the honeycomb structure part, the upper limit of the opening ratio of the cell is preferably 0.94 or less, more preferably 0.92 or less, and further preferably 0.90 or less.

[0112] The thickness of the peripheral wall 103 is not particularly limited, and is preferably determined based on the following viewpoints. First, from the viewpoint of strengthening the honeycomb structure portion, the thickness of the peripheral wall 103 is preferably 0.05 mm or more, more preferably 0.06 mm or more, and further preferably 0.08 mm or more. On the other hand, from the viewpoint of increasing the resistance to suppress the initial current, and from the viewpoint of reducing the pressure loss during air circulation, the thickness of the peripheral wall 103 is preferably 1.0 mm or less, more preferably 0.5 mm or less, further preferably 0.4 mm or less, and further preferably 0.3 mm or less.

[0113] In this specification, the thickness of the outer peripheral wall 103 refers to the length in the normal direction of the outer peripheral surface from the boundary between the outer peripheral wall 103 and the outermost cell 104 or partition wall 106 to the outer peripheral surface of the honeycomb structure part in a cross section perpendicular to the direction in which the flow path extends.

[0114] The length of the honeycomb structure in the direction in which the flow path extends and the cross-sectional area perpendicular to the direction in which the flow path extends can be adjusted according to the required size of the heater component and are not particularly limited. For example, in the case of a compact heater component that ensures the specified function, the length of the honeycomb structure in the direction in which the flow path extends can be 2 to 50 mm, typically 5 to 50 mm, and the cross-sectional area perpendicular to the direction in which the flow path extends can be 30 to 400 cm 2 , typically 50 to 150 cm 2 .

[0115] The partition walls 106 constituting the honeycomb structure are made of a material capable of generating heat by passage of electricity, specifically, a material having a PTC (Positive Temperature Coefficient) property. If necessary, the outer peripheral wall 103 may also be made of a material having a PTC property like the partition walls 106 .

[0116] In the case where a functional material layer is provided on the partition wall 106, the functional material layer can be heated by heat transfer from the heat-generating partition wall 106 (and the peripheral wall 103 as required). In addition, the material having the PTC property has the following characteristics, that is, when the temperature rises and exceeds the Curie point, the resistance value rises sharply and the current is difficult to flow. Therefore, with respect to the partition wall 106 (and the peripheral wall 103 as required), when the heater component 100 reaches a high temperature, the current flowing through them is limited, and therefore, the excessive heating of the heater component 100 is suppressed. Therefore, it is also possible to suppress the thermal degradation of the functional material layer caused by excessive heating.

[0117] From the viewpoint of obtaining moderate heat generation, the lower limit of the volume resistivity of the material having PTC characteristics at 25°C is preferably 0.5Ω·cm or more, more preferably 1Ω·cm or more, further preferably 5Ω·cm or more, and further preferably 10Ω·cm or more. From the viewpoint of making it generate heat at a low driving voltage, the upper limit of the volume resistivity of the material having PTC characteristics at 25°C is preferably 30Ω·cm or less, more preferably 20Ω·cm or less, further preferably 18Ω·cm or less, and further preferably 16Ω·cm or less. Therefore, the range of the volume resistivity of the material having PTC characteristics at 25°C can be, for example, 10Ω·cm or more and 30Ω·cm or less. In this specification, the volume resistivity of the material having PTC characteristics at 25°C is measured in accordance with JIS K6271:2008.

[0118] From the viewpoint of being able to generate heat when energized and having PTC characteristics, the outer peripheral wall 103 and the partition wall 106 are preferably made of barium titanate (BaTiO 3 ) as the main component, more preferably barium titanate (BaTiO 3 ) is a ceramic composed of a material whose main component is a crystal particle. It should be noted that in this specification, "main component" means: a component that accounts for more than 50% by mass of the total component. BaTiO 3 The content of the crystalline particles can be determined by fluorescent X-ray analysis. Other crystalline particles can also be measured in the same manner as this method.

[0119] BaTiO in which a portion of Ba is replaced by rare earth elements 3The composition formula of the crystal particles can be expressed as (Ba 1- x A x )TiO 3 In the composition formula, A represents one or more rare earth elements, and 0.0001≤x≤0.010.

[0120] A may be a rare earth element, but is not particularly limited thereto, and is preferably one or more selected from the group consisting of La, Ce, Pr, Nd, Eu, Gd, Dy, Ho, Er, Y, and Yb, and more preferably La. From the viewpoint of suppressing excessive resistance at room temperature, x is preferably 0.001 or more, and more preferably 0.0015 or more. On the other hand, from the viewpoint of suppressing excessive resistance at room temperature due to insufficient sintering, x is preferably 0.009 or less.

[0121] BaTiO in which a portion of Ba is replaced by rare earth elements 3 The content of BaTiO crystal particles in the ceramic is not particularly limited as long as it is an amount that becomes the main component, but is preferably 90% by mass or more, more preferably 92% by mass or more, and further preferably 94% by mass or more. 3 The upper limit of the content of the crystalline particles is not particularly limited, but is usually 99% by mass or less, and preferably 98% by mass or less.

[0122] From the viewpoint of reducing the environmental load, the material used for the peripheral wall 103 and the partition wall 106 is preferably substantially free of lead (Pb). Specifically, the Pb content in the peripheral wall 103 and the partition wall 106 is preferably 0.01 mass % or less, more preferably 0.001 mass % or less, and further preferably 0 mass %. With a low Pb content, air heated by contact with the heating partition wall 106, for example, can be safely blown toward living things such as humans. It should be noted that the Pb content in the peripheral wall 103 and the partition wall 106, if converted to PbO, is preferably less than 0.03 mass %, more preferably less than 0.01 mass %, and further preferably 0 mass %. The lead content can be solved using ICP-MS (inductively coupled plasma mass spectrometry).

[0123] From the viewpoint of efficiently heating the air, the lower limit of the Curie point of the material constituting the outer peripheral wall 103 and the partition wall 106 is preferably 100° C. or higher, more preferably 110° C. or higher, and even more preferably 125° C. or higher. In addition, from the viewpoint of safety as a component placed indoors, particularly in a vehicle compartment or near a vehicle compartment, the upper limit of the Curie point is preferably 250° C. or lower, more preferably 225° C. or lower, even more preferably 200° C. or lower, even more preferably 150° C. or lower, and even more preferably 130° C. or lower. Therefore, the Curie point of the material constituting the outer peripheral wall 103 and the partition wall 106 may be, for example, in the range of 100° C. or higher and 130° C. or lower.

[0124] The Curie point of the material constituting the outer peripheral wall 103 and the partition wall 106 can be adjusted by the type and amount of the shifting agent. 3 ) has a Curie point of about 120°C, but the Curie point can be moved to a lower temperature by replacing part of Ba and Ti with one or more of Sr, Sn and Zr.

[0125] In this specification, the Curie point is measured by the following method. The sample is mounted on a sample holder for measurement, assembled in a measurement tank (e.g., MINI-SUBZERO MC-810P manufactured by Espec Co., Ltd.), and a DC resistance meter (e.g., multimeter 3478A manufactured by YOKOGAWA HEWLETT PACKARD, LTD.) is used to measure the change in the resistance of the sample relative to the temperature change when the temperature is increased from 10°C. Based on the resistance-temperature graph obtained by the measurement, the temperature at which the resistance value reaches twice the resistance value at room temperature (20°C) is set as the Curie point.

[0126] (1-2. Electrode layer)

[0127] The first electrode layer 102a is provided on the first end surface 101a, and the second electrode layer 102b is provided on the second end surface 101b. By applying a voltage between the first electrode layer 102a and the second electrode layer 102b, the honeycomb structure can generate heat by Joule heat.

[0128] Specifically, the first electrode layer 102a covers a part or all of the surface of the partition wall 106 forming the first end face 101a. The second electrode layer 102b covers a part or all of the surface of the partition wall 106 forming the second end face 101b. In order to make it easy for the current to spread to the entire first end face 101a, the first electrode layer 102a preferably covers more than 80% of the area of ​​the portion (partition wall portion and peripheral wall portion) at the first end face 101a except the opening portion of the partition 104, more preferably covers more than 90%, and further preferably covers more than 99%. Similarly, in order to make the current spread to the entire second end face 101b, the second electrode layer 102b preferably covers more than 80% of the area of ​​the portion (partition wall portion and peripheral wall portion) at the second end face 101b except the opening portion of the partition 104, more preferably covers more than 90%, and further preferably covers more than 99%.

[0129] As the first electrode layer 102a and the second electrode layer 102b, there is no particular limitation, for example, a metal or alloy containing at least one selected from Cu, Ag, Al, Ni and Si can be used. In a preferred embodiment, the first electrode layer 102a and the second electrode layer 102b contain pure aluminum and / or an aluminum alloy. In addition, an ohmic electrode that can be in ohmic contact with the peripheral wall 103 and / or the partition wall 106 having PTC characteristics can also be used. The ohmic electrode can be, for example, an ohmic electrode containing at least one selected from Al, Au, Ag and In as a base metal, and containing at least one selected from Ni, Si, Zn, Ge, Sn, Se and Te for n-type semiconductors as a dopant. In addition, the first electrode layer 102a and the second electrode layer 102b can be a single-layer structure or a stacked structure of more than two layers. In the case where the first electrode layer 102a and the second electrode layer 102b have a stacked structure of more than two layers, the material of each layer can be the same type or different types. In a preferred embodiment, the first electrode layer 102 a and the second electrode layer 102 b have a single layer of pure aluminum, a two-layer structure of an Al—Ni alloy layer and a pure silver layer, or a two-layer structure of an Al—Ni alloy layer and a pure aluminum layer.

[0130] The thickness of the first electrode layer 102a and the second electrode layer 102b is not particularly limited and can be appropriately set according to the formation method of the first electrode layer 102a and the second electrode layer 102b. As the formation method of the first electrode layer 102a and the second electrode layer 102b, metal precipitation methods such as sputtering, evaporation, electrolytic precipitation, and chemical precipitation can be cited. In addition, the electrode layer can also be formed by a method of sintering after applying an electrode paste, or by spraying. In addition, the electrode layer can also be made by joining a metal plate or alloy plate such as a stamping metal with a through hole to a portion corresponding to the opening of the compartment.

[0131] The average thickness of the first electrode layer 102a and the second electrode layer 102b is not limited, and can be, for example, 5 μm or more and 100 μm or less. The lower limit of the average thickness of the first electrode layer 102a and the second electrode layer 102b is 5 μm or more, preferably 10 μm or more, and more preferably 20 μm or more, thereby obtaining the advantage of being able to avoid abnormal heating at the electrode layer. The upper limit of the average thickness of the first electrode layer 102a and the second electrode layer 102b is 100 μm or less, preferably 80 μm or less, and more preferably 60 μm or less, thereby obtaining the advantage of being able to suppress the rigidity of the electrode layer and not being easy to peel off from the end face of the honeycomb structure.

[0132] The average thickness of the first electrode layer 102a is measured in the following order. First, a cross-sectional image of the first electrode layer at about 50 times magnification is obtained using a scanning electron microscope or the like. As a cross section, it is a cross section of the honeycomb structure part parallel to the direction in which the flow path extends. In the cross-sectional image, Figure 1B As shown in the partial enlarged view of FIG. 1 , the first electrode layer is visible in each partition wall. Therefore, for each first electrode layer, the thickness T at the center position of the length of the partition wall forming the first end surface covered by the first electrode layer in the direction perpendicular to the direction in which the flow path extends is measured at two locations in one cross-sectional image. 1 The thickness direction is parallel to the direction in which the flow path extends. In this way, a large number of cross-sectional images of the first electrode layer are obtained without bias from the vicinity of the first end surface of the heater member, and the thickness T of the first electrode layer at more than 10 locations is measured as a whole. 1 The total thickness T 1 The average value of is defined as the average thickness of the first electrode layer. The average thickness of the second electrode layer 102b is also measured in the same manner.

[0133] The terminal is preferably arranged at the periphery. Therefore, if the thickness of the electrode layer at the periphery and the connection part with the terminal is large, the material of the electrode layer melts during bonding, and the bonding area with the terminal can be fully ensured, thereby improving the bonding strength with the terminal. In addition, since the bonding area with the terminal can be fully ensured, the conductivity between the electrode layer and the terminal can be improved. Accordingly, the heater component 100 preferably satisfies at least one of the following conditions (1) and (2), and more preferably satisfies both conditions.

[0134] (1) The average value of the thickness of the first electrode layer 102a at the outer peripheral portion of the first end surface 101a and at the connection portion with the first terminal 109a is larger than the average value of the thickness of the first electrode layer 102a at other portions.

[0135] (2) The average value of the thickness of the second electrode layer 102b at the outer peripheral portion of the second end surface 101b and at the connection portion with the second terminal 109b is larger than the average value of the thickness of the second electrode layer 102b at other portions.

[0136] The average value of the thickness of the first electrode layer 102a (second electrode layer 102b) at the peripheral portion of the first end face 101a (second end face 101b) and the connection portion with the first terminal 109a (second terminal 109b) is preferably 1.1 to 2.0 times, and more preferably 1.5 to 1.6 times, the average value of the thickness of the first electrode layer 102a (second electrode layer 102b) at other portions.

[0137] The average value of the thickness of the first electrode layer 102a (second electrode layer 102b) at the outer periphery of the first end face 101a (second end face 101b) and the connection portion with the first terminal 109a (second terminal 109b) is not limited, and can be, for example, 5.5 μm or more and 200 μm or less. The lower limit of the average value is 5.5 μm or more, preferably 11 μm or more, and more preferably 22 μm or more, thereby obtaining the advantage of ensuring good conduction performance. The upper limit of the average value is 200 μm or less, preferably 160 μm or less, and more preferably 120 μm or less, thereby obtaining the advantage of being able to reduce the pressure loss during air supply by ensuring the opening of the compartment 104.

[0138] The average value of the thickness of the first electrode layer 102a at the outer periphery of the first end face 101a and the connection portion with the first terminal 109a is measured in the following order. First, a cross-sectional image of the first electrode layer at about 50 times the outer periphery of the first end face and the connection portion with the first terminal is obtained using a scanning electron microscope or the like. As a cross section, it is a cross section of the honeycomb structure part parallel to the direction in which the flow path extends. In the cross-sectional image, as shown in FIG. Figure 1B As shown in the partial enlarged view of FIG. 1 , the first electrode layer is visible for each partition wall. Therefore, for each first electrode layer at the peripheral portion of the first end face and the connection portion with the first terminal, in one cross-sectional image, the thickness T at the center position of the length of the partition wall of the first end face covered by the first electrode layer in the direction perpendicular to the direction in which the flow path extends is measured at two locations. 1 The thickness direction is parallel to the direction in which the flow path extends. In this way, a large number of cross-sectional images of the first electrode layer at the outer periphery of the first end surface and the connection portion with the first terminal are obtained without bias from the vicinity of the first end surface of the heater member, and the thickness T of the first electrode layer at more than 10 locations is measured as a whole. 1 The total thickness T 1The average value of is set as the average thickness of the first electrode layer 102a at the outer periphery of the first end face 101a and the connection portion with the first terminal 109a. The average thickness of the second electrode layer 102b at the outer periphery of the second end face 101b and the connection portion with the second terminal 109b is also measured in the same order. It should be noted that the definition of the outer periphery is explained below.

[0139] The average value of the thickness of the first electrode layer 102a at the portion other than the outer periphery of the first end face 101a and the connection portion with the first terminal 109a is measured in the following order. First, a cross-sectional image of the first electrode layer at a magnification of about 50 times is obtained at the portion other than the outer periphery of the first end face and the connection portion with the first terminal using a scanning electron microscope or the like. As a cross section, it is a cross section of the honeycomb structure portion parallel to the direction in which the flow path extends. In the cross-sectional image, as shown in FIG. Figure 1B As shown in the partial enlarged view of FIG. 1 , the first electrode layer is visible for each partition wall. Therefore, for each first electrode layer at a portion other than the outer periphery of the first end face and the connection portion with the first terminal, in one cross-sectional image, the thickness T at the center position of the length of the partition wall in the direction perpendicular to the direction in which the flow path extends, which forms the first end face covered by the first electrode layer, is measured at two locations. 1 The thickness direction is parallel to the direction in which the flow path extends. In this way, a large number of cross-sectional images of the first electrode layer at portions other than the outer periphery of the first end surface and the connection portion with the first terminal are obtained without bias from the vicinity of the first end surface of the heater member, and the thickness T of the first electrode layer at more than 10 locations is measured as a whole. 1 The total thickness T 1 The average value of is set as the average thickness of the first electrode layer 102a at the portion other than the outer periphery of the first end face 101a and the connection portion with the first terminal 109a. The average thickness of the second electrode layer 102b at the portion other than the outer periphery of the second end face 101b and the connection portion with the second terminal 109b is also measured in the same order. It should be noted that the definition of the peripheral portion is explained below.

[0140] As described above, when the thickness of the electrode layer at the peripheral portion and the connection portion with the terminal is large, the terminal is firmly connected to the electrode layer, and the conduction performance between the electrode layer and the terminal can be improved. On the other hand, in order to increase the degree of freedom of the area to be connected to the terminal, it is preferred to increase the thickness of the electrode layer of the entire peripheral portion. Accordingly, the heater component 100 preferably satisfies at least one of the following (3) and (4), and more preferably satisfies both conditions.

[0141] (3) The average value of the thickness of the first electrode layer 102a in the entire outer periphery of the first end surface 101a is larger than the average value of the thickness of the first electrode layer 102a in other portions.

[0142] (4) The average value of the thickness of the second electrode layer 102b in the entire outer peripheral portion of the second end surface 101b is larger than the average value of the thickness of the second electrode layer 102b in other portions.

[0143] The average value of the thickness of the first electrode layer 102a at the entire periphery of the first end face 101a is measured in the following order. First, a cross-sectional image of the first electrode layer at about 50 times the periphery of the first end face is obtained using a scanning electron microscope or the like. As a cross section, it is a cross section of the honeycomb structure part parallel to the direction in which the flow path extends. In the cross-sectional image, Figure 1B As shown in the partial enlarged view of FIG. 1 , the first electrode layer is visible for each partition wall. Therefore, for each first electrode layer at the peripheral portion of the first end face, in one cross-sectional image, the thickness T at the center position of the length of the partition wall of the first end face covered by the first electrode layer in the direction perpendicular to the direction in which the flow path extends is measured at two locations. 1 The thickness direction is parallel to the direction in which the flow path extends. In this way, cross-sectional images of the first electrode layer at the outer peripheral portion of the first end surface are obtained at equal intervals along the circumferential direction from the vicinity of the first end surface of the heater member, and the thickness T of the first electrode layer at more than 10 locations is measured as a whole. 1 The total thickness T 1 The average value of is set as the average thickness of the first electrode layer 102a at the entire periphery of the first end face 101a. The average thickness of the second electrode layer 102b at the entire periphery of the second end face 101b is also measured in the same manner. It should be noted that the definition of the periphery is explained below.

[0144] The average value of the thickness of the first electrode layer 102a at the portion other than the peripheral portion of the first end face 101a is measured in the following order. First, a cross-sectional image of the first electrode layer at a magnification of about 50 at the portion other than the peripheral portion of the first end face is obtained using a scanning electron microscope or the like. As a cross section, it is a cross section of the honeycomb structure part parallel to the direction in which the flow path extends. In the cross-sectional image, as shown in FIG. Figure 1B As shown in the partial enlarged view of FIG. 1 , the first electrode layer is visible for each partition wall. Therefore, for each first electrode layer at a portion other than the peripheral portion of the first end surface, in one cross-sectional image, the thickness T at the center position of the length of the partition wall of the first end surface covered by the first electrode layer in the direction perpendicular to the direction in which the flow path extends is measured at two locations. 1The thickness direction is parallel to the direction in which the flow path extends. In this way, a large number of cross-sectional images of the first electrode layer at the first end surface other than the peripheral portion are obtained without bias from the vicinity of the first end surface of the heater member, and the thickness T of the first electrode layer at more than 10 locations is measured as a whole. 1 The total thickness T 1 The average value of is set as the average thickness of the first electrode layer 102a at the portion other than the peripheral portion of the first end face 101a. The average thickness of the second electrode layer 102b at the portion other than the peripheral portion of the second end face 101b is also measured in the same manner. It should be noted that the definition of the peripheral portion is explained below.

[0145] The lower limit of the volume resistivity of the first electrode layer 102a and the second electrode layer 102b at 25°C is not particularly limited, and the generally achievable range is 1.0×10 -7 From the viewpoint of making the temperature distribution uniform by allowing the current to fully spread in the surface, the upper limit of the volume resistivity of the first electrode layer 102a and the second electrode layer 102b at 25°C is preferably 1.0×10 -5 Ω·cm or less, more preferably 1.0×10 -6 Ω·cm or less, more preferably 5.0×10 -7 Ω·cm or less, more preferably 3.0×10 -7 Therefore, the volume resistivity of the first electrode layer 102a and the second electrode layer 102b at 25°C may be in the range of, for example, 1.0×10 -7 Ω·cm or more and 1.0×10 -5 In this specification, the volume resistivity of the first electrode layer 102a and the second electrode layer 102b at 25°C is measured in accordance with JIS K6271:2008.

[0146] (1-3. First and second functional material containing layers)

[0147] The first functional material-containing layer 107a can cover a portion of the outer surface of the first electrode layer 102a, and the second functional material-containing layer 107b can cover a portion of the outer surface of the second electrode layer 102b. The functional material-containing layer exists on the end surface side of the heater component, so that the function brought by the functional material can be imparted to the heater component. For example, when the first functional material-containing layer 107a and the second functional material-containing layer 107b contain a hygroscopic material, it is possible to suppress the migration of metal components in the electrode layers and the occurrence of a short circuit between the electrode layers. The outer surface of the first electrode layer 102a refers to the surface on the opposite side of the surface where the first electrode layer 102a contacts the first end surface 101a. The outer surface of the second electrode layer 102b refers to the surface on the opposite side of the surface where the second electrode layer 102b contacts the second end surface 101b.

[0148] The reason why the first functional material-containing layer 107a covers "a portion" of the outer surface of the first electrode layer 102a is that the portion of the outer surface of the first electrode layer 102a to which the first terminal 109a is connected should not be covered by the first functional material-containing layer 107a, and therefore, is not entirely covered. Similarly, the reason why the second functional material-containing layer 107b covers "a portion" of the outer surface of the second electrode layer 102b is that the portion of the outer surface of the second electrode layer 102b to which the second terminal 109b is connected should not be covered by the second functional material-containing layer 107b, and therefore, is not entirely covered.

[0149] In order to improve the performance brought by the functional material, the first functional material-containing layer 107a preferably covers more than 80% of the area of ​​the portion of the outer surface of the first electrode layer 102a that is not connected to the first terminal 109a, more preferably covers more than 90%, and further preferably covers more than 99%. Similarly, the second functional material-containing layer 107b preferably covers more than 80% of the area of ​​the portion of the outer surface of the second electrode layer 102b that is not connected to the second terminal 109b, more preferably covers more than 90%, and further preferably covers more than 99%.

[0150] The first functional material-containing layer 107a and the second functional material-containing layer 107b are preferably insulating. Foreign flying objects are easily attached near the first end face 101a and the second end face 101b. If the flying objects are conductive, they will cause short circuits. By making the first functional material-containing layer 107a and the second functional material-containing layer 107b insulating, short circuits caused by flying objects can be prevented. In this specification, the first functional material-containing layer 107a and the second functional material-containing layer 107b are insulating, which means that the first functional material-containing layer 107a and the second functional material-containing layer 107b respectively meet the following conditions related to resistance.

[0151] The coordinate value of the center of gravity O of the first end face 101a (second end face 101b) is set to 0, and the coordinate axis is obtained in the direction from the center of gravity O toward the outer contour C of the first end face 101a (second end face 101b), and the coordinate value at the outer contour C is set to 1.00R. In addition, the resistance at 25°C between two points on the outer surface of the first functional material-containing layer 107a (second functional material-containing layer 107b) whose distance between the line segment connecting the center of gravity O and an arbitrary point D with a coordinate value of 0.90R is the farthest is measured by the branch method (refer to Figure 1A ). The outer surface of the first functional material-containing layer 107a (the second functional material-containing layer 107b) refers to the surface on the opposite side of the surface where the first functional material-containing layer 107a (the second functional material-containing layer 107b) contacts the first electrode layer 102a (the second electrode layer 102b). Next, the point D is rotated and moved by 30° with the center of gravity O as the rotation center, and the resistance is measured in the same manner. For each rotation of point D by 30°, the resistance between the center of gravity O and point D is measured once (12 locations) for one cycle. The lower limit of the resistance at the 12 locations obtained is 1.0×10 4 When Ω or more, the first functional material-containing layer 107a (the second functional material-containing layer 107b) is defined as being insulating.

[0152] It should be noted that when the first terminal 109a (second terminal 109b) exists between the line segment connecting point D and the center of gravity O at the position obtained by rotating and moving point D, point D is further rotated and moved to a position where the first terminal 109a (second terminal 109b) does not exist for measurement.

[0153] The lower limit of the resistance of the first functional material-containing layer 107a and the second functional material-containing layer 107b when the resistance is measured in the above order is preferably 1.0×10 5 Ω or more, more preferably 5.0×10 5 The upper limit of the resistance of the first functional material-containing layer 107a and the second functional material-containing layer 107b is not particularly set, and the resistance range when the resistance is measured in the above-mentioned order is usually 1.0×10 5 Ω~1.0×10 7 Ω, typically 2.0×10 5 Ω~1.0×10 6 Ω.

[0154] The first functional material-containing layer 107a and the second functional material-containing layer 107b preferably contain a hygroscopic material. In this specification, a hygroscopic material refers to a substance having the property that the mass (g) of water that can be adsorbed per 1g of its dry mass after being left for one hour at room temperature (25°C) and a relative humidity of 50% is 5g / g or more. The hygroscopic material preferably has the function of being able to adsorb water at -20 to 40°C and to release it at a high temperature of 60°C or more, preferably 70 to 180°C. In this way, when the hygroscopic material has the function of adsorbing water at low temperatures and releasing it at high temperatures, the hygroscopic material can be used multiple times by repeatedly turning on and off the power.

[0155] The type of hygroscopic material is not particularly limited, and examples thereof include silica gel, sepiolite, calcium oxide, diatomaceous earth, activated carbon, activated clay, zeolite, white carbon, calcium chloride, magnesium chloride, potassium acetate, sodium hydrogen phosphate, sodium citrate, water-absorbent polymer, crystalline aluminum silicate, amorphous aluminum silicate, etc. Among them, zeolite and amorphous aluminum silicate are preferred, and amorphous aluminum silicate is more preferred, because they can release moisture in a relatively low temperature range. The hygroscopic material can be used alone or in combination of two or more. The above-mentioned hygroscopic materials are examples and are not limited to these materials.

[0156] The first functional material-containing layer 107a and the second functional material-containing layer 107b may contain an adhesive. As the adhesive, both organic adhesives and inorganic adhesives can be cited, and inorganic adhesives are preferred. The type of inorganic adhesive is not particularly limited, and examples thereof include: aluminum sol, silica sol, montmorillonite, boehmite, γ-alumina, and attapulgite. These inorganic adhesives can be used alone or in combination of two or more. Among them, aluminum sol and silica sol are preferred, and silica sol is more preferred because it is easy to ensure the adhesive force.

[0157] The first functional material-containing layer 107a and the second functional material-containing layer 107b may contain a functional material having a function of adsorbing a component to be removed in the air such as carbon dioxide and / or an organic gas component, in addition to the hygroscopic material or in place of the hygroscopic material. It is particularly preferred to contain a functional material having a function of being able to adsorb carbon dioxide and / or an organic gas component at -20 to 40°C and desorb at a high temperature of 60°C or higher, preferably 70 to 180°C. In this way, when the functional material has the function of adsorbing the component to be removed in the air at a low temperature and desorbing at a high temperature, the functional material can be used multiple times by repeatedly energizing and de-energizing.

[0158] Organic gas components contained in the air that can be removed include, for example, volatile organic compounds (VOCs), odor components, etc. Specific examples of harmful volatile components include ammonia, acetic acid, isovaleric acid, nonenal, formaldehyde, toluene, xylene, p-dichlorobenzene, ethylbenzene, styrene, chlorpyrifos, di-n-butyl phthalate, tetradecane, di-2-ethylhexyl phthalate, diazinon, acetaldehyde, N-methylcarbamic acid-2-(1-methylpropyl)phenyl ester, etc.

[0159] The above-mentioned hygroscopic materials also have such functions, and some of them are repeated in the description. However, as the types of functional materials, for example, zeolite, silica gel, activated carbon, alumina, silicon dioxide, low-crystalline clay, amorphous aluminosilicate complex, etc. can be cited. The type of functional material can be appropriately selected according to the type of the component to be removed. The functional material can be used alone or in combination of two or more.

[0160] The first functional material-containing layer 107a and the second functional material-containing layer 107b may contain a catalyst for the purpose of further purifying the removal target component or improving the capture function of the functional material (including the hygroscopic material) to capture the removal target component. As a catalyst, it is preferred to have a function of promoting the redox reaction. Examples of catalysts having such a function include metal catalysts such as Pt, Pd, and Ag, CeO 2 、ZrO 2 Oxide catalysts, etc. The catalyst may be used alone or in combination of two or more.

[0161] The average thickness of at least one of the first functional material-containing layer 107a and the second functional material-containing layer 107b, preferably both, is not limited and can be, for example, 10 μm or more and 500 μm or less. The lower limit of the average thickness of at least one of the first functional material-containing layer 107a and the second functional material-containing layer 107b, preferably both, is 10 μm or more, preferably 30 μm or more, and more preferably 50 μm or more, thereby obtaining the advantages of ensuring insulation and easily exerting the functions of the functional materials. The upper limit of the average thickness of the first functional material-containing layer 107a and the second functional material-containing layer 107b is 500 μm or less, preferably 300 μm or less, and more preferably 200 μm or less, thereby obtaining the advantages of reducing the rigidity of the functional material-containing layer and not being easy to peel off.

[0162] The average thickness of the first functional material-containing layer 107a is measured in the following order. First, a cross-sectional image of the first functional material-containing layer is obtained at about 50 times magnification using a scanning electron microscope or the like. As the cross section, it is a cross section of the honeycomb structure part parallel to the direction in which the flow path extends. In the cross-sectional image, Figure 1BAs shown in the partial enlarged view of FIG. 1 , the first functional material-containing layer is visible for each partition wall. Therefore, for each first functional material-containing layer, in one cross-sectional image, the thickness T at the center position of the length of the partition wall forming the first end face indirectly covered by the first functional material-containing layer in the direction perpendicular to the direction in which the flow path extends is measured at two locations. 2 The thickness direction is parallel to the direction in which the flow path extends. In addition, a large number of cross-sectional images of the first functional material-containing layer are obtained without bias near the first end surface of the heater component, and the thickness T of the first functional material-containing layer at more than 10 locations is measured. 2 The total thickness T 2 The average value of is defined as the average thickness of the first functional material-containing layer. The average thickness of the second functional material-containing layer 107 b is also measured in the same manner.

[0163] The first functional material-containing layer 107a preferably covers a portion or all of the outer surface of the first electrode layer 102a and other exposed surfaces of the first electrode layer 102a (e.g., the surface of the first electrode layer 102a parallel to the thickness direction), and more preferably covers all of them. Similarly, the second functional material-containing layer 107b preferably covers a portion or all of the outer surface of the second electrode layer 102b and other exposed surfaces of the second electrode layer 102b (e.g., the surface of the second electrode layer 102b parallel to the thickness direction), and more preferably covers all of them.

[0164] (1-4.Terminal)

[0165] The first terminal 109a is connected to the outer surface of the first electrode layer 102a (when the first functional material-containing layer 107a is provided, it is preferably the portion of the outer surface of the first electrode layer 102a that is not covered by the first functional material-containing layer 107a). The second terminal 109b is connected to the outer surface of the second electrode layer 102b (when the second functional material-containing layer 107b is provided, it is preferably the portion of the outer surface of the second electrode layer 102b that is not covered by the second functional material-containing layer 107b). The first terminal 109a (the second terminal 109b) is preferably at least partially arranged on the outer periphery of the first end face 101a (the second end face 101b), and more preferably all of it is arranged on the outer periphery.

[0166] As for the connection method between the first electrode layer 102a and the first terminal 109a, and between the second electrode layer 102b and the second terminal 109b, the two can be connected without any particular limitation, and the connection can be made by, for example, welding, brazing or mechanical contact. The material of the first terminal 109a and the second terminal 109b is not particularly limited, and can be, for example, metal. As the metal, a metal single substance and an alloy can be used. From the perspective of not being easily oxidized in an environment with high humidity, not being easily migrated or electro-corroded even under wet conditions, and selecting a material that is easy to join with the electrode, it is preferred to contain one or more selected from pure aluminum, aluminum alloy and stainless steel, and can be made of, for example, pure aluminum, aluminum alloy or stainless steel. In addition, an alloy containing at least one selected from the group consisting of Cr, Fe, Co, Ni, Cu and Ti can also be used, among which Fe-Ni alloy and phosphor bronze can be preferably used. From the perspective of avoiding electro-corrosion, the terminal is preferably made of a material close to the electrode layer on the end surface. As an example, it is preferred that both the electrode layer and the terminal are pure aluminum and / or aluminum alloy.

[0167] The shapes of the first terminal 109a and the second terminal 109b are not limited, and may be, for example, flat plates. The plate thickness of the terminals is not limited, and may be, for example, 0.1 to 4 mm, preferably 0.3 to 2 mm.

[0168] The area of ​​the portion of the first end face 101a that is (indirectly) covered by the first terminal 109a through the connection with the first electrode layer 102a by the first terminal 109a is not particularly limited. If the first terminal 109a is too small, it is difficult to connect the current-carrying component to the first terminal 109a. On the contrary, if the first terminal 109a is too large, the area of ​​the opening of the compartment 104 is blocked, and the flow rate of air that can flow through the heater component 100 is reduced. Therefore, relative to the area of ​​the first end face 101a, the lower limit of the proportion of the area covered by the first terminal 109a is preferably 0.5% or more, more preferably 1% or more, and further preferably 2% or more. In addition, relative to the area of ​​the first end face 101a, the upper limit of the proportion of the area covered by the first terminal 109a is preferably 10% or less, more preferably 8% or less, and further preferably 5% or less. Therefore, the ratio of the area covered by the first terminal 109a to the area of ​​the first end face 101a can be, for example, 0.5% to 10%. The ratio of the area covered by the second terminal 109b to the area of ​​the second end face 101b is similar.

[0169] The lower limit of the volume resistivity of the first terminal 109a and the second terminal 109b at 25°C is not particularly limited, and the generally achievable range is 1.0×10 -7From the viewpoint of reducing the heat energy loss at the terminal, the upper limit of the volume resistivity of the first terminal 109a and the second terminal 109b at 25°C is preferably 1.0×10 -6 Ω·cm or less, more preferably 5.0×10 -7 Ω·cm or less, more preferably 3.0×10 -7 Ω·cm or less, more preferably 2.0×10 -7 Therefore, the volume resistivity of the first terminal 109a and the second terminal 109b at 25°C may be in the range of, for example, 1.0×10 -7 Ω·cm or more and 1.0×10 -6 In this specification, the volume resistivity of the first terminal 109a and the second terminal 109b at 25°C is measured in accordance with JIS K6271:2008.

[0170] (1-5. Third and Fourth Functional Material-Containing Layers)

[0171] The third functional material-containing layer 111a can cover a portion of the outer surface of the first terminal 109a, and the fourth functional material-containing layer 111b can cover a portion of the outer surface of the second terminal 109b. By having the functional material-containing layer on the outer surface of the terminal, the function brought by the functional material can be imparted to the heater component. For example, when the third functional material-containing layer 111a and the fourth functional material-containing layer 111b contain hygroscopic materials, it is possible to suppress the migration of metal components in the terminal and short circuit. The outer surface of the first terminal 109a refers to the surface on the opposite side of the surface where the first terminal 109a contacts the first electrode layer 102a. The outer surface of the second terminal 109b refers to the surface on the opposite side of the surface where the second terminal 109b contacts the second electrode layer 102b.

[0172] The third functional material-containing layer 111a covers "a portion" of the outer surface of the first terminal 109a because the portion of the outer surface of the first terminal 109a to which the power supply component 105a is connected should not be covered by the third functional material-containing layer 111a, and therefore, not all of it is covered. Similarly, the fourth functional material-containing layer 111b covers "a portion" of the outer surface of the second terminal 109b because the portion of the outer surface of the second terminal 109b to which the power supply component 105b is connected should not be covered by the fourth functional material-containing layer 111b, and therefore, not all of it is covered.

[0173] In order to improve the performance brought by the functional material, the third functional material-containing layer 111a preferably covers more than 80% of the area of ​​the portion of the outer surface of the first terminal 109a that is not connected to the current-carrying component 105a, more preferably covers more than 90%, and further preferably covers more than 99%. Similarly, the fourth functional material-containing layer 111b preferably covers more than 80% of the area of ​​the portion of the outer surface of the second terminal 109b that is not connected to the current-carrying component 105b, more preferably covers more than 90%, and further preferably covers more than 99%.

[0174] For the same reasons as the first functional material-containing layer 107a and the second functional material-containing layer 107b, the third functional material-containing layer 111a and the fourth functional material-containing layer 111b are preferably insulating. The third functional material-containing layer 111a and the fourth functional material-containing layer 111b are insulating, which means that the third functional material-containing layer 111a and the fourth functional material-containing layer 111b respectively satisfy the following conditions related to resistance.

[0175] The resistance between any two points at a distance of 3 mm on the outer surface of the third functional material-containing layer 111a (fourth functional material-containing layer 111b) at 25°C was measured by the shunt method. The two points were selected so that there was no conducting component 105a between the line segment connecting the two points. The lower limit of the resistance obtained when the measurement points were staggered and measured at three locations was 1.0×10 4 Ω or above, it is defined that the third functional material-containing layer 111a (the fourth functional material-containing layer 111b) is insulating.

[0176] The lower limit of the resistance of the third functional material-containing layer 111a and the fourth functional material-containing layer 111b when the resistance is measured in the above order is preferably 1.0×10 5 Ω or more, more preferably 5.0×10 5 In the third functional material-containing layer 111a and the fourth functional material-containing layer 111b, the upper limit of the resistance is not particularly set, and the resistance range when the resistance is measured in the above order is usually 5.0×10 5 Ω~1.0×10 7 Ω, typically 1.0×10 6 Ω~5.0×10 6 Ω.

[0177] The functional materials contained in the third functional material-containing layer 111 a and the fourth functional material-containing layer 111 b are as described in the description of the first functional material-containing layer 107 a and the second functional material-containing layer 107 b , including preferred embodiments.

[0178] The third functional material-containing layer 111 a and the fourth functional material-containing layer 111 b may contain a binder. The binder is as described in the description of the first functional material-containing layer 107 a and the second functional material-containing layer 107 b including preferred embodiments.

[0179] The third functional material-containing layer 111a and the fourth functional material-containing layer 111b may contain a catalyst for the purpose of further purifying the removal target component or improving the capture function of the functional material (including the functional material) to capture the removal target component. The catalyst, including the preferred embodiment, is as described in the description of the first functional material-containing layer 107a and the second functional material-containing layer 107b.

[0180] The average thickness of the third functional material-containing layer 111a and the fourth functional material-containing layer 111b is not limited, and can be, for example, 10 μm or more and 500 μm or less. The lower limit of the average thickness of the third functional material-containing layer 111a and the fourth functional material-containing layer 111b is 10 μm or more, preferably 20 μm or more, and more preferably 30 μm or more, thereby obtaining the advantages of ensuring insulation and easily exerting the functions of the functional materials. The upper limit of the average thickness of the third functional material-containing layer 111a and the fourth functional material-containing layer 111b is 500 μm or less, preferably 300 μm or less, and more preferably 200 μm or less, thereby obtaining the advantages of reducing the rigidity of the functional material-containing layer and not being easy to peel off.

[0181] The average thickness of the third functional material-containing layer 111a is determined by measuring the thickness of the third functional material-containing layer at five or more locations using a cross-section method in accordance with JIS K5600-1-7:2014. The average thickness of the fourth functional material-containing layer 111b is measured in the same manner.

[0182] The third functional material-containing layer 111a preferably covers a portion or all of the outer surface of the first terminal 109a and other exposed surfaces of the first terminal 109a (e.g., the surface parallel to the plate thickness direction when the first terminal 109a is in a flat plate shape), and more preferably covers all of them. Similarly, the fourth functional material-containing layer 111b preferably covers a portion or all of the outer surface of the second terminal 109b and other exposed surfaces of the second terminal 109b (e.g., the surface parallel to the plate thickness direction when the second terminal 109b is in a flat plate shape), and more preferably covers all of them.

[0183] (1-6. Fifth functional material-containing layer)

[0184] It is preferred to have a fifth functional material-containing layer 113 that covers a portion or all of the surface of the partition wall 106 that forms the flow path inside the compartment 104. Since air containing the removal target component passes through the flow path inside the compartment 104, by covering the surface of the partition wall 106 that forms the flow path with the functional material, the performance of the heater member 100 as a whole can be improved by the functional material.

[0185] In order to improve the performance brought by the functional material, the fifth functional material-containing layer 113 preferably covers 80% or more of the surface area of ​​the partition wall 106 forming the flow path inside the compartment 104, more preferably covers 90% or more, and further preferably covers 99% or more. The ratio of the surface area of ​​the partition wall 106 forming the flow path inside the compartment 104 to the area covered by the fifth functional material-containing layer 113 is measured in the following order.

[0186] (1) A cross section passing through the center of gravity O of the first end surface 101 a (second end surface 101 b ) and parallel to the direction in which the compartment 104 extends is cut out of the heater member 100 .

[0187] (2) The obtained cross section is imaged, and by using image analysis, for each cell 104, the ratio of the length of the portion covered by the fifth functional material-containing layer 113 to the length in the cell extension direction of the surface of the partition wall 106 forming the flow path inside the cell 104 is calculated. The average value of the ratio measured for all cells 104 in the cross section is regarded as the ratio of the area covered by the fifth functional material-containing layer 113 to the area of ​​the surface of the partition wall 106 forming the flow path inside the cell 104. As an image analysis, the following method can be used, that is, on an image taken by an optical microscope (magnification 50 times), the brightness of each pixel constituting the fifth functional material-containing layer and the partition wall is measured, and the average value is used as a threshold value for binary processing to distinguish the area of ​​the fifth functional material-containing layer and the partition wall. The length of the portion of the partition wall covered by the fifth functional material-containing layer is determined, and divided by the length of the cell (the length of the honeycomb structure), thereby being able to calculate the ratio of the length of the portion covered by the fifth functional material-containing layer.

[0188] For the same reason as the first functional material containing layer 107a and the second functional material containing layer 107b, the fifth functional material containing layer 113 is preferably insulating. The fifth functional material containing layer 113 being insulating means that the fifth functional material containing layer 113 satisfies the following conditions.

[0189] A cross section of the honeycomb structure parallel to the direction in which the flow path extends is cut out of the heater member 100 to expose the fifth functional material-containing layer 113 covering the surface of the partition wall 106. The resistance between two points at any five locations 3 mm apart in the extending direction of the partition 104 at 25°C is measured by the shunt method. If the obtained resistance is 1.0×10 4 Ω or more, it is defined that the fifth functional material-containing layer 113 covering the cell has insulating properties. The fifth functional material-containing layer 113 covering other cells can also be measured in the same manner. However, if it is known that the material forming the fifth functional material-containing layer 113 is substantially the same, the result will be the same, so the measurement can be omitted.

[0190] The lower limit of the resistance of the fifth functional material-containing layer 113 when the resistance is measured in the above-mentioned procedure is preferably 1.0×10 5 Ω or more, more preferably 5.0×10 5 The upper limit of the resistance of the fifth functional material-containing layer 113 is not particularly set, and the resistance range when the resistance is measured in the above-mentioned order is usually 5.0×10 5 Ω~1.0×10 7 Ω, typically 1.0×10 6 Ω~5.0×10 6 Ω.

[0191] The functional material contained in the fifth functional material-containing layer 113 is as described in the description of the first functional material-containing layer 107 a and the second functional material-containing layer 107 b including preferred embodiments.

[0192] The fifth functional material-containing layer 113 may contain a binder. The binder is as described in the description of the first functional material-containing layer 107a and the second functional material-containing layer 107b, including preferred embodiments.

[0193] The fifth functional material-containing layer 113 may contain a catalyst for the purpose of further purifying the removal target component or improving the capture function of the functional material (including the functional material) to capture the removal target component. The catalyst, including the preferred embodiment, is as described in the description of the first functional material-containing layer 107a and the second functional material-containing layer 107b.

[0194] The average thickness of the fifth functional material-containing layer 113 is not limited, and can be, for example, 10 μm or more and 500 μm or less. The lower limit of the average thickness of the fifth functional material-containing layer 113 is 10 μm or more, preferably 20 μm or more, and more preferably 30 μm or more, thereby obtaining the advantage of easily exerting the function of the functional material. The upper limit of the average thickness of the fifth functional material-containing layer 113 is 500 μm or less, preferably 300 μm or less, and more preferably 200 μm or less, thereby obtaining the advantage of being able to maintain the opening area of ​​the compartment at a large level and suppress the ventilation resistance at a low level.

[0195] The average thickness of the fifth functional material-containing layer 113 is measured in the following order. First, a cross-sectional image of the fifth functional material-containing layer 113 at about 50 times magnification is obtained using a scanning electron microscope or the like. As a cross section, it is a cross section of the honeycomb structure part parallel to the direction in which the flow path extends. In the cross-sectional image, Figure 1B As shown in the partial enlarged view of , two fifth functional material-containing layers 113 sandwiching the partition wall are seen for each partition wall, so the thickness of each fifth functional material-containing layer 113 is calculated by dividing the overall cross-sectional area from the first end face 101a to the second end face 101b of each fifth functional material-containing layer 113 by the length from the first end face 101a to the second end face 101b of the partition wall covered by the fifth functional material-containing layer. In addition, a large number of cross-sectional images of the fifth functional material-containing layer 113 are obtained without bias from the heater member, and the thickness of more than 5 fifth functional material-containing layers 113 is measured. The average value of the thicknesses of all the fifth functional material-containing layers 113 measured is set as the average thickness of the fifth functional material-containing layer.

[0196] It should be noted that the first to fifth classifications of various functional material-containing layers are for convenience of description. Therefore, it is not necessary to form separate layers, and functional material-containing layers of different classifications can be continuous and can be formed simultaneously in a single process.

[0197] (1-7. Power-carrying parts)

[0198] The first terminal 109a and the second terminal 109b can be connected to the conducting parts 105a and 105b, respectively. As the conductive materials constituting the conducting parts 105a and 105b, stainless steel, aluminum, aluminum alloy, copper alloy, and copper can be cited. Regarding the connection method between the first terminal 109a and the conducting part 105a, and between the second terminal 109b and the conducting part 105b, it is not particularly limited as long as the two are conductive. For example, they can be connected by welding, brazing, or mechanical contact. In one embodiment, the conducting parts 105a and 105b can be the wire itself between the power source and the first terminal 109a (second terminal 109b), that is, copper wire, copper alloy wire, aluminum wire, aluminum alloy wire, and stainless steel wire. In another embodiment, the conducting parts 105a and 105b can be intermediate parts that connect the wire and the first terminal 109a (second terminal 109b). The intermediate member can be connected to the electric wire by any method such as welding, soldering, brazing, riveting, and bolting, or other methods.

[0199] (2. Heater component assembly having an end-surface clamping frame)

[0200] A heater component according to one embodiment of the present invention is provided as a heater component assembly held in a frame. The protection of the frame prevents the heater component from being damaged when it is placed in a ventilation path, ensures electrical insulation from surrounding components, and has a shape that is easy to assemble in an air conditioning system. Figure 2A and Figure 2B 2 shows an example of a heater member assembly including a frame 120 that holds the heater member 100 from the first end surface 101 a side and the second end surface 101 b side.

[0201] The frame body 120 includes a first frame portion 121 and a second frame portion 122 for sandwiching the heater member from the first end surface 101 a side and the second end surface 101 b side.

[0202] The first frame portion is a resin-made first frame portion 121 disposed on the first end face 101a side, and includes: a flange portion 121b disposed on the outer peripheral side of the outer peripheral contour C of the first end face 101a, and a retaining portion 121a disposed on the inner peripheral side of the outer peripheral contour C of the first end face 101a and applying pressure to at least a portion of the outer peripheral portion of the first end face 101a. In addition, the second frame portion 122 is a resin-made second frame portion 122 disposed on the second end face 101b side, and includes: a flange portion 122b disposed on the outer peripheral side of the outer peripheral contour C of the second end face 101b, and a retaining portion 122a disposed on the inner peripheral side of the outer peripheral contour C of the second end face 101b and applying pressure to at least a portion of the outer peripheral portion of the second end face 101b.

[0203] In this specification, the coordinate value of the center of gravity O of the first end face 101a (second end face 101b) is set to 0, and a coordinate axis is drawn in the direction from the center of gravity O toward the outer contour C of the first end face 101a (second end face 101b). If the coordinate value at the outer contour C is set to 1.00R, the set of points located between 0.90R and 1.00R is set to the outer periphery of the first end face 101a (second end face 101b).

[0204] In one embodiment, the first frame 121 (second frame 122) is annular in shape and can be designed in specific shape and size according to the shape and size of the first end surface 101a (second end surface 101b) of the heater member 100.

[0205] The holding portion 121a (122a) can apply pressure to the first end surface 101a (second end surface 101b) on the inner peripheral side of the outer peripheral portion. However, if the holding portion 121a (122a) is enlarged, it is easy to hinder the air flow entering and exiting the heater member 100. Therefore, the holding portion 121a (122a) preferably applies pressure only to the outer peripheral portion of the first end surface 101a (second end surface 101b).

[0206] In addition, from the viewpoint of not hindering the air flow in and out of the heater member 100, the area of ​​the portion of the first end face 101a (second end face 101b) to which the pressure is applied by the retaining portion 121a (122a) is preferably 10% or less of the entire area of ​​the first end face 101a (second end face 101b), more preferably 8% or less, further preferably 5% or less, further preferably 2% or less, further preferably 1.8% or less, further preferably 1.6% or less. In addition, from the viewpoint of improving the holding performance for the heater member 100, the area of ​​the portion of the first end face 101a (second end face 101b) to which the pressure is applied by the retaining portion 121a (122a) is preferably 1% or more of the entire area of ​​the first end face 101a (second end face 101b), more preferably 1.2% or more, further preferably 1.4% or more. Therefore, the ratio of the area of ​​the portion of the first end surface 101a (second end surface 101b) subjected to pressure by the holding portion 121a (122a) to the entire area of ​​the first end surface 101a (second end surface 101b) can be, for example, 1% to 10%.

[0207] From the viewpoint of not hindering the airflow in and out of the heater component 100, the upper limit of the width W of the retaining portion 121a (122a) is preferably less than 7 mm, more preferably less than 5 mm, and further preferably less than 4 mm. In addition, from the viewpoint of improving the holding performance for the heater component 100, the lower limit of the width W of the retaining portion 121a (122a) is preferably more than 1 mm, more preferably more than 2 mm, and further preferably more than 3 mm. Therefore, the range of the width W of the retaining portion 121a (122a) can be, for example, more than 1 mm and less than 7 mm. Here, the width W of the retaining portion 121a (122a) refers to: the length of the retaining portion 121a (122a) in the direction from the outer peripheral contour C of the first end face 101a (second end face 101b) toward the center of gravity O of the first end face 101a (second end face 101b).

[0208] The resin constituting at least one of the first frame 121 and the second frame 122, preferably both, preferably has a certain degree of softness so that the heater member 100 is not easily damaged. Therefore, in one embodiment, the upper limit of the Rockwell hardness of the resin constituting at least one of the first frame 121 and the second frame 122, preferably both, measured in accordance with ASTM D785-2008R15 is preferably 150HRR or less, more preferably 130HRR or less, and further preferably 120HRR or less. In another embodiment, the upper limit of the Rockwell hardness of the resin constituting at least one of the first frame 121 and the second frame 122, preferably both, measured in accordance with ASTM D785-2008R15 is preferably 120HRM or less, more preferably 100HRM or less, and further preferably 90HRM or less. The resin constituting at least one of the first frame 121 and the second frame 122, preferably both, can satisfy the above-mentioned conditions related to the upper limit of either the Rockwell hardness HRR or HRM, and preferably satisfies both conditions.

[0209] On the other hand, from the viewpoint of improving the holding performance of the heater component 100, the resin constituting at least one of the first frame portion 121 and the second frame portion 122, preferably both, preferably has a certain degree of hardness. Therefore, in one embodiment, the lower limit of the Rockwell hardness of the resin constituting at least one of the first frame portion 121 and the second frame portion 122, preferably both, measured in accordance with ASTM D785-2008R15 is preferably 70HRR or more, more preferably 80HRR or more, and further preferably 90HRR or more. In another embodiment, the lower limit of the Rockwell hardness of the resin constituting at least one of the first frame portion 121 and the second frame portion 122, preferably both, measured in accordance with ASTM D785-2008R15 is preferably 40HRM or more, more preferably 50HRM or more, and further preferably 70HRM or more. The resin constituting at least one of the first frame portion 121 and the second frame portion 122 , and preferably both of them, may satisfy the above-mentioned condition regarding the lower limit of either Rockwell hardness HRR or HRM, and preferably both of them.

[0210] Therefore, in one embodiment, the Rockwell hardness of the resin constituting at least one of the first frame portion 121 and the second frame portion 122, preferably both, measured in accordance with ASTM D785-2008R15 is, for example, 70 HRR or more and 150 HRR or less. In another embodiment, the Rockwell hardness of the resin constituting at least one of the first frame portion 121 and the second frame portion 122, preferably both, is, for example, 40 HRM or more and 120 HRM or less.

[0211] There is no particular restriction on the type of resin constituting the first frame portion 121 and the second frame portion 122. From the viewpoint of heat resistance, the resin constituting at least one of the first frame portion 121 and the second frame portion 122, and preferably both of them, preferably contains one or both of polyetheretherketone (PEEK) and polybutylene terephthalate (PBT). More preferably, the total content of polyetheretherketone (PEEK) and polybutylene terephthalate (PBT) is 80% by mass or more, and further preferably, the total content is 90% by mass or more, and the total content can be 100% by mass.

[0212] The resin constituting the first frame portion 121 and the second frame portion 122 preferably has heat resistance. Therefore, the lower limit of the load deflection temperature measured in accordance with JIS K7191-1:2015 of the resin constituting at least one of the first frame portion 121 and the second frame portion 122, preferably both, is preferably 145°C or more, more preferably 160°C or more, and further preferably 180°C or more. The upper limit of the load deflection temperature is not particularly set, but is usually 300°C or less, typically 250°C or less, from the perspective of ease of availability. Therefore, the load deflection temperature of the resin constituting at least one of the first frame portion 121 and the second frame portion 122, preferably both, is in the range of, for example, 145°C or more and 300°C or less.

[0213] The resin constituting the first frame portion 121 and the second frame portion 122 preferably has a high melting point that does not melt when heated. Therefore, the lower limit of the melting point of the resin constituting at least one of the first frame portion 121 and the second frame portion 122, preferably both, is preferably 250°C or more, more preferably 280°C or more, and further preferably 300°C or more. The upper limit of the melting point is not particularly set, but is usually 400°C or less, typically 350°C or less, from the perspective of ease of availability. Therefore, the melting point of the resin constituting at least one of the first frame portion 121 and the second frame portion 122, preferably both, is, for example, in the range of 250°C or more and 400°C or less.

[0214] In this specification, the melting point of a resin refers to the lowest temperature among the temperatures at which an endothermic peak due to melting is observed when measuring by TG-DTA (thermogravimetry-differential thermal analysis).

[0215] The resin constituting the first frame portion 121 and the second frame portion 122 preferably has a low thermal conductivity in order to reduce heat loss. Therefore, the upper limit of the thermal conductivity of the resin constituting at least one of the first frame portion 121 and the second frame portion 122, preferably both, measured in accordance with JISR1611:2010 at 25°C is preferably 0.5 W / m / K or less, more preferably 0.3 W / m / K or less, and further preferably 0.2 W / m / K or less. The lower limit of the thermal conductivity is not particularly set, but from the perspective of ease of acquisition, it is usually 0.1 W / m / K or more, and typically 0.15 W / m / K or more. Therefore, the range of the thermal conductivity of the resin constituting at least one of the first frame portion 121 and the second frame portion 122, preferably both, is, for example, 0.1 W / m / K or more and 0.5 W / m / K or less.

[0216] The resin constituting the first frame portion 121 and the second frame portion 122 is preferably insulating in order to suppress short circuits. Therefore, the lower limit of the volume resistivity of the resin constituting at least one of the first frame portion 121 and the second frame portion 122, preferably both, at 25° C. measured by the bridge method according to JIS C2139:2008 is preferably 1.0×10 16 Ω·cm or more, more preferably 2.0×10 16 Ω·cm or more, more preferably 5.0×10 16 The upper limit of the volume resistivity is not particularly set, but is usually 1.0×10 18 Ω·cm or less, typically 1.0×10 17 Therefore, the volume resistivity of the resin constituting at least one of the first frame portion 121 and the second frame portion 122, preferably both of them, is in the range of, for example, 1.0×10 16 Ω·cm or more and 1.0×10 18 Ω·cm or less.

[0217] The holding portion 121a (122a) can directly apply pressure to the first end face 101a (second end face 101b), but it is preferred to apply pressure indirectly via the buffer material 127. The holding portion 121a (122a) applies pressure indirectly via the buffer material 127 to the first end face 101a (second end face 101b), so that the first end face 101a (second end face 101b) is not easily damaged. In addition, the buffer material 127 can also deform in accordance with the thermal deformation of the heater component 100, thereby relieving thermal stress. Thus, cracks in the heater component 100 can be suppressed.

[0218] From the viewpoint of ensuring the deformation amount sufficient for the buffering effect, the lower limit of the thickness in the compression direction of the buffer material 127 compressed by the pressure applied to the retaining portion 121a (122a) is preferably 0.5 mm or more, more preferably 1.0 mm or more, and further preferably 2.0 mm or more. From the viewpoint of ensuring the surface pressure of the heater component and retaining the heater component without damage, the upper limit of the thickness in the compression direction of the buffer material 127 compressed by the pressure applied to the retaining portion 121a (122a) is preferably 7.0 mm or less, more preferably 5.0 mm or less, and further preferably 4.0 mm or less. Therefore, the thickness in the compression direction of the buffer material 127 compressed by the pressure applied to the retaining portion 121a (122a) can range from, for example, 0.5 mm or more to 7.0 mm or less.

[0219] The lower limit of the pressure received by the buffer material 127 from the holding portion 121a (122a) is preferably 0.002 MPa or more, and more preferably 0.005 MPa or more. The upper limit of the pressure received by the buffer material 127 from the holding portion 121a (122a) is preferably 0.2 MPa or less, and more preferably 0.1 MPa or less. Therefore, the pressure received by the buffer material 127 from the holding portion 121a (122a) is preferably, for example, 0.002 MPa to 0.2 MPa, and more preferably 0.005 MPa to 0.1 MPa. The pressure received by the buffer material 127 from the holding portion 121a (122a) is solved based on the Young's modulus and displacement of the buffer material 127.

[0220] From the viewpoint of ensuring the surface pressure maintained for the honeycomb heater component, the lower limit of the Young's modulus of the buffer material 127 is preferably 0.05 MPa or more, more preferably 0.06 MPa or more, and further preferably 0.1 MPa or more. From the viewpoint of ensuring the deformation amount for obtaining a sufficient buffering effect, the upper limit of the Young's modulus of the buffer material 127 is preferably 0.3 MPa or less, more preferably 0.25 MPa or less, and further preferably 0.2 MPa or less. Therefore, the range of the Young's modulus of the buffer material 127 can be, for example, 0.05 MPa or more and 0.3 MPa or less.

[0221] The Young's modulus of the cushioning material 127 is obtained from the relationship between the surface pressure and the thickness change (displacement amount) when the sheet-shaped cushioning material is compressed by gradually applying surface pressure.

[0222] The type of material constituting the buffer material 127 is not particularly limited. From the viewpoint of ensuring sufficient deformation, it is preferably made of rubber, and more preferably made of rubber sponge. Sponge refers to a porous body. Rubber and rubber sponge can contain various rubbers such as natural rubber, styrene-butadiene rubber, butadiene rubber, chloroprene rubber, ethylene-propylene rubber, butyl rubber, fluororubber, acrylonitrile-butadiene rubber, silicone rubber, isoprene rubber, urethane rubber, chlorosulfonated polyethylene, hydrogenated nitrile rubber, epichlorohydrin rubber, acrylic rubber, ethylene acrylic rubber, norbornene rubber, etc. These rubbers can be contained alone or in a mixture of two or more. Among them, the buffer material 127 is more preferably made of silicone rubber sponge with silicone rubber as the main component (preferably 60% by mass or more, more preferably 80% by mass or more).

[0223] In one embodiment, the first frame portion 121 and the second frame portion 122 can be provided in a state separated from each other. In this case, the first frame portion 121 and the second frame portion 122 can be connected by a fastener 124. By connecting with the fastener 124, the advantage of easily adjusting the pressure applied by the retaining portion 121a (122a) to the first end face 101a (second end face 101b) is obtained. The fastener 124 can be fixed to the flange portion 121b (flange portion 122b). As the fastener 124, there is no limitation, and a combination of a bolt and a nut can be cited. A recess 125 for accommodating the fastener 124 can be provided in the first frame portion 121 and the second frame portion 122. By providing the recess 125, the fastener 124 is not easily accidentally deviated. The number and positions of the parts where the first frame 121 and the second frame 122 are connected by the fasteners 124 can be appropriately set in a manner that can stably hold the heater component 100. As an example, it is preferable to set 4 to 8 parts at equal intervals in the circumferential direction of the flange 121b (flange 122b) when the heater component assembly is viewed from the first end surface 101a (second end surface 101b) side (see Figure 2A ).

[0224] When the first frame portion 121 and the second frame portion 122 are separated from each other, other methods for connecting the two are not limited, and examples thereof include a method of connecting by a fitting structure and a method of connecting by an adhesive.

[0225] Figure 3A and Figure 3B 2 shows another example of a heater member assembly including a frame 120 that holds the heater member 100 from the first end surface 101 a side and the second end surface 101 b side. Figure 3A and Figure 3B The holding portion 121a of the first frame portion 121 of the frame body 120 shown in the figure has a portion that presses the first terminal 109a toward the first end surface 101a. Figure 3A and Figure 3B The holding portion 122 a of the second frame portion 122 of the illustrated frame body 120 has a portion that presses the second terminal 109 b toward the second end surface 101 b .

[0226] The holding portion 121a (holding portion 122a) has a portion that presses the first terminal 109a (second terminal 109b) toward the first end surface 101a (second end surface 101b), thereby preventing the first terminal 109a (second terminal 109b) from falling off. In addition, the conductive characteristics between the first terminal 109a (second terminal 109b) and the first electrode layer 102a (second electrode layer 102b) are improved.

[0227] In order to improve the effect of preventing the first terminal 109a from falling off, the retaining portion 121a of the first frame portion 121 preferably has a portion 126a that partially protrudes toward the inner circumference, and the protruding portion 126a constitutes at least a part of the portion that presses the first terminal 109a toward the first end face 101a. Similarly, in order to improve the effect of preventing the second terminal 109b from falling off, the retaining portion 122a of the second frame portion 122 preferably has a portion 126b that partially protrudes toward the inner circumference, and the protruding portion 126b constitutes at least a part of the portion that presses the second terminal 109b toward the second end face 101b.

[0228] When the proportion of the area of ​​the portion of the outer surface of the first terminal 109a (second terminal 109b) that is pressed toward the first end face 101a (second end face 101b) by the portion 126a (126b) protruding toward the inner circumference of the retaining portion 121a (122a) is large, the effect of preventing the first end face 101a (second end face 101b) from falling off is improved. From this aspect, the lower limit of the proportion of the area is preferably 10% or more, more preferably 15% or more, and further preferably 20% or more. On the other hand, when the proportion of the area is small, it is easy to ensure space for the current-carrying components and to easily engage the current-carrying components 105a (105b). From this aspect, the upper limit of the proportion of the area is preferably 80% or less, more preferably 75% or less, and further preferably 70% or less. Therefore, the range of the proportion of the area can be, for example, 10 to 80%.

[0229] Since only the holding portion 121a (holding portion 122a) partially protrudes toward the inner circumference, the area of ​​the opening of the compartment 104 that is blocked can be reduced. When the portion 126a (126b) that partially protrudes toward the inner circumference in order to press the first terminal 109a (second terminal 109b) toward the first end surface 101a (second end surface 101b) is viewed from the first end surface 101a (second end surface 101b) side (refer to Figure 3A), the upper limit of the ratio of the area of ​​the portion 126a (126b) partially protruding toward the inner circumference (when there are multiple portions 126a (126b) partially protruding toward the inner circumference, it refers to their total area.) to the area of ​​the first end face 101a (second end face 101b) is preferably 10% or less, more preferably 5% or less, and further preferably 3% or less. On the other hand, from the viewpoint of improving the effect of preventing the first terminal 109a (second terminal 109b) from falling off, the lower limit of the ratio of the area of ​​the portion 126a (126b) partially protruding toward the inner circumference to the area of ​​the first end face 101a (second end face 101b) is preferably 0.5% or more, more preferably 1% or more, and further preferably 2% or more. Therefore, the range of the ratio of the area of ​​the portion 126a (126b) partially protruding toward the inner circumference to the area of ​​the first end face 101a (second end face 101b) can be, for example, 0.5% or more and 10% or less.

[0230] It should be explained that Figure 3A and Figure 3B In the heater component assembly, Figure 2A and Figure 2B The same symbols represent the components as in Figure 2A and Figure 2B The description of the heater component assembly is described in the description of the heater component assembly, so the description is omitted.

[0231] Figure 2A and Figure 2B The heater assembly shown and Figure 3A and Figure 3B In the heater assembly shown in FIG. 1 , there is a gap between the first frame portion 121 and the second frame portion 122, and the outer peripheral surface of the outer peripheral wall 103 of the heater component 100 is exposed. Figure 4A and Figure 4B As shown, the frame 120 may include a third frame portion 123 made of resin surrounding the outer peripheral surface 103 e of the outer peripheral wall 103 , so as to improve the protection performance of the frame 120 for the heater member 100 .

[0232] The third frame portion 123 may be connected to the first frame portion 121 or the second frame portion 122, or may be integrally formed with the first frame portion 121 or the second frame portion 122. In addition, the third frame portion 123 may have a through hole for the fastener 124 to pass through.

[0233] The material such as Rockwell hardness, type, load deflection temperature, melting point, thermal conductivity, and volume resistivity of the resin constituting the third frame portion 123 are as described in the description of the first frame portion 121 and the second frame portion 122 including the preferred embodiment.

[0234] The third frame portion 123 may not be in contact with the outer peripheral wall 103. From the viewpoint of stably holding the heater component 100 in the frame body 120, the third frame portion 123 may be in contact with the outer peripheral wall 103. From the viewpoint of improving the protection performance for the heater component 100, the buffer material 131 may be interposed between the third frame portion 123 and the outer peripheral wall 103. When the buffer material 131 is interposed between the third frame portion 123 and the outer peripheral wall 103, from the viewpoint of improving the protection performance for the heater component 100 and stably holding the heater component 100 in the frame body 120, the buffer material 131 is preferably in a compressed state by being sandwiched between the third frame portion 123 and the outer peripheral wall 103.

[0235] From the viewpoint of ensuring the deformation amount to obtain a sufficient buffering effect, the lower limit of the thickness in the compression direction of the buffer material 131 compressed by being sandwiched between the third frame portion 123 and the peripheral wall 103 is preferably 0.5 mm or more, more preferably 1.0 mm or more, and further preferably 2.0 mm or more. Considering the need to ensure that the heater component maintains the surface pressure and does not damage the heater component, the upper limit of the thickness in the compression direction of the buffer material 131 compressed by being sandwiched between the third frame portion 123 and the peripheral wall 103 is preferably 7.0 mm or less, more preferably 5.0 mm or less, and further preferably 4.0 mm or less. Therefore, the range of the thickness in the compression direction of the buffer material 131 compressed by being sandwiched between the third frame portion 123 and the peripheral wall 103 can be, for example, 0.5 mm or more and 7.0 mm or less.

[0236] The lower limit of the pressure to which the buffer material 131 is subjected when sandwiched between the third frame portion 123 and the peripheral wall 103 is preferably 0.002 MPa or more, and more preferably 0.005 MPa or more. The upper limit of the pressure to which the buffer material 131 is subjected is preferably 0.2 MPa or less, and more preferably 0.1 MPa or less. Therefore, the pressure to which the buffer material 131 is subjected is preferably, for example, 0.002 MPa to 0.2 MPa, and more preferably 0.005 MPa to 0.1 MPa. The pressure to which the buffer material 131 is subjected is solved based on the Young's modulus and displacement of the buffer material 131.

[0237] From the viewpoint of ensuring the surface pressure maintained for the honeycomb heater component, the lower limit of the Young's modulus of the buffer material 131 is preferably 0.05 MPa or more, more preferably 0.06 MPa or more, and further preferably 0.1 MPa or more. From the viewpoint of ensuring the deformation amount for obtaining a sufficient buffering effect, the upper limit of the Young's modulus of the buffer material 131 is preferably 0.3 MPa or less, more preferably 0.25 MPa or less, and further preferably 0.2 MPa or less. Therefore, the range of the Young's modulus of the buffer material 131 can be, for example, 0.05 MPa or more and 0.3 MPa or less.

[0238] The method for measuring the Young's modulus of the cushioning material 131 is as described in the description of the cushioning material 127 .

[0239] The material constituting the cushioning material 131 is as described in the description of the cushioning material 127 including preferred embodiments.

[0240] It should be explained that Figure 4A and Figure 4B In the heater component assembly, Figure 3A and Figure 3B The same symbols represent the components as in Figure 3A and Figure 3B The description of the heater component assembly is described in the description of the heater component assembly, so the description is omitted.

[0241] Figure 5A and Figure 5B 2 shows another example of a heater member assembly including a frame 120 that holds the heater member 100 from the first end surface 101 a side and the second end surface 101 b side. Figure 5A and Figure 5B The holding portion 121a of the first frame portion 121 of the frame body 120 shown in the figure has a plurality of portions 126a that partially protrude toward the inner circumference. Figure 5A and Figure 5B The holding portion 122 a of the second frame portion 122 of the frame body 120 shown in the figure has a plurality of portions 126 b that partially protrude toward the inner circumference side.

[0242] Figure 5A and Figure 5B In the first frame portion 121 of the frame body 120 shown in the figure, only the portion 126a partially protruding toward the inner peripheral side constitutes the holding portion 121a that applies pressure to at least a portion of the outer peripheral portion of the first end surface 101a. Figure 5A and Figure 5B In the second frame portion 122 of the frame body 120 shown in the figure, only a portion 126b partially protruding toward the inner peripheral side constitutes a holding portion 122a for applying pressure to at least a portion of the outer peripheral portion of the second end surface 101b.

[0243] When only the portion 126a partially protruding toward the inner circumference side constitutes the holding portion 121a that applies pressure to at least a portion of the outer circumference of the first end surface 101a, the protruding portion 126a is preferably provided at a plurality of locations in order to stably hold the heater member 100. Similarly, when only the portion 126b partially protruding toward the inner circumference side constitutes the holding portion 122a that applies pressure to at least a portion of the outer circumference of the second end surface 101b, the protruding portion 126b is preferably provided at a plurality of locations in order to stably hold the heater member 100.

[0244] When the protruding portion 126a (126b) is provided at a plurality of locations, it is preferred that the protruding portion 126a (126b) is provided at 4 to 8 locations at equal intervals in the circumferential direction of the first frame portion 121 (second frame portion 122) when the heater assembly is viewed from the first end surface 101a (second end surface 101b) and / or is provided point-symmetrically with the center of gravity O as the center of symmetry (see Figure 5A ).

[0245] At least one of the protruding portions 126a (126b) preferably has a portion that presses the first terminal 109a (second terminal 109b) toward the first end face 101a (second end face 101b). The other protruding portions 126a (126b) do not need to play a role in pressing the first terminal 109a (109b) toward the first end face 101a (second end face 101b), and it is sufficient for them to play a role as the retaining portion 121a (121b) that applies pressure to at least a portion of the outer periphery of the first end face 101a (second end face 101b).

[0246] When only the portion 126a (126b) partially protruding toward the inner circumference constitutes the holding portion 121a (122a) that applies pressure to at least a portion of the outer circumference of the first end surface 101a (second end surface 101b), when the protruding portion 126a (126b) is viewed from the first end surface 101a (second end surface 101b) side (refer to Figure 5A ), the upper limit of the ratio of the area of ​​the portion 126a (126b) that partially protrudes toward the inner circumference (when there are multiple portions 126a (126b) that partially protrude toward the inner circumference, it refers to their total area.) to the area of ​​the first end face 101a (second end face 101b) is preferably 1.0% or less, more preferably 0.8% or less, and further preferably 0.5% or less. On the other hand, from the viewpoint of improving the effect of preventing the first terminal 109a (second terminal 109b) from falling off, the lower limit of the ratio of the area of ​​the portion 126a (126b) that partially protrudes toward the inner circumference (when there are multiple portions 126a (126b) that partially protrude toward the inner circumference, it refers to their total area.) to the area of ​​the first end face 101a (second end face 101b) is preferably 0.1% or more, more preferably 0.3% or more, and further preferably 0.4% or more. Therefore, the ratio of the area of ​​the portion 126a (126b) partially protruding toward the inner circumference to the area of ​​the first end surface 101a (second end surface 101b) may be in the range of, for example, 0.1% to 1.0%.

[0247] Figure 5A and Figure 5BIn the frame 120 shown, the first frame portion 121 (the second frame portion 122) has a passage 130a (130b) for the conducting component 105a (105b) that passes from the inner peripheral side to the outer peripheral side. The conducting component 105a (105b) is inserted into the passage 130a (130b) and has an end portion 105c (105d) that can be electrically connected to an electric wire on the outer peripheral surface side of the first frame portion 121 (the second frame portion 122).

[0248] in addition, Figure 5A and Figure 5B The frame 120 shown is divided into two parts, and the two parts are connected by a connecting portion 150 having a fitting structure. In the illustrated embodiment, the dividing portion 154 is located at the second frame portion 122, but there is no particular limitation on the position of the dividing portion 154. For example, the dividing portion 154 can be freely set at the first frame portion 121, the third frame portion 123, the boundary between the first frame portion 121 and the third frame portion 123, and the boundary between the second frame portion 122 and the third frame portion 123, etc., in addition to being set at the second frame portion 122.

[0249] The connecting portion 150 shown in the figure has a convex portion 151 and a concave portion 152 of a press-fitting type. If the convex portion 151 is pressed into the concave portion 152 while being elastically deformed, the connecting state is maintained by the restoring force of the convex portion 151 and the concave portion 152. The connecting portion 150 may have other interlocking structures such as a snap-fitting type in addition to the press-fitting type. It is preferred that a cushioning material 132 is sandwiched between the two parts. The cushioning material 132 sandwiched and compressed between the two parts plays a role of a spring by elastic deformation, and can prevent the loosening of the connecting state between the two parts.

[0250] From the viewpoint of ensuring the surface pressure maintained for the honeycomb heater component, the lower limit of the Young's modulus of the buffer material 132 is preferably 0.05MPa or more, more preferably 0.06MPa or more, more preferably Pa or more, more preferably 0.06MPa or more, and more preferably MPa or more. From the viewpoint of ensuring the deformation amount for obtaining a sufficient buffering effect, the upper limit of the Young's modulus of the buffer material 132 is preferably 0.3MPa or less, more preferably 0.25MPa or less, and more preferably 0.2MPa or less. Therefore, the range of the Young's modulus of the buffer material 132 can be, for example, 0.05MPa or more and 0.3MPa or less.

[0251] The method for measuring the Young's modulus of the cushioning material 132 is as described in the description of the cushioning material 127 .

[0252] The material constituting the cushioning material 132 is as described in the description of the cushioning material 127 including preferred embodiments.

[0253] It should be explained that Figure 5A and Figure 5B In the heater component assembly, Figure 4A and Figure 4B The same symbols represent the components as in Figure 4A and Figure 4B The description of the heater component assembly is described in the description of the heater component assembly, so the description is omitted.

[0254] (3. Method for manufacturing heater member)

[0255] Next, a method for producing the heater member of the present invention will be described illustratively.

[0256] The method for manufacturing the honeycomb structure portion constituting the heater member includes a molding step and a firing step.

[0257] In the molding process, the BaCO 3 Powder, TiO 2 A raw material of ceramics containing powder of nitrate or hydroxide of rare earth is molded into a form to produce a honeycomb molded body having a relative density of 60% or more.

[0258] The ceramic raw material can be obtained by dry-mixing various powders in a desired composition.

[0259] The green material can be obtained by adding a dispersion medium, a binder, a plasticizer, and a dispersant to a ceramic raw material and kneading the mixture. The green material may contain additives such as a displacement agent, a metal oxide, a property improving agent, and a conductor powder as required.

[0260] The blending amount of the components other than the ceramic raw material is not particularly limited as long as the relative density of the honeycomb formed body becomes 60% or more.

[0261] Here, in the present specification, the "relative density of the honeycomb formed body" refers to the ratio of the density of the honeycomb formed body to the true density of the entire ceramic raw material. Specifically, it can be solved by the following formula.

[0262] Relative density of honeycomb molded body (%) = Density of honeycomb molded body (g / cm 3 ) / True density of ceramic raw material as a whole (g / cm 3 )×100

[0263] The density of the honeycomb molded body can be measured by the Archimedean method using pure water as the medium. In addition, the true density of the entire ceramic raw material can be obtained by dividing the total mass (g) of each raw material by the total actual volume (cm 3 ) to solve.

[0264] Examples of the dispersion medium include water and a mixed solvent of water and an organic solvent such as alcohol, and water can be particularly preferably used.

[0265] Examples of the binder include organic binders such as methylcellulose, hydroxypropoxycellulose, hydroxyethylcellulose, carboxymethylcellulose, and polyvinyl alcohol. In particular, it is preferred to use methylcellulose and hydroxypropoxycellulose in combination. The binder may be used alone or in combination of two or more, but preferably does not contain an alkali metal element.

[0266] Examples of the plasticizer include polyoxyethylene alkyl ether, polycarboxylic acid-based polymers, and alkyl phosphate esters.

[0267] As the dispersant, a surfactant such as polyoxyethylene alkyl ether, ethylene glycol, dextrin, fatty acid soap, polyol, etc. may be used. The dispersant may be used alone or in combination of two or more.

[0268] The honeycomb molded body can be produced by extrusion molding a blank. During the extrusion molding, a die having a desired overall shape, cell shape, cell wall thickness, cell density, etc. can be used.

[0269] The lower limit of the relative density of the honeycomb formed body obtained by extrusion molding is preferably 60% or more, more preferably 65% ​​or more. By controlling the relative density of the honeycomb formed body within such a range, the honeycomb formed body can be densified and the electrical resistance at room temperature can be reduced. It should be noted that the upper limit of the relative density of the honeycomb formed body is not particularly limited, but is usually 80% or less, preferably 75% or less.

[0270] The honeycomb formed body may be dried before the firing step. The drying method is not particularly limited, and for example, conventionally known drying methods such as hot air drying, microwave drying, dielectric drying, reduced pressure drying, vacuum drying, and freeze drying may be used. Among them, a drying method combining hot air drying with microwave drying or dielectric drying is preferred in terms of being able to quickly and uniformly dry the entire formed body.

[0271] The sintering process includes: after maintaining at 1150-1250° C., heating it to a maximum temperature of 1360-1430° C. at a heating rate of 20-600° C. / hour, and maintaining it for 0.5-10 hours.

[0272] By maintaining the honeycomb molded body at a maximum temperature of 1360 to 1430° C. for 0.5 to 10 hours, a BaTiO2 in which a part of Ba is replaced by a rare earth element can be obtained. 3 A honeycomb structure composed mainly of crystal particles.

[0273] In addition, by maintaining the temperature at 1150-1250°C, the Ba generated during the sintering process is2 TiO 4 Since the crystal particles are easily removed, the honeycomb structure can be densified.

[0274] Furthermore, by setting the heating rate from 1150 to 1250° C. to the maximum temperature of 1360 to 1430° C. to 20 to 600° C. / hour, 1.0 to 10.0 mass % of Ba can be generated in the honeycomb structure. 6 Ti 17 O 40 Crystalline particles.

[0275] The holding time at 1150 to 1250° C. is not particularly limited, but is preferably 0.5 to 10 hours. By setting such a holding time, the Ba generated during the sintering process is 2 TiO 4 Crystalline particles can be removed easily and stably.

[0276] The calcining step preferably includes maintaining the temperature at 900 to 950°C for 0.5 to 5 hours. By maintaining the temperature at 900 to 950°C for 0.5 to 5 hours, BaCO 3 The honeycomb structure part having a predetermined composition can be easily obtained by efficiently decomposing the honeycomb.

[0277] Note that a degreasing step for removing the binder may be performed before the calcining step. The atmosphere of the degreasing step is preferably an air atmosphere so that the organic components can be completely decomposed.

[0278] Furthermore, from the viewpoint of controlling electrical characteristics and manufacturing cost, the atmosphere of the firing step is preferably an air atmosphere.

[0279] The firing furnace used in the firing step and the degreasing step is not particularly limited, and an electric furnace, a gas furnace, or the like can be used.

[0280] By joining a pair of electrode layers (the first electrode layer 102a and the second electrode layer 102b) to the honeycomb structure portion thus obtained, a heater component can be manufactured. The first electrode layer 102a and the second electrode layer 102b can be formed on the first end face 101a and the second end face 101b of the honeycomb structure portion by a metal precipitation method such as sputtering, evaporation, electrolytic deposition, and chemical precipitation. In addition, the first electrode layer 102a and the second electrode layer 102b can also be formed by sintering after applying electrode paste to the first end face 101a and the second end face 101b of the honeycomb structure portion. In addition, it can also be formed by spraying. The first electrode layer 102a and the second electrode layer 102b can be composed of a single layer or a plurality of electrode layers with different compositions. When the first electrode layer 102a and the second electrode layer 102b are formed on the end face using the above method, if the thickness of the electrode layer is set in a manner that does not make it too large, it is possible to prevent the compartment from being blocked.

[0281] The method for forming the first electrode layer 102a and the second electrode layer 102b is not limited, and examples thereof include: sintering of electrode paste, dry plating such as sputtering and evaporation, wet plating such as electrolytic deposition and chemical deposition, and joining of metal plates or alloy plates. Each method has a preferred thickness range. In the sintering of electrode paste, the preferred thickness range can be about 5 to 30 μm, in dry plating such as sputtering and evaporation, the preferred thickness range can be about 100 to 1000 nm, in spraying, the preferred thickness range can be about 10 to 100 μm, and in wet plating such as electrolytic deposition and chemical deposition, the preferred thickness range can be about 5 to 30 μm. In addition, in the joining of metal plates or alloy plates, the thickness of the electrode layer can be about 5 to 100 μm.

[0282] Next, the first terminal 109a is connected to the outer surface of the first electrode layer 102a, and the second terminal 109b is connected to the outer surface of the second electrode layer 102b. As described above, the connection method of the two can be: welding, soldering or mechanical contact. In addition, when the electrode paste used to form the first electrode layer 102a (the second electrode layer 102b) is sintered, the first terminal 109a (the second terminal 109b) can be sintered at the same time to achieve connection.

[0283] Next, the conducting members 105a and 105b are connected to the first terminal 109a and the second terminal 109b, respectively, as necessary. As a method for connecting the two, as described above, welding, soldering, or mechanical contact methods can be cited.

[0284] Next, a first functional material-containing layer 107a covering a portion of the outer surface of the first electrode layer 102a and a second functional material-containing layer 107b covering a portion of the outer surface of the second electrode layer 102b are formed. In a preferred embodiment, a third functional material-containing layer 111a covering a portion of the outer surface of the first terminal 109a and a fourth functional material-containing layer 111b covering a portion of the outer surface of the second terminal 109b are also formed. In a more preferred embodiment, a fifth functional material-containing layer 113 covering a portion or all of the surface of the partition wall 106 forming the flow path inside the compartment 104 is also formed.

[0285] The first functional material-containing layer 107a, the second functional material-containing layer 107b, the third functional material-containing layer 111a, the fourth functional material-containing layer 111b and the fifth functional material-containing layer 113 can be formed separately or simultaneously. These functional material-containing layers can be formed simultaneously using, for example, the following process. The heater component before forming the functional material-containing layer is immersed in a slurry containing functional materials such as hygroscopic materials, adhesives and dispersion media for a predetermined time, and the excess slurry on the outer peripheral surface of the honeycomb structure is removed by blowing and wiping. Thereafter, the slurry is dried, thereby forming these functional material-containing layers. For example, the heater component can be dried while being heated to a temperature of about 120 to 600°C. A series of steps of impregnation, slurry removal, and drying can be performed only once, but by repeating them multiple times, a functional material-containing layer of a desired thickness can be provided on the surface of an electrode layer, etc.

[0286] As the adhesive, an organic adhesive may be used, but an inorganic adhesive is preferably used because smoke may be generated due to heat and components in the smoke may flow into the vehicle cabin, thereby deteriorating the vehicle cabin environment. Preferred types of the inorganic adhesive are as described above.

[0287] The dispersion medium can be water, an organic solvent (e.g., toluene, xylene, ethanol, n-butanol, ethyl acetate, butyl acetate, terpineol, dihydroterpineol, Texanol, ethylene glycol monobutyl ether acetate, diethylene glycol monoethyl ether acetate, diethylene glycol monoethyl ether, diethylene glycol monobutyl ether acetate, diethylene glycol monobutyl ether) or a mixture thereof.

[0288] (4. Air conditioning system)

[0289] According to one embodiment of the present invention, an air conditioning system having the above-mentioned heater member is provided, which can be used to improve the indoor space of various vehicles such as automobiles, buildings such as houses, offices, factories, stores, warehouses, and cold storages, and transportation vehicles such as ships and airplanes.

[0290] (4-1. First Air Conditioning System 1000)

[0291] Figure 6 1 is a schematic diagram showing a configuration of a first air conditioning system 1000 according to an embodiment of the present invention.

[0292] The first air conditioning system 1000 includes:

[0293] at least one heater member 100;

[0294] a power source 200 such as a battery, which applies a voltage to the heater member 100;

[0295] The inflow pipe 400 connects the interior of the vehicle compartment or the like with the inlet end surface of the heater member 100;

[0296] an outflow pipe 500 having a first path 500a connecting the outlet end surface of the heater member 100 and the interior of the chamber; and

[0297] The ventilator 600 allows air from the room to flow into the inlet end surface of the heater member 100 through the inlet pipe 400 .

[0298] Figure 6 In the air conditioning system shown, the heater component 100 is configured in such a way that the inlet end face is the first end face 101a and the outlet end face is the second end face 101b. However, the heater component 100 may also be configured in such a way that the inlet end face is the second end face 101b and the outlet end face is the first end face 101a. The heater component 100 may be one, but may also be configured in series or in parallel.

[0299] The outflow pipe 500 may have a second path 500b that connects the outlet end surface of the heater member 100 to the outside of the vehicle, in addition to the first path 500a. In addition, the outflow pipe 500 may have a switching valve 300 that can switch the air flow flowing through the outflow pipe 500 between the first path 500a and the second path 500b.

[0300] The first air conditioning system 1000 may have the following operation modes.

[0301] The first mode is to cut off the applied voltage from the power source 200, switch the switching valve 300 so that the air flowing through the outflow pipe 500 passes through the first path 500a, and turn on the ventilator 600;

[0302] Second mode: the applied voltage from the power source 200 is turned on, the switching valve 300 is switched so that the air flowing through the outflow pipe 500 passes through the second path 500 b , and the ventilator 600 is turned on.

[0303] The first air conditioning system 1000 may include a control unit 900 capable of switching between the first mode and the second mode. The control unit 900 may be configured to, for example, alternately execute the first mode and the second mode. By repeatedly switching between the first mode and the second mode at a certain cycle, the removal target components such as water vapor in the room can be stably discharged to the outside of the vehicle.

[0304] In the first mode, the removal target component in the air is removed. Specifically, the air from the room flows in from the inlet end face of the heater component 100 through the inlet pipe 400, passes through the heater component 100, and flows out from the outlet end face of the heater component 100. The removal target component of the air from the room is captured by functional materials such as dehumidification materials during the passage through the heater component 100 and is removed. The air from the outlet end face of the heater component 100, from which the removal target has been removed, passes through the first path 500a of the outflow pipe 500 and returns to the room. The air can also be supplied to other air conditioning systems (e.g., HVAC of a vehicle).

[0305] In the second mode, the functional material such as the dehumidifying material is regenerated. Specifically, the air from the room flows in from the inlet end face of the heater member 100 through the inlet pipe 400, flows out from the outlet end face of the heater member 100 after passing through the heater member 100. The heater member 100 generates heat due to the power supply, and the functional material carried on the heater member 100 is heated, so that the removal target component captured by the functional material is separated from the functional material or reacts.

[0306] In order to promote the detachment of the removal target components captured by the functional material, it is preferred to heat the functional material to a temperature above the detachment temperature depending on the type of the functional material. When a hygroscopic material is used as the functional material, it is preferred to heat at least a portion of the hygroscopic material, preferably all of it, to 70 to 150°C, more preferably to 80 to 140°C, and further preferably to 90 to 130°C. In addition, the second mode is preferably performed until the functional material is fully regenerated. Although it also depends on the type of functional material, for example, when a hygroscopic material is used as the functional material, in the second mode, the functional material is preferably heated to the above temperature range in 1 to 10 minutes, more preferably heated to the above temperature range in 2 to 8 minutes, and further preferably heated to the above temperature range in 3 to 6 minutes.

[0307] In the second mode, the air from the room carries the removal target components separated from the functional material while passing through the heater member 100 and flows out from the outlet end surface of the heater member 100. The air containing the removal target components flowing out from the outlet end surface of the heater member 100 passes through the second path 500b of the outlet pipe 500 and is discharged to the outside.

[0308] For example, the power source 200 and the pair of terminals 109a and 109b of the heater member 100 are electrically connected by the wire 810, and the power switch 910 provided therebetween is operated to switch on and off the voltage applied to the heater member 100. The control unit 900 can operate the power switch 910.

[0309] For example, the control unit 900 and the ventilator 600 are electrically connected by wire 820 or wirelessly, and the ventilator 600 is switched on and off by operating a switch (not shown) of the ventilator 600 by the control unit 900. The ventilator 600 may also be configured such that the ventilation volume can be changed by the control unit 900.

[0310] For example, the control unit 900 and the switching valve 300 may be electrically connected via the wire 830 or wirelessly, and the switching valve 300 may be switched by operating a switch (not shown) of the switching valve 300 using the control unit 900 .

[0311] The switching valve 300 is not particularly limited as long as it is a valve that has a function of switching the flow path by electric drive, and examples thereof include a solenoid valve and an electric valve. In one embodiment, the switching valve 300 includes an opening and closing door 312 supported by a rotating shaft 310, and an actuator 314 such as a motor that performs a swing operation on the rotating shaft 310. The actuator 314 is configured to be controllable by the control unit 900.

[0312] From the viewpoint of stably ensuring the above functions, the first air conditioning system 1000 preferably configures the heater component 100 at a position close to the room. Accordingly, from the viewpoint of preventing electric shock, the driving voltage is preferably below 60V. The honeycomb structure portion used for the heater component 100 has a low resistance at room temperature, and therefore, the honeycomb structure portion can be heated with this low driving voltage. It should be noted that the lower limit of the driving voltage is not particularly limited, and is preferably above 10V. If the driving voltage is less than 10V, the current when the honeycomb structure portion is heated becomes larger, and therefore, it is necessary to make the wire 810 thicker. Therefore, the driving voltage of the first air conditioning system 1000 can be, for example, above 10V and below 60V.

[0313] Figure 6In the illustrated embodiment, the ventilator 600 is provided on the upstream side of the heater member 100. More specifically, the ventilator 600 is provided in the middle of the inflow pipe 400 connecting the heater member 100 and the indoor room, and the air that has passed through the ventilator 600 flows in in a manner of being pressed against the heater member 100. As another method, the ventilator 600 may be provided on the downstream side of the heater member 100. In this case, the ventilator 600 may be provided in the middle of the outflow pipe 500, for example, and the air that has passed through the inflow pipe 400 flows in in a manner of being sucked into the heater member 100.

[0314] Example

[0315] [1. Specifications of honeycomb structure]

[0316] A honeycomb structure having the following specifications was prepared.

[0317] The shape of the cross section and end surface of the honeycomb structure part perpendicular to the direction in which the flow path extends: quadrilateral (radius of curvature 6 mm or more)

[0318] · Opening shape of the cell perpendicular to the direction in which the flow path extends: square with rounded corners

[0319] ·Thickness of the wall: 0.100mm

[0320] ·Thickness of outer wall: 0.3mm

[0321] Compartment density: 80 compartments / cm 2

[0322] Compartment spacing: 1.11mm

[0323] ·Compartment opening ratio: 0.797

[0324] ·Dimensions of the cross section of the honeycomb structure part perpendicular to the direction in which the flow paths extend: 90 mm×90 mm

[0325] · Length of the honeycomb structure in the direction in which the flow path extends: 12 mm

[0326] ·Volume resistivity of the material constituting the outer wall and partition wall at 25°C: 15Ω·cm

[0327] · Curie point of the material constituting the outer wall and partition wall: 120℃

[0328] · Material constituting the outer wall and partition wall: Barium titanate

[0329] Density of the material constituting the outer wall and partition wall: 5750kg / m 3

[0330] Specific heat of the material constituting the outer wall and partition walls: 550 J / kg / K

[0331] [2. Characteristics of the functional material (hygroscopic material) used]

[0332] As a hygroscopic material, commercially available amorphous aluminum silicate was prepared. 5 g of amorphous aluminum silicate dried at 180°C for more than 2 hours was placed in a thermostat at room temperature (25°C) and a relative humidity of 50% for one hour. Based on the increased mass of the amorphous aluminum silicate taken out of the thermostat, the mass (g) of water that can be absorbed per 1 g of dry mass was calculated, and the result was 15 g / g.

[0333] 5 g of amorphous aluminum silicate dried at 180°C for 2 hours was placed in a thermostat at a relative humidity of 50% and left at various temperatures for one hour to investigate the change in mass. Based on this, the temperature range in which the mass (g) of water that can be adsorbed per 1 g of dry mass is 5 g / g or more was found to be 10°C to 25°C.

[0334] 5 g of amorphous aluminum silicate dried at 180°C for more than 2 hours was placed in a thermostat at room temperature (25°C) and a relative humidity of 50% for one hour to allow it to absorb moisture. The mass change of the amorphous aluminum silicate after moisture absorption was investigated after it was placed in a thermostat at a relative humidity of 50% for 0.1 hour at various temperatures. The lowest temperature at which the mass reduction ratio of the amorphous aluminum silicate after moisture absorption reached 30% was defined as the moisture desorption temperature, which was 70°C.

[0335] [3. Manufacturing of Heater Component Assembly]

[0336] The heater component assemblies of the following embodiments and comparative examples were manufactured for various analysis and test needs.

[0337] <Example 1>

[0338] A paste obtained by mixing aluminum powder and a binder resin was applied to both end surfaces (the first end surface 101a and the second end surface 101b) of the honeycomb structure, and sintered. A pair of electrode layers (the first electrode layer 102a and the second electrode layer 102b) (volume resistivity at 25°C: 2.0×10 -7 Ω·cm).

[0339] The ratio (coverage rate) of the area of ​​the first end face 101a (second end face 101b) covered by the first electrode layer 102a (second electrode layer 102b) to the area of ​​the portion of the first end face 101a (second end face 101b) other than the opening portion of the partition 104 (the partition wall portion and the outer peripheral wall portion) is calculated based on the areas of the two, and the result is 99%.

[0340] Furthermore, the above-described measurement method was used to measure the average value of the entire thickness of the first electrode layer 102a (second electrode layer 102b), the average value of the thickness at portions other than the peripheral portion, and the average value of the thickness at the peripheral portion. The results are shown in Table 1-1.

[0341] It should be noted that the conditions for the first electrode layer 102a and the second electrode layer 102b are the same.

[0342] Next, pure aluminum (A1050) (volume resistivity at 25°C: 2.0×10 -7 The rectangular plate-shaped first terminal 109a and the second terminal 109b with a plane size of 100 mm×4 mm and a thickness of 1 mm are connected to the outer peripheries of the first end face 101a and the second end face 101b of the outer surfaces of the first electrode layer 102a and the second electrode layer 102b by soldering.

[0343] The ratio (coverage rate) of the area covered by the first terminal 109a (second terminal 109b) to the area of ​​the first end surface 101a (second end surface 101b) was calculated based on the areas of both and was 3%.

[0344] It should be noted that the conditions for the first terminal 109 a and the second terminal 109 b are the same.

[0345] Next, amorphous aluminum silicate powder, silicon dioxide powder, and solvent (water) were mixed and stirred at a mass ratio of amorphous aluminum silicate: silicon dioxide: solvent = 95:5:100 to prepare a hygroscopic material slurry. The obtained hygroscopic material slurry was applied to the outer surface of the first electrode layer 102a and the outer surface of the second electrode layer 102b by a brush coating method, and then dried in a dryer at 190°C for 2 hours to form a first functional material-containing layer 107a and a second functional material-containing layer 107b, thereby preparing a heater component.

[0346] It should be noted that the first functional material-containing layer 107 a and the second functional material-containing layer 107 b are produced under the same conditions.

[0347] The ratio (coverage rate) of the area covered by the first functional material-containing layer 107a (the second functional material-containing layer 107b) on the outer surface of the first electrode layer 102a (the second electrode layer 102b) to the area of ​​the portion not connected to the first terminal 109a (the second terminal 109b) was calculated based on the areas of both and the result was 95% or more. In addition, the average thickness of the first functional material-containing layer 107a (the second functional material-containing layer 107b) was measured using the above-mentioned measurement method and the result was 200 μm.

[0348] The resistance of the first functional material-containing layer 107a and the second functional material-containing layer 107b were measured at 12 locations in the above order. The resistance range (minimum value to maximum value) at this time was 3.0×10 6 ~4.0×10 6 Ω.

[0349] The heater member obtained in the above order is clamped from the first end surface 101a side and the second end surface 101b side by the frame body 120 having the first frame portion 121 and the second frame portion 122 but not having the third frame portion 123, and assembled Figure 3A , Figure 3B The heater assembly of the structure shown in FIG. 1 is a heater assembly. The outer peripheral shapes of the first frame portion 121 and the second frame portion 122 are substantially quadrilateral shapes corresponding to the outer peripheral shapes of the heater member. In addition, no cushioning material is used at any position.

[0350] The first frame portion 121 and the second frame portion 122 have a portion 126 a partially protruding toward the inner peripheral side, and the protruding portion 126 a constitutes at least a part of a portion pressing the first terminal 109 a toward the first end surface 101 a .

[0351] The first frame 121 and the second frame 122 are formed by injection molding or cutting of a base material. The first frame 121 and the second frame 122 are connected by a combination of bolts and nuts. Four connection locations are set at equal intervals in the circumferential direction of the flange 121b (flange 122b).

[0352] Table 1-1 shows the following conditions for commercially available resins used in the first frame portion 121 and the second frame portion 122. The conditions for the resins used in the first frame portion 121 and the second frame portion 122 are the same.

[0353] R1: Resin type (Comparative Example 1 is made of metal)

[0354] R2: Rockwell hardness (HRR and HRM) measured according to ASTM D785-2008R15

[0355] R3: Thermal conductivity at 25°C measured in accordance with JIS R1611:2010

[0356] R4: Deflection temperature under load specified in JIS K7191-1:2015

[0357] R5: Melting point

[0358] R6: Volume resistivity at 25°C measured in accordance with JIS C2139:2008

[0359] Regarding the obtained heater member assembly, the structural conditions of the holding portion 121a (122a) are shown in Table 1-1. The structural conditions of the holding portion 121a and the holding portion 122a are the same.

[0360] S1: Ratio of the area of ​​the portion of the first end surface 101a (second end surface 101b) that is subjected to pressure by the holding portion 121a (122a) to the entire area of ​​the first end surface 101a (second end surface 101b)

[0361] S2: Range of the width W of the holding portion 121a (122a) (If there is a portion partially protruding toward the inner peripheral side, this portion is also considered as the range of the width of the holding portion.)

[0362] S3: The number of the portions 126a (126b) of the retaining portion 121a (122a) that protrude inwardly

[0363] S4: Ratio of the area of ​​the portion 126a (126b) of the retaining portion 121a (122a) that partially protrudes toward the inner circumference (when there are multiple portions 126a (126b) that partially protrude toward the inner circumference, it refers to the total area of ​​these portions) to the area of ​​the first end face 101a (second end face 101b) when viewed from the first end face 101a (second end face 101b) side

[0364] S5: Is it that only the portion 126a (126b) of the holding portion 121a (122a) that partially protrudes toward the inner circumference constitutes the holding portion 121a (122a) that applies pressure to at least a portion of the outer circumference of the first end surface 101a (second end surface 101b)?

[0365] S6: Ratio of the area of ​​the portion of the outer surface of the first terminal 109a (second terminal 109b) pressed toward the first end surface 101a (second end surface 101b) by the portion 126a (126b) of the holding portion 121a (122a) protruding toward the inner circumference

[0366] <Examples 2, 3, 7, 8>

[0367] The heater component assembly was assembled under the same conditions as in Example 1, except that the commercially available resin used in the first frame portion 121 and the second frame portion 122 was changed to the conditions described in Table 1-1. The conditions of the resin used in the first frame portion 121 and the second frame portion 122 were the same.

[0368] <Examples 4 to 6>

[0369] The heater component assembly was assembled under the same conditions as in Example 1 except that the sheet-shaped cushioning material was arranged between the retaining portion 121a of the first frame portion 121 and the first end face 101a and between the retaining portion 122a of the second frame portion 122 and the second end face 101b under the conditions described in Table 1-2 using commercially available cushioning materials of the type and Young's modulus described in Table 1-2. In the table, the thickness displacement rate of the compressed cushioning material in the compression direction was solved using the following formula. Displacement rate (%) = (1 - thickness of the cushioning material after compression / thickness of the cushioning material before compression) × 100

[0370] <Examples 9, 10, 13, 14>

[0371] The heater component assembly was assembled under the same conditions as in Example 1, except that the structural conditions of the holding portion 121a (122a) were changed to the conditions described in Table 1-1. The structural conditions of the holding portion 121a and the holding portion 122a were the same.

[0372] <Example 11>

[0373] The heater component assembly was assembled under the same conditions as in Example 1 except that the average thickness at the outer periphery of the first electrode layer 102a and the second electrode layer 102b was changed to the value described in Table 1-1 using a hand roller.

[0374] <Example 12>

[0375] The heater component assembly was assembled under the same conditions as in Example 1 except that the frame 120 having the third frame 123 in addition to the first frame 121 and the second frame 122 was used. The outer peripheral shapes of the first frame 121, the second frame 122, and the third frame 123 were substantially quadrilaterals corresponding to the outer peripheral shape of the heater component. In addition, no buffer material was used between the third frame 123 and the peripheral wall 103. The conditions of the resin used in the third frame 123 were the same as those of the first frame 121 and the second frame 122.

[0376] <Comparative Example 1>

[0377] The heater component assembly was assembled under the same conditions as in Example 1, except that the materials of the first frame 121 and the second frame 122 were changed to metal (SUS304) having the properties shown in Table 1-1. The conditions of the first frame 121 and the second frame 122 were the same.

[0378] [4. Characteristics of heater component assembly]

[0379] <Water release performance>

[0380] The frame was removed from the heater member assembly of each example and comparative example obtained in the above-mentioned order, and a sample of 25 mm in diameter (flow path length was unchanged) was cut out from the heater member, and the sample was inserted into a quartz glass tube having a wall thickness of 1 mm, an inner diameter of 25 mm, and a length of 26 mm, and then mounted on MEXA-6000FT manufactured by HORIBA, and nitrogen gas heated to 120° C. was flowed through the flow path of the sample at 40 L / min for 1 hour to dry the sample, and then the introduction of nitrogen gas was stopped, and water vapor gas adjusted to 0.6% was introduced at 25° C. and 50 L / min for 10 minutes, and then the introduction of water vapor gas was stopped, and nitrogen gas heated to 120° C. was introduced at 15 L / min for 10 minutes, and the water release performance of the sample was measured. It should be noted that, regarding Example 12, the sample was inserted into a polyetheretherketone resin tube having a wall thickness of 1 mm, an inner diameter of 25 mm, and a length of 26 mm instead of the quartz glass tube, and the test was carried out in this state. Regarding Comparative Example 1, the sample was inserted into a metal tube made of SUS304 having a wall thickness of 1 mm, an inner diameter of 25 mm, and a length of 26 mm instead of the quartz glass tube, and the test was conducted in this state. The water release performance was evaluated based on the following criteria.

[0381] ○: Water release exceeds 0.0353 g / cm 3 And less than 0.0367g / cm 3

[0382] ◎: Water release is 0.0367g / cm 3 above

[0383] ×: Water release is 0.0353 g / cm 3 the following

[0384] <Bondability between the first electrode layer (second electrode layer) and the first terminal (second terminal)>

[0385] Remove the frame from the heater component assembly, place the obtained heater component horizontally (the direction in which the compartment extends is the horizontal direction) on the measuring table and fix it, push the connected terminal vertically from the upper surface, and find the maximum stress when the stress-displacement curve is obtained during the push. The bonding between the first electrode layer and the first terminal and the bonding between the second electrode layer and the second terminal are measured separately, and the average value is set as the measured value. It should be noted that the measuring device uses a conventional universal testing machine (INSTRON6800). The bonding is evaluated based on the following criteria.

[0386] ○: More than 0.95MPa and less than 1.05MPa

[0387] ◎:1.05MPa or more

[0388] ×: 0.95 MPa or less

[0389] <Retention of heater components>

[0390] A voltage of 13 V was applied between the first terminal and the second terminal of the heater component assembly of each embodiment and comparative example obtained in the above order to energize the heater component. At the same time, air (25° C.) was circulated through the flow path of the heater component assembly at a flow rate of 40 L / min. The heater component was heated for 3 minutes to confirm that the heater component reached an average of 120° C. or more. The energization was stopped, and then air at 25° C. was circulated at 750 L / min for 3 minutes to cool the heater component to an average of 25° C. or less. Thereafter, a voltage of 13 V was applied again, and air (25° C.) was circulated through the flow path of the heater component assembly at a flow rate of 40 L / min. Whether the heater component could reach an average of 120° C. or more without being damaged or falling off from the frame during heating for 3 minutes was investigated. The retention of the heater component in the frame was evaluated based on the following criteria.

[0391] ○: During reheating, the heater member was not damaged or dropped from the housing, and the average temperature reached 120°C or higher.

[0392] ×: During reheating, the heater member was damaged or fell off from the frame.

[0393] <Pressure loss>

[0394] When air (25° C.) was flowed from one end surface side at a flow rate of 750 L / min into the flow path of the heater member assembly of each example and comparative example obtained in the above-described procedure, the pressure loss between the two end surfaces was measured. Evaluation was performed based on the following criteria.

[0395] 0:Pressure loss exceeds 58.2Pa and is less than 60Pa

[0396] ◎: Pressure loss is 58.2Pa or less

[0397] According to the above test results, it can be understood that the resin frame has lower thermal conductivity than the metal frame, which can reduce heat loss and improve water release performance. In addition, according to the results of the hot and cold tests, it can be understood that the resin frame has higher retention performance for the heater component than the metal frame, that is, higher protection performance for the heater component.

[0398]

Table 1-1

[0399]

[0400]

Table 1-2

[0401]

Claims

1. A heater component assembly comprising a heater component and a frame, The heater component assembly is characterized in that The heater component comprises: A honeycomb structure part, the honeycomb structure part has an outer peripheral wall and partition walls and can generate heat when powered, the partition walls contain a material having PTC characteristics and are arranged on the inner peripheral side of the outer peripheral wall to partition into a plurality of compartments, the plurality of compartments forming a flow path extending from the first end face to the second end face; a first electrode layer covering a part or the whole of the surface of the partition wall forming the first end face; a second electrode layer covering a part or the whole of the surface of the partition wall forming the second end face; a first terminal connected to an outer surface of the first electrode layer; as well as a second terminal connected to an outer surface of the second electrode layer, The frame body includes a first frame portion and a second frame portion for clamping the heater member from the first end surface side and the second end surface side. The first frame portion is a resin-made first frame portion arranged on the first end face side, and includes a flange portion arranged on the outer peripheral side of the outer peripheral contour of the first end face, and a retaining portion arranged on the inner peripheral side of the outer peripheral contour of the first end face and applying pressure to at least a portion of the outer peripheral portion of the first end face. The second frame portion is a second frame portion made of resin and arranged on the side of the second end face, and has a flange portion arranged on the outer peripheral side of the outer peripheral contour of the second end face, and a retaining portion arranged on the inner peripheral side of the outer peripheral contour of the second end face and applying pressure relative to at least a portion of the outer peripheral portion of the second end face.

2. The heater component assembly according to claim 1, wherein: The Rockwell hardness of the resin constituting the first frame portion and / or the second frame portion measured in accordance with ASTM D785-2008R15 is 150 HRR or less and / or 120 HRM or less.

3. The heater component assembly according to claim 1 or 2, characterized in that The deflection temperature under load of the resin constituting the first frame portion and / or the second frame portion measured in accordance with JIS K7191-1:2015 is 145° C. or higher.

4. The heater component assembly according to claim 1 or 2, characterized in that The melting point of the resin constituting the first frame portion and / or the second frame portion is 250° C. or higher.

5. The heater component assembly according to claim 1 or 2, characterized in that The resin constituting the first frame portion and / or the second frame portion has a thermal conductivity of 0.5 W / m / K or less at 25° C. as measured in accordance with JIS R1611:2010.

6. The heater component assembly according to claim 1 or 2, characterized in that The volume resistivity of the resin constituting the first frame portion and / or the second frame portion at 25° C. measured in accordance with JIS C2139:2008 is 1.0×10 16 Ω·cm or more.

7. The heater component assembly according to claim 1 or 2, characterized in that The resin constituting the first frame portion and / or the second frame portion includes one or two selected from polyetheretherketone and polybutylene terephthalate (PBT).

8. The heater component assembly according to claim 1 or 2, characterized in that The ratio of the area of ​​the first end surface to which the pressure is applied by the holding portion of the first frame portion relative to the area of ​​the first end surface is 10% or less, and / or A ratio of an area of ​​the second end surface to which pressure is applied by the holding portion of the second frame portion relative to an area of ​​the second end surface is 10% or less.

9. The heater component assembly according to claim 1 or 2, characterized in that The ratio of the area of ​​the first end surface to which the pressure is applied by the holding portion of the first frame portion relative to the area of ​​the first end surface is 2% or less, and / or A ratio of an area of ​​the second end surface to which pressure is applied by the holding portion of the second frame portion relative to an area of ​​the second end surface is 2% or less.

10. The heater component assembly according to claim 1 or 2, characterized in that The holding portion of the first frame portion has a portion that presses the first terminal toward the first end surface, and / or The holding portion of the second frame portion has a portion that presses the second terminal toward the second end surface.

11. The heater component assembly according to claim 1 or 2, characterized in that A cushioning material is sandwiched between the holding portion of the first frame portion and the first end surface, and / or A cushioning material is interposed between the holding portion of the second frame portion and the second end surface.

12. The heater component assembly according to claim 1 or 2, characterized in that The frame body includes a third frame portion made of resin and surrounding an outer peripheral surface of the outer peripheral wall of the heater member.

13. The heater component assembly of claim 12, wherein: A cushioning material is interposed between the third frame portion and the outer peripheral wall.

14. The heater component assembly according to claim 1 or 2, characterized in that The first frame portion and the second frame portion are divided from each other and connected by a fastener.

15. The heater component assembly according to claim 1 or 2, characterized in that The first frame portion and the second frame portion are divided from each other and connected by a fitting structure.

16. The heater component assembly according to claim 1 or 2, characterized in that The first frame portion and the second frame portion are divided from each other and connected with an adhesive.

17. The heater component assembly according to claim 1 or 2, characterized in that The average thickness of the first electrode layer at the outer periphery of the first end surface and the connection portion with the first terminal is greater than the average thickness of the first electrode layer at other portions, and / or An average value of the thickness of the second electrode layer at an outer peripheral portion of the second end surface and a connection portion with the second terminal is larger than an average value of the thickness of the second electrode layer at other portions.

18. The heater component assembly of claim 1 or 2, wherein: The average value of the thickness of the first electrode layer in the entire periphery of the first end surface is greater than the average value of the thickness of the first electrode layer in other portions, and / or An average value of the thickness of the second electrode layer in the entire outer peripheral portion of the second end surface is larger than an average value of the thickness of the second electrode layer in other portions.

Citation Information

Patent Citations

  • Air cleaning system for vehicle, and control method of the air cleaning system for vehicle

    JP2020104774A

  • Heating element for heating passenger compartment, method of use thereof, and heater for heating passenger compartment

    WO2020036067A1