Steel sheet manufacturing method, trimming device, manufacturing device, rolled steel sheet, coil, and blank

By directly applying lubricating oil on the surface of the steel plate and using a lubricating oil attachment device to supply the cutting area, the problem of edge chipping of the rotary knife when cutting high-tensile steel plates is solved, and the yield of the steel plate and the stability of the production line are improved.

CN118742407APending Publication Date: 2024-10-01JFE STEEL CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202280093154.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2022-03-10
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

When cutting high-tensile steel plates with the existing technology, the rotary knife is prone to chipping, leading to increased friction, damage to the steel plate, and adhesion of iron powder, affecting the normal operation of the production line.

Method used

Before cutting, apply lubricating oil directly on the surface of the steel plate to reduce the friction between the knife and the steel plate and reduce the frequency of edge chipping. The lubricating oil is evenly supplied through the lubricating oil attachment device to ensure lubrication of the cutting area.

Benefits of technology

It significantly reduces the chipping frequency of the rotary knife, improves the yield of the steel plate, reduces the indentation of the steel plate and the shedding of iron powder, and improves the stability of the production line and product quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118742407A_ABST
    Figure CN118742407A_ABST
Patent Text Reader

Abstract

The tipping frequency is further improved, and the yield of steel plate manufacturing is increased. By directly applying lubricating oil to a steel plate (1) before trimming, insufficient supply of oil is eliminated, and the tipping frequency of an edge trimmer is suppressed by reducing friction. Namely, the method for manufacturing the steel plate (1) has a process for cutting the edge portion of the steel plate (1) by means of a rotary blade (2), and in the process for cutting the steel plate (1) by means of the rotary blade (2), lubricating oil adheres to the positions to be cut by means of the rotary blade (2) on the surfaces (1a, 1b) of the steel plate (1) before cutting.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a cutting technology for cutting the edge (end in the width direction of the plate) of a steel plate, and a technology for manufacturing a steel plate including the cutting process, and a manufactured steel plate and a coil and a blank made of the steel plate. In particular, the present invention is a technology suitable for manufacturing a high-tensile steel plate (high-tensile strength steel plate) having a tensile strength of 590 MPa or more, that is, a steel plate having a plate thickness of 0.4 mm or more. Background Art

[0002] For example, in hot-dip galvanizing plants and cold rolling plants, there is a process (equipment) for trimming the edges (ends in the width direction) of steel plates according to the product width. In recent years, the demand for high-tensile steel plates has increased in the fields of automobiles and building materials. Therefore, in the manufacture of steel plates, a process of cutting high-tensile steel plates using a rotating knife (trimming knife) is sometimes performed.

[0003] However, when cutting a high-tensile steel plate (hereinafter also referred to as a high-strength steel plate), the rotary blade may not be able to withstand the load from the steel plate and may break the blade, thereby producing a material that has not been trimmed (untrimmed material). In particular, if a high-tensile steel plate with a tensile strength of 590 MPa or more, such as a steel plate with a thickness of 0.4 mm or more, is cut, the load applied to the blade during trimming is high and the blade breakage is unavoidable.

[0004] In this regard, there is a method of applying cutting oil (lubricating oil) to a rotating rotary blade, for example, as described in Patent Document 1. In Patent Document 1, the cutting oil is directly sprayed on the rotary blade to apply the cutting oil, so that the blade and the steel plate have lubricity, thereby reducing friction.

[0005] Prior art literature

[0006] Patent Literature

[0007] Patent Document 1: Japanese Patent Application Publication No. 2005-153116 Summary of the invention

[0008] Problems to be solved by the invention

[0009] The chipping of the rotary blade caused by cutting is considered to occur when stress is concentrated on the corner (blade) of the blade. As the load generated on the blade, it is estimated that there are two types of vertical resistance accompanied by shear load and lateral force caused by friction between the steel plate and the blade.

[0010] Regarding the lateral force, it is considered that it can be suppressed by reducing the friction between the steel plate and the knife.

[0011] As shown in Patent Document 1, a method of directly supplying cutting oil to a rotating blade is used as a measure to improve lubricity between the blade and the steel plate and reduce friction. However, it is desired to further improve the frequency of chipping.

[0012] In addition, according to the inventor's research, it is also assumed that the steel plate side is damaged due to chipping of the rotating blade during cutting. In the case where the end face of the steel plate is damaged, in the processing line of manufacturers such as automobile companies that purchase rolled steel plates and coils as products by the rotating blade cutting process and the subsequent process, the iron powder that falls off from the damaged part of the steel plate adheres to the steel plate being processed, which easily causes indentations on the steel plate. In addition, there is a possibility that the iron powder adheres to the processing equipment and causes failure.

[0013] The present invention focuses on the above-mentioned points, and aims to further improve the chipping frequency and increase the yield of steel sheet production.

[0014] Methods used to solve problems

[0015] The inventors studied the effect of cutting by directly applying cutting oil to a rotary blade, and found that the frequency of chipping needs to be further improved.

[0016] That is, the following findings were obtained as disadvantages of the technique of directly applying cutting oil to the rotary blade.

[0017] (1) When cutting oil is directly applied to the rotating rotary blade, the oil is scattered due to the centrifugal force of the rotation of the rotary blade, resulting in a state where the cutting oil is insufficiently supplied to the cutting portion. It should be noted that although it is also possible to consider supplying oil to the blade at a position close to the cutting portion, it is difficult to do so if interference with other equipment is taken into consideration. In addition, even if a large amount of oil is directly supplied to the rotating blade, during the process of the blade cutting the steel plate, the blade may slide on the steel plate after the blade contacts the steel plate. Moreover, due to the sliding of the blade, the oil is immediately removed at the tip of the blade.

[0018] (2) In addition, this leads to insufficient penetration of oil between the blade and the steel plate. Therefore, even if a large amount of oil is applied to the blade, the effect of improving the chipping is small, and in particular, the chipping during cutting cannot be fully suppressed for high-strength steel plates above 590 MPa.

[0019] Furthermore, there arises the problem of the above-mentioned generation of iron powder due to chipping.

[0020] (3) In contrast, by directly applying lubricating oil to the steel plate before trimming with a rotating knife, it is possible to effectively prevent the oil from running out at the tip of the trimming knife even when the knife is sliding on the steel plate after the knife contacts the steel plate, and it is possible to significantly prevent chipping of the blade even when cutting high-strength steel plates.

[0021] The present invention is based on the knowledge that lubricating oil is directly applied (attached) to a steel plate before trimming to eliminate insufficient oil supply and to reduce friction to suppress the frequency of chipping of the trimmer.

[0022] In addition, the steel plate manufactured by the method of the present invention can suppress the adverse effects of iron powder generated by cutting with a rotating knife with chipped edges, and has established a technology that significantly suppresses the generation of indentations in steel plate manufacturing production lines, automobile stamping production lines, etc. after edge cutting.

[0023] That is, in order to solve the problem, the main purpose of one embodiment of the present invention is a method for manufacturing a steel plate having an edge portion that is processed by cutting the steel plate using a rotating knife, wherein, in the process of cutting the steel plate using the above-mentioned rotating knife, lubricating oil is attached to the position on the surface of the steel plate before cutting at which the rotating knife is to be cut.

[0024] In addition, the present invention is a steel plate manufacturing device, which is a trimming device for cutting the edge of a conveyed steel plate using a rotating knife, wherein a lubricating oil adhering device is provided upstream of the rotating knife for adhering lubricating oil to the position of the steel plate to be cut by the rotating knife.

[0025] Furthermore, one embodiment of the present invention is a rolled steel plate, a coil, or a billet having a smooth end surface (first cut surface) in a cut surface in the width direction.

[0026] The rolled steel plate refers to a steel plate manufactured in a manufacturing line including a rolling process. In addition, at least one end face in the width direction of the rolled steel plate of the present embodiment includes a cut surface.

[0027] Effects of the Invention

[0028] According to the aspect of the present invention, the lubricating oil can be supplied more reliably between the blade and the steel plate, the frequency of chipping can be further improved, and the yield rate of steel plate manufacturing can be improved.

[0029] In addition, according to the method of the present invention, a steel plate or coil having a smooth end surface (first cut surface) at the cut surface of the edge (end in the width direction) can be provided. As a result, according to the method of the present invention, a steel plate or the like can be provided which suppresses the indentation in the steel plate manufacturing line or the automobile stamping line by suppressing the shedding of iron powder.

[0030] That is, the steel plate obtained by the cutting method of the present invention, the coil material and the blank composed of the steel plate can suppress the generation of iron powder generated by cutting with a rotary knife (trimmer) with chipped edges. As a result, the generation of indentations in processing lines such as steel plate manufacturing lines and automobile stamping lines after edge cutting can be significantly suppressed. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 It is a side view for demonstrating the trimming device of the steel plate based on embodiment of this invention.

[0032] Figure 2 It is a top view for explaining the steel plate trimming device based on embodiment of this invention.

[0033] Figure 3 It is a side view for explaining another configuration example of the lubricating oil adhesion device.

[0034] Figure 4 These are SEM observations of sheared surfaces (cut surfaces), (a) is the case of Comparative Example 2, and (b) is the case of Comparative Example 7.

[0035] Figure 5 This is a picture obtained by SEM observation of a sheared surface (cut surface). DETAILED DESCRIPTION

[0036] Next, embodiments of the present invention will be described with reference to the drawings.

[0037] In this embodiment, the trimming equipment (trimming process) of the surface treated steel plate manufacturing line in the steel plate manufacturing is taken as an example for description. The present invention can also be applied to the manufacturing plants of rolled steel plates such as cold rolled steel plates and hot rolled steel plates.

[0038] "Steel plates to be processed"

[0039] This embodiment is applicable even to high-tensile steel plates, especially high-tensile steel plates with a tensile strength of 590 MPa or more, that is, steel plates with a thickness of 0.4 mm or more. This embodiment can also be applied to high-tensile steel plates with a thickness of 4.0 mm or less.

[0040] Examples of steel plates cut by a rotary blade include GI, GA, EG, CRS, tin-plated steel plates, Zn-plated steel plates, and Al-plated steel plates. However, the steel plates are not limited thereto, and any steel plates can be applied. This embodiment can also be applied to steel plates to which a solid lubricating film is applied to GI or GA, or to steel plates to which an organic coating is applied.

[0041] In addition, the inventors discovered the following new problem during their investigation: when cutting high-strength steel plates with a tensile strength of 1180 MPa or more, poor trimming materials due to chipping occur at an extremely high frequency of about 8% of the manufactured coils, requiring offline re-trimming of the poor materials. In response to this problem, when the present invention is applied, it is confirmed that the occurrence rate of poor trimming can be significantly reduced even for high-strength steel plates of 1180 MPa and 1470 MPa grades with a plate thickness of 0.4 mm or more, which have previously experienced significant poor trimming due to chipping.

[0042] Regarding the high-tensile strength steel sheet to be processed in the present embodiment, its composition contains, for example, by mass %, C: 0.03% to 0.35%, Si: 0.01% to 3.00%, Mn: 0.50% to 3.50%, Al: 0.001% to 1.000%, P: 0.100% to 0.0100%, S: 0.0200% to 0.0200%, and the balance is Fe and inevitable impurities.

[0043] In addition, in this specification, the % mark about a component represents mass % unless otherwise specified.

[0044] Next, the reasons for limiting the composition of the steel sheet will be described.

[0045] ·C: 0.03% or more and 0.35% or less

[0046] C has the effect of increasing the strength of the steel strip. For this reason, C needs to be 0.03% or more. On the other hand, when C exceeds 0.35%, the weldability required when used as a raw material for automobiles and home appliances deteriorates. Therefore, the amount of C can be set to 0.03% or more and 0.35% or less.

[0047] From the viewpoint of obtaining a high-strength material having a tensile strength of 1180 MPa or more, the amount of C is preferably set to 0.10% or more. From the viewpoint of obtaining a high-strength material having a tensile strength of 1320 MPa or more, the amount of C is preferably set to 0.13% or more.

[0048] ·Si: 0.01% or more and 3.00% or less

[0049] Si is an element effective in strengthening steel and improving ductility, and for this reason, Si needs to be 0.01% or more. On the other hand, when Si exceeds 3.00%, Si forms oxides on the surface, and the appearance of the coating deteriorates. Therefore, the amount of Si can be set to 0.01% or more and 3.00% or less.

[0050] ·Mn: 0.50% or more and 3.50% or less

[0051] Mn is an element useful for improving hardenability and the strength of steel sheets. This effect cannot be obtained when Mn is less than 0.50%. On the other hand, when the content of Mn is greater than 3.50%, segregation of Mn occurs and workability decreases. Therefore, the Mn amount is preferably 0.50% or more and 3.50% or less.

[0052] From the viewpoint of obtaining a high-strength material with a tensile strength of 1180 MPa or more, the Mn content is preferably set to 1.00% or more. In the case of cooling after annealing using a relatively slow cooling device such as a gas jet cooling device, from the viewpoint of obtaining a steel plate of 1180 MPa grade, Mn is more preferably set to 2.20% or more.

[0053] Al: 0.001~1.000%

[0054] Al is added for the purpose of deoxidizing molten steel. This goal cannot be achieved when the Al content is less than 0.001%. On the other hand, when Al exceeds 1.000%, Al forms oxides on the surface, and the appearance of the coating (surface appearance) deteriorates. Therefore, the Al content can be set to 0.001% or more and 1.000% or less.

[0055] ·P: 0.100% or less

[0056] P is one of the elements that are inevitably contained. Since there is a concern that the cost will increase in order to make P less than 0.005%, P is preferably 0.005% or more. On the other hand, as P increases, the slab manufacturability deteriorates. In addition, containing P will inhibit the alloying reaction, resulting in uneven plating. In order to suppress these situations, it is necessary to set the P content to less than 0.100%. Therefore, the P amount can be set to less than 0.100%. Preferably, it is less than 0.050%.

[0057] ·S: 0.0100% or less

[0058] S is an element that is inevitably contained in the steelmaking process. However, when a large amount of S is contained, weldability deteriorates. Therefore, S can be set to 0.0100% or less. Since there is a concern that the cost will increase if S is less than 0.0002%, S is preferably set to 0.0002% or more.

[0059] N: 0.0200% or less

[0060] N is an element that is inevitably contained in the steelmaking process. However, when N is contained in large amounts, ductility deteriorates. Therefore, N can be set to 0.0200% or less. There is no lower limit, but it takes a lot of cost to reduce it to 0.0005% or less, so the lower limit is about 0.0005%.

[0061] Other components that may be added are described.

[0062] The high-tensile steel sheet to be processed in the present embodiment may contain, as necessary, B: 0.0002% to 0.0050% inclusive, Nb: 0.005% to 0.100% inclusive, Ti: 0.005% to 0.200% inclusive, Cr: 0.005% to 1.000% inclusive, Mo: 0.005% to 1.000% inclusive, Cu: 0.005% to 1.000% inclusive, and Ni: 0.005% to 1.000% inclusive. , Sb: 0.001% to 0.200%, Zr: 0.005% to 0.100%, V: 0.005% to 0.200%, W: 0.005% to 0.100%, Sn: 0.001% to 0.200%, Ca: 0.0002% to 0.0050%, REM: 0.0002% to 0.0050%, Mg: 0.0002% to 0.0050%.

[0063] When these elements are added, appropriate contents and reasons for their limitations are as follows.

[0064] ·B: 0.0002% or more and 0.0050% or less

[0065] When B is 0.0002% or more, a quenching promotion effect can be obtained. On the other hand, when the content of B is greater than 0.0050%, castability and chemical conversion treatment properties deteriorate. Therefore, when B is contained, the amount of B can be set to more than 0.0002% and less than 0.0050%. From the viewpoint of obtaining a sufficient hardenability promotion effect, B is preferably set to more than 0.0005%, and from the viewpoint of reducing inclusions, B is preferably set to less than 0.0025%.

[0066] Nb: 0.005% or more and 0.100% or less

[0067] When Nb is 0.005% or more, the effect of strength adjustment (strength improvement) can be obtained. On the other hand, when Nb is greater than 0.100%, it leads to increased costs. In addition, inclusions increase, which impairs the castability and ductility of the steel plate. Therefore, when Nb is contained, the amount of Nb can be set to more than 0.005% and less than 0.100%. From the viewpoint of obtaining the effect of increasing strength by refining the structure and improving the delayed fracture resistance, Nb is further preferably added to 0.01% or more. In addition, from the viewpoint of reducing inclusions, Nb is further preferably set to less than 0.06%.

[0068] ·Ti: 0.005% or more and 0.200% or less

[0069] When Ti is 0.005% or more, the effect of strength adjustment (strength improvement) can be obtained. On the other hand, when Ti is greater than 0.200%, inclusions increase, which damages the castability and ductility of the steel plate. In addition, it leads to deterioration of chemical conversion treatment properties. Therefore, when Ti is contained, the amount of Ti can be set to more than 0.005% and less than 0.200%. From the viewpoint of obtaining the effect of increasing strength by refining the structure and improving the delayed fracture resistance, Ti is further preferably added to more than 0.01%. In addition, from the viewpoint of reducing inclusions, Ti is further preferably set to less than 0.15%.

[0070] Cr: 0.005% or more and 1.000% or less

[0071] When Cr is 0.005% or more, a hardenability effect can be obtained. On the other hand, when Cr is greater than 1.000%, Cr is enriched on the surface, so chemical conversion treatment, plating properties, and weldability deteriorate. Therefore, when Cr is contained, the Cr amount can be set to 0.005% or more and 1.000% or less.

[0072] ·Mo: 0.005% or more and 1.000% or less

[0073] When Mo is 0.005% or more, the effect of strength adjustment (strength improvement) can be obtained. On the other hand, when Mo is greater than 1.000%, the chemical conversion treatment property is deteriorated and the cost is increased. Therefore, when Mo is contained, the Mo amount can be set to 0.0005% or more and 1.000% or less.

[0074] ·Cu: 0.005% or more and 1.000% or less

[0075] When Cu is 0.005% or more, the delayed fracture resistance improvement effect can be obtained. On the other hand, when Cu is greater than 1.000%, the chemical conversion treatment property deteriorates and the cost increases. Therefore, when Cu is contained, the Cu amount can be set to 0.005% or more and 1.000% or less. From the viewpoint of improving the delayed fracture resistance, it is further preferred to add 0.05% or more of Cu. In addition, from the viewpoint of preventing the chemical conversion treatment property from deteriorating, Cu is further preferably set to 0.2% or less.

[0076] ·Ni: 0.005% or more and 1.000% or less

[0077] When Ni is 0.005% or more, the effect of promoting the formation of the residual γ phase can be obtained. On the other hand, when Ni is greater than 1.000%, the cost increases. Therefore, when Ni is contained, the Ni amount can be set to 0.005% or more and 1.000%.

[0078] ・Sb: 0.001% or more and 0.200% or less

[0079] Sb can be contained from the viewpoint of inhibiting nitridation and oxidation on the surface of the steel plate or decarburization of tens of micrometers on the surface of the steel plate caused by oxidation. By inhibiting nitridation and oxidation, the amount of martensite generated on the surface of the steel plate is prevented from decreasing, and fatigue properties and surface quality are improved. Such an effect can be obtained when Sb is 0.001% or more. On the other hand, when Sb is greater than 0.200%, toughness deteriorates. Therefore, when Sb is contained, the amount of Sb can be set to 0.001% or more and 0.200% or less. From the viewpoint of improving fatigue resistance, Sb is preferably added at 0.002% or more, and from the viewpoint of obtaining high toughness, Sb is further preferably set to 0.100% or less.

[0080] ·Zr: 0.005% or more and 0.100% or less

[0081] When Zr is 0.005% or more, the effect of high strength can be obtained. On the other hand, when Zr is greater than 0.100%, inclusions increase, which impairs the castability and ductility of the steel sheet. Therefore, when Zr is contained, the Zr amount can be set to 0.005% or more and 0.100% or less.

[0082] ·V: 0.005% or more and 0.200% or less

[0083] When V is 0.005% or more, the effect of high strength can be obtained. On the other hand, when V is greater than 0.200%, inclusions increase, which impairs the castability and ductility of the steel sheet. Therefore, when V is contained, the V amount can be set to 0.005% or more and 0.200% or less.

[0084] W: 0.005% or more and 0.100% or less

[0085] When W is 0.005% or more, the effect of high strength can be obtained. On the other hand, when W is greater than 0.100%, inclusions increase, which impairs the castability and ductility of the steel sheet. Therefore, when W is contained, the W content can be set to 0.005% or more and 0.100% or less.

[0086] Sn: 0.001% or more and 0.200% or less

[0087] Sn can be contained from the viewpoint of inhibiting nitridation and oxidation on the surface of the steel plate or decarburization of tens of micrometers on the surface of the steel plate caused by oxidation. By inhibiting nitridation and oxidation, the amount of martensite generated on the surface of the steel plate is prevented from decreasing. As a result, fatigue properties and surface quality are improved. Such an effect can be obtained when Sn is 0.001% or more. On the other hand, when Sn is greater than 0.200%, toughness deteriorates. Therefore, when Sn is contained, the amount of Sn can be set to 0.001% or more and 0.200% or less. From the viewpoint of improving fatigue resistance, it is preferred to add 0.002% or more of Sn, and from the viewpoint of obtaining high toughness, Sn is further preferably set to 0.100% or less.

[0088] ·Ca: 0.0002% or more and 0.0050% or less

[0089] Ca has the effect of spheroidizing the morphology of inclusions and improving bendability and delayed fracture resistance. From the viewpoint of obtaining such an effect, 0.0002% or more of Ca can be added. However, when Ca is added in large amounts, the cost increases, so Ca is preferably set to 0.0050% or less.

[0090] ・REM (Rare Earth Metal): 0.0002% or more and 0.0050% or less

[0091] REM has the effect of spheroidizing the morphology of inclusions and improving bendability and delayed fracture resistance. From the perspective of obtaining such an effect, 0.0002% or more of REM can be added. However, when a large amount of REM is added, the cost increases. Therefore, REM is preferably set to 0.0050% or less.

[0092] Mg: 0.0002% or more and 0.0050% or less

[0093] Mg has the effect of spheroidizing the morphology of inclusions and improving bendability and delayed fracture resistance. From the viewpoint of obtaining such an effect, it is preferred to add 0.0002% or more of Mg. However, when adding a large amount of Mg, it leads to an increase in cost, so Mg is preferably set to 0.0050% or less.

[0094] The steel sheet having the above-described composition can be manufactured by a known or arbitrary method. For example, a slab having the above-described composition can be heated and hot-rolled to produce a hot-rolled steel sheet, the hot-rolled steel sheet can be pickled, and then the hot-rolled steel sheet can be cold-rolled to produce a cold-rolled steel sheet as required. In addition, the surface of the steel sheet may also be subjected to the surface treatment described above.

[0095] "First Implementation Method"

[0096] Figure 1 It is a figure explaining the structure of the trimming device provided in the trimming equipment.

[0097] like Figure 1 As shown, in this embodiment, the steel sheet 1 subjected to plating or other surface treatment is conveyed to the trimming equipment along the conveyor line, and the sheet width direction end portion (edge ​​portion) of the steel sheet 1 being conveyed is trimmed.

[0098] (structure)

[0099] The trimming device of the present embodiment includes a rotating blade 2, a calendering roller 7, and a lubricating oil adhering device. In addition, the trimming device of the present embodiment includes a film thickness equalization device. It may also include at least one of the calendering roller 7 and the film thickness equalization device. It should be noted that, in the present embodiment, the calendering roller 7 also serves as the film thickness equalization device.

[0100] <Spinning Knife 2>

[0101] like Figure 1 and Figure 2 As shown, the rotary blade 2 has a pair of rotary blades 2A and 2B (upper blade 2A and lower blade 2B) that can clamp the steel plate 1 and cut the steel plate 1 from the plate thickness direction. Figure 2 As shown, the contact position between the blade tips of the pair of rotating blades 2A and 2B becomes the cutting position.

[0102] Figure 2 The symbol L in represents the position of the steel plate 1 before cutting, which is assumed to pass through the cutting position. Figure 1 and Figure 2 Reference numeral 10 in the figure denotes lubricating oil adhered to the steel plate 1 by the lubricating oil adhering device.

[0103] like Figure 1 As shown, the pair of rotating blades 2A and 2B are set so that the rotation direction at the cutting position is the same as the conveying direction.

[0104] The rotary blade 2 performs trimming processing of the edge portion (end portion) of the cut steel plate 1 according to the product width before, for example, the exit-side inspection.

[0105] <Lubricant adhesion device>

[0106] like Figure 1 As shown, the lubricating oil attachment device is arranged at a position upstream of the setting position of the rotating blade 2 in the steel plate conveying direction, that is, at a position that can face the surfaces 1a and 1b of the steel plate 1 before cutting. Figure 2 As shown, the lubricant oil adhering device is a device that preliminarily adheres the lubricant oil 10 to the area including the position (position indicated by symbol L) to be cut by the rotating blade 2 on the surface 1 a , 1 b of the steel plate 1 .

[0107] The lubricating oil attaching device of this embodiment has a spray device 3 (injection nozzle), and the spray device 3 sprays the lubricating oil onto the surfaces 1a and 1b of the steel plate 1 to attach the lubricating oil to the surfaces 1a and 1b of the steel plate 1. The spray device 3 is connected to an oil tank 4 for storing the lubricating oil and a compressor or other air supply device 5 for supplying air. The spray device 3 can be configured as follows: according to the instruction from the controller 6, the air and the lubricating oil are mixed at the front end of the nozzle to make the lubricating oil mist, and the mist lubricating oil can be sprayed onto the surfaces 1a and 1b of the steel plate 1.

[0108] [Water content of lubricating oil]

[0109] The water content of the lubricating oil is preferably less than 3000 ppm.

[0110] In this state, lubricating oil still adheres to the end of the steel plate after being cut by the rotary blade 2. If the water content of the adhered lubricating oil is 3000 ppm or more and the water content is high, the flat surface or cut surface of the steel plate may rust due to the water contained in the lubricating oil during the period from cutting by the rotary blade 2 to processing the steel plate into a product by an automobile manufacturer, a home appliance manufacturer, etc. This makes it difficult to use this embodiment in the manufacture of steel plates for automobiles and home appliances.

[0111] On the other hand, by setting the water content of the lubricating oil to less than 3000 ppm, rust formation on the flat surface or cut surface of the steel sheet can be suppressed.

[0112] From the viewpoint of suppressing rust for a longer period of time, the water content of the lubricating oil is more preferably 2000 ppm or less.

[0113] The lower limit of the water content of the lubricating oil is 0 ppm. In consideration of the cost required for dehydration, the lower limit of the water content of the lubricating oil is preferably 20 ppm or more.

[0114] It should be noted that "ppm" in this specification means ppm by weight.

[0115] [Spray volume]

[0116] The spray volume has the same meaning as the amount attached to the steel plate surface.

[0117] For manufacturers that process steel plates in the automotive industry, for example, after stamping the steel plates or the blanks after trimming the steel plates and before the chemical conversion treatment and electrodeposition coating process, there is a cleaning process of degreasing the oil (stamping oil, rust-proof oil) attached to the steel plates using an alkaline cleaning solution. At this time, the more oil is attached, the more significantly the degreasing performance in the degreasing process deteriorates, which has an adverse effect on the chemical conversion treatment and coating performance. Therefore, when manufacturing steel plates for such purposes, it is difficult to supply a larger amount of cutting oil in the conventional method of directly applying oil to a rotating blade and cutting the steel plates because the oil will be excessively transferred from the rotating blade to the steel plate, resulting in poor degreasing.

[0118] Meanwhile, the inventors have conducted various studies and have obtained new knowledge that the following effects can be obtained when a method is adopted in which lubricating oil is directly applied (attached) to a steel sheet before trimming and then cut.

[0119] That is, the inventors have confirmed that even if the amount of lubricating oil supplied to the steel sheet is the same, the frequency of chipping can be suppressed more when lubricating oil is directly supplied (attached) to the steel sheet and cutting is performed compared to when oil is directly applied to the trimming rotary blade.

[0120] The reason for this is not necessarily clear, but it is considered to be due to a new mechanism of retaining oil at the blade tip as described below.

[0121] That is, when the lubricant is directly applied to the rotating blade as in the past, no new lubricant is supplied after the blade contacts the steel plate. Therefore, the oil supply to the blade tip cannot be suppressed during the process of the blade deforming the steel plate while the blade corner, i.e., the blade tip, slides on the steel plate until the steel plate is cut. Therefore, it is presumed that the lateral force caused by the friction between the steel plate and the blade acts strongly on the blade during this process.

[0122] On the other hand, when the lubricant is directly applied (attached) to the steel plate before trimming, after the knife contacts the steel plate, during the process of cutting as the knife tip slides on the surface of the steel plate, there is also lubricant applied (attached) to the area on the new surface of the steel plate in front of the knife tip sliding. Therefore, the lubricant is continuously supplied. As a result, it is believed that oil shortage is suppressed and the friction between the steel plate and the knife is reduced. Thus, when the lubricant is directly applied (attached) to the steel plate, chipping is significantly suppressed. In addition, during the sliding process, the oil locally accumulated between the knife tip and the steel plate is generated on the chip side removed by trimming, so poor degreasing caused by accumulated oil is also less likely to occur.

[0123] As described above, when lubricating oil is directly applied (attached) to the steel plate, the amount of lubricating oil supplied to the steel plate for trimming can be reduced, compared with the case where oil is directly applied to the rotary blade.

[0124] It should be noted that when a large amount of lubricating oil is applied to the entire steel plate, a large amount of lubricating oil needs to be removed in the degreasing production line, and the frequency of changing the liquid is significantly increased. Therefore, it is very difficult to implement realistically from the perspective of cost and production line operability. In addition, when the steel plate is applied as a whole, the load on the earth's environment is also significantly increased. In the cutting method of the present invention, a significant effect can be obtained by applying the coating only in the vicinity of the rotating blade, so this problem can also be solved.

[0125] That is, by applying this embodiment, it is not necessary to apply (attach) a large amount of oil in order to obtain a significant effect of suppressing chipping. As a result, there is an advantage that the effect can be obtained with an amount of oil attached within a range that does not impair the degreasing properties required by automobile manufacturers and the like.

[0126] Thus, according to the present invention, the frequency of chipping can be suppressed with a small amount of lubricating oil attached, compared with a method of directly applying oil to a rotary blade and cutting a steel plate. As a result, according to the present invention, it is found that the present invention has the advantages of being applicable to applications such as automobile frames and body parts, and is also excellent in environmental protection. In addition, according to the present invention, scattering can be prevented, and the area where the lubricating oil is attached to the steel plate can be limited.

[0127] Here, regarding the spray amount of the lubricating oil, the oil flow rate and the like are adjusted so that the lubricating oil can be continuously and evenly applied (adhered) to the edge portions of the surfaces 1 a and 1 b of the steel plate 1 .

[0128] For example, in order to ensure a certain oil coating density or higher on the surfaces 1 a and 1 b of the steel plate 1 , the spray amount is set as shown in the following formula (1).

[0129] That is, the lower limit of the spray amount is set according to the conveying speed of the steel sheet, for example, according to the following formula (1). More preferably, the lower limit of the spray amount is set according to the formula (2).

[0130] The lower limit of spray volume = 1.00 [mL / m 2 ]×0.04(:Width of spray area)[m]×Conveying speed[mpm]×60[min / h] …(1)

[0131] The lower limit of spray volume = 7.24 [mL / m 2 ]×0.04(:Width of spray area)[m]×Conveying speed[mpm]×60[min / h]…(2)

[0132] By setting the spray amount to be equal to or greater than the amount specified by formula (1) per single surface, a particularly good effect of suppressing chipping can be obtained. It should be noted that the lower limit of the spray amount specified by formula (1) corresponds to 1.00 mL / m 2The oil coating density is the amount of lubricating oil attached to the surface of the steel plate per unit area. By further setting the spray amount to be greater than the amount specified by formula (2), a better effect of suppressing edge chipping can be obtained. Therefore, the lower limit of the spray amount is preferably set within this range. It should be noted that the lower limit of the spray amount specified by formula (2) corresponds to 7.24 mL / m 2 The oil coating density is preferably formed on the steel plate surface on the upper blade side (upper surface) where the chipping occurs initially. It is further preferred that the oil coating density is formed on both the upper blade side and the lower blade side.

[0133] Here, the provisions in formula (1) and formula (2) are based on the premise that the width of the spray area (adhesion area) is from the edge of the steel plate to 0.04m. In the case where the width is different, the spray amount can be obtained by substituting other values ​​instead of 0.04m. [mpm] is the distance (m) that the steel plate passes per minute.

[0134] When the width of the spray area is set to 0.01 m and the conveying speed is set to 40 mpm, it is set to 0.02 L / hour in formula (1) and 0.17 L / hour in formula (2). These values ​​can be considered as the lower limit of the spray amount in the case of excellent chipping suppression and the lower limit of the spray amount in the case of further suppressing chipping. It should be noted that the values ​​when converted to oil coating density are as described above.

[0135] There is no particular upper limit on the spray volume.

[0136] However, in the case of excessive oiling, the oil 10 attached to the edge of the steel plate 1 falls from the steel plate, which may have an adverse effect on the production line equipment here and there. Therefore, the spray amount is preferably very small. From this point of view, the spray amount of the lubricating oil is preferably set to less than 60L / hour for both sides combined. The reason for setting the spray amount as the total of both sides is that the oil flows out from both the upper and lower surfaces, and when the coil is made, the oil on both sides flows out as a whole. In the case of spraying on both sides, a spray amount of less than 60L / hour for both sides corresponds to less than 15mL / m 2 In the case of spraying only on one side, it corresponds to less than 30mL / m 2 Here, the width of the spray area is set to 0.15m, and the conveying speed of the steel plate is set to 230mpm. This corresponds to the conditions of the width of the spray area and the upper limit of the conveying speed of the steel plate.

[0137] In addition, from the viewpoint of ensuring the excellent degreasing property required for automobile steel sheets, the oil coating density is preferably set to 10 mL / m 2This is because the degreasing time is significantly affected by the oil density. In the case of single-sided spraying, the oil density is 10mL / m 2 The following corresponds to the spray volume of lubricating oil below 20L / hour. In the case of double-sided spraying, the oil coating density is 10mL / m 2 The following corresponds to a spray amount of lubricating oil of 40 L / hour or less. Here, the spray amount of lubricating oil is calculated by setting the width of the spray area to 0.15 m and the conveying speed of the steel plate to 230 mpm. From the perspective of ensuring better degreasing performance, the oil coating density is preferably set to 5 mL / m 2 In the case of single-sided spraying, the oil coating density corresponds to a spray volume of lubricating oil of 10 L / hour or less, and in the case of double-sided spraying, the oil coating density corresponds to a spray volume of lubricating oil of 20 L / hour or less. By controlling the oil coating density within this range, the time required for degreasing treatment performed by automobile manufacturers and the like can be reduced.

[0138] It should be noted that in this embodiment, the lubricating oil is not directly sprayed but supplied in the form of mist. Therefore, the supply of the lubricating oil can be naturally suppressed.

[0139] Here, when the lubricating oil is applied (attached) by dripping, the range of the dripping amount is the same as that of the above-mentioned spraying. It should be noted that in the case of dripping, the calculation can be performed by replacing the (width of the spraying area) in formula (1) and formula (2) with the (width of the dripping area).

[0140] [Spray pressure]

[0141] The spray pressure is set to, for example, 0.09 MPa or more and 0.12 MPa or less.

[0142] The spray pressure is not particularly limited as long as it is set so that the oil can be evenly applied to a predetermined spray area.

[0143] [Spray area]

[0144] The spray region preferably has a region of ±20 mm in the width direction of the steel sheet 1 with respect to the position L serving as the cutting position.

[0145] When the width of the spray region (spray width) is 40 mm or less, a sufficient lubrication region cannot be ensured at the cutting position, and chipping may occur.

[0146] There is no particular upper limit on the width of the spray area. However, if excessive oil is applied, the oil 10 attached to the edge of the steel plate 1 will fall off the steel plate, which may adversely affect the production line equipment thereafter, so the width of the spray area is preferably very small.

[0147] When the manufactured steel plate is used for automobile purposes, excellent degreasing performance is required from the viewpoints of increasing the degreasing speed, reducing the poor degreasing, reducing the frequency of changing the liquid, and reducing the environmental load. Therefore, it is preferred to reduce the width of the spray area as much as possible. From such a viewpoint, the width of the coating area is preferably set to less than ±100mm (200mm width). In addition, the width of the spray area is preferably set to less than ±40mm (80mm width) by precisely controlling the lubricating oil coating density on the steel plate. In addition, the width of the spray area is more preferably set to less than ±20mm (40mm width), and further preferably set to less than ±10mm (20mm width).

[0148] [Distance between the spraying part of the spray device 3 and the steel plate 1]

[0149] The distance between the spraying part of the spray device 3 and the steel plate 1 is preferably 40 mm or more. If the distance is less than 40 mm, the nozzle of the spray device 3 may interfere with the steel plate 1 when the steel plate 1 with a defective shape passes through.

[0150] There is no particular upper limit on the distance between the spraying portion of the spray device 3 and the steel plate 1. The greater the distance, the lower the density of the lubricating oil (oil coating density) attached to the surfaces 1a and 1b of the steel plate 1, and the wider the width of the spray area. However, if the oil coating density and the spray area are within the range of the distance that can ensure the preset target range, there is no upper limit on the distance.

[0151] In the present embodiment, the spray nozzles are arranged facing the upper surface 1 a and the lower surface 1 b of the steel plate 1 , and the lubricating oil is attached to the positions on both the front and back surfaces of the steel plate 1 to be cut by the rotary blade 2 .

[0152] The spray nozzle may be disposed on only one of the front and back surfaces 1 a and 1 b of the steel sheet 1 .

[0153] [Lubricating oil viscosity]

[0154] The viscosity of the lubricating oil is preferably 3 mm when the liquid temperature of the lubricating oil is 40°C. 2 / s or more and 130mm 2 / s or less. When the viscosity of the lubricating oil is less than 3mm 2 / s, the cutting surface of the rotating blade and the steel plate act with high surface pressure. Therefore, the rotating blade and the steel plate may come into direct contact due to oil failure. In the cutting of high-strength steel plates with a strength of 1180MPa or more, from the perspective of suppressing oil failure even at a higher surface pressure, the viscosity of the lubricating oil is more preferably 8mm when the liquid temperature of the lubricating oil is 40°C. 2 / s or more.

[0155] In addition, when the viscosity of the lubricating oil is greater than 130 mm 2 / s, the diffusion and penetration of the lubricant on the steel plate surface after the lubricant adheres to the steel plate surface is insufficient, and there may be a lack of lubricant in some areas. In addition, when the rotary knife cuts the steel plate, the lubricant is not supplied to the side of the rotary knife, and the side of the rotary knife may directly contact the steel plate. Therefore, the viscosity of the lubricant is preferably set to 130mm 2 In addition, from the viewpoint of distributing the attached oil more evenly, the viscosity of the lubricating oil is more preferably set to 100 mm when the liquid temperature of the lubricating oil is 40°C. 2 / s or less. It should be noted that the measurement of viscosity is based on JIS Z8803. The measurement of viscosity can be performed using, for example, a rotational viscometer.

[0156] There is no particular regulation on the type of lubricating oil. For example, as lubricating oil, stamping oil, rust-proof oil, cutting oil, etc. can be exemplified. From the viewpoint of stably suppressing chipping even when cutting high-strength steel plates, extreme pressure additives can also be added to these lubricating oils.

[0157] [Lubricating oil particle size]

[0158] The average diameter of the droplets after spraying is set to a range of, for example, 1 μm or more and 2000 μm or less. There is no particular lower limit for the average diameter of the droplets. However, if the particle size is too small, it will scatter around, and the adhesion rate to the steel plate will decrease. In addition, the scattered oil will scatter around, and from the perspective of disaster prevention, there are concerns about risks. There is no particular upper limit for the average diameter of the droplets. However, the adhesion amount becomes uneven, and there is a concern that chipping is likely to occur. From the perspective of suppressing chipping, the more preferred range of the average diameter of the droplets is 100 μm or less.

[0159] [Retention time from when the lubricant adheres to the steel plate to when cutting starts]

[0160] There is no particular regulation for the holding time from the time the lubricating oil adheres to the steel plate to the time the cutting starts. However, from the viewpoint of making the oil particles attached to the steel plate surface dispersed on the steel plate surface to form a uniform adhesion state, the holding time is preferably set to 1 second or more. When the diameter of the attached lubricating oil particles is large, the time for the oil particles attached to the steel plate surface to be dispersed on the steel plate surface to form a uniform adhesion state becomes longer. Therefore, when the particle diameter of the lubricating oil is greater than 2000 μm, the holding time is preferably set to 3 seconds or more.

[0161] [Material of Rotary Knife]

[0162] There is no particular provision for the constituent material of the rotary blade. Examples of the constituent material of the rotary blade include carbon tool steel, alloy tool steel, high-speed tool steel, and the like. From the viewpoint of stably suppressing tooth chipping in the cutting of high-tensile steel plates having a tensile strength of 1180 MPa or more, alloy tool steel and high-speed tool steel are preferably used as the constituent material of the rotary blade. In addition, it is more preferred to subject the surface of the rotary blade to surface hardening treatments such as quenching, nitriding / carburizing, and TD treatment, and surface coating treatments such as PVD, CVD, plating, and spraying.

[0163] <Calendering roll 7>

[0164] The pair of rolling rolls 7 are arranged so as to sandwich and hold the steel sheet 1 .

[0165] The pair of rolling rolls 7 is set between the rotating blade 2 in the conveying direction of the steel sheet 1 and the position where the lubricating oil is attached by the lubricating oil attaching device.

[0166] The region of the steel sheet 1 gripped by the pair of rolling rolls 7 is set to include at least the position of the steel sheet 1 to be cut by the rotating blade 2 .

[0167] The pair of rolling rolls 7 suppresses vibration of the steel sheet 1 and enables more stable cutting by the rotating blade 2 .

[0168] In addition, it also has the function of pressing and extending the lubricating oil 10 adhering to the steel plate 1 toward the surfaces 1 a and 1 b of the steel plate 1 , making the adhering lubricating oil 10 uniform and improving the adhesion to the steel plate.

[0169] [Film thickness uniformity equipment]

[0170] The film thickness equalization tool is arranged between the rotating blade and the lubricating oil attachment position, and is a tool for making the film thickness of the lubricating oil attached to the steel plate surface uniform. In other words, the film thickness equalization tool is a tool for uniformly adjusting the amount of lubricating oil attached to the attachment area, especially near the cutting part (10 to 100 mm width), when the lubricating oil attached by dripping or spraying is unevenly distributed.

[0171] The film thickness equalizing tool is preferably used to equalize the film thickness during the period from when the lubricating oil adheres to the steel plate until it is cut by the rotating blade.

[0172] In this embodiment, the film thickness uniformizing device is provided between the spray device or the oil dripping device of the lubricating oil and the rotating blade.

[0173] In this embodiment, a pair of rolling rollers 7 are illustrated as an example of a film thickness uniformizing device. As a film thickness uniformizing device, a flat member or a rolled member composed of one or more of bristles or felt, rubber, resin, and metal can be used. These film thickness uniformizing devices can be fixed devices or devices that rotate or swing for the purpose of making the film thickness of the lubricating oil more uniform. Any structure that can make the amount of lubricating oil attached to the surface of the steel plate uniform by pressing or scraping the surface of the lubricating oil can be used.

[0174] When the lubricating oil is unevenly distributed, it causes chipping. In contrast, by using a film thickness equalization tool, it has a significant effect of suppressing chipping, and can stably suppress chipping. In addition, when the lubricating oil is unevenly distributed, it causes the degreasing performance to deteriorate. However, by using a film thickness equalization tool, this can be suppressed.

[0175] <Other structures>

[0176] This embodiment has a felt 9 impregnated with lubricating oil. The felt 9 directly supplies the lubricating oil to the rotating blade 2. It should be noted that the lubricating oil is appropriately supplied to the felt 9. Since the lubricating oil directly supplied to the rotating blade 2 is scattered by the centrifugal force of the rotation of the rotating blade 2, it is preferred that the amount of lubricating oil supplied by the spray device 3 is larger than the amount of lubricating oil supplied by the felt 9.

[0177] In the present embodiment, the felt 9 may not be provided.

[0178] [Gap between upper blade 2A and lower blade 2B of rotating blade 2]

[0179] The gap between the upper blade 2A and the lower blade 2B of the rotating blade 2 is preferably in the range of 5% or more and 19% or less relative to the plate thickness of the steel plate 1. In the cutting of high-tension steel plates with a tensile strength of 590 MPa or more, chipping is easily generated in the gap of about 20% that is not a problem in existing soft steel plates. By controlling the gap between the upper blade 2A and the lower blade 2B of the rotating blade 2 to be in the range of 5% or more and 19% or less, even in the cutting of high-tension steel plates with a tensile strength of 590 MPa or more, trimming chipping and the iron powder generated thereby can be suppressed. As a result, indentations in cutting and subsequent processing can be suppressed. From the viewpoint of suppressing chipping of high-tension steel plates with a tensile strength of 980 MPa or more, the gap between the upper blade 2A and the lower blade 2B of the rotating blade 2 is more preferably in the range of 5% or more and 14% or less. In addition, from the viewpoint of suppressing chipping of high-tension steel plates with a tensile strength of 1180 MPa or more, it is further preferably in the range of 5% or more and 13% or less.

[0180] [Contact angle between the upper blade of the rotating blade 2 and the steel plate in the vertical direction]

[0181] The contact angle between the upper blade 2A of the rotating blade 2 and the steel plate 1 in the vertical direction in the rotation direction is preferably greater than 3 degrees and less than 13 degrees. In the cutting of high-tensile steel plates with a tensile strength of more than 590 MPa, chipping is prone to occur at a contact angle of about 14 degrees, which would not be a problem with soft steel plates in the past. When the contact angle is greater than 13 degrees, the contact area between the rotating blade 2 and the steel plate 1 becomes smaller, and it is necessary to apply bending deformation to the chips, and the deformation resistance becomes higher. As a result, in the cutting of high-tensile steel plates, very high stress is concentrated on the tip of the rotating blade 2, and chipping becomes obvious. When the contact angle is less than 3 degrees, sufficient cutting depth in the direction of the plate thickness cannot be ensured, resulting in poor cutting. By controlling the contact angle within the range of more than 3 degrees and less than 13 degrees, even in the cutting of high-tensile steel plates with a tensile strength of more than 590 MPa, the chipping of the rotating blade 2 and the iron powder generated thereby can be suppressed, and indentation can be suppressed.

[0182] [Angle between the rotation direction of the rotary blade 2 and the conveying direction of the steel plate]

[0183] The angle formed by the rotation direction of the rotating knife 2 and the conveying direction of the steel plate is preferably greater than 0.01 degrees and less than 0.5 degrees in the direction of forming an opening angle on the rear side of the conveying. In the cutting of high-tensile steel plates with a tensile strength of more than 590 MPa, high surface pressure is generated due to the re-contact between the rotating knife 2 and the cut end surface of the steel plate 1, which easily causes accumulation of adhesion on the tip of the knife. When adhesion accumulates on the tip of the knife, large stress is applied to the tip of the knife due to the narrowing of the local gap, causing chipping. From the viewpoint of avoiding such a phenomenon, the angle formed by the rotation direction of the rotating knife 2 and the conveying direction of the steel plate 1 is preferably greater than 0.01 degrees and less than 0.5 degrees in the direction of forming an opening angle on the rear side of the conveying.

[0184] (Variation Example)

[0185] (1) In the above description, the case where the lubricating oil adhering device is constituted by the spray device 3 is exemplified. Figure 3 Another example of the lubricating oil adhesion device will be described.

[0186] Figure 3 The lubricating oil adhering device shown is configured as follows: it is provided with an oil dripping device 20, and the lubricating oil supplied from the oil storage tank 21 is continuously dripped onto the upper surface 1a of the steel plate 1 according to the instruction from the controller 22. It should be noted that the lubricating oil cannot be dripped onto the lower surface 1b of the steel plate 1. Therefore, it is more preferable to arrange the spraying device 3 opposite to the lower surface 1b of the steel plate 1, and spray the lubricating oil onto the lower surface 1b as well.

[0187] The oil droplets 23 dropped onto the surface 1 b of the steel sheet 1 in the conveying direction are stretched by the rolling rolls 7 , and the oil droplets attached to the steel sheet 1 are uniformed in the conveying direction.

[0188] (2) Alternatively, the lubricating oil adhering device may be constituted by brush bristles, and the lubricating oil may be adhered to the steel plate 1 by the brush bristles.

[0189] However, when applying with a brush, unlike the spray device 3 or the like that supplies the lubricating oil 10 in a non-contact manner, the brush is brought into direct contact with the surfaces 1a and 1b of the steel plate 1. Therefore, when applying with a brush, it is difficult to apply the brush to a steel plate manufacturing line that vibrates by conveying the steel plate 1 at a high speed. For example, there are application problems such as the need to stop the production line during application or the need for an operator to enter the production line.

[0190] (3) In addition, the lubricating oil adhering device may be a planar member or a rolled member made of one or more of felt, rubber, resin, and metal. Furthermore, the lubricating oil may be attached to these members and then attached to the steel plate 1. In addition, these lubricating oil adhering devices may be fixed devices or devices that rotate or swing for the purpose of making the oil adhere more evenly.

[0191] For example, when the lubricant oil adhering device is in the form of a roll, the rolling roller 7 can also be used as the lubricant oil adhering device. By adhering lubricant oil to the outer peripheral surface of the rolling roller 7 and supplying lubricant oil to the steel sheet, the rolling roller 7 can perform both the function of the rolling roller and the function of the lubricant oil adhering device.

[0192] (4) In addition, a lubricating oil removal device for removing excess lubricating oil may be provided before or after the position where the rotating blade is set in the traveling direction of the steel plate. In this case, the amount of lubricating oil adhered to the steel plate can be adjusted by removing part of the lubricating oil adhered to the steel plate before or after cutting with the rotating blade.

[0193] For example, when the produced steel sheet is used in an application requiring excellent degreasing properties such as automobiles, it is preferred to adhere lubricating oil to 10 mL / m 2 After that, the lubricant oil removal device was used to adjust the amount of lubricant oil to 10 mL / m 2 However, in this case, since a lubricating oil removal device is required, there arises a problem of increased cost.

[0194] (5) Furthermore, the removed lubricating oil may be circulated in the lubricating oil adhering device and reused.

[0195] (Rolled steel plates, coils and billets)

[0196] Next, a rolled steel plate and the like according to this embodiment will be described based on the present invention.

[0197] The steel plate manufacturing method according to the present embodiment is a technique suitable for manufacturing a rolled steel plate.

[0198] The rolled steel plate of the present embodiment is manufactured by a facility having a rolling process of rolling a slab using a rolling mill and the above-mentioned cutting process, and has a strip shape. It should be noted that the rolled steel plate is also simply referred to as a steel plate hereinafter.

[0199] Here, in the above-mentioned cutting method, before cutting with the rotating blade 2, oil is applied to the portion of the steel plate to be cut. The end face of the steel plate in the width direction cut by the cutting method of this embodiment becomes a smooth cut end face. In this embodiment, the portion of the smooth cut end face is called a first cut face. The first cut face is a predetermined structure as described later.

[0200] Here, it is preferred that the cut end face formed in the width direction of the steel plate is the first cut face in the entire length direction of the steel plate. However, the cut end face formed in the width direction of the steel plate may be the first cut face in only a portion of the length direction of the steel plate. For example, the cut faces of the front end and the rear end of the steel plate, where the conveying speed during cutting tends to become unstable, may not be the first cut faces. In addition, the cut face of a portion of the length direction may not be the first cut face. For example, there may be an end face portion where the amount of local oil applied is too small and does not meet the requirements of the first cut face. However, more than 50%, preferably more than 70%, and more preferably more than 90% of the length direction of the cut end face formed in the width direction of the steel plate is the first cut face.

[0201] Furthermore, the strip-shaped steel plate is rolled into a coil by a winding device to form a coil.

[0202] Furthermore, the steel sheet formed by unwinding the rolled steel sheet or coil is appropriately cut out to form a blank for stamping. In the blank of this embodiment, at least one end surface of the steel sheet at both ends in the width direction is constituted by a first cut surface.

[0203] Here, since the chipping of the rotating blade 2 also depends on the strength of the steel plate, setting conditions, etc., it cannot be strictly determined, but it occurs in a cutting length of hundreds of meters to tens of thousands of meters. Therefore, from the perspective of improving productivity, a region that is not locally oiled can be formed within a range of hundreds of meters in the length direction of the steel plate. Even if there is a region that is not locally oiled, the effect of suppressing chipping, the effect of suppressing the indentation caused by it, and the effect of suppressing conveying failures, poor coil winding shape, and poor punching dimensional accuracy can be obtained by having a region that meets the necessary conditions of the present invention.

[0204] In addition, in steel plates and coils, from the perspective of fully enjoying the above-mentioned effects, the three locations of the front end (5 to 10 m from the front end of the coil), the middle of the length, and the tail end (5 to 10 m from the tail end of the coil) are measured, and preferably more than 50% of the area meets the requirements of the first cutting surface described below. Here, the ratio of the area is calculated as follows: the area sandwiched by the qualified part and the qualified part is qualified, the area sandwiched by the qualified part and the unqualified part is half of the area in the interval is qualified, half of the area is unqualified, and the area sandwiched by the unqualified part is unqualified. In the case where the above-mentioned locations cannot be measured, the adjacent areas are measured.

[0205] In addition, in the case of a blank, the end portion in the width direction having the first cut surface is a straight side parallel to the rolling direction. In addition, the blank must satisfy the following provisions of the first cut surface. The blank is a flat plate material on the premise of performing a stamping process. The length of the end face of the blank material consisting of the first cut surface is, for example, 100 mm to 2500 mm, for example, a rectangular plate material. However, the blank material may also have punching holes such as process holes.

[0206] In addition, the steel plate of the present embodiment is composed of a high-tensile steel plate having a tensile strength TS of 590 MPa or more.

[0207] The steel plate may be any of a hot-rolled steel plate, a cold-rolled steel plate, a hot-rolled steel plate, a steel plate subjected to surface treatment on a cold-rolled steel plate, and a high-hardness cold-rolled plate subjected to cold rolling on a hot-rolled steel plate. It should be noted that the strength of the high-hardness cold-rolled plate is not the strength after annealing after trimming, and the TS of the raw material in the trimming process may be 590 MPa or more.

[0208] The surface of the steel plate of the present embodiment may also be subjected to surface treatment. Examples of the steel plate subjected to surface treatment include GI, GA, EG, CRS, tin-plated steel plates, Zn-plated steel plates, Al-plated steel plates, etc. However, this is not limited thereto, and any steel plate may be applied as the steel plate. The present invention may also be applied to, for example, steel plates to which solid lubricating films are applied to GI and GA, and steel plates to which organic coatings are applied. The above-mentioned surface treatment is preferably performed before the cutting process of the edge portion of the steel plate.

[0209] In this embodiment, the plate thickness of the steel plate is 0.4 mm or more, where the cutting load becomes high and the chipping becomes obvious, and 0.8 mm or more is more suitable. On the other hand, the effect of the present invention can be fully obtained even if the plate thickness is below 4.0 mm, so this range is also the scope of the present invention.

[0210] [Shearing surface ratio]

[0211] According to the tensile strength TS (MPa) of the steel plate, the shear plane ratio (%) of at least a portion of the cut planes in the longitudinal direction of the steel plate, i.e., the first cut plane, is set to the range of the following formulas (3) to (6).

[0212] <TS: 590MPa or more and less than 980MPa>

[0213] 19-0.0146×TS≤shear surface ratio≤48-0.0300×TS …Formula (3)

[0214] <TS: 980MPa or more and less than 1180MPa>

[0215] 10-0.00526×TS≤shear surface ratio≤36-0.0180×TS …Formula (4)

[0216] <TS: 1180MPa or more and less than 1320MPa>

[0217] 10-0.00526×TS≤shear surface ratio≤27-0,108×TS …Formula (5)

[0218] <TS: 1320MPa or more and less than 1850MPa>

[0219] 3≤shear surface ratio≤16-0.0254×TS …Formula (6)

[0220] Here, when the lubricating oil is not applied directly to the steel plate 1 but to the rotating blade 2, as described above, oil shortage is likely to occur at the blade tip, resulting in large friction and large plastic deformation on the shear section. Therefore, the cut surface has a cross-sectional shape with a high shear surface ratio. The cut surface accompanied by large plastic deformation lacks residual ductility. Therefore, iron powder is likely to fall off from the end face during the cutting process and subsequent processing, and the fallen iron powder causes indentations, increasing the incidence of surface defects. This effect is particularly evident in high-tensile steel plates above 980MPa, and even more evident in high-tensile steel plates above 1180MPa.

[0221] On the other hand, according to the present invention, when cutting is performed by directly applying lubricating oil to a steel plate, the friction force on the first cut surface is reduced in a high-tensile steel plate having a strength of 590 MPa or more over a wide range.

[0222] Therefore, the inventors have obtained the knowledge that the shear plane ratio of the first cut surface can be suppressed within the range described in equations (1) to (4) by applying the cutting method of the present invention. As a result, the steel plate formed by applying the cutting method of the present invention and the coil and billet formed by the steel plate can further suppress the falling of iron powder from the end surface in the cutting process and the subsequent conveying process, rolling process, annealing process, steel plate winding process, etc., and can reduce the indentation caused by the re-adhesion of the fallen iron powder in each process.

[0223] It should be noted that, from the viewpoint of suppressing the falling of iron powder, the lower limit of the shear plane ratio in the formulas (1) to (4) is not necessarily limited, and the lower limit obtained by the cutting method of the present invention is described.

[0224] In addition, by controlling the shear plane ratio within such a range, the plastic flow of the material in the vertical direction of the end face can be suppressed. As a result, the collapsed edge, burr and flash can be suppressed to be small, and the steel plate with the end face shape with high dimensional accuracy can be made. Such a steel plate can prevent transportation failure and poor winding shape in the cutting and subsequent transportation process, rolling process, annealing process, steel plate winding process, etc. In addition, in the stamping process of automobile manufacturers, it can also suppress the poor dimensional accuracy of stamped parts.

[0225] Here, if Figure 4 As shown in FIG. 1 , the area ratio of the sheared surface of the cut surface is determined by observing the cut surface by SEM at a magnification that allows observation of an area in the range of 2 to 2.5 times the plate thickness, and observing a total length of 100 mm in the rolling direction. The sample for observation can be cut separately, but it is cut from a range of no more than 150 mm in length in the rolling direction. The area ratio of the sheared surface is the value obtained by dividing the total area of ​​the measured sheared surface by the total area of ​​the sheared surface and the fracture surface.

[0226] It should be noted that Figure 4 (a) is a conventional example in which the steel plate is not directly coated, P1 is the center line of the boundary between the shear surface and the fracture surface, and P2 is a line that shifts the position of P1 toward the fracture surface by "plate thickness × 4%". Figure 4 (b) is an example of the case where the present invention is applied to a steel plate.

[0227] Here, in the case of conventional blank processing using a punching die, cutting using a cutting machine, and process hole processing using a punching punch, the vertical angle between the cutting knife and the steel plate is about 0 to about 2 degrees. In contrast, in the cutting using the rotating knife 2 of the present invention, since the steel plate 1 is clamped by the rotating knife 2 with a certain curvature, the angle is usually larger than the above. In the present invention, as described above, it is preferred to control the angle to be greater than 3 degrees and less than 13 degrees, as a result, Figure 4 (b) and Figure 5 As shown by the arrow and dotted line in the figure, sometimes a faint stripe pattern corresponding to the angle at the time of cutting appears parallel to each other on the fracture surface of the cut section. In the present invention, it is allowed to generate a stripe pattern on the fracture surface, and the angle formed by the direction of the stripe pattern and the side view in the thickness direction of the steel plate is 3 degrees or more and 13 degrees or less. The angle formed by the direction of the stripe pattern and the side view in the thickness direction of the steel plate can be measured by using the same SEM method as the determination of the area ratio of the shear surface.

[0228] [Number of convex parts at the boundary between the shear surface and the fracture surface]

[0229] The number of convex portions at the boundary between the shear surface and the fracture surface of the first cut surface is set to 5 / 100 mm or less. The number of convex portions at the boundary between the shear surface and the fracture surface corresponds to the disorder of the shear surface at the boundary between the shear surface and the fracture surface.

[0230] Here, when the lubricating oil is not applied directly to the steel plate but to the knife, as described above, the oil is easily cut off at the knife, and the blade is easily broken. In addition, since the contact surface pressure between the steel plate and the rotating knife becomes high, it is easy to cause a part of the newly cut surface of the cut steel plate to adhere to the metal mold. When such edge breaking and adhesion occur, the boundary line between the shear surface and the fracture surface of the cut end surface becomes wavy (refer to Figure 4 (a)). In addition, when the shape is wavy, iron powder is likely to fall off particularly from this portion, increasing the frequency of indentation.

[0231] On the other hand, by setting the number of convex portions at the boundary between the shear surface and the fracture surface of the cut end surface to 5 / 100 mm or less (refer to Figure 4 (b) Figure 5 ), which can significantly suppress the frequency of indentation.

[0232] In addition, in the region where the boundary line is wavy, large collapsed edges, burrs, and flashes are likely to occur locally. As a result, in the coil having such regions, poor dimensional accuracy of stamped parts is likely to occur during transportation failures and stamping processes of automobile manufacturers. Coils that control the number of convex portions within the above range can solve these problems.

[0233] The number of convex parts was measured using SEM at the same magnification and observation length as the measurement of the shear surface ratio. In each observation field, the boundary line between the shear surface and the fracture surface was drawn with a straight line, and the number of shear surfaces that protruded from the boundary line to the fracture surface side by more than 4% of the plate thickness was measured as convex parts. That is, the convex part is composed of a protruding shape that protrudes from the fracture surface side by more than 4% of the plate thickness.

[0234] Regarding the position of the boundary line, a line roughly parallel to the upper end of the shear surface is set, and the height of the line is set so that the area of ​​the shear surface below the line is equal to the area of ​​the fracture surface above the line. The number of convex parts is set to the value obtained by dividing the total number of convex parts by the total observation length.

[0235] On the first cut surface, the number of convex portions at the boundary between the shear surface and the fracture surface of the cut end surface is controlled to be less than 5 / 100 mm, which can be achieved by applying the cutting method of the present invention. For example, it is preferred to apply the lubricant at 0.900 g / m 2 Oil density above (corresponding to 1.00mL / m 2 The oil coating density) is directly applied on the steel plate before trimming the edge, and the gap of the rotating blade 2 and the contact angle when the upper blade of the rotating blade 2 contacts the steel plate 1 are adjusted. When the gap of the rotating blade 2 is small, a secondary shear surface is formed, and the number of convex parts increases. When the gap is large, the shear surface ratio increases, the tool loss becomes significant, and when the cutting length increases, chipping occurs at a high frequency, and the number of convex parts increases. When the contact angle between the rotating blade 2 and the steel plate 1 is small, the cutting range is expanded at the same time, and the cross-sectional morphology is difficult to stabilize. On the other hand, when the contact angle is large, the bending deformation loads overlap greatly, and a large load is applied to the blade tip, which is prone to chipping. Therefore, the number of convex parts increases.

[0236] [Amount of oil applied to the area 5 mm from the cut surface]

[0237] As described above, when the present invention is applied, chipping can be effectively suppressed by applying lubricating oil only to the peripheral area of ​​the rotating blade 2 (near the area to be cut). Therefore, from the viewpoint of ensuring excellent degreasing properties, it is preferred to apply a large amount of lubricating oil only to the edge portion and then cut the manufactured steel plate. In addition, by making the amount of oil applied near the first cut surface remain much more than in the central portion in the width direction of the steel plate, it is possible to more effectively prevent the iron powder at the edge portion of the steel plate 1 from falling off and scattering after cutting. Therefore, it is preferred that in the cut end face of the steel plate 1, the amount of oil applied in the area from the end face of the first cut surface to 5 mm inside the central direction of the steel plate width is 0.2 g / m more than the amount of oil applied at the central position of the rolled steel plate width. 2 Here, the amount of oil applied means the amount of oil applied per single side.

[0238] The above-mentioned control of the amount of oil applied is preferably implemented on at least one side of the front and back sides of the steel plate. Since the steel plate surface on the upper knife side, that is, the steel plate surface on the shear surface side of the upper surface, has a particularly large influence on the occurrence of chipping, it is preferred to increase the amount of oil applied to the edge of the steel plate surface on the upper knife side. From the viewpoint of particularly stably suppressing chipping, it is preferred to increase the amount of oil applied to the edge of both the steel plate surfaces on the upper knife side and the lower knife side. However, from the viewpoint of reducing the frequency of changing the chemical solution in the degreasing process, it is not necessary to perform additional oiling on the steel plate surface on the lower knife side, which has a smaller influence, and only increase the amount of oil applied to the steel plate surface on the upper knife side.

[0239] Generally, the upper limit of the normal oiling of the steel sheet 1 is about 2.5 g / m 2 The amount of oil applied to the steel plate surface in the region 5 mm from the end surface at the first cut surface position is preferably set to 2.7 g / m 2 Here, the amount of oil applied refers to the amount of oil applied per single side. The above-mentioned amount of oil applied is preferably controlled on at least one side of the front and back sides of the steel plate, and the amount of oil applied is preferably controlled within the above-mentioned range on the steel plate surface on the shear surface side.

[0240] In addition, from the perspective of further enjoying the chipping suppression effect, it is preferably set to 7.24 mL / m 2 This corresponds to 6.5 g / m 2 Therefore, the amount of oil applied to the area from the first cut surface to 5 mm is more preferably set to 6.5 g / m 2 Here, the amount of oil applied refers to the amount of oil applied per single side. The above-mentioned amount of oil applied is preferably controlled on at least one side of the front and back sides of the steel plate, and the amount of oil applied is preferably controlled within the above-mentioned range on the steel plate surface on the shear surface side.

[0241] On the other hand, if excessive oil is applied, there is a concern that the oil at the edge will drip and cause adverse effects on production line equipment. Therefore, the amount of oil applied to the area from the first cut surface to 5 mm is preferably set to less than 27 g / m 2 (corresponding to less than 30mL / m 2 In addition, from the viewpoint of ensuring the excellent degreasing property required for automobile steel sheets, the oiling amount in the area from the first cut surface to 5 mm is preferably set to 9 g / m 2 Below (corresponding to 10mL / m 2 From the perspective of further reducing the degreasing time, the amount of oil applied to the area 5 mm from the first cut surface is more preferably set to 4.5 mL / m 2 Below (corresponding to 5mL / m 2 Here, the density of oil is 0.9 g / cm 3 .

[0242] The upper limit of the amount of oil applied to the center of the rolled steel plate width is about 2.5 g / m 2 Therefore, in order to make the oiling amount of the edge within the above range, the amount of oiling in the area from the end face of the first cut surface to 5 mm inside the center direction of the steel plate width is preferably increased by less than 24.5 g / m 2 , more preferably 6.5 g / m 2 Below, more preferably 2.0 / m 2 the following.

[0243] Here, the amount of oil applied is calculated by cutting 6 samples with a width of 5 mm and a length of 200 mm from the cut end surface and the center of the steel plate width, and measuring the weight changes before and after alkali degreasing. If the sample cannot be ensured in sufficient quantity in the blank, the film thickness can be measured, and the density of the oil is set to 0.9 g / cm 3 And convert it into attachment weight per unit area.

[0244] (effect)

[0245] In this embodiment, lubricating oil is directly applied (attached) to the steel plate 1 before trimming to eliminate the insufficient supply of oil at the cutting position. Therefore, in this embodiment, the frequency of chipping of the trimmer is suppressed by reducing friction, and even if the rotary blade needs to be rotated at high speed for cutting, the yield rate of steel plate manufacturing is improved.

[0246] For example, a spray device 3 capable of continuously applying oil to both the front and back surfaces 1a and 1b of the steel plate 1 is provided in front of the trimming machine. Furthermore, by applying oil to the cut position of the steel plate 1 before cutting using the spray device 3, insufficient oil penetration at the cut position can be eliminated. Therefore, even if the steel plate 1 to be cut is set to a high-tensile steel plate 1, the upper blade and the lower blade constituting the pair of rotating blades 2A and 2B can be continuously and uniformly and fully oiled. Therefore, insufficient oil penetration can be eliminated and chipping can be suppressed.

[0247] In addition, in this embodiment, the amount of lubricating oil applied to the steel sheet can be reduced compared to the case where lubricating oil is supplied to the rotating blade. Therefore, the generation of rust in the manufactured steel sheet can be reduced compared to the case where lubricating oil is supplied to the rotating rotating blade.

[0248] Furthermore, by pressing the oil with the calender roll 7 , the oil can be supplied to the cutting position more stably.

[0249] Similarly, using Figure 3The oil dripping device 20 shown applies oil to the end of the steel plate 1 before trimming, and can also eliminate insufficient oil penetration at the cutting position. Therefore, even if the steel plate 1 to be cut is set to a high-tensile steel plate 1, the upper blade and the lower blade constituting the pair of rotating blades 2A and 2B can be continuously and evenly and fully oiled, thereby eliminating insufficient oil penetration and suppressing chipping.

[0250] Here, the spray amount and drop amount of lubricating oil are preferably set according to the conveying speed of the steel sheet so that the lubricating oil can be continuously and evenly applied (attached) to both the front and back surfaces of the steel sheet 1 by setting the supply air pressure, oil flow rate, and oil consumption.

[0251] In addition, the rolled steel plate, coil and blank having the first cut surface formed by the cutting method of the present invention have the first cut surface that becomes a smooth end surface. Therefore, since the shedding of iron powder after cutting is suppressed compared with the past, the generation of indentations caused by the shedding of iron powder can be suppressed. That is, it is possible to provide a rolled steel plate, coil and blank with good quality.

[0252] (Example)

[0253] Next, examples will be described based on this embodiment.

[0254] "First Embodiment"

[0255] In the first embodiment, the steel plate 1 to be cut was set to a hot-dip galvanized steel plate (tensile strength 1180 MPa, plate thickness 1.2 mm), and an experiment was conducted on the generation of untrimmed material (material not trimmed) in the trimming equipment.

[0256] As the conditions for trimming, it was performed under the following conditions.

[0257] ·Conveying speed of steel plate 1: Maximum 230 [mpm]

[0258] · Trimming amount of plate end: 10~20[mm]

[0259] <Example 1>

[0260] In Example 1, the above-mentioned spray device 3 is used as the lubricating oil attachment device (refer to Figure 1 ).

[0261] The conditions of the spray device 3 are set as follows.

[0262] ·Steel plate conveying speed: 230 [mpm]

[0263] · Oiling range of spray device 3: 40 [mm] from the end surface in the width direction of the steel plate, only the upper surface

[0264] Oil usage: 4.0 [L / hour] (Oil density: 7.25 [mL / m 2 ])

[0265] Supply air pressure: 0.4~0.6[MPa]

[0266] <Example 2>

[0267] In Example 2, the above-mentioned oil dripping device 20 is used as the lubricating oil attachment device (refer to Figure 3 ).

[0268] The conditions of the oil dripping device 20 are set as follows.

[0269] ·Steel plate conveying speed: 80 [mpm]

[0270] Oiling range: 40mm from the end surface in the width direction of the steel plate

[0271] Oil usage: 0.8 [L / hour] (Oil density: 4.15 [mL / m 2 ])

[0272] Supply air pressure: 0.4~0.6[MPa]

[0273] <Example 3>

[0274] In Example 3, the above-mentioned spray device 3 is used as the lubricating oil attachment device (refer to Figure 1 ).

[0275] The conditions of the spray device 3 are set as follows.

[0276] ·Steel plate conveying speed: 60 [mpm]

[0277] · Oiling range of spray device 3: 40 [mm] from the end surface in the width direction of the steel plate, only the upper surface

[0278] Oil usage: 4.0 [L / hour] (Oil density: 14.0 [mL / m 2 ])

[0279] Supply air pressure: 0.4~0.6[MPa]

[0280] Oil moisture content: 700ppm

[0281] Here, the steel sheet manufactured by the method of Example 3 was wound into a coil, stored in a warehouse for 100 days, and then checked for rust in the lubricating oil adhesion area, but no rust was found.

[0282] The reason why the period of 100 days is set is that it is assumed that the coil is stored at a manufacturer such as an automobile manufacturer until the steel sheet is press-formed.

[0283] <Example 4>

[0284] In Example 4, the above-mentioned spray device 3 is used as the lubricating oil attachment device (refer to Figure 1 ).

[0285] The conditions of the spray device 3 are set as follows.

[0286] ·Steel plate conveying speed: 40 [mpm]

[0287] · Oiling range of spray device 3: 11 [mm] from the end surface in the width direction of the steel plate, upper and lower surfaces

[0288] Oil usage: 0.05 [L / hour] per single side, 0.1 [L / hour] per double side (Oil density: 1.88 [mL / m 2 ])

[0289] Supply air pressure: 0.4~0.6[MPa]

[0290] Oil moisture content: 700ppm

[0291] Here, the steel sheet manufactured by the method of Example 4 was wound into a coil, stored in a warehouse for 100 days, and then checked for rust in the lubricating oil adhesion area, but no rust was found.

[0292] <Example 5>

[0293] In Example 5, the above-mentioned spray device 3 is used as the lubricating oil attachment device (refer to Figure 1 ).

[0294] The conditions of the spray device 3 are set as follows.

[0295] ·Steel plate conveying speed: 80 [mpm]

[0296] · Oiling range of spray device 3: 80 [mm] from the end surface in the width direction of the steel plate, only the upper surface

[0297] Oil consumption: 11.1 [L / hour] (Oil density: 29.0 [mL / m 2 ])

[0298] Supply air pressure: 0.4~0.6[MPa]

[0299] Oil type: NOX-RUST550 (manufactured by Japan Parkersei Co., Ltd.)

[0300] Oil viscosity: 17.0mm 2 / s

[0301] <Example 6>

[0302] In Example 5, the above-mentioned spray device 3 is used as the lubricating oil attachment device (refer to Figure 1 ).

[0303] The conditions of the spray device 3 are set as follows.

[0304] ·Steel plate conveying speed: 80 [mpm]

[0305] · Oiling range of spray device 3: 15 [mm] from the end surface in the width direction of the steel plate, upper and lower surfaces

[0306] Oil usage: 0.58 [L / hour] per single side, 1.16 [L / hour] per double side (Oil density: 8.00 [mL / m 2 ])

[0307] Supply air pressure: 0.4~0.6[MPa]

[0308] Oil type: NOX-RUST550 (manufactured by Japan Parkersei Co., Ltd.)

[0309] Oil viscosity: 17.0mm 2 / s(Lubricating oil temperature is 40℃)

[0310] The average particle size of the oil spray droplets is 5.0 μm.

[0311] · Holding time from oil adhering to steel plate to cutting: 1 second

[0312] <Comparative Example 1>

[0313] In Comparative Example 1, no lubricant oil attaching device was used. Instead, lubricant oil was supplied to both of the pair of rotating blades 2 using felt 9 (refer to the configuration position of the felt 9). Figure 1 ).

[0314] In Comparative Example 1, the conveying speed of the steel plate was set to 60 mpm, and the lubricating oil supply to the rotating blade was set to 4.0 L / hour for the total of the upper blade and the lower blade. The coating width for the upper and lower blades was set to 12 mm (oil coating density: 46.3 mL / m 2 ])

[0315] <Evaluation>

[0316] The evaluation was performed by the improvement in the probability of occurrence of fluctuations caused by untrimmed materials.

[0317] The fluctuation occurrence probability is the ratio of the amount (total weight of defective coils) of the trimmed material loading amount (total weight of 5 to 10 coils manufactured) of the applicable material that fluctuates (is judged as defective material) due to chipping and becomes untrimmed material.

[0318] The evaluation results are as follows.

[0319] Comparative Example 1 (when oil is applied only to felt 9) ... 8.2%

[0320] Example 1 (Oil spray) ... 0.0%

[0321] Example 2 (when oil is added) ... 7.1%

[0322] Example 3 (Oil spray) ... 0.0%

[0323] Example 4 (Oil spray) ... 0.0%

[0324] Example 5 (Oil spray) ... 0.0%

[0325] Example 6 (Oil spray) ... 0.0%

[0326] This evaluation revealed that Examples 1 to 6 according to the present invention could suppress the frequency of chipping of the trimmer compared to Comparative Example 1. As a result, it was found that the yield of steel sheet production could be improved in the present invention.

[0327] Here, the following two points are considered as reasons why the probability of occurrence of fluctuation in Example 2 is lower than that in Examples 1 and 3 to 6.

[0328] That is, (1) the oil dripping device 20 is a dripping device, so only the surfaces 1a and 1b can be oiled, and the chipping of the back surface (lower blade) is not reduced. (2) In addition, since it is a dripping device, it cannot be applied (adhered) continuously, so the load is applied to the blade in the unoiled part, and the chipping frequency of the surfaces 1a and 1b (upper blade) is significantly reduced, but not zero.

[0329] "Second Embodiment"

[0330] Next, a second embodiment will be described.

[0331] <Comparative Example 2>

[0332] In Comparative Example 2, the following steel plates were used as steel plates.

[0333] Steel plate: TS1020MPa, thickness 1.8mm

[0334] Ingredients:

[0335] C: 0.09%, Si: 0.60%, Mn: 2.50%, P: 0.012%, S: 0.0013%, sol.Al: 0.045%, N: 0.0025%, Nb: 0.040%, Cr: 0.550%, Cu: 0.006%, Mo: 0.010%, Ni: 0.010%, Ti: 0.025%, B: 0.0016%, the balance is Fe and unavoidable impurities

[0336] In Comparative Example 2, the lubricating oil applying device was not used, and lubricating oil was directly applied to both of the pair of rotary blades 2 using the felt 9 for lubrication.

[0337] The experimental conditions of Comparative Example 2 are as follows.

[0338] ·Steel plate conveying speed: 180 [mpm]

[0339] · Lubricating oil supply to the rotary knife: 6.0 [L / hour] for the total of the upper knife and the lower knife

[0340] Coating width: 12mm for upper and lower blades respectively (oil density: 23[mL / m 2 ])

[0341] Oil density in the center of the steel plate width: 1.5[g / m 2 ]

[0342] Rotating blade diameter: φ300mm

[0343] · Gap of rotating blade: 12% of steel plate thickness

[0344] Overlap of rotating blade: 0.3mm

[0345] ·Vertical contact angle between upper knife and steel plate: 11 degrees

[0346] · Angle between the rotation direction of the rotary blade and the conveying direction of the steel plate: 0.15 degrees on the rear side of the conveying

[0347] Cutting position: 12mm from the edge

[0348] <Example 7>

[0349] In Example 7, the following steel plates were used as steel plates.

[0350] Steel plate: TS1020MPa, thickness 2.0mm

[0351] Ingredients:

[0352] C: 0.09%, Si: 0.60%, Mn: 2.50%, P: 0.012%, S: 0.0012%, sol.Al: 0.044%, N: 0.0026%, Nb: 0.040%, Cr: 0.550%, Cu: 0.006%, Mo: 0.010%, Ni: 0.010%, Ti: 0.025%, B: 0.0016%, the balance is Fe and unavoidable impurities

[0353] In addition, the above-mentioned spray device 3 is used as the lubricating oil attachment device (refer to Figure 1 ).

[0354] In Example 7, the conditions of the spray device 3 were set as follows, and lubricating oil was applied before trimming.

[0355] ·Steel plate conveying speed: 230 [mpm]

[0356] · Oiling range of spray device 3: 20 [mm] from the end surface in the width direction of the steel plate, only the upper surface

[0357] Oil usage: 2.0 [L / hour] (Oil density: 7.25 [mL / m 2 ])

[0358] Supply air pressure: 0.4~0.6[MPa]

[0359] Oil density in the center of the steel plate width: 1.5[g / m 2 ]

[0360] · Oil application within 5 mm of the edge: 4.9 [g / m 2 ] Lower surface 1.5[g / m 2 ]

[0361] After trimming, a portion of the lubricant (1.6 g / m 2 )remove

[0362] · Lubricating oil spray area: implemented on both edges.

[0363] For the total length of 900 m, the front 150 m and the rear 150 m were not sprayed toward the edge.

[0364] (The amount of oil applied is the same as that of the center part) Other than that, spray.

[0365] Rotating blade diameter: φ300mm

[0366] · Gap of rotating blade: 9% of steel plate thickness

[0367] Overlap of rotating blade: 0.3mm

[0368] ·Vertical contact angle between upper knife and steel plate: 11 degrees

[0369] · Angle between the rotation direction of the rotary blade and the conveying direction of the steel plate: 0.15 degrees on the rear side of the conveying

[0370] Cutting position: 10mm from the edge

[0371] <Example 8>

[0372] In Example 8, the following steel plates were used as steel plates.

[0373] Steel plate: TS1220MPa, thickness 1.2mm

[0374] Ingredients:

[0375] C: 0.12%, Si: 0.45%, Mn: 2.50%, P: 0.008%, S: 0.0012%, sol.Al: 0.030%, N: 0.0020%, Nb: 0.040%, Cr: 0.400%, Cu: 0.010%, Mo: 0.010%, Ni: 0.010%, Ti: 0.017%, B: 0.0012%, the balance is Fe and unavoidable impurities

[0376] In addition, the above-mentioned spray device 3 is used as the lubricating oil attachment device (refer to Figure 1 ).

[0377] In Example 8, the conditions of the spray device 3 were set as follows, and lubricating oil was applied before trimming.

[0378] ·Steel plate conveying speed: 230 [mpm]

[0379] · Oiling range of spray device 3: 20 [mm] from the end surface in the width direction of the steel plate, only the upper surface

[0380] Oil usage: 0.9 [L / hour] (Oil density: 2.8 [mL / m 2 ])

[0381] Supply air pressure: 0.4~0.6[MPa]

[0382] · Oil amount in the center of the steel plate width: 1.5[g / m 2 ]

[0383] · Oil application within 5 mm of the edge: 2.5 [g / m 2 ], lower surface 1.5[g / m 2 ]

[0384] · Lubricant spray area: For the entire length, upper surface, and both edges.

[0385] Rotating blade diameter: φ300mm

[0386] · Gap of rotating blade: 9% of steel plate thickness

[0387] Overlap of rotating blades: 0mm

[0388] ·Vertical contact angle between upper knife and steel plate: 7 degrees

[0389] · Angle between the rotation direction of the rotary blade and the conveying direction of the steel plate: 0.09 degrees on the rear side of the conveying

[0390] Cutting position: 10mm from the edge

[0391] <Example 9>

[0392] In Example 9, the following steel plates were used as steel plates.

[0393] Steel plate: TS1480MPa, thickness 1.4mm

[0394] Ingredients:

[0395] C: 0.20%, Si: 0.95%, Mn: 3.20%, P: 0.008%, S: 0.0009%, sol.Al: 0.025%, N: 0.0020%, Nb: 0.013%, Cr: 0.050%, Cu: 0.150%, Mo: 0.100%, Ni: 0.080%, Ti: 0.012%, B: 0.0012%, Sb: 0.005%, the balance is Fe and unavoidable impurities

[0396] In addition, the above-mentioned spray device 3 is used as the lubricating oil attachment device (refer to Figure 1 ).

[0397] In Example 9, the conditions of the spray device 3 were set as follows, and lubricating oil was applied before trimming.

[0398] ·Steel plate conveying speed: 115 [mpm]

[0399] · Oiling range of spray device 3: 40 [mm] from the end surface in the width direction of the steel plate, upper and lower surfaces

[0400] Oil usage: 3.1 [L / hour] per single side, 6.2 [L / hour] per double side (Oil density: 11.2 [mL / m 2 ])

[0401] Supply air pressure: 0.4~0.6[MPa]

[0402] · Oil amount in the center of the steel plate width: 1.5[g / m 2 ]

[0403] · Oil amount within 5mm of the edge: 3.8[g / m 2 ]

[0404] After trimming, part of the applied lubricant is removed.

[0405] · Lubricant spray area: For the entire length, upper and lower surfaces, and on both edges.

[0406] Rotating blade diameter: φ300mm

[0407] · Gap of rotating blade: 9% of steel plate thickness

[0408] Overlap of rotating blade: 0.1mm

[0409] ·Vertical contact angle between upper knife and steel plate: 8 degrees

[0410] · Angle between the rotation direction of the rotary blade and the conveying direction of the steel plate: 0.20 degrees on the rear side of the conveying

[0411] Cutting position: 20mm from the edge

[0412] <Example 10>

[0413] In Example 10, the following steel plates were used as steel plates.

[0414] Steel plate: TS1220MPa, thickness 2.0mm

[0415] Ingredients:

[0416] C: 0.12%, Si: 0.45%, Mn: 2.50%, P: 0.008%, S: 0.0012%, sol.Al: 0.030%, N: 0.0020%, Nb: 0.040%, Cr: 0.400%, Cu: 0.010%, Mo: 0.010%, Ni: 0.010%, Ti: 0.017%, B: 0.0012%, the balance is Fe and unavoidable impurities

[0417] In addition, the above-mentioned spray device 3 is used as the lubricating oil attachment device (refer to Figure 1 ).

[0418] In Example 10, the conditions of the spray device 3 were set as follows, and lubricating oil was applied before trimming.

[0419] ·Steel plate conveying speed: 230 [mpm]

[0420] · Oiling range of spray device 3: 20 [mm] from the end surface in the width direction of the steel plate, upper and lower surfaces

[0421] Oil usage: 0.8 [L / hour] per single side, 1.6 [L / hour] per double side (Oil density: 2.8 [mL / m 2 ])

[0422] Supply air pressure: 0.4~0.6[MPa]

[0423] · Oil amount in the center of the steel plate width: 1.5[g / m 2 ]

[0424] · Oil amount within 5mm of the edge: 2.5[g / m 2 ]

[0425] · Lubricant spray area: For the entire length, upper and lower surfaces, and on both edges.

[0426] Rotating blade diameter: φ300mm

[0427] · Gap of rotating blade: 4% of steel plate thickness

[0428] Overlap of rotating blades: 2.5mm

[0429] ·Vertical contact angle between upper knife and steel plate: 14 degrees

[0430] · Angle between the rotation direction of the rotary blade and the conveying direction of the steel plate: 0 degrees on the rear side of the conveyor

[0431] Cutting position: 10mm from the edge

[0432] <Evaluation>

[0433] In the evaluation, 20 coils (variety: GA) were passed through the CGL under the same manufacturing conditions and the edges of all the coils were trimmed along the entire length. Then, the rate of indentation of the soft steel (caused by foreign matter other than adhesion in the furnace) when about 500 tons of mild steel were passed through the plate was evaluated. The rate of indentation is the weight ratio of the coil parts where indentation was confirmed and removed in the passed coil of mild steel. It should be noted that the parts of the coil where the weight of each coil after removing the indentation part is less than 1.5 tons are insufficient in terms of the product weight and are therefore unqualified. In addition, the shear surface ratio and the frequency of convexity generation were evaluated in the central part of the length of the passed coil.

[0434] Examples of SEM observation of the steel plates of Comparative Example 2 and Example 7 are shown in FIG. Figure 4 middle. Figure 4 (a) corresponds to Comparative Example 2, Figure 4 (b) corresponds to Example 7.

[0435] Depend on Figure 4 It can be seen that in the steel plate where the lubricating oil is applied only to the trimming blade using the felt, the shear surface ratio is large, and the shear surface is a cross-sectional boundary with a wavy shape ( Figure 4 (a)), whereas in the steel plate to which the lubricant was directly applied, the shear plane ratio was small and the boundary between the shear plane and the fracture plane was clearly a straight line ( Figure 4 (b)).

[0436] Table 1 shows the evaluation results of each steel plate.

[0437]

[0438] In Examples 7 to 9 based on the present invention, the shear surface ratio and the frequency of convex portions are within the scope of the invention, and the rate of indentation is suppressed to less than 1.0%. On the other hand, in Comparative Example 2 in which lubricating oil is not directly applied to the steel plate, the gap, the vertical contact angle between the upper blade and the steel plate, and the angle between the rotation direction of the rotating blade and the conveying direction of the steel plate are not appropriate.

[0439] It should be noted that in Example 10, the cutting method of the present invention was used, but as a steel plate, the shear plane ratio and the frequency of convex portion generation were outside the scope of the invention, and the indentation generation rate was greater than 1.0%. However, compared with Comparative Example 2, the shear plane ratio and the frequency of convex portion generation of Example 10 were smaller.

[0440] It can be seen from this that, compared with the conventional case of directly applying lubricating oil to the rotating blade, the steel plate having the first cut surface formed by the cutting method of the present invention can suppress the shedding of iron powder after cutting, and can provide a steel plate of higher quality than before.

[0441] In addition, the steel sheets of Examples 7 and 9 were subjected to alkali degreasing treatment in a degreasing line before stamping automobile parts, and it was confirmed that no degreasing failure occurred.

[0442] (other)

[0443] The present invention can also adopt the following structure.

[0444] (1) This embodiment is a method for manufacturing a steel plate having an edge portion that is cut by a rotating knife, wherein, during the process of cutting the steel plate by the rotating knife, lubricating oil is attached to a position on the surface of the steel plate before cutting at which the rotating knife is to be cut.

[0445] According to this structure, even if the lubricating oil attached to the rotating blade splashes due to the centrifugal force of the rotating blade, the insufficient oil supply at the cutting position can be eliminated by attaching the lubricating oil to the surface of the steel plate, and the frequency of chipping of the trimmer can be suppressed by reducing friction, thereby improving the yield of steel plate manufacturing.

[0446] (2) In the present embodiment, the rotary blade is a pair of rotary blades that can clamp the steel plate and cut the steel plate by clamping the steel plate with the pair of rotary blades, and the lubricating oil is attached to at least one of the front and back surfaces of the steel plate. The lubricating oil is preferably attached to both the front and back surfaces of the steel plate.

[0447] According to this configuration, the steel plate can be cut more stably by using a pair of rotating blades.

[0448] (3) The lubricating oil is adhered to the surface of the steel plate by spraying the lubricating oil, for example.

[0449] According to this configuration, the lubricating oil can be made to adhere to the surface of the steel plate more uniformly.

[0450] The lubricating oil preferably has an average droplet diameter of 1 μm or more and 2000 μm or less after spraying.

[0451] (4) The lubricating oil is adhered to the surface of the steel plate, for example.

[0452] According to this configuration, the lubricating oil can be attached to the surface of the steel plate.

[0453] Here, the method of attaching the lubricating oil to the upper surface side of the steel plate and the method of attaching the lubricating oil to the lower surface side of the steel plate may be different.

[0454] For example, the lubricating oil may be attached by dripping the lubricating oil onto the upper surface of the steel plate and spraying the lubricating oil onto the lower surface of the steel plate.

[0455] (5) The amount of lubricating oil adhered to the surface is adjusted to less than 30 mL / m 2 .

[0456] (6) The water content of the lubricating oil is 3000 ppm or less.

[0457] (7) The viscosity of the above lubricating oil is 3 mm when the liquid temperature of the lubricating oil is 40°C. 2 / s or more and 130mm 2 / s or less.

[0458] (8) A film thickness equalizing tool for equalizing the film thickness of the lubricating oil attached to the surface of the steel plate is provided between the rotating blade and the attachment position of the lubricating oil.

[0459] (9) In the present embodiment, a pair of rolling rollers for holding the steel plate are provided between the rotating blade and the attachment position of the lubricating oil, and the area of ​​the steel plate 1 held by the pair of rolling rollers at least includes the position of the steel plate 1 to be cut by the rotating blade.

[0460] According to this configuration, the lubricating oil adhering to the steel sheet is stretched by the rolling rolls. As a result, the adhering lubricating oil becomes more uniform along the conveying direction of the steel sheet.

[0461] (10) In the present embodiment, the steel plate is cut by the rotary blade while being conveyed, and the rotary blade performs cutting by rotating in the forward direction relative to the conveying direction of the steel plate.

[0462] According to this configuration, the load on the rotating blade can be suppressed to be small compared to the case where the rotating blade is rotated in the reverse direction.

[0463] (11) The steel plate to be cut may be a high-tensile steel plate, and the plate thickness of the steel plate may be 0.4 mm or more, for example.

[0464] According to the method for manufacturing a steel plate of the present embodiment, the steel plate to be cut is a high-tensile steel plate, and even if the steel plate has a thickness of 0.4 mm or more, continuous cutting with a good yield is possible.

[0465] (12) This embodiment is a trimming device for cutting an edge of a conveyed steel plate using a rotary blade, wherein a lubricating oil adhering device for adhering lubricating oil to a position of the steel plate to be cut by the rotary blade is provided upstream of the rotary blade.

[0466] According to this configuration, even if the lubricating oil attached to the rotating blade splashes due to the centrifugal force of the rotating blade, the lubricating oil can be attached to the surface of the steel plate to eliminate insufficient oil supply at the cutting position, and the frequency of chipping of the trimmer can be suppressed by reducing friction.

[0467] (13) This embodiment is a manufacturing apparatus for the steel plate 1 including the above-mentioned trimming apparatus.

[0468] According to this configuration, the frequency of chipping of the trimmer can be suppressed, thereby improving the yield rate of steel sheet production.

[0469] (14) The composition of the steel sheet contains, by mass%, C: 0.03% to 0.35%, Si: 0.01% to 3.00%, Mn: 0.50% to 3.50%, Al: 0.001% to 1.000%, P: 0.100% to 0.0100%, S: 0.0200% to 0.0200%, and further contains B: 0.0050% to 0.0050%, Nb: 0.100% to 0.0100%, and Ti: 0.200% to 0.0000% , Cr: less than 1.000%, Mo: less than 1.00%, Cu: less than 1.000%, Ni: less than 1.000%, Sb: less than 0.200%, Zr: less than 0.100%, V: less than 0.200%, W: less than 0.100%, Sn: less than 0.200%, Ca: less than 0.0050%, REM: less than 0.0050%, Mg: less than 0.0050%, one or more of the following, the balance being Fe and inevitable impurities.

[0470] (15) The rotating blade comprises a pair of rotating blades which can clamp the steel plate relative to each other and use the pair of rotating blades to clamp and cut the steel plate. The gap between the upper blade and the lower blade of the pair of rotating blades is greater than 5% and less than 19%. The contact angle between the upper blade in the rotating direction of the rotating blade and the steel plate in the vertical direction is greater than 3 degrees and less than 13 degrees. The angle formed by the rotating direction of the rotating blade and the conveying direction of the steel plate in the direction of forming an opening angle on the rear side of the conveying is greater than 0.01 degrees and less than 0.5 degrees.

[0471] (16) A trimming device that uses a rotary blade to cut an edge of a conveyed steel plate, wherein a lubricating oil attaching device is provided upstream of the rotary blade to lubricate a portion of the steel plate to be cut by the rotary blade.

[0472] (17) A steel plate manufacturing apparatus comprising the steel plate trimming apparatus of the present invention.

[0473] (18) A rolled steel plate, wherein at least one end face at both ends in the width direction includes a cut surface, wherein the tensile strength TS of the steel plate is greater than or equal to 590 MPa and less than or equal to 980 MPa, and the shear surface ratio (%) of at least a portion of the cut surface in the length direction of the steel plate, i.e., the first cut surface, satisfies the formula (1), and the number of convex portions at the boundary between the shear surface of the first cut surface and the fracture surface is less than or equal to 5 / 100 mm.

[0474] 19-0.0146×TS≤shear surface ratio≤48-0.0300×TS …Formula (1)

[0475] (19) A rolled steel plate, wherein at least one end face at both ends in the width direction includes a cut surface, wherein the tensile strength TS of the steel plate is greater than or equal to 980 MPa and less than or equal to 1180 MPa, and the shear surface ratio (%) of at least a portion of the cut surface in the length direction of the steel plate, i.e., the first cut surface, satisfies the formula (2), and the number of convex portions at the boundary between the shear surface of the first cut surface and the fracture surface is less than or equal to 5 / 100 mm.

[0476] 10-0.00526×TS≤shear surface ratio≤36-0.0180×TS …Formula (2)

[0477] (20) A rolled steel plate, wherein at least one end face at both ends in the width direction includes a cut surface, wherein the tensile strength TS of the steel plate is greater than or equal to 1180 MPa and less than or equal to 1320 MPa, the shear surface ratio (%) of at least a portion of the cut surface in the length direction of the steel plate, i.e., the first cut surface, satisfies the formula (3), and the number of convex portions at the boundary between the shear surface and the fracture surface of the cut surface is less than or equal to 5 / 100 mm.

[0478] 10-0.00526×TS≤shear surface ratio≤27-0.0108×TS …Formula (3)

[0479] (21) A rolled steel plate, wherein at least one end face at both ends in the width direction includes a cut surface, wherein the tensile strength TS of the steel plate is greater than or equal to 1320 MPa and less than or equal to 1850 MPa, and the shear surface ratio (%) of at least a portion of the cut surface in the length direction of the steel plate, i.e., the first cut surface, satisfies the formula (4), and the number of convex portions at the boundary between the shear surface and the fracture surface of the first cut surface is less than or equal to 5 / 100 mm.

[0480] 3≤shear surface ratio≤16-0.0254×TS …Formula (4)

[0481] (22) With respect to the amount of oil applied to at least one of the surfaces of the steel sheet facing each other in the thickness direction, the amount of oil applied to the region extending from the width direction end face formed by the first cut surface to a distance of 5 mm is 0.2 g / m greater than the amount of oil applied to the center position in the width direction. 2 above.

[0482] (23) The amount of oil applied to the steel plate surface in the region 5 mm from the width direction end face formed by the first cut surface is 2.7 g / m 2 above.

[0483] (24) The amount of oil applied to the steel plate surface in the region from the widthwise end face formed by the first cut surface to 5 mm is 6.5 g / m 2above.

[0484] (25) The composition of the steel sheet contains, by mass%, C: 0.03% to 0.35%, Si: 0.01% to 3.00%, Mn: 0.50% to 3.50%, Al: 0.001% to 1.000%, P: 0.100% to 0.0100%, S: 0.0200% to 0.0200%, and further contains B: 0.0050% to 0.0050%, Nb: 0.100% to 0.0100%, and Ti: 0.200% to 0.0000% , Cr: less than 1.000%, Mo: less than 1.00%, Cu: less than 1.000%, Ni: less than 1.000%, Sb: less than 0.200%, Zr: less than 0.100%, V: less than 0.200%, W: less than 0.100%, Sn: less than 0.200%, Ca: less than 0.0050%, REM: less than 0.0050%, Mg: less than 0.0050%, one or more of the following, the balance being Fe and inevitable impurities.

[0485] (26) The steel sheet has a composition comprising, by mass%, C: 0.10% to 0.35% and Mn: 1.00% to 3.50%.

[0486] (27) In the composition of the above steel sheet, Mn is contained in an amount of 2.2% or more by mass%.

[0487] (28) A coil material obtained by winding the rolled steel sheet of the present invention into a coil shape.

[0488] (29) A blank material for stamping obtained by processing the rolled steel plate of the present invention, wherein at least one end face includes the first cut surface.

[0489] Explanation of symbols

[0490] 1 Steel Plate

[0491] 1a, 1b Steel plate surface

[0492] 2 Rotating Knife

[0493] 2A, 2B a pair of rotating blades

[0494] 3. Spray device (lubricating oil attachment device)

[0495] 7 calendering rollers

[0496] 9 Felt

[0497] 20 Oil drop device (lubricating oil adhesion device)

Claims

1. A method for manufacturing a steel plate, comprising a process of cutting an edge of the steel plate using a rotating knife, characterized in that: In the process of cutting the steel plate with the rotary blade, lubricating oil is attached to a position on the surface of the steel plate before cutting, where the steel plate is to be cut with the rotary blade.

2. The method for manufacturing a steel plate according to claim 1, characterized in that: The rotating blade has a pair of rotating blades that can clamp the steel plate and face each other, and the steel plate is clamped and cut by the pair of rotating blades. The lubricating oil is attached to at least one of the front and back surfaces of the steel plate.

3. The method for manufacturing a steel plate according to claim 1 or claim 2, characterized in that: The lubricating oil is adhered to the surface of the steel plate by spraying the lubricating oil.

4. The method for manufacturing a steel plate according to claim 3, characterized in that: The average diameter of the droplets of the sprayed lubricating oil is 1 μm or more and 2000 μm or less.

5. The method for manufacturing a steel plate according to claim 1 or claim 2, characterized in that: The lubricating oil is adhered by dropping the lubricating oil onto the surface of the steel plate.

6. The method for manufacturing a steel plate according to any one of claims 1 to 5, characterized in that: The lubricating oil is adhered by dripping the lubricating oil onto the upper surface of the steel plate and spraying the lubricating oil onto the lower surface of the steel plate.

7. The method for manufacturing a steel plate according to any one of claims 1 to 6, characterized in that: The amount of lubricant oil adhered was adjusted to less than 30 mL / m 2 .

8. The method for manufacturing a steel plate according to any one of claims 1 to 7, characterized in that: The water content of the lubricating oil is 3000 ppm or less.

9. The method for manufacturing a steel plate according to any one of claims 1 to 8, characterized in that: The viscosity of the lubricating oil is 3 mm when the liquid temperature of the lubricating oil is 40°C. 2 / s or more and 130mm 2 / s or less.

10. The method for manufacturing a steel plate according to any one of claims 1 to 9, characterized in that: A film thickness equalizing tool for equalizing the film thickness of the lubricating oil attached to the surface of the steel plate is provided between the rotating blade and the attachment position of the lubricating oil.

11. The method for manufacturing a steel plate according to any one of claims 1 to 10, characterized in that: A pair of rolling rolls for holding the steel sheet is provided between the rotating blade and the lubricant oil attachment position, and a region of the steel sheet held by the pair of rolling rolls includes at least a position of the steel sheet to be cut by the rotating blade.

12. The method for manufacturing a steel plate according to any one of claims 1 to 11, characterized in that: The process of cutting the steel plate by the rotary knife is performed on the steel plate during transportation. The rotary blade cuts the steel plate by rotating in the forward direction relative to the conveying direction of the steel plate.

13. The method for manufacturing a steel plate according to any one of claims 1 to 12, characterized in that: The steel plate is a high-tensile steel plate, and the plate thickness of the steel plate is greater than or equal to 0.4 mm.

14. The method for manufacturing a steel plate according to claim 13, characterized in that: The steel sheet comprises, by mass%, C: 0.03% to 0.35%, Si: 0.01% to 3.00%, Mn: 0.50% to 3.50%, Al: 0.001% to 1.000%, P: 0.100% to 1.000%, S: 0.0100% to 1.000%, N: 0.0200% to 1.000%, B: 0.0050% to 1.000%, Nb: 0.100% to 1.000%, Ti: 0.200% to 1.000%, and C. One or more of r: less than 1.000%, Mo: less than 1.00%, Cu: less than 1.000%, Ni: less than 1.000%, Sb: less than 0.200%, Zr: less than 0.100%, V: less than 0.200%, W: less than 0.100%, Sn: less than 0.200%, Ca: less than 0.0050%, REM: less than 0.0050%, Mg: less than 0.0050%, and the balance is Fe and inevitable impurities.

15. The method for manufacturing a steel plate according to any one of claims 1 to 14, characterized in that: The rotating blade has a pair of rotating blades that can clamp the steel plate and face each other, and the steel plate is clamped and cut by the pair of rotating blades. The gap between the upper blade and the lower blade of the pair of rotating blades is greater than 5% and less than 19%. The contact angle between the upper blade of the rotating blade and the steel plate in the vertical direction in the rotating direction is 3 degrees or more and 13 degrees or less. The angle formed by the rotation direction of the rotating blade and the conveying direction of the steel plate is 0.01 degrees or more and 0.5 degrees or less in the direction forming an opening angle on the conveying rear side.

16. A steel plate trimming device, which utilizes a rotary knife to cut the edge of a conveyed steel plate, characterized in that: A lubricant oil adhering device for adhering lubricant oil to a position of the steel plate to be cut by the rotary blade is provided upstream of the rotary blade. 17 . A steel plate manufacturing device comprising the steel plate trimming device according to claim 16 .

18. A rolled steel plate, wherein at least one end surface of both ends in the width direction includes a cut surface, characterized in that: The tensile strength TS of the steel plate is greater than or equal to 590 MPa and less than 980 MPa. The shear surface ratio (%) of at least a portion of the cut surface in the length direction of the steel plate, i.e., the first cut surface, satisfies the formula (1), The number of convex portions at the boundary between the shear surface and the fracture surface of the first cut surface is 5 / 100 mm or less, 19-0.0146×TS≤shear plane ratio≤48-0.0300×TS …Formula (1).

19. A rolled steel plate, wherein at least one end surface of both ends in the width direction includes a cut surface, characterized in that: The tensile strength TS of the steel plate is greater than or equal to 980 MPa and less than 1180 MPa. The shear surface ratio (%) of at least a portion of the cut surface in the length direction of the steel plate, i.e., the first cut surface, satisfies the formula (2), The number of convex portions at the boundary between the shear surface and the fracture surface of the first cut surface is 5 / 100 mm or less, 10-0.00526×TS≤shear surface ratio≤36-0.0180×TS …Formula (2).

20. A rolled steel plate, wherein at least one end surface of both ends in the width direction includes a cut surface, characterized in that: The tensile strength TS of the steel plate is greater than or equal to 1180 MPa and less than 1320 MPa. The shear surface ratio (%) of at least a portion of the cut surface in the length direction of the steel plate, i.e., the first cut surface, satisfies the formula (3), The number of convex portions at the boundary between the shear surface and the fracture surface of the cut surface is 5 / 100 mm or less, 10-0.00526×TS≤shear surface ratio≤27-0.0108×TS …Formula (3).

21. A rolled steel plate, wherein at least one end surface of both ends in the width direction includes a cut surface, characterized in that: The tensile strength TS of the steel plate is greater than or equal to 1320 MPa and less than 1850 MPa. The shear surface ratio (%) of at least a portion of the cut surface in the length direction of the steel plate, i.e., the first cut surface, satisfies the formula (4), The number of convex portions at the boundary between the shear surface and the fracture surface of the first cut surface is 5 / 100 mm or less, 3≤shear plane ratio≤16-0.0254×TS ...Formula (4).

22. The rolled steel plate according to any one of claims 18 to 21, characterized in that Regarding the amount of oil applied to at least one of the steel plate surfaces that are opposite to each other in the plate thickness direction, The amount of oil applied in the region 5 mm from the widthwise end face formed by the first cut face is 0.2 g / m greater than the amount of oil applied at the center position in the widthwise direction. 2 above.

23. The rolled steel plate according to any one of claims 18 to 22, characterized in that: The amount of oil applied to the steel plate surface in the region 5 mm from the width direction end surface formed by the first cut surface was 2.7 g / m 2 above.

24. The rolled steel plate according to claim 23, characterized in that The amount of oil applied to the steel plate surface in the region 5 mm from the width direction end surface formed by the first cut surface was 6.5 g / m 2 above.

25. The rolled steel plate according to any one of claims 18 to 24, characterized in that: The steel sheet comprises, by mass%, C: 0.03% to 0.35%, Si: 0.01% to 3.00%, Mn: 0.50% to 3.50%, Al: 0.001% to 1.000%, P: 0.100% to 1.000%, S: 0.0100% to 1.000%, N: 0.0200% to 1.000%, B: 0.0050% to 1.000%, Nb: 0.100% to 1.000%, Ti: 0.200% to 1.000%, and C. One or more of r: less than 1.000%, Mo: less than 1.00%, Cu: less than 1.000%, Ni: less than 1.000%, Sb: less than 0.200%, Zr: less than 0.100%, V: less than 0.200%, W: less than 0.100%, Sn: less than 0.200%, Ca: less than 0.0050%, REM: less than 0.0050%, Mg: less than 0.0050%, and the balance is Fe and inevitable impurities.

26. The rolled steel plate according to claim 25, characterized in that The steel sheet includes, by mass%, C: 0.10% to 0.35% and Mn: 1.00% to 3.50%.

27. The rolled steel plate according to claim 26, characterized in that The steel sheet contains, in terms of mass%, Mn: 2.20% or more.

28. A coil material obtained by winding the rolled steel sheet according to any one of claims 18 to 27 into a coil shape.

29. A blank material for stamping obtained by processing the rolled steel plate according to any one of claims 18 to 27, characterized in that: At least one end surface includes the first cutting surface.