C02 immobilized ceramic, and method for producing CO2 immobilized product

By using γ-2CaO·SiO2 and 2CaO·Al2O3·SiO2 ceramic materials for carbonation treatment under low temperature and high humidity conditions, the problems of low efficiency and high cost of the existing CO2 immobilization technology are solved, and the efficient immobilization of CO2 is achieved. Expand its application in a variety of materials.

CN118742384APending Publication Date: 2024-10-01DENKA CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202380017397.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-02-10
Filing Date
2023-01-30
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Existing CO2 immobilization technology has problems such as low efficiency, high cost and low carbonation rate during the manufacturing process. It is especially difficult to effectively immobilize CO2 when using early-strength Portland cement.

Method used

Ceramic materials containing γ-2CaO·SiO2 and 2CaO·Al2O3·SiO2 are used, and carbonation treatment is carried out under conditions of less than 75°C and/or 50% RH or more, and the reactivity of γ-C2S and C2AS is used to immobilize CO2.

Benefits of technology

It achieves efficient immobilization of CO2, improves the carbonation rate, and can be used as a variety of materials, such as cement additives, mortar, concrete aggregate, etc., and is suitable for industrial and construction fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004946811060000131
    Figure BDA0004946811060000131
  • Figure BDA0004946811060000141
    Figure BDA0004946811060000141
  • Figure BDA0004946811060000151
    Figure BDA0004946811060000151
Patent Text Reader

Abstract

The CO2 immobilized ceramic according to the present invention comprises: a gamma crystal phase comprising [gamma]-2CaO. SiO2 ([gamma]-C2S); and 2CaO. Al2O3. SiO2 (C2AS).
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a CO2-fixed ceramic and a method for producing a CO2-fixed product. Background Art

[0002] As a measure to reduce greenhouse gases, concrete products that forcibly absorb or carbonate CO2 during manufacturing (hereinafter referred to as CO2 absorbing concrete) have been partially put into practical use. CO2 absorbing concrete, a type of CCUS technology (abbreviation for Carbon dioxide Capture, Utilization and Storage), was also mentioned in the "Carbon Recycling Technology Roadmap" published by the Ministry of Economy, Trade and Industry of Japan in 2019, and technical development is being carried out for its popularization and expansion.

[0003] Patent Document 1 discloses a method for forcibly absorbing or carbonating CO2 when manufacturing concrete. Specifically, a method for fixing carbon dioxide is disclosed, which includes a contact step of bringing a gas containing carbon dioxide into contact with a cementitious hardened body, thereby fixing the carbon dioxide contained in the gas containing carbon dioxide to the cementitious hardened body.

[0004] It should be noted that the cementitious hardened body of Patent Document 1 is obtained by filling a mold with a cement paste prepared by mixing early-strength Portland cement and water, and then water-curing the mixture (Paragraph 0019 of Patent Document 1).

[0005] Prior art literature

[0006] Patent Literature

[0007] Patent Document 1: Japanese Patent Application Publication No. 2020-15659 Summary of the invention

[0008] Problems to be solved by the invention

[0009] An object of the present invention is to provide a CO 2 fixing ceramic capable of fixing CO 2 by carbonation, and a method for producing a CO 2 fixing product using the same.

[0010] Means for solving problems

[0011] The inventors of the present application have discovered that by using ceramics containing γ-2CaO·SiO2 and 2CaO·Al2O3·SiO2, it is possible to realize a CO2-fixing ceramic that can fix CO2 by carbonation, thereby completing the present invention.

[0012] According to one aspect of the present invention, the following CO 2 fixed ceramics and methods for producing CO 2 fixed products are provided.

[0013] 1. A CO2 fixation ceramic comprising:

[0014] A γ crystalline phase composed of γ-2CaO·SiO2 (γ-C2S); and

[0015] 2CaO·Al2O3·SiO2(C2AS).

[0016] 2. The CO2 fixation ceramic as described in 1., which contains a glass phase and / or CaO·2Al2O3 (CA2).

[0017] 3. The CO 2 immobilization ceramic as described in 1. or 2., wherein the content of the above-mentioned γ-C 2 S in 100 mass % of the CO 2 immobilization ceramic is 30 mass % or more and 98 mass % or less.

[0018] 4. The CO 2 immobilization ceramic according to any one of 1. to 3., wherein the content of the C 2 AS is 0.5 mass % or more and 50 mass % or less relative to 100 mass % of the γ-C 2 S.

[0019] 5. The CO 2 immobilization ceramic according to any one of 1. to 4., comprising a hetero phase present in the γ crystalline phase, wherein the hetero phase contains the C 2 AS.

[0020] 6. The CO2-fixing ceramic according to 5., wherein the γ-crystalline phase does not contain Al2O3.

[0021] 7. The CO 2 fixation ceramic according to any one of 1. to 6., comprising a β crystal phase composed of β-2CaO·SiO 2 (β-C 2 S).

[0022] 8. The CO2-fixing ceramic according to 7., wherein the β-crystalline phase contains Al2O3.

[0023] 9. The CO 2 immobilization ceramic according to 7. or 8., wherein the content of the β-C 2 S is 1.0% by mass or more and 50% by mass or less relative to 100% by mass of the γ-C 2 S.

[0024] 10. The CO 2 fixation ceramic according to any one of 1. to 9., comprising disaccharides.

[0025] 11. The CO 2 immobilization ceramic according to 10., wherein the content of the disaccharide is 0.5 parts by mass or more and 10 parts by mass or less in 100 parts by mass of the CO 2 immobilization ceramic.

[0026] 12. The CO 2 fixation ceramic according to 10. or 11., wherein the disaccharide contains trehalose.

[0027] 13. The CO 2 immobilization ceramic according to any one of 1. to 12., which is in powder form.

[0028] 14. A method for producing a CO2-fixed product, comprising the step of performing a carbonation treatment on the CO2-fixed ceramic described in any one of 1. to 13. under conditions of less than 75°C and / or 50%RH or more.

[0029] Effects of the Invention

[0030] According to the present invention, a CO 2 fixation ceramic having excellent CO 2 fixation ability and a method for producing a CO 2 fixed product using the same are provided. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] [ Figure 1 ] is the SEM image of immobilized ceramic A.

[0032] [ Figure 2 ] is the SEM image of immobilized ceramic B. DETAILED DESCRIPTION

[0033] The outline of the CO 2 immobilization ceramic according to the present embodiment will be described.

[0034] The CO 2 immobilization ceramic of the present embodiment includes: a γ crystal phase composed of γ-2CaO·SiO 2 (hereinafter, sometimes abbreviated as γ-C 2 S); and 2CaO·Al 2 O 3 ·SiO 2 (hereinafter, sometimes abbreviated as C 2 AS).

[0035] According to the findings of the inventors of the present application, it has been confirmed that CO 2 can be fixed in a relatively short time by using a CO 2 fixing ceramic containing γ-C 2 S and C 2 AS.

[0036] The detailed mechanism is still uncertain, but generally, when carbonation curing is performed on powders with good reactivity with CO2, such as γ-C2S, it will become agglomerates and hinder the intrusion of CO2, and the reaction will stagnate. On the other hand, it is believed that by allowing C2AS as a stable phase to exist appropriately, it will not become an excessively dense agglomerate, and CO2 will intrude into the interior to cause the reaction to proceed.

[0037] According to the present embodiment, it is possible to provide a CO 2 fixing ceramic that can fix CO 2 by carbonation.

[0038] According to the CO 2 immobilization ceramic of the present embodiment, CO 2 fixation can be promoted by carbonation treatment under relatively low temperature and / or relatively high humidity conditions such as less than 75° C. and / or 50% RH or more.

[0039] The CO2-fixed ceramic of this embodiment can be used for various purposes, such as a capture material for absorbing CO2 gas discharged from industrial facilities, power generation facilities, or transportation vehicles including automobiles, a chemical heat storage material for storing waste heat in a factory or renewable energy whose power generation varies depending on the weather, and a CO2 absorbent that can absorb CO2 in exhaled air for safe anesthesia and accurate inspection using medical equipment. In addition, the CO2-fixed ceramic can also be used as a cement additive (mixed material).

[0040] [Method for producing CO2 fixed product]

[0041] An example of the method for producing a CO 2 fixed product according to the present embodiment includes a step of subjecting a CO 2 fixed ceramic to a carbonation treatment at 75° C. or lower and / or 50% RH or higher.

[0042] The method of carbonation treatment is not particularly limited, and examples thereof include a method of treating the carbonation mixture by appropriately heating and / or humidifying (adding water) in a gas atmosphere containing CO 2 to achieve predetermined temperature and humidity conditions.

[0043] The temperature of the carbonation treatment is, for example, preferably 5°C or higher and lower than 75°C, and more preferably 5°C or higher and 50°C or lower.

[0044] The relative humidity during the carbonation treatment is preferably 50% RH or more and 100% RH or less, and more preferably 80% RH or more and 100% RH or less.

[0045] As the above-mentioned gas containing CO2, waste gas generated from cement factories and coal-fired power plants, waste gas generated from exhaust gas treatment in coating factories, etc. can be used. The proportion of CO2 in the gas containing CO2 is preferably 5% by volume or more, preferably 10% by volume or more, and more preferably 15% by volume or more.

[0046] In addition, the gas containing CO 2 may contain moisture (water vapor).

[0047] The CO2-fixed ceramic of this embodiment can not only effectively fix CO2 in the atmosphere, but also can be further effectively utilized as a concrete material. That is, the CO2-fixed product can be used as a cement additive (mixed material), or can be directly used as a material such as mortar, concrete aggregate, roadbed material, fill material, backfill material, etc. In addition, the CO2-fixed product can be used as a filler and extender material for paint, ink, and rubber.

[0048] Hereinafter, the CO 2 immobilization ceramics according to the present embodiment will be described in detail.

[0049] The CO2-fixed ceramics include an inorganic sintered product containing γ-C2S and C2AS. The inorganic sintered product is a molded product or a powdered product having a predetermined shape obtained by heating and sintering an inorganic raw material.

[0050] In addition, the CO2-fixing ceramic can be configured in a powder form.

[0051] For example, by appropriately controlling the CaO / SiO2 molar ratio according to the Al2O3 content contained in the inorganic raw material, it is possible to realize a CO2-fixing ceramic that is entirely powdered.

[0052] In addition, the CO2-fixed ceramic contains not only inorganic substances such as inorganic sintered products but also organic substances such as disaccharides described later. The CO2-fixed ceramic containing organic substances is obtained by mixing a powdered inorganic sintered product with disaccharides, for example.

[0053] γ-C2S is known to have α-type, β-type, γ-type and other crystal forms. Their crystal structures and densities are different from each other. Among them, γ-C2S as a γ-type has a neutralization inhibition effect. By implementing forced carbonation, γ-C2S is used to improve the densification of cement hardened materials.

[0054] γ-C2S constitutes the γ crystal phase of the CO2-immobilized ceramic. The γ crystal phase may be contained in the CO2-immobilized ceramic as an inorganic matrix.

[0055] The lower limit of the content of γ-C 2 S is, for example, 30 parts by mass or more, preferably 35 parts by mass or more, and more preferably 40 parts by mass or more, based on 100 parts by mass of the CO 2 immobilization ceramic.

[0056] On the other hand, the upper limit of the content of γ-C 2 S is, for example, 98 parts by mass or less, preferably 95 parts by mass or less, and more preferably 93 parts by mass or less, based on 100 parts by mass of the CO 2 immobilization ceramic.

[0057] By being within such a range, the carbonation rate can be increased.

[0058] The CO2 fixation ceramic may include a heterogeneous phase present in the gamma crystalline phase.

[0059] The heterogeneous phase exists along the interior of a crystal grain composed of a γ crystal phase composed of γ-C 2 S or along the interface of the crystal grains in at least one SEM image of a fracture surface of the CO 2 -fixed ceramic.

[0060] In SEM images, a grain may contain one or more than two different phases.

[0061] The CO2-fixed ceramic preferably contains C2AS as a component constituting a heterogeneous phase. Thus, the carbonation rate can be further improved.

[0062] It should be noted that components other than C2AS may inevitably exist in the heterophase.

[0063] The lower limit of the content of C2AS is, for example, 0.5 mass % or more, preferably 1.0 mass % or more, and more preferably 2.0 mass % or more relative to 100 mass % of γ-C2S. This allows CO2 to be fixed in a short time.

[0064] On the other hand, the upper limit of the content of C2AS is, for example, below 50 mass %, preferably below 40 mass %, more preferably below 30 mass %, relative to 100 mass % of γ-C2S. Thus, the reduction of excessive carbonation rate can be avoided.

[0065] In the present embodiment, the existence of the above-mentioned heterogeneous phase and the content of the components constituting the heterogeneous phase can be controlled by appropriately selecting, for example, the type and amount of each component contained in the CO2-fixed ceramic, the preparation method of the CO2-fixed ceramic, etc. Among these, as elements for making the existence of the above-mentioned heterogeneous phase and the content of the components constituting the heterogeneous phase in the desired state, for example, there can be cited: using a raw material mixture containing a CaO raw material, a SiO2 raw material, and an Al2O3 raw material; using a rotary kiln lined with high-purity aluminum bricks in the furnace; and / or applying alumina mortar of a specified concentration on the surface of the bricks inside the kiln; appropriately adjusting the conditions of firing temperature, dry pulverization, and granulation size; and the like.

[0066] The content of each mineral component in the CO2-fixed ceramic can be confirmed by conventional analytical methods. For example, for a crushed sample, the generated mineral composition can be confirmed by powder X-ray diffraction, and the data can be analyzed by the Rietveld method to quantify the mineral composition. In addition, the mineral composition amount can also be calculated based on the identification results of the chemical composition and powder X-ray diffraction.

[0067] The CO2-fixing ceramic may be configured so that Al2O3 is not included in the γ-crystalline phase. This can increase the carbonation rate.

[0068] The CO 2 fixing ceramic may be constituted to include a β crystal phase composed of β-2CaO·SiO 2 (hereinafter, sometimes also abbreviated as β-C 2 S).

[0069] The lower limit of the content of β-C2S is, for example, 1.0 mass % or more, preferably 2.0 mass % or more, and more preferably 3.0 mass % or more relative to 100 mass % of γ-C2S. This allows CO2 to be fixed in a short time.

[0070] On the other hand, with regard to the upper limit of the content of β-C2S, with respect to 100 quality % of γ-C2S, for example, be below the 50 quality %, be preferably below the 30 quality %, more preferably below the 20 quality %.Thus, can avoid the reduction of the carbonation rate that becomes dense piece caused by carrying out hydration reaction.

[0071] The CO 2 fixing ceramics containing β-C 2 S may be configured to contain Al 2 O 3 in the β crystal phase.

[0072] The CO 2 fixing ceramic may contain a glass phase and / or CaO·2Al 2 O 3 (hereinafter, sometimes abbreviated as CA 2 ).

[0073] The lower limit of the glass phase content is, for example, 20% by mass or more, preferably 30% by mass or more, and more preferably 40% by mass or more relative to 100% by mass of γ-C2S. Thus, a CO2-fixed ceramic that is entirely powdered can be realized.

[0074] On the other hand, the upper limit of the glass phase content is, for example, 120 mass % or less, preferably 100 mass % or less, and more preferably 90 mass % or less, relative to 100 mass % of γ-C2S. Thus, a CO2-fixed ceramic can be powdered as a whole.

[0075] The lower limit of the CA2 content is, for example, 0.01% by mass or more, preferably 0.05% by mass or more, and more preferably 0.1% by mass or more relative to 100% by mass of γ-C2S. Thus, a CO2-fixed ceramic that is entirely powdered can be realized.

[0076] On the other hand, the upper limit of the CA2 content is, for example, 20% by mass or less, preferably 18% by mass or less, and more preferably 15% by mass or less relative to 100% by mass of γ-C2S. Thus, a CO2-fixed ceramic can be powdered as a whole.

[0077] The water content of the CO 2 immobilization ceramic is preferably 10% by mass or less, and more preferably 0.01 to 10% by mass, for example. This allows the surface of the CO 2 immobilization ceramic to be properly kept in contact with the gas containing CO 2 .

[0078] The moisture content can be determined from the difference between the mass of the sample before drying and the mass after heat drying at 105° C. In addition, the moisture content of the CO2-fixed ceramic can be adjusted by adding an appropriate amount of water and stirring after heat drying at 105° C.

[0079] The average particle size of the CO2 fixed ceramic is preferably 1 to 100 μm, more preferably 1 to 70 μm. By making the average particle size 1 to 70 μm, the dissolution of Ca into the water on the particle surface can be promoted, thereby promoting the carbonation reaction. The average particle size can be measured and obtained by a laser diffraction / scattering particle size distribution measuring device.

[0080] The Blaine specific surface area of ​​the CO2-fixing ceramic is preferably, for example, 1,000 to 10,000 cm 2 / g, more preferably 2,500 to 10,000 cm 2 / g. By making the specific surface area 2,500 to 10,000 cm 2 / g, the contact area between the particles and the water on the particle surface increases, which promotes the dissolution of Ca and thus can promote the carbonation reaction.

[0081] The Blaine specific surface area can be determined by measuring with a Blaine air permeation apparatus described in JIS R 5201.

[0082] In this specification, the so-called fixation of CO2 means that the material is carbonated and CO2 and the material form a carbonate compound.

[0083] In this embodiment, when the CO2-fixed ceramic contacts CO2, a carbonate compound is formed by carbonation, thereby the carbonate compound can be formed (fixed) inside and / or on the surface of the CO2-fixed ceramic. The substance obtained by fixing CO2 in the form of a carbonate compound to the CO2-fixed ceramic is called a CO2-fixed product.

[0084] In addition, the carbonation of such CO 2 -fixed ceramics can be promoted by a predetermined carbonation treatment.

[0085] As the carbonation treatment, a relatively low temperature and / or relatively high humidity condition can be adopted, for example, a condition of less than 75°C and / or 50%RH or more can be adopted. CO2 can be fixed on the CO2 fixed ceramic of the present embodiment by carbonation treatment not only under high temperature conditions but also under relatively low temperature conditions.

[0086] In this specification, the carbonation rate is the ratio of the CaO component in the CO2-fixing ceramic to the CO2 that can be theoretically fixed. The carbonation rate can be calculated according to the following formula.

[0087] Formula (1): Carbonation rate = (ΔM × 56.08) / (M × wCaO × 44.01)

[0088] In the above formula (1), ΔM represents the increase in mass [g] caused by carbonation, M represents the mass of the CO2 fixed ceramic before carbonation [g], and wCaO represents the CaO [wt%] in the CO2 fixed ceramic before carbonation.

[0089] In the above formula (1), the mass increase due to carbonation refers to the mass obtained by subtracting the weight of the sample before carbonation from the weight of the sample after carbonation. CaO in the CO2-fixed ceramic before carbonation can be measured by fluorescent X-ray analysis.

[0090] A method for producing CO2-fixing ceramics will be described.

[0091] An example of a method for producing a CO 2 -fixed ceramic includes a step of firing a raw material mixture including a CaO raw material, a SiO 2 raw material, and an Al 2 O 3 raw material using, for example, a kiln.

[0092] As the CaO raw material, a material commercially available as an industrial raw material can be used, for example, one or more selected from the group consisting of limestone, fly ash, quicklime, slaked lime, and acetylene generation shavings can be used. Among them, slaked lime and by-product slaked lime can be used.

[0093] As SiO2 raw material, commercially available materials as industrial raw materials can be used, for example, silica, silica sand, quartz, diatomaceous earth etc. can be enumerated. These raw materials can be used alone, or two or more can be combined and used. It should be noted that if the CaO raw material and the Al2O3 raw material contain the required amount of SiO2, the above raw materials may not be used.

[0094] For example, when coal ash containing SiO 2 is used as the CaO raw material, the above-mentioned SiO 2 raw material does not need to be added.

[0095] Here, coal ash (fly ash and others) is a general term for combustion ash obtained by burning coal, such as coal combustion ash discharged from a boiler of a thermal power plant. As the coal ash, for example, ash generated from a coal-fired power plant, generated by burning pulverized coal, collected when the combustion gas of a combustion boiler passes through an air waste heat unit or an economizer, collected by an electric dust collector, and coal ash dropped into the furnace bottom of a combustion boiler can be used.

[0096] As Al2O3 raw materials, substances commercially available as industrial raw materials can be used, for example, one or more selected from the group consisting of bauxite, aluminum hydroxide, and aluminum slag ash. The aluminum slag ash can be mainly composed of aluminum hydroxide. Among them, bauxite can be used.

[0097] These raw materials are blended so as to have a predetermined mineral composition ratio after firing, mixed and pulverized to obtain a raw material mixture.

[0098] The method of mixed pulverization is not particularly limited, and dry pulverization or wet pulverization can be applied. In the case of wet pulverization, dehydration treatment is required for subsequent granulation. In addition, when quicklime is used as the raw material, it is preferably carried out in a dry manner.

[0099] In addition, by adjusting the input ratio of the raw materials, the γ-C2S / C2AS ratio in the CO2-fixed ceramic can be controlled.

[0100] The raw material mixture may be granulated before firing. The granulated product may be adjusted to an appropriate size, for example, 0.5 to 3.0 cm.

[0101] The calcination temperature may be, for example, 1,200°C to 1,600°C, preferably 1,300°C to 1,550°C, and more preferably 1,400°C to 1,450°C.

[0102] A rotary kiln or the like can be used for firing.

[0103] For example, a rotary kiln can be used in which the bricks of the firing zone are made of high-purity alumina bricks having an Al2O3 content of 99% or more by mass, and / or the inner surface of the bricks in the firing zone of the rotary kiln can be coated with alumina mortar adjusted to an appropriate concentration before firing.

[0104] The CO 2 -fixed ceramic can be obtained as an inorganic fired product (clinker) obtained by firing an inorganic raw material, or can be obtained as a powdered inorganic fired product by pulverizing the clinker.

[0105] In addition to the inorganic calcined product containing the above-mentioned inorganic components such as γ-C2S and C2AS, the CO2-fixed ceramic may also contain disaccharides as other organic components. By including disaccharides, a chelate is further formed with Ca dissolved in the surface water of the inorganic calcined product, which can promote further dissolution.

[0106] The CO2-fixing ceramic preferably contains one or more disaccharides selected from the group consisting of trehalose, maltose, and sucrose, for example. Among them, it is more preferable to contain trehalose which has a high effect of promoting the carbonation reaction.

[0107] From the viewpoint of the effect of promoting the carbonation reaction, the CO2 immobilized ceramic preferably contains 0.5 to 10 parts by mass of disaccharides, and more preferably contains 5 to 10 parts by mass of disaccharides, relative to 100 parts by mass of the CO2 immobilized ceramic. In addition, in order to obtain a sufficient carbonation promoting effect, the content of trehalose in the disaccharides is preferably 90% by mass or more, and more preferably 95% by mass or more, in 100% by mass of the disaccharides.

[0108] The above describes the embodiments of the present invention. However, these are examples of the present invention, and various configurations other than the above can be adopted. In addition, the present invention is not limited to the above embodiments, and modifications, improvements, etc. within the scope that can achieve the object of the present invention are included in the present invention.

[0109] Example

[0110] Hereinafter, the present invention will be described in detail with reference to examples, but the present invention is not limited by any of the descriptions of these examples.

[0111] <Production of CO₂ Immobilization Ceramics>

[0112] (Using Raw Materials)

[0113] · By - product slaked lime: Slaked lime by - produced after reacting calcium carbide with water to produce acetylene. SiO₂ is 0.8% by mass, Al₂O₃ is 0.6% by mass, Fe₂O₃ is 0.3% by mass, CaO is 68.5% by mass, MgO is 0.02% by mass, Na₂O is 0.01% by mass, K₂O is 0.01% by mass, SO₃ is 0.5% by mass. The loss on ignition (L.O.I.) is 24.1% by mass.

[0114] · Silica: Silica fine powder, SiO₂ is 99.3% by mass, Al₂O₃ is 0.01% by mass, Fe₂O₃ is 0.0% by mass, CaO is 0.0% by mass, MgO is 0.04% by mass, Na₂O is 0.02% by mass, K₂O is 0.3% by mass, SO₃ is 0.04% by mass, and the loss on ignition (L.O.I.) is 0.6% by mass.

[0115] · Alumina: Al₂O₃ is 99.03% by mass, SiO₂ is 0.14% by mass, Fe₂O₃ < 0.01% by mass, CaO < 0.01% by mass, TiO₂ is 0.06% by mass, and the loss on ignition (L.O.I.) is 0.82% by mass.

[0116] [Experimental Example 1]

[0117] (Immobilization Ceramic A)

[0118] As raw materials containing CaO and SiO₂, the above - mentioned by - product slaked lime and silica were mixed and pulverized dry in such a way as to achieve the CaO / SiO₂ molar ratio shown in Table 1, and a mixed raw material was obtained. The obtained mixed raw material was granulated to produce granules with a diameter of about 1 cm to 2.5 cm.

[0119] The obtained granules were put into a rotary kiln whose sintering zone bricks were made of high-purity alumina bricks (Al2O3 content was 99% or more by mass), and sintered at a combustion point temperature (Japanese: sintering point temperature) of 1,400°C. During the cooling process to room temperature, powdered clinker was synthesized. The obtained clinker powder was used as CO2 fixed ceramic A.

[0120] It should be noted that CO2 immobilized ceramics are sometimes simply referred to as "immobilized ceramics".

[0121] (Immobilized ceramics B, C)

[0122] Instead of silica, the above-mentioned alumina is used, and the CaO / SiO2 molar ratio and Al2O3 content shown in Table 1 are adopted. Except for this, the same operation is performed as the fixed ceramic A to synthesize a clinker powder with the mineral proportions shown in Table 1, which is used as CO2 fixed ceramics B and C.

[0123] (Immobilized ceramic D)

[0124] Calcium carbonate powder with a purity of 99.0% by mass or more and silicon oxide powder with a purity of 99.0% by mass or more were mixed in a manner such that the molar ratio of CaO / SiO2 was 2.0, and heat-treated at 1,400°C for 2 hours, and slowly cooled in an electric furnace to synthesize γ-C2S powder. The obtained γ-C2S powder was used as CO2 fixed ceramic D.

[0125] C2AS and C 12 A7 is not dissolved in the γ-C2S powder obtained here and is not contained in the γ-C2S powder.

[0126] The elemental surface analysis was performed using the obtained SEM images and an energy dispersive X-ray analyzer (EDS), and the results confirmed that in the fixed ceramics A to C, C2AS existed in the γ crystal phase composed of γ-C2S, and the γ crystal phase did not contain Al2O3. In addition, in the fixed ceramics of the fixed ceramics A to C, β-C2S was confirmed, and it was confirmed that Al2O3 was contained in the β crystal phase composed of β-C2S.

[0127] Furthermore, the fracture surfaces of the obtained clinker powders of the immobilized ceramics A to C were observed using SEM, and as a result, it was confirmed that C2AS existed in the γ crystal phase composed of γ-C2S.

[0128] Figure 1 SEM image of the fracture surface of the clinker with immobilized ceramic A, Figure 2 This is a SEM image showing a fracture surface of a clinker in which ceramic B is immobilized. Figure 1 , 2In the figure, arrow A (white area) indicates C2AS, and arrow B (gray area) indicates γ-C2S.

[0129] [Calculation of Carbonation Rate]

[0130] 25 g of the obtained immobilized ceramics A to D were placed in plastic cups respectively, and carbonation treatment was carried out in a constant temperature and humidity room under the conditions of 20° C., 80% RH, and a CO 2 concentration of 20% by volume.

[0131] After carbonation at each prescribed time (1 day, 3 days, 7 days) shown in Table 1, it was dried at 105°C for 24 hours, the mass of the sample thus obtained was measured, and the carbonation rate was calculated based on the following formula (1) according to the mass change before and after the carbonation treatment. The results are shown in Table 1.

[0132] Formula (1): Carbonation rate = (ΔM × 56.08) / (M × wCaO × 44.01)

[0133] In the above formula (1), ΔM represents the increased mass [g] caused by carbonation, M represents the mass [g] of the immobilized ceramic before carbonation, and wCaO represents the content [wt%] of CaO in the immobilized ceramic before carbonation. The increased mass caused by carbonation is the mass obtained by deducting the sample weight before carbonation from the sample weight after carbonation. The content of CaO in the CO2 immobilized ceramic before carbonation is measured by fluorescent X-ray analysis.

[0134] [Table 1]

[0135]

[0136] In Table 1, γ-C2S represents γ-2CaO·SiO2, β-C2S represents β-2CaO·SiO2, and C2AS represents 2CaO·Al2O3·SiO2.

[0137] In Table 1, the ratio of the mineral composition was calculated based on the results of the chemical composition quantitatively determined using fluorescent X-rays and the identification results by powder X-ray diffraction.

[0138] [Experimental Example 2]

[0139] Various additives were added and mixed to 100 parts by mass of the CO 2 immobilization ceramic A in predetermined proportions as shown in Table 2, thereby obtaining a CO 2 immobilization ceramic E.

[0140] The obtained CO 2 immobilized ceramic E was subjected to carbonation treatment in the same manner as in Experimental Example 1, and the carbonation rate was calculated. The results are shown in Table 2.

[0141] [Table 2]

[0142] [Table 2]

[0143]

[0144] [Experimental Example 3]

[0145] The carbonation treatment was carried out in the same manner as in Experimental Example 1 except that the CO2-fixed ceramic A was used and the conditions of the carbonation treatment in the constant temperature and humidity chamber were changed to the conditions shown in Table 3, and the carbonation rate was calculated. The results are shown in Table 3.

[0146] [Table 3]

[0147] [Table 3]

[0148]

[0149] According to the results in Table 1, compared with Comparative Example 1, the CO2 immobilized ceramics of Examples 1 to 3 achieved a high carbonation rate.

[0150] According to the results in Table 2, when disaccharides were added, the carbonation effect was large. In particular, when trehalose was added, the carbonation effect was greater.

[0151] According to the results of Table 3, a good carbonation rate can be obtained by setting the carbonation temperature to 75° C. or lower and / or 50% RH or higher.

[0152] By using the CO 2 immobilized ceramics of Examples 1 to 3 and performing a carbonation treatment under relatively low temperature and / or relatively high humidity conditions, a CO 2 immobilized product can be obtained in which CO 2 is immobilized.

[0153] Such CO2 fixed products can be used as cement additives in the fields of civil engineering and construction, and can also be used directly as aggregates for mortar and concrete, roadbed materials, fill materials, backfill materials, etc. In addition, they can be effectively used as filler and extender materials for paints, inks, and rubber.

[0154] This application claims the benefit of priority based on Japanese patent application No. 2022-019300, filed on February 10, 2022, the disclosure of which is incorporated herein in its entirety.

Claims

1. A CO2 fixation ceramic comprising: A γ crystalline phase composed of γ-2CaO·SiO2 (γ-C2S); and 2CaO·Al2O3·SiO2(C2AS).

2. The CO2 fixation ceramic according to claim 1, comprising a glass phase and / or CaO·2Al2O3 (CA2).

3. The CO2 fixation ceramic according to claim 1 or 2, wherein: In 100 mass % of the CO 2 immobilization ceramic, the content of the γ-C 2 S is 30 mass % or more and 98 mass % or less.

4. The CO2-fixing ceramic according to any one of claims 1 to 3, wherein The content of the C2AS is 0.5% by mass or more and 50% by mass or less relative to 100% by mass of the γ-C2S. 5 . The CO 2 immobilization ceramic according to claim 1 , comprising a hetero phase present in the γ crystalline phase, wherein the hetero phase includes the C 2 AS.

6. The CO2 fixation ceramic according to claim 5, wherein: The γ crystal phase does not contain Al2O3.

7. The CO2-fixing ceramic according to any one of claims 1 to 6, comprising a β-crystalline phase composed of β-2CaO·SiO2 (β-C2S).

8. The CO2 fixation ceramic according to claim 7, wherein: The β crystal phase contains Al2O3.

9. The CO2 fixation ceramic according to claim 7 or 8, wherein: The content of the β-C2S is 1.0% by mass or more and 50% by mass or less relative to 100% by mass of the γ-C2S.

10. The CO2-fixing ceramic according to any one of claims 1 to 9, comprising a disaccharide.

11. The CO2 fixation ceramic according to claim 10, wherein: The content of the disaccharide in 100 parts by mass of the CO 2 immobilization ceramic is 0.5 parts by mass or more and 10 parts by mass or less.

12. The CO2 fixation ceramic according to claim 10 or 11, wherein: The disaccharide comprises trehalose.

13. The CO2-fixing ceramic according to any one of claims 1 to 12, which is in powder form.

14. A method for producing a CO2-fixed product, comprising the step of performing a carbonation treatment on the CO2-fixed ceramic according to any one of claims 1 to 13 under conditions of less than 75°C and / or 50%RH or more.

Citation Information

Patent Citations

  • Ceramic product with oriented particles and method for the production thereof

    CN107124880A

  • Method for preparing high-carbonization-activity cementing material from industrial waste residues

    CN113880466A

  • Weed control material and usage of the same

    JP2019058091A

  • Ceramic product with oriented particles and method for the production thereof

    US20170129816A1