Carbon fiber for sliding and method for producing carbon fiber for sliding
Through the combination of uncarbonized carbon fiber fired in the range of 400 to 550°C and the resin composition, the problem of damage to the sliding parts of the submersible pump when using carbon fiber is solved, and good sliding properties and wear resistance are achieved.
Patent Information
- Application Number
- CN202380023410.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-04
- Filing Date
- 2023-02-27
- Publication Date
- 2024-10-01
AI Technical Summary
When using carbon fiber for existing submersible pump sliding parts, it is easy to damage the target material, and it is difficult to obtain good sliding properties and strength from uncarbonized carbon fiber.
Use uncarbonized carbon fiber fired in the range of 400 to 550°C as carbon fiber for sliding, mix it into the resin composition, and adjust the 5% weight reduction temperature through thermogravimetry to ensure that the target material is not damaged during processing and improve sliding performance and wear resistance.
It achieves good sliding properties, wear resistance and mechanical strength without damaging the target material, and is suitable for applications such as submersible pumps.
Smart Images

Figure CN118742679A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a carbon fiber for sliding and a method for producing the carbon fiber for sliding.
[0002] More specifically, the present invention relates to a carbon fiber for sliding which, when blended into a sliding resin composition and processed into a sliding part, exhibits good sliding properties without damaging the counterpart part, and a method for producing such a carbon fiber for sliding. Background Art
[0003] Existing submersible pumps are used for various purposes, such as water pumping devices for pumping water from rivers and oceans, and water circulation in water heaters, floor heating equipment, automobile engines, inverters, batteries or fuel cells, etc.
[0004] An example of the submersible pump (water pump) includes the following structures 1) to 5) including a predetermined sliding member (sliding bearing, thrust receiving member) (for example, refer to Patent Document 1).
[0005] 1) Impeller
[0006] 2) Shaft for fixing the impeller
[0007] 3) Sliding bearing fixed to the impeller, which is used to support the impeller to rotate freely relative to the shaft support
[0008] 4) Thrust bearing components that slide with the end faces of the sliding bearing
[0009] 5) The casing and cover that contain the impeller and form the pump chamber
[0010] The sliding bearing, which is a sliding component, is a cylindrical bearing that receives loads on the inner diameter and the end surface and has the same thickness on the end surface, and is an injection molded product made of a resin composition having a linear polyphenylene sulfide resin as a base resin.
[0011] That is, it is characterized in that it is an injection molded product derived from a resin composition containing at least carbon fiber and at least one selected from polytetrafluoroethylene resin and graphite in a predetermined base resin, and the carbon fiber is a carbide sintered at 1000 to 1500°C.
[0012] Furthermore, there has been proposed a sliding part using, as a reinforcing material, predetermined uncarbonized carbonaceous fibers different from the uncarbonized carbon fibers serving as the sliding carbon fibers of the present invention (for example, see Patent Document 2).
[0013] More specifically, the sliding member is a sintered body obtained by sintering a composite body having a predetermined shape and composed of the following blending components 1) to 3).
[0014] For example, a raw material pitch is supplied to a spinning machine, and is extruded from a nozzle under pressure based on an inert gas while being heated to 300°C to obtain raw material fibers. Subsequently, the obtained raw material fibers are kept in an oxidizing atmosphere at about 150 to 500°C for about 0.5 to 5 hours to obtain carbon fibers that are not dissolved, and a sliding part is formed by containing a specified amount of uncarbonized carbon fibers.
[0015] 1) Uncarbonized carbon fibers heat treated at a temperature below 550°C
[0016] 2) Boron compounds and other inorganic powders or inorganic fibers
[0017] 3) Inorganic powder or its inorganic fiber having self-sintering properties in which uncarbonized carbonaceous fibers and boron compounds are embedded
[0018] It should be noted that uncarbonized carbonaceous fibers are carbonaceous fibers that have not been subjected to carbonization treatment at a normal temperature, and are defined as carbonaceous fibers that have been heat-treated (burned) at a temperature of 550° C. or less and still have room for further carbonization.
[0019] Furthermore, according to the embodiment of Patent Document 2, the composites composed of 1) to 3) are all heated to 1000°C in a normal pressure, non-oxidizing atmosphere or a nitrogen atmosphere for primary sintering, and then heated to 1300°C, 1700°C or 2000°C in the atmosphere for secondary sintering. Therefore, the uncarbonized carbonaceous fibers of Patent Document 2 are finally heat-treated at a temperature substantially above 1000°C.
[0020] [Prior art literature]
[0021] [Patent Document]
[0022] [Patent Document 1] Japanese Patent No. 6639592 (claims, etc.)
[0023] [Patent Document 2] Japanese Patent Application Laid-Open No. 3-237062 (claims, etc.) Summary of the invention
[0024] However, the sliding component (sliding bearing, etc.) used for the submersible pump (water pump) described in Patent Document 1 is characterized in that carbide fired at 1000 to 1500° C. is used as reinforcing fiber for a predetermined resin.
[0025] Therefore, there is a problem that the mixed carbon fiber (carbide) damages the counterpart material. This problem also exists when a graphite fired at 2000° C. or higher is used as the carbon fiber.
[0026] As a countermeasure, it is conceivable not to use carbon fibers. However, in this case, there is a problem that the strength of the sliding member (sliding bearing) is insufficient and sufficient wear resistance cannot be obtained depending on the use conditions.
[0027] In addition, in the sliding member described in Patent Document 2, it is necessary to use uncarbonized carbonaceous fibers fired at an extremely low temperature, and there is a problem that it is difficult to obtain good sliding properties.
[0028] That is, for example, it is necessary to use the following uncarbonized carbonaceous fibers: raw material fibers are obtained by extruding raw pitch from a nozzle at 300-400°C under pressure based on an inert gas, and then maintaining the raw material pitch at about 150-500°C for about 0.5-5 hours in an oxidizing atmosphere to form uncarbonized carbonaceous fibers.
[0029] This is to improve the interface adhesion with the self-sintering carbonaceous powder. Ultimately, if the temperature is not raised to 1000°C for a sintering process in a non-oxidizing atmosphere or a nitrogen atmosphere at normal pressure as described above, and then the temperature is raised to 1300°C, 1700°C or 2000°C for a sintering process in the atmosphere, the desired strength cannot be obtained.
[0030] Moreover, the sliding part described in Patent Document 2 is an invention related to a reinforced carbon composite material based on carbon fibers, the so-called C / C composite material. Therefore, there is no description or consideration at all about the situation of combining the uncarbonized carbonaceous fibers described in Patent Document 2 with a resin composition.
[0031] In view of this, the inventors conducted intensive research and found that by using uncarbonized carbon fibers (hereinafter sometimes referred to as sliding carbon fibers) whose 5 wt% reduction temperature obtained by thermogravimetric measurement under specified conditions is within a specified range as carbon fibers blended in a sliding resin composition, when a sliding part is made by specified processing, the friction coefficient is low, the wear amount is reduced, and good sliding properties can be obtained, etc., thereby completing the present invention.
[0032] That is, an object of the present invention is to provide a carbon fiber for sliding, which is blended in a resin composition for sliding and, when the resin composition for sliding is made into a sliding part by a predetermined process, exhibits good sliding properties without damaging the mating part, and an efficient method for producing such a carbon fiber for sliding.
[0033] According to the present invention, there is provided a sliding carbon fiber blended in a sliding resin composition for use in making a sliding part by a predetermined process, wherein the 5 wt% reduction temperature (hereinafter sometimes referred to as TG5) based on thermogravimetric measurement is set to a value within the range of 400 to 550° C., thereby being able to solve the above-mentioned problems.
[0034] In this way, by regulating the 5 weight % reduction temperature based on thermogravimetric measurement of the sliding carbon fiber as an additive for use in the sliding resin composition within a specified range, when processed into a specified sliding part, the counterpart material (for example, metals such as stainless steel and aluminum alloy) will not be damaged, and good sliding properties can be exhibited for a long time.
[0035] In addition, such a sliding carbon fiber has excellent uniform mixing properties with various resin components and can exhibit good sliding properties with a relatively small blending amount.
[0036] Furthermore, if such a sliding carbon fiber is mixed with a sliding resin composition and processed into a predetermined sliding part, sufficient characteristics such as heat resistance, mechanical strength, low linear expansion coefficient, friction coefficient and wear amount, antistatic property, etc. can be exerted.
[0037] Furthermore, when the sliding carbon fiber of the present invention is constituted, the tensile modulus measured in accordance with JIS R7606:2000 is preferably a value within the range of 10 to 35 GPa.
[0038] In this way, when the tensile modulus of the sliding carbon fibers is specified and they are combined and processed into a specified sliding member, it is easy to adjust the linear expansion coefficient, friction coefficient and wear amount to values below the specified values.
[0039] When the sliding carbon fiber of the present invention is formed, the tensile elongation measured in accordance with JIS R7606:2000 is preferably within a range of 2 to 5%.
[0040] In this way, by specifying the tensile elongation of the sliding carbon fiber, when the sliding resin composition is made by combining such sliding carbon fiber and then processed into a specified sliding part, the linear expansion coefficient, friction coefficient and wear amount can be more easily adjusted to values below the specified values, thereby improving durability and wear resistance.
[0041] When the sliding carbon fiber of the present invention is formed, the saturated moisture content measured in accordance with JIS K 7209:2000 is preferably set to a value within a range of 1 to 8% by weight.
[0042] By specifying the saturated moisture content of the sliding carbon fibers in this manner, dimensional changes in sliding components and the like caused by water absorption of the sliding carbon fibers can be suppressed, and dimensional accuracy can be easily maintained.
[0043] When the sliding carbon fiber of the present invention is configured, it is preferred that the carbon content of the surface as determined by XPS elemental analysis be within a range of 85 to 96% by weight relative to the total weight.
[0044] By specifying the carbon amount on the surface of the sliding carbon fiber based on XPS elemental analysis, when such sliding carbon fiber is blended to form a sliding resin composition and then processed into a specified sliding part, excellent sliding properties can be more quantitatively exhibited for a long period of time.
[0045] In addition, when the sliding carbon fiber of the present invention is formed, it is preferable that the volume resistivity is set to 1×10 0 ~1×10 4 The value is within the range of Ω·cm.
[0046] By limiting the volume resistivity of the sliding carbon fibers in this way, when such carbon fibers are blended to form a sliding resin composition and then processed into a predetermined sliding part, not only durability and wear resistance but also conductivity and antistatic properties can be easily adjusted.
[0047] In addition, the resin component of the sliding resin composition formulated with the sliding carbon fiber of the present invention is preferably at least one selected from the group consisting of polyphenylene sulfide resin, polyethersulfone resin, polyetheretherketone resin, polyimide resin, polyamide resin, polyacetal resin, polytetrafluoroethylene resin, polyketone resin, thermosetting phenolic resin, epoxy resin, melamine resin, diallyl phthalate resin and unsaturated polyester resin.
[0048] Thus, by adding a predetermined carbon fiber for sliding, the resin component when the sliding resin composition is prepared is limited, and when processed into a predetermined sliding part, good mechanical strength can be obtained, and further, more excellent durability, wear resistance, etc. can be exerted.
[0049] It should be noted that when the sliding carbon fiber of the present invention is combined to form a sliding resin composition, the sliding resin composition contains at least the compounding components (a) to (c), or the compounding components (a), (b), (d), or (a) to (d). Here, the compounding component (a) is the above-mentioned resin component, the compounding component (b) is the sliding carbon fiber of the present invention, the compounding component (c) is the inorganic material described later, and the compounding component (d) is the lubricating additive described later.
[0050] Furthermore, when a polytetrafluoroethylene resin is used as the compounding component (a), the lubricating additive as the compounding component (d) is not an essential compounding component in constituting the sliding resin composition of the present invention and may be omitted.
[0051] Another aspect of the present invention is a method for producing a sliding carbon fiber to be blended with a sliding resin composition, the method comprising the following steps (1) to (2).
[0052] (1) A step of preparing raw material fibers for carbon fibers.
[0053] (2) A calcining step in which the raw material fibers of the carbon fibers are calcined at a calcining temperature in the range of 600 to 800° C. so that the 5 wt % reduction temperature of the obtained sliding carbon fibers based on thermogravimetric measurement is in the range of 400 to 550° C.
[0054] By such a process, as an additive for use in a sliding resin composition, it is easy, stable, and efficient to manufacture a sliding carbon fiber having a 5 wt% reduction temperature (TG5) within a specified range, so that when it is processed into a specified sliding part through the sliding resin composition, the target part will not be damaged, and good sliding properties, wear resistance, etc. can be exhibited for a long time.
[0055] Furthermore, the sliding carbon fiber produced in this manner has excellent uniform mixing properties with various resin components, and can exhibit good sliding properties, wear resistance, etc. with a relatively small blending amount. BRIEF DESCRIPTION OF THE DRAWINGS
[0056] Figure 1 (a) to (c) are graphs provided for explaining the relationship between the firing temperature of carbon fibers and the linear expansion coefficient, friction coefficient, and wear amount of sliding parts.
[0057] Figure 2 This is a diagram for explaining the relationship between the calcination temperature of carbon fibers and the 5 wt% reduction temperature (TG5) of carbon fibers.
[0058] Figure 3 (a) to (b) are graphs provided to explain the relationship between the calcination temperature of carbon fibers and the tensile elastic modulus and tensile elongation of carbon fibers.
[0059] Figure 4 This is a diagram for explaining the relationship between the calcination temperature of carbon fibers and the volume resistivity (logarithmic expression) of carbon fibers.
[0060] Figure 5 (a) to (c) are graphs provided to explain the relationship between the blending amount of sliding carbon fibers and the linear expansion coefficient, friction coefficient, and wear amount of the sliding component.
[0061] Figure 6 (a) to (c) are diagrams provided to illustrate the relationship between the weight ratio of the sliding carbon fiber as the compounding component (b) / the compounding component (c), i.e., the inorganic material, and the linear expansion coefficient, friction coefficient, and wear amount in the sliding part.
[0062] Figure 7(a) to (c) are diagrams provided to illustrate the relationship between the weight ratio of the sliding carbon fiber as the compounding component (b) / the compounding component (d) i.e. the lubricating additive and the linear expansion coefficient, friction coefficient and wear amount in the sliding part. DETAILED DESCRIPTION
[0063] [First embodiment]
[0064] The first embodiment is a sliding carbon fiber that is blended with a sliding resin composition for use in a sliding part, wherein the 5 wt% reduction temperature based on thermogravimetric measurement is set to a value within a range of 400 to 550°C.
[0065] That is, Figure 1 As shown in (a) to (c), the sliding carbon fiber of the present invention is to control the linear expansion coefficient, friction coefficient, and wear amount in the sliding parts from the sliding resin composition. Figure 2 As shown, it refers to uncarbonized carbon fibers having a 5 wt% reduction temperature (hereinafter, sometimes abbreviated as TG5) measured by a thermogravimetric measuring device (TGA) within a prescribed range under prescribed conditions.
[0066] Hereinafter, the carbon fiber for sliding according to the first embodiment will be described in more detail with reference to the drawings as appropriate.
[0067] 1. Types
[0068] The type of sliding carbon fiber is characterized in that the 5 wt% reduction temperature (TG5) measured using TGA under the conditions of an air flow rate of 100 ml / min and a heating rate of 5°C / min is set to a value within the range of 400 to 550°C.
[0069] The reason for this is that when the TG5 is less than 400°C, heat resistance, mechanical strength, etc. are excessively reduced, and when processed into a predetermined sliding part, durability, etc. are significantly reduced.
[0070] On the other hand, when TG5 exceeds 550°C, the heat resistance and mechanical strength of the steel itself are improved, but when processed into a predetermined sliding part, the friction coefficient increases.
[0071] Therefore, it is more preferable that the TG5 of the uncarbonized carbon fibers be a value within a range of 430 to 500°C, and further preferably a value within a range of 450 to 490°C.
[0072] In addition, this TG5 can be measured using TGA, and in the obtained weight reduction graph, the temperature at which the weight is reduced by 5% by weight from the initial weight (100% by weight) is used as a reference.
[0073] Here, refer to Figure 2, the relationship between the calcination temperature (°C) of carbon fiber (including carbon fiber for sliding and other carbon fiber, the same below) and the 5 weight % reduction temperature (TG5) of TGA, which is one of its thermal decomposition temperatures, is described.
[0074] Right now, Figure 2 The horizontal axis is represented by the sintering temperature (° C.) of the carbon fiber, and the vertical axis is represented by the TG5 value (° C.) of the carbon fiber.
[0075] Furthermore, as described later, Figure 2 The characteristic curves in FIG. 1 are based on the results of TG5 of carbon fibers used in Examples 1 to 3 and Comparative Examples 1 and 2 that differed only in the firing temperature.
[0076] In addition, in the drawings, Example 1 is described as Example 1 and Comparative Example 1 is described as Comparative Example 1, and the same shall apply hereinafter.
[0077] According to the Figure 2 It can be understood from the characteristic curve that the TG5 value tends to decrease slightly as the sintering temperature (° C.) of the carbon fiber decreases.
[0078] More specifically, when the sintering temperature of the carbon fiber is greater than 1200°C, TG5 is greater than 550°C, and when the sintering temperature of the carbon fiber is 600-800°C, TG5 is a value in the range of 400-550°C, and when the sintering temperature of the carbon fiber is less than 600°C, TG5 is sometimes less than 400°C.
[0079] Therefore, according to Figure 2 As a result of the characteristic curve shown, it can be said that by adjusting the firing temperature of the carbon fibers to a predetermined range, even the firing temperature of the uncarbonized carbon fibers can be controlled to a temperature at which the predetermined heat resistance is exhibited.
[0080] In addition, the carbon fiber for sliding can basically limit TG5 to a value within a predetermined range by limiting the firing temperature to a relatively low level.
[0081] That is, the carbide described in Patent Document 1 and the like in the prior art is a carbon fiber sintered at least at 1000°C, preferably 1300 to 1500°C, and its TG5 is found to be higher than 700°C.
[0082] In addition, the uncarbonized carbonaceous fibers described in Patent Document 2 of the prior art are fired at a temperature of 500°C or lower, and it is separately found that the carbonization degree thereof is quite low, and TG5 is less than 400°C.
[0083] Therefore, regarding the type of the carbon fiber for sliding, when producing the carbon fiber for sliding, it is usually preferred to set the calcining temperature to be within the range of 600 to 800°C.
[0084] Therefore, the carbonization degree of TG5 of the sliding carbon fiber is higher than that of uncarbonized carbon fibers fired at a temperature below 500°C, and on the other hand, it is lower than that of carbides fired at a temperature above 1000°C, and is a low-temperature carbide that is clearly different from these previous carbon fibers.
[0085] That is, as described later, the sliding carbon fiber has significant differences in properties compared to uncarbonized carbon fibers (low-temperature carbides) and carbides in terms of tensile elastic modulus, tensile elongation, XPS elemental analysis (carbon content), volume resistivity, saturated moisture content, etc., and can be clearly distinguished.
[0086] Furthermore, the calcination time of the sliding carbon fiber is preferably 0.1 to 20 hours under the above-mentioned predetermined temperature conditions.
[0087] The reason for this is that if the calcination time is outside the prescribed numerical range, uncarbonized carbon fibers having desired properties cannot be obtained even under prescribed temperature conditions.
[0088] More specifically, if the sintering time is less than 0.1 hour, carbonization is insufficient even under predetermined temperature conditions, and the mechanical strength and wear resistance of the obtained sliding part may be significantly reduced.
[0089] On the other hand, when the calcination time exceeds 20 hours, carbonization may become excessive even under the prescribed temperature conditions, and the friction coefficient may increase.
[0090] Therefore, it is more preferably 0.2 to 15 hours, and even more preferably 0.3 to 10 hours.
[0091] 2. Morphology
[0092] The average fiber diameter (diameter) of the sliding carbon fibers is usually 30 μm or less, preferably 3 to 25 μm, and more preferably 5 to 20 μm, and can be appropriately determined depending on the application, ease of use, and the like.
[0093] Similarly, the average length of the sliding carbon fibers is usually 500 μm or less, preferably 50 to 450 μm, and more preferably 100 to 400 μm, but this can be appropriately determined according to the application, ease of use, and the like.
[0094] 3. Tensile elastic modulus
[0095] Furthermore, the tensile elastic modulus of the sliding carbon fibers is usually preferably a value within a range of 10 to 35 GPa.
[0096] The reason for this is that if the tensile elastic modulus of the sliding carbon fiber is a value less than 10 GPa, when it is processed into a predetermined sliding part, the mechanical strength and wear resistance may be significantly reduced.
[0097] On the other hand, if the tensile elastic modulus of the sliding carbon fiber exceeds 35 GPa, the friction coefficient of the obtained sliding component may increase.
[0098] Therefore, the tensile elastic modulus of the sliding carbon fibers is more preferably set to a value within the range of 13 to 30 GPa, and further preferably set to a value within the range of 16 to 25 GPa.
[0099] It should be noted that the tensile modulus of the uncarbonized carbon fibers can be measured in accordance with JIS R 7606:2000.
[0100] Here, refer to Figure 3 (a) The relationship between the calcination temperature and the tensile modulus of carbon fibers (including carbon fibers for sliding and other carbon fibers) is described.
[0101] Right now, Figure 3 The horizontal axis of (a) represents the sintering temperature (° C.) of the carbon fiber, and the vertical axis represents the value of the tensile elastic modulus (GPa) of the carbon fiber.
[0102] Furthermore, as described later, Figure 3 The characteristic curve in (a) is based on the tensile elastic modulus of carbon fibers used in Examples 1 to 3 and Comparative Examples 1 and 2 that differ only in the firing temperature.
[0103] Depend on Figure 3 From the characteristic curve in (a), it can be seen that the value of the tensile modulus of the carbon fiber tends to significantly increase as the sintering temperature of the carbon fiber increases.
[0104] More specifically, when the carbon fiber is fired at a temperature lower than 600° C., the tensile modulus is lower than 10 GPa, and when the carbon fiber is fired at a temperature of 450° C., the tensile modulus is a relatively low value lower than 1 GPa.
[0105] It was also found that when the carbon fiber is fired at a temperature of 600 to 800°C, the tensile modulus reaches a value of at least 10 GPa, and when other manufacturing conditions (stretching conditions, firing time) are changed, a maximum value of about 35 GPa is obtained.
[0106] Furthermore, when the sintering temperature of the carbon fibers is higher than 1200° C., the tensile modulus becomes a value higher than 35 GPa.
[0107] Therefore, it can be said that by adjusting the firing temperature of the carbon fibers to a predetermined range, the tensile modulus of the carbon fibers can be reliably controlled to a value within a desired range.
[0108] 4. Tensile elongation
[0109] In addition, the tensile elongation of the sliding carbon fiber is usually preferably a value within the range of 2 to 5%.
[0110] The reason for this is that if the tensile elongation of the sliding carbon fiber is a value less than 2%, the friction coefficient of the obtained sliding member may increase.
[0111] On the other hand, if the tensile elongation of the sliding carbon fiber exceeds 5%, when processed into a sliding part, the mechanical strength and wear resistance may be significantly reduced.
[0112] Therefore, the tensile elongation is more preferably set to a value within the range of 2.1 to 4%, and further preferably set to a value within the range of 2.2 to 3%.
[0113] In addition, the tensile elongation of the sliding carbon fiber can be measured in accordance with JIS R 7606:2000.
[0114] Here, combined Figure 3 (b) The relationship between the calcination temperature and the tensile elongation of carbon fibers (including carbon fibers for sliding and other carbon fibers) is described.
[0115] Right now, Figure 3 The horizontal axis of (b) represents the calcination temperature (°C) of the carbon fiber, and the vertical axis represents the tensile elongation value (%) of the carbon fiber.
[0116] Moreover, as described later, Figure 3 The characteristic curve in (b) is based on the tensile elongation of the carbon fibers used in Examples 1 to 3 and Comparative Examples 1 and 2, in which only the sintering temperature of the carbon fibers was different.
[0117] From this Figure 3 It can be understood from the characteristic curve described in (b) that when the calcination temperature of the carbon fiber is at least less than 600° C., the value of the tensile elongation of the carbon fiber tends to become significantly smaller as the calcination temperature becomes lower.
[0118] More specifically, when the calcination temperature of the carbon fibers is lower than 600° C., the tensile elongation becomes a value significantly lower than 2%.
[0119] It was also found that when the carbon fiber is fired at a temperature of 600 to 800°C, the tensile elongation reaches at least 2% and when other manufacturing conditions (stretching conditions, firing time) are changed, a maximum value of 5% can be achieved.
[0120] Furthermore, when the sintering temperature of the carbon fiber exceeds 800° C., the tensile elongation becomes a small value less than 2%.
[0121] Therefore, it can be said that by adjusting the calcining temperature of the carbon fibers to a predetermined range, the value of the tensile elongation of the carbon fibers can be accurately controlled to a value within a desired range.
[0122] 5.XPS elemental analysis (carbon content)
[0123] The carbon content of the surface of the sliding carbon fiber as determined by XPS elemental analysis is preferably a value within a range of 85 to 96 wt % relative to 100 wt % of the total amount.
[0124] The reason is that by regulating the carbon amount to a value within a prescribed range, unlike conventional carbides (graphite) and uncarbonized carbonaceous fibers, when processed into prescribed sliding parts, a sliding resin composition having a linear expansion coefficient, a friction coefficient and a wear amount that are respectively below prescribed values can be more easily and stably provided.
[0125] More specifically, this is because if the carbon content is less than 85% by weight, the mechanical strength and wear resistance of the obtained sliding part may be significantly reduced.
[0126] On the other hand, when the carbon amount is a value exceeding 96% by weight, the friction coefficient may increase.
[0127] Therefore, the carbon amount is more preferably within a range of 86 to 95% by weight, and further preferably within a range of 88 to 94% by weight, based on the total amount.
[0128] It should be noted that the carbon content can be measured according to XPS elemental analysis based on a standard curve of carbon element.
[0129] 6. Volume resistivity
[0130] In addition, the volume resistivity of the sliding carbon fiber is usually preferably 1×10 0 ~1×10 4 The value is within the range of Ω·cm.
[0131] The reason is that by setting the volume resistivity to a value within a specified range, when processed into a specified sliding part, unlike conventional carbides and uncarbonized carbonaceous fibers, a sliding part having excellent electrical insulation, antistatic properties, etc. can be provided more easily and quantitatively stably.
[0132] More specifically, if the volume resistivity is less than 1×10 0The value of Ω·cm is lower than that of Ω·cm, and the antistatic property becomes good, but the electrical insulation in the sliding parts becomes insufficient, and sparks may occur.
[0133] On the other hand, if the volume resistivity is greater than 1×10 4 If the value of Ω·cm is too low, the electrical insulation becomes good. On the contrary, static electricity may accumulate in the sliding member, and the antistatic property may become insufficient.
[0134] Therefore, it is more preferable to set the volume resistivity to 5×10 0 ~5×10 3 The value is preferably within the range of Ω·cm, and more preferably 1×10 1 ~1×10 3 The value is within the range of Ω·cm.
[0135] The volume resistivity can be measured by a four-terminal method using a commercially available digital voltmeter or the like.
[0136] Here, combined Figure 4 , the relationship between the sintering temperature and volume resistivity of carbon fibers (including carbon fibers for sliding and other carbon fibers) is described.
[0137] Right now, Figure 4 The horizontal axis represents the sintering temperature (° C.) of the carbon fiber, and the vertical axis represents the volume resistivity value (Ω·cm) of the carbon fiber in a logarithmic representation.
[0138] Moreover, if Figure 4 As described later, the characteristic curve in is based on the volume resistivity of the carbon fibers used in Examples 1 to 3 and Comparative Examples 1 and 2 in which only the sintering temperature of the carbon fibers was different.
[0139] Depend on Figure 4 From the characteristic curve in FIG, it can be seen that the higher the sintering temperature of the carbon fiber, the more rapidly the volume resistivity tends to decrease.
[0140] More specifically, if the sintering temperature of carbon fiber is lower than 600°C, the volume resistivity becomes significantly greater than 1×10 4 The value of Ω·cm.
[0141] In addition, when the sintering temperature of carbon fiber is 600 to 800°C, the volume resistivity can easily reach 1×10 0 ~1×10 4 The value is within the range of Ω·cm.
[0142] Furthermore, when the sintering temperature of carbon fiber exceeds 1200°C, the volume resistivity becomes less than 1×10 -1 Small value of Ω·cm.
[0143] Therefore, by adjusting the sintering temperature of the carbon fiber to a predetermined range, the volume resistivity value can be accurately controlled to a value within the predetermined range, and the handling of the carbon fiber becomes easy, and it can be said that the desired antistatic properties can be obtained in the sliding parts.
[0144] 7. Saturated moisture content
[0145] The saturated moisture content of the sliding carbon fibers can be measured in accordance with JIS K 7209:2000 which specifies the method for determining the water absorption rate in plastics, and is usually preferably within a range of 1 to 8% by weight.
[0146] The reason for this is that by regulating the saturated water content to a value within a predetermined range and processing the material into a predetermined sliding part, when used for a bearing for a submersible pump or the like, excellent sliding properties can be obtained more easily and quantitatively over a long period of time.
[0147] More specifically, when the saturated moisture content is less than 1% by weight, it may be difficult to exhibit excellent sliding properties and the like.
[0148] On the other hand, when the saturated moisture content is a value exceeding 8% by weight, the dimensional change due to water absorption becomes large, and it may become difficult to maintain dimensional accuracy.
[0149] Therefore, the saturated moisture content is more preferably within a range of 1.5 to 7% by weight, and further preferably within a range of 2 to 6% by weight.
[0150] The saturated moisture content is measured in accordance with JIS K 7209:2000 and can be measured as a ratio of the increased weight due to absorbed moisture to the initial weight.
[0151] 8. Amount of coordination
[0152] (1) Mixing amount 1
[0153] In the sliding resin composition, the amount of the sliding carbon fiber as the compounding component (b) is preferably within a range of 10 to 400 parts by weight relative to 100 parts by weight of the resin component as the compounding component (a).
[0154] The reason is that by regulating the amount of the sliding carbon fiber as the compounding component (b) to a value within a prescribed range, when processed into a prescribed sliding part, a sliding resin composition having a friction coefficient, wear amount, and linear expansion coefficient below prescribed values can be more easily and stably provided.
[0155] More specifically, if the blending amount of the sliding carbon fiber is less than 10 parts by weight, it may be difficult to adjust the linear expansion coefficient to within a specified range when processed into a specified sliding part, or the wear resistance may decrease, resulting in increased wear.
[0156] On the other hand, if the amount of the sliding carbon fiber blended is greater than 400 parts by weight, when the sliding resin composition is processed into a sliding part, it may be difficult to adjust the friction coefficient value to within a predetermined range or the molding processability when processed into a sliding part may be significantly reduced.
[0157] Therefore, the blending amount of the sliding carbon fiber is more preferably within a range of 30 to 300 parts by weight, and further preferably within a range of 50 to 200 parts by weight.
[0158] Here, refer to Figure 5 (a) The relationship between the blending amount of the sliding carbon fiber and the linear expansion coefficient measured in accordance with JIS K 7197:2012 when processed into a predetermined sliding member (hereinafter, sometimes simply referred to as the linear expansion coefficient) is described.
[0159] Right now, Figure 5 The horizontal axis of (a) represents the amount (parts by weight) of the sliding carbon fiber relative to 100 parts by weight of the resin component (a), and the vertical axis represents the linear expansion coefficient (1×10 -5 / ℃).
[0160] Furthermore, as described later, Figure 5 The characteristic curve in (a) is based on the results of the linear expansion coefficient of the sliding parts of Examples 1, 4 to 5 and Comparative Examples 3 and 4, which have the same types of compounding components (a) to (d) and the same compounding amounts of compounding components (a) and (c) to (d) and differ only in the compounding amount of compounding component (b).
[0161] By Figure 5 From the characteristic curve shown in (a), it can be seen that the linear expansion coefficient tends to slightly decrease as the blending amount of the sliding carbon fiber increases.
[0162] More specifically, if the blending amount of the sliding carbon fiber is less than 10 parts by weight, the linear expansion coefficient becomes greater than 5×10 -5 / ℃, when the value is 10 parts by weight or more, the linear expansion coefficient becomes 5×10 -5 / ℃ or below.
[0163] Furthermore, when the blending amount of the sliding carbon fiber exceeds 400 parts by weight, the linear expansion coefficient becomes approximately 4×10 -5 / ℃ or so.
[0164] Next, refer to Figure 5 (b) illustrates the relationship between the blending amount of sliding carbon fiber and the friction coefficient when processed into a predetermined sliding part.
[0165] Right now, Figure 5 The horizontal axis of (b) represents the blending amount (parts by weight) of the sliding carbon fiber, and the vertical axis represents the friction coefficient (-) obtained when the sliding member is processed according to Example 1 described later.
[0166] and, Figure 5 The characteristic curve in (b) is Figure 5 (a) Similarly, the results related to the friction coefficient of Examples 1, 4 to 5 and Comparative Examples 3 and 4 are given.
[0167] From this Figure 5 It can be understood from the characteristic curve described in (b) that the friction coefficient tends to increase as the blending amount of the sliding carbon fiber increases.
[0168] More specifically, when the amount of the sliding carbon fibers as the compounding component (b) is within the range of 5 to 150 parts by weight relative to 100 parts by weight of the resin component as the compounding component (a), a value of about 0.05 can be obtained as the friction coefficient.
[0169] Furthermore, as the blending amount of the sliding carbon fiber increases, the friction coefficient gradually increases, and when it exceeds 400 parts by weight, the friction coefficient tends to be larger than 0.4.
[0170] Next, refer to Figure 5 (c) illustrates the relationship between the blending amount of sliding carbon fiber and the wear amount when processed into a predetermined sliding part.
[0171] Right now, Figure 5 The horizontal axis of (c) represents the blending amount (parts by weight) of the sliding carbon fiber, and the vertical axis represents the wear loss (μm) under predetermined conditions when processed into a sliding part according to Example 1 described later.
[0172] and, Figure 5 The characteristic curve in (c) is Figure 5 (a) Similarly, the results are based on the wear amount of Examples 1, 4 to 5 and Comparative Examples 3 and 4.
[0173] According to the Figure 5 It can be understood from the characteristic curve (c) that as the blending amount of the sliding carbon fiber increases, the wear amount temporarily decreases and then tends to increase.
[0174] More specifically, when the amount of the sliding carbon fiber as the compounding component (b) is less than 10 parts by weight relative to 100 parts by weight of the resin component as the compounding component (a), the wear loss is a value larger than 100 μm.
[0175] When the blending amount of the sliding carbon fiber was in the range of 10 to 400 parts by weight, a low value of 100 μm or less was obtained, although some variation was observed depending on the conditions.
[0176] Therefore, by Figure 5 (a) to (c) show that by controlling the blending amount of the sliding carbon fiber to a value within a range of, for example, 10 to 400 parts by weight, the value of the linear expansion coefficient in the sliding component, the friction coefficient as the sliding property, and the wear amount can be adjusted with high accuracy.
[0177] (2) Mixing amount 2
[0178] In addition, it is also preferable to determine the blending amount of the sliding carbon fibers as the blending component (b) in relation to the blending amount of the inorganic material as the blending component (c).
[0179] More specifically, the weight ratio of the compounded component (b) / the compounded component (c) (hereinafter, sometimes simply referred to as the compounded amount ratio b / c) is preferably set to a value within the range of 1 / 1 to 10 / 1.
[0180] The reason for this is that by limiting the blending ratio b / c in the sliding resin composition, when processed into a sliding part, the linear expansion coefficient, friction coefficient and wear amount can be more easily adjusted to values below specified values.
[0181] More specifically, if the ratio b / c of the blending amount is less than 1 / 1, it may be difficult to adjust the amount of wear and the like to a predetermined numerical range when processed into a sliding part.
[0182] On the other hand, if the ratio b / c of the blending amount is a value larger than 10 / 1, it may be difficult to adjust the friction coefficient, wear amount, etc. within a predetermined numerical range.
[0183] Therefore, the ratio b / c of the blending amount is more preferably a value within the range of 1.5 / 1 to 8 / 1, and further preferably a value within the range of 2 / 1 to 6 / 1.
[0184] Here, refer to Figure 6 (a) Regarding the blending amount of the sliding carbon fiber, the relationship between the blending amount ratio b / c and the linear expansion coefficient is described.
[0185] Right now, Figure 6The horizontal axis of (a) is the ratio of the compounding amount, i.e., compounding component (b) / compounding component (c) (-), and the vertical axis is the linear expansion coefficient (1×10 -5 / ℃).
[0186] Moreover, as described later, Figure 6 The data of the characteristic curve (a) are based on the results of the linear expansion coefficient of the sliding parts of Examples 1, 4 to 5 and Comparative Examples 3 and 4, in which the types of the compounding components (a) to (d) and the compounding amounts of the compounding components (a) and (c) to (d) are the same and only the compounding amount of the compounding component (b) is different.
[0187] According to the Figure 6 From the characteristic curve in (a), it can be seen that as the value of the ratio b / c of the compounding amount increases, the linear expansion coefficient decreases and tends to stabilize.
[0188] More specifically, when the ratio b / c of the blending amount is around 0 / 1, the linear expansion coefficient becomes larger than 5×10 -5 / ℃, if the ratio b / c of the above-mentioned compounding amount is about 1 / 1, the linear expansion coefficient is 5×10 -5 / ℃.
[0189] In addition, if the ratio b / c of the blending amount is further about 10 / 1, 4×10 -5 / ℃ or so.
[0190] In addition, refer to Figure 6 (b) Regarding the blending amount of the sliding carbon fiber, the relationship between the blending amount ratio b / c and the friction coefficient when processed into a predetermined sliding part is described.
[0191] Right now, Figure 6 The horizontal axis of (b) shows the ratio of the blending amount, i.e., blending component (b) / blending component (c) (-), and the vertical axis shows the friction coefficient (-) obtained when the sliding part is processed according to Example 1 described later.
[0192] and, Figure 6 (b) The data of the characteristic curve and Figure 6 (a) Similarly, the friction coefficients of the sliding parts of Examples 1, 4 to 5 and Comparative Examples 3 and 4.
[0193] According to the Figure 6 It can be understood from the characteristic curve in (b) that the friction coefficient tends to increase as the ratio b / c of the blending amount increases.
[0194] More specifically, when the blending ratio b / c is around 0 / 1 to around 5 / 1, the friction coefficient is about 0.05, but then gradually increases. When the blending ratio b / c is greater than 10 / 1, a value greater than 0.1 is obtained, and a value greater than 0.5 is obtained around 15 / 1.
[0195] In addition, refer to Figure 6 (c) Regarding the blending amount of the sliding carbon fiber, the relationship between the blending amount ratio b / c and the wear amount when processed into a sliding part is described.
[0196] Right now, Figure 6 The horizontal axis of (c) is expressed as the ratio of the blending amount, i.e., blending component (b) / blending component (c) (-), and the vertical axis is expressed as the wear amount (μm) under predetermined conditions when processed into a sliding part according to Example 1 described later.
[0197] and, Figure 6 (c) The data of the characteristic curve and Figure 6 (a) Similarly, the wear amount of the sliding parts of Examples 1, 4 to 5 and Comparative Examples 3 and 4.
[0198] According to the Figure 6 From the characteristic curve in (c), it can be seen that as the ratio b / c of the blending amount increases, the wear amount temporarily decreases and then tends to increase.
[0199] More specifically, when the ratio b / c of the blending amount is around 0 / 1, the wear amount is greater than 100 μm, when the ratio b / c of the blending amount is around 1 / 1, it decreases to less than 100 μm, and when it is greater than 10 / 1, it increases to a value greater than 100 μm.
[0200] Therefore, by Figure 6 (a) to (c) show that if the blending ratio b / c is within a range of, for example, 1 / 1 to 10 / 1, the linear expansion coefficient, the friction coefficient as the sliding property, and the wear amount in the sliding member can be adjusted with higher accuracy.
[0201] (3) Mixing amount 3
[0202] In addition, it is also preferred that the amount of the sliding carbon fibers as the compounding component (b) be determined in relation to the amount of the lubricating additive as the compounding component (d).
[0203] More specifically, the weight ratio of the compounded component (b) / the compounded component (d) (hereinafter, sometimes simply referred to as the compounded amount ratio b / d) is preferably set to a value within the range of 1 / 1 to 10 / 1.
[0204] The reason for this is that by limiting the blending ratio b / d in the sliding resin composition, when processed into a sliding part, the linear expansion coefficient, friction coefficient and wear loss can be more easily adjusted to values below predetermined values.
[0205] More specifically, if the ratio b / d of the blending amount is less than 1 / 1, it may be difficult to adjust the amount of wear and the like to a predetermined numerical range when processed into a sliding part.
[0206] On the other hand, if the ratio b / d of the blending amount is a value larger than 10 / 1, it may be difficult to adjust the friction coefficient, wear amount, etc. within a predetermined numerical range.
[0207] Therefore, the ratio b / d of the blending amount is more preferably set to a value within the range of 1.5 / 1 to 8 / 1, and further preferably set to a value within the range of 2 / 1 to 6 / 1.
[0208] Here, refer to Figure 7 (a) The relationship between the ratio b / d of the blending amount and the linear expansion coefficient is described with respect to the blending amount of the sliding carbon fiber.
[0209] Right now, Figure 7 The horizontal axis of (a) is the ratio of the compounding amount, i.e., compounding component (b) / compounding component (d) (-), and the vertical axis is the linear expansion coefficient (1×10 -5 / ℃).
[0210] Moreover, as described later, Figure 7 The data of the characteristic curve (a) are based on the results of the linear expansion coefficient of the sliding parts of Examples 1, 4 to 5 and Comparative Examples 3 and 4, which have the same types of compounding components (a) to (d) and the same compounding amounts of compounding components (a) and (c) to (d) and only the compounding amount of compounding component (b) is different.
[0211] According to the Figure 7 From the characteristic curve in (a), it can be seen that as the value of the ratio b / d of the compounding amount increases, the linear expansion coefficient decreases and tends to stabilize.
[0212] More specifically, when the ratio b / d of the blending amount is around 0 / 1, the linear expansion coefficient becomes larger than 5×10 -5 / ℃, if the ratio b / d of the above-mentioned compounding amount becomes 1 / 1 or more, the linear expansion coefficient is 5×10 -5 / ℃ below.
[0213] In addition, if the ratio b / d of the blending amount is further about 10 / 1, 4×10 -5 / ℃ or so.
[0214] In addition, refer to Figure 7 (b) Regarding the blending amount of the sliding carbon fiber, the relationship between the blending amount ratio b / d and the friction coefficient when processed into a predetermined sliding part is described.
[0215] Right now, Figure 7 The horizontal axis of (b) shows the ratio of the blending amount, i.e., blending component (b) / blending component (d) (-), and the vertical axis shows the friction coefficient (-) obtained when the predetermined sliding member is processed according to Example 1 described later.
[0216] and, Figure 7 (b) The data of the characteristic curve and Figure 7 (a) Similarly, the results are based on the friction coefficients of the sliding parts of Examples 1, 4 to 5 and Comparative Examples 3 and 4.
[0217] According to the Figure 7 As can be understood from the characteristic curve in (b), the friction coefficient tends to become larger as the ratio b / d of the blending amount increases.
[0218] More specifically, when the ratio b / d of the blending amount is in the range of approximately 0 / 1 to approximately 5 / 1, the friction coefficient is approximately 0.05, but when the ratio b / d of the blending amount is approximately 10 / 1, a value of less than 0.2 is obtained.
[0219] In addition, refer to Figure 7 (c) Regarding the blending amount of the sliding carbon fiber, the relationship between the blending amount ratio b / d and the wear amount when processed into a predetermined sliding part is described.
[0220] Right now, Figure 7 The horizontal axis of (c) is expressed as the ratio of the blending amount, i.e., blending component (b) / blending component (d) (-), and the vertical axis is expressed as the wear amount (μm) under predetermined conditions when processed into a predetermined sliding part according to Example 1 described later.
[0221] and, Figure 7 (c) The data of the characteristic curve and Figure 7 (a) Similarly, the results are based on the wear amount of the sliding parts of Examples 1, 4 to 5 and Comparative Examples 3 and 4.
[0222] According to the Figure 7 From the characteristic curve in (c), it can be seen that as the ratio b / d of the blending amount increases, the wear amount temporarily decreases and then tends to increase.
[0223] More specifically, when the ratio b / d of the blending amount is around 0 / 1, the wear amount is greater than 100 μm, when the ratio b / d of the blending amount is around 1 / 1, it decreases to less than 100 μm, and when it further exceeds 10 / 1, it increases to a value greater than 100 μm.
[0224] Therefore, from Figure 7 (a) to (c) It can be understood that if the blending ratio b / d is a value within the range of, for example, 1 / 1 to 10 / 1, the linear expansion coefficient, the friction coefficient as sliding property, and the wear amount in the sliding component can be adjusted with higher accuracy.
[0225] [Second embodiment]
[0226] The second embodiment is a method for producing a sliding carbon fiber, which is a method for producing a sliding carbon fiber to be blended with a sliding resin composition, and is characterized by comprising the following steps (1) to (2).
[0227] (1) Process of preparing raw material fibers for carbon fibers
[0228] (2) a calcining step in which the raw material fiber of the carbon fiber is calcined at a calcining temperature in the range of 600 to 800° C., and the 5 wt % reduction temperature of the obtained sliding carbon fiber based on thermogravimetric measurement is set to a value in the range of 400 to 550° C.
[0229] Through such a process, it is easy, stable and efficient to manufacture sliding carbon fibers having a 5 wt% reduction temperature (TG5) within a specified range, so that when processed into sliding parts through a sliding resin composition, they can exhibit good sliding properties, wear resistance, etc. for a long time.
[0230] In addition, if the sliding carbon fiber is manufactured in this way, it becomes easy to adjust its own various properties (linear expansion coefficient, tensile elastic modulus, tensile elongation, friction coefficient, etc.), and when it is processed into a sliding part with a specified amount, it can exhibit good sliding properties, wear resistance, etc. for a long time.
[0231] 1. Process 1
[0232] (1) Raw material fiber selection process
[0233] Step 1 is a step of preparing raw material fibers of carbon fibers.
[0234] As raw materials of carbon fibers before calcination, there are pitch-based isotropic materials and PAN-based materials, and as the first stage, these are selected as necessary and melt-spinned.
[0235] (2) Melt Spinning Process
[0236] 1) Melt spinning process of asphalt-based materials
[0237] The asphalt-based isotropic material is produced according to a known production method, and is usually produced by directly using asphalt obtained from petroleum or coal as a raw material.
[0238] Therefore, materials such as asphalt can be prepared from ethylene bottom oil (petroleum-based) derived from naphtha, coal tar (coal-based), etc. as starting materials, and can obtain pitch suitable for spinning by removing low-boiling components and making it heavier by heat treatment.
[0239] However, it is preferable to introduce oxygen crosslinking or the like so as not to develop a graphite crystal structure during heat treatment.
[0240] Next, the obtained pitch is preferably ejected from a spinneret having a plurality of fine holes to form fibers.
[0241] Next, it is washed with water, stretched, subjected to oil-adhering and drying treatments, and is usually heated at 200 to 300° C. to be infusible, and further stretched, thereby producing raw material fibers based on a material such as a pitch-based material.
[0242] In addition, when spinning a pitch-based isotropic material, it is usually preferable to adopt a short fiber continuous spinning method.
[0243] Furthermore, in the case of spinning a pitch-based isotropic material, it is also preferable to adopt a vortex method in which a spiral airflow is generated near the spinning nozzle to perform stretching by a rotational force.
[0244] 3) Melt spinning process of PAN-based materials
[0245] The PAN-based material is also preferably produced according to a known production method.
[0246] Therefore, it is preferred that acrylonitrile (AN) as a monomer is first dissolved in a solvent, a polymerization catalyst is added, and then the mixture is heated at a predetermined temperature for a predetermined time, thereby obtaining polyacrylonitrile (PAN) having a high molecular weight.
[0247] Next, the obtained PAN is preferably discharged from a spinneret having a plurality of fine holes to form fibers, followed by water washing, primary stretching, oiling and drying treatment, and further secondary stretching to produce PAN fibers.
[0248] 2. Process 2
[0249] (1) Carbonization process / graphitization process of pitch-based isotropic materials
[0250] The spun pitch-based isotropic material is preferably heat-treated and carbonized in a carbonization furnace in an inert gas atmosphere at 1000 to 1300°C.
[0251] Next, the pitch-based material or the like is subjected to a heating treatment in a graphite furnace, preferably in an inert gas atmosphere, at 2000 to 3000° C. to be graphitized.
[0252] However, in the present invention, there is a feature that the graphitization step is not performed but only the carbonization step (firing step) is performed at 600 to 800°C.
[0253] Furthermore, it is important to adjust the 5 wt % reduction temperature of the obtained sliding carbon fiber by thermogravimetric measurement to a value within the range of 400 to 550°C.
[0254] (2) Carbonization process / graphitization process of PAN-based materials
[0255] In the case of a spun PAN-based material, a flame resistant treatment step is first performed.
[0256] Therefore, it is preferred to heat the spun PAN-based material at 200 to 300° C. in an air atmosphere while continuously passing the material through a refractory furnace to convert the material into refractory fibers that do not melt even at high temperatures.
[0257] Next, in the carbonization step, the obtained refractory fibers are preferably subjected to a heat treatment at 1000 to 1500° C. in an inert gas atmosphere (nitrogen atmosphere) while being continuously passed through a charcoal furnace to be converted into carbonized carbon fibers.
[0258] Furthermore, the PAN-based material is graphitized by heating it in a graphite furnace, preferably at 2000 to 3000° C. in an inert gas atmosphere.
[0259] However, the present invention is characterized in that the graphitization step is not performed and only the carbonization step (firing step) at 600 to 800° C. is performed.
[0260] Furthermore, it is important to adjust the 5 wt % reduction temperature of the obtained sliding carbon fiber by thermogravimetric measurement to a value within the range of 400 to 550°C.
[0261] [Third Embodiment]
[0262] The third embodiment is a sliding resin composition characterized in that it is a sliding carbon fiber blended in the sliding resin composition, the sliding resin composition is formed into a sliding part by a predetermined processing, the sliding resin composition contains the sliding carbon fiber, the 5 weight% reduction temperature of the sliding carbon fiber based on thermogravimetric measurement is set to a value in the range of 400 to 550°C, and at least contains blended components (a) to (c), or blended components (a), (b), (d), or (a) to (d).
[0263] (a) Resin component: 100 parts by weight
[0264] (b) 5 wt% uncarbonized carbon fibers with a reduction temperature of 400 to 550°C: 10 to 400 parts by weight
[0265] (c) Inorganic materials: 10 to 80 parts by weight
[0266] (d) Lubricating additive: 10 to 80 parts by weight
[0267] 1. Compounding ingredients (a)
[0268] (1) Types
[0269] The type of the resin component as the compounded component (a) is not particularly limited, and any known resin component used for sliding parts can be appropriately used.
[0270] More specifically, it is preferred that the resin composition be at least one heat-resistant resin selected from the group consisting of polyphenylene sulfide resin (PPS), polyethersulfone resin (PES), polyetheretherketone resin (PEEK), polyimide resin (PI), polyamide resin (PA), polyacetal resin (POM), polytetrafluoroethylene resin (PTFE), polyketone resin (PK), thermosetting phenolic resin (PF), epoxy resin (EP), melamine resin (MF), diallyl phthalate resin (PDAP) and unsaturated polyester resin (UP).
[0271] The reason is that by adding a predetermined sliding carbon fiber, the resin component when the sliding resin composition is prepared is limited, and when processed into a predetermined sliding part, good mechanical strength can be obtained, and further, better durability, wear resistance, etc. can be exerted.
[0272] Among the above-mentioned resin components, polyphenylene sulfide resin, polyetheretherketone resin, polyethersulfone resin, polyamide resin, and polyacetal resin are more preferable.
[0273] It should be noted that the resin component (heat-resistant resin) as the compounding component (a) can be used as the main component. As a standard, when the total amount of the resin component is set to 100 weight %, it is preferably 50 weight % or more, more preferably 70 weight % or more, and further preferably 90 weight % or more.
[0274] Among these heat-resistant resins, polyphenylene sulfide resin (including modified products of polyphenylene sulfide resin, sometimes referred to as PPS resin) is the most suitable resin component as the compounding component (a).
[0275] The reason is that PPS resin is generally a crystalline, translucent thermoplastic resin with a melting point of about 280°C and a glass transition temperature of 93°C. It has extremely high rigidity, excellent heat resistance, dimensional stability, abrasion resistance, low water absorption, etc.
[0276] In addition, PPS resins are classified into a cross-linked type, a linear type, and a semi-cross-linked type according to their molecular structures, and each of these types can be used alone or in combination of two or more types.
[0277] Furthermore, in order to form a sliding bearing that takes into account abrasive wear forms such as a water-repellent state where no water film is formed or a state where foreign matter is bitten, a straight-chain type having toughness is also preferred among PPS resins.
[0278] When a polyamide resin is used as the compounding component (a), it is preferably at least one resin selected from the group consisting of PA6 (polyamide 6, hereinafter also referred to as the abbreviation), PA11, PA12, PA66, PA610, PA4T, PA6T, PA6I, PA9T, PA10T and PAM5T.
[0279] (2) Quantity
[0280] The amount of the resin component as the compounding component (a) can be determined in consideration of the heat resistance, moldability, mechanical strength, etc. of the obtained sliding part. Generally, the compounding amount of the compounding component (a) is preferably set to a value in the range of 10 to 80 wt % relative to the total amount (100 wt %) of the sliding resin composition.
[0281] The reason is that when the amount of the compounding component (a) is less than 10% by weight, the amount of the sliding carbon fiber (e.g., a sintered product at 600 to 800°C) as the compounding component (b) and the inorganic material (talc, etc.) as the compounding component (c) increases, and the melt viscosity of the sliding resin composition becomes too high, which deteriorates the molding processability and sometimes makes it difficult to obtain a sliding part that exhibits excellent sliding properties.
[0282] On the other hand, when the amount of the compounded component (a) exceeds 80% by weight, the amount of the sliding carbon fiber as the compounded component (b) and the inorganic material as the compounded component (c) is reduced, and it becomes difficult to adjust the linear expansion coefficient of the obtained sliding part, and the mechanical strength and the like are significantly reduced, and sometimes it is impossible to exhibit excellent sliding properties.
[0283] Therefore, the amount of the component (a) is more preferably within a range of 15 to 60% by weight, and even more preferably within a range of 20 to 40% by weight, relative to the total amount of the sliding resin composition.
[0284] 2. Compounding ingredients (b)
[0285] Since the contents related to the sliding carbon fibers can be the same as those described in the first embodiment, re-explanation thereof will be omitted here.
[0286] 3. Compounding ingredients (c)
[0287] (1) Types
[0288] It is preferred that a predetermined amount of an inorganic material is added as the compounding component (c), and that the mechanical strength, heat resistance, sliding properties, surface smoothness, etc. of the sliding part obtained by performing a predetermined process are improved.
[0289] Therefore, the type of the inorganic material is not particularly limited, but it is preferable to mix an inorganic material having a Mohs hardness of 6 or less.
[0290] More specifically, at least one of mica, talc, graphite, gypsum, kaolinite, zinc oxide, titanium oxide, zirconium oxide and the like is preferably added.
[0291] The reason for this is that these inorganic materials have a Mohs hardness of 6 or less and are low in hardness, so when they are made into sliding parts, the sliding resistance with the counterpart part can be reduced and the friction coefficient can be suppressed to a low level.
[0292] In addition, among these inorganic materials, if it is talc, mica, graphite, gypsum, kaolinite or a mixture thereof with a Mohs hardness of less than 4 (for example, the mixing weight ratio of talc / mica: 90 / 10 to 10 / 90), even a relatively small amount of the mixed amount can exhibit good sliding properties, etc., and therefore it can be said to be more suitable.
[0293] Furthermore, if the compounding component (c) is talc (hydrous magnesium silicate: Mg3Si4O 10 (OH)2 as the main component of the mineral) is relatively cheap and can be mixed evenly with the resin component as the compounding component (a), so it is preferred.
[0294] Furthermore, when talc or a mixture of talc and mica is used as the compounding component (c), the apparent density is relatively uniform and low.
[0295] More specifically, in the case of talc, the apparent density measured in accordance with JIS K 5101-12:2004 is preferably 0.1 to 0.8 g / ml, more preferably 0.2 to 0.7 g / ml, and still more preferably 0.3 to 0.6 g / ml.
[0296] Furthermore, these inorganic materials are more preferable because they can provide a smooth surface without hindering the predetermined fluidity even when the sliding parts are manufactured by injection molding, compression molding, or the like.
[0297] (2) Quantity
[0298] The invention is characterized in that the amount of the inorganic material as the compounding component (c) is usually within a range of 10 to 80 parts by weight relative to 100 parts by weight of the resin component as the compounding component (a).
[0299] The reason for this is that if the amount of the compounded component (c) is less than 10 parts by weight, when processed into a sliding part, the slidability and durability may be significantly reduced.
[0300] On the other hand, when the amount of the compounded component (c) is greater than 80 parts by weight, the melt viscosity of the sliding resin composition becomes high, and the molding processability when processing into a sliding part may be significantly reduced.
[0301] Therefore, the amount of the compounding component (c) is more preferably 15 to 60 parts by weight, and even more preferably 20 to 50 parts by weight, relative to 100 parts by weight of the resin component as the compounding component (a).
[0302] 4. Compounding ingredients (d)
[0303] (1) Types
[0304] Furthermore, as the compounded component (d), it is preferred to compound a lubricating additive which is different from the resin component of the compounded component (a) and which exhibits a lubricating effect or the like.
[0305] The reason for this is that by adding such a lubricating additive, the sliding properties of the processed sliding parts can be significantly improved by interacting with the components (a) to (b) or the components (a) to (c) constituting the sliding resin composition.
[0306] Furthermore, the type of the lubricating additive is not particularly limited as long as it is a compound that exerts a prescribed lubricating effect, and is preferably at least one of polytetrafluoroethylene (PTFE), perfluoroalkoxyalkane (PFA), ethylene-tetrafluoroethylene copolymer (ETFE), perfluoroethylene-propylene copolymer (FEP), polyvinylidene fluoride (PVDF), silicone grease, silicone oil, silicone powder, and the like.
[0307] In particular, PTFE etc. has a low friction coefficient and can also exhibit good wear resistance. In addition, even a relatively wide range of mixing amounts can be uniformly mixed and dispersed with respect to the resin component as the mixing component (a), such as PPS resin.
[0308] That is, when PTFE or the like is used, the average particle size (D50 by laser diffraction method) is preferably within a range of 1 to 50 μm, more preferably 3 to 20 μm, and still more preferably 5 to 10 μm.
[0309] (2) Quantity
[0310] The invention is characterized in that the amount of the lubricating additive as the compounding component (d) is usually within a range of 10 to 80 parts by weight relative to 100 parts by weight of the resin component as the compounding component (a).
[0311] The reason for this is that if the amount of the compounded component (d) is less than 10 parts by weight, even if it is added to the sliding resin composition, the effect of addition such as imparting lubricity may not be exhibited.
[0312] On the other hand, if the amount of the compounded component (d) is greater than 80 parts by weight, it may be difficult to adjust the linear expansion coefficient and the like of the processed lubricated member to a predetermined value or less.
[0313] Therefore, the amount of the compounding component (d) is more preferably 15 to 60 parts by weight, and even more preferably 20 to 40 parts by weight, relative to 100 parts by weight of the resin component as the compounding component (a).
[0314] 5. Other ingredients (e)
[0315] (1) Types
[0316] Furthermore, it is also preferable to mix|blend as a compound other than the components (a)-(d) as a compounding component (e), and mix|blend various additives for achieving various purposes.
[0317] For example, as various additives, in order to further improve the friction characteristics, it is preferred to add at least one of modified polyolefin resins, lubricating oils such as mineral oil, ester oil, silicone oil, waxes such as polyethylene wax, oxidized polyethylene wax, ester wax, partially saponified wax, graphite, boron nitride, molybdenum disulfide, and tungsten disulfide.
[0318] In particular, among the oxidized polyethylene waxes, those with a melting point of 120° C. or higher are preferred because they help to achieve uniform mixing of various ingredients even when a relatively small amount is added while maintaining the mechanical strength and heat resistance of the sliding parts, and because adjustment of lubricity, moldability, etc. becomes easy.
[0319] On the other hand, graphite is a suitable compounding component (e) because lubricity, moldability, conductivity, hiding power, etc. can be easily adjusted by appropriately changing its compounding amount and form (average particle size, flaky shape).
[0320] (2) Quantity
[0321] When graphite or the like is added as the component (e), the amount thereof is usually preferably within a range of 1 to 50 parts by weight relative to 100 parts by weight of the resin component as the component (a).
[0322] The reason for this is that, although it depends on the type of the compounded component (e), if the compounded amount is less than 1 part by weight, compounding effects, particularly effects on friction characteristics, lubricity, etc., may not be achieved.
[0323] On the other hand, if the amount of the compounding component (e) is greater than 50 parts by weight, it may be difficult to uniformly mix with the resin component of the compounding component (a), or it may be difficult to adjust the lubricity, moldability, conductivity, hiding power, etc.
[0324] Therefore, the amount of the compounding component (e) is more preferably 1.5 to 30 parts by weight, and even more preferably 2 to 10 parts by weight, relative to 100 parts by weight of the resin component as the compounding component (a).
[0325] [Fourth Embodiment]
[0326] A fourth embodiment is a sliding part derived from a sliding resin composition, the sliding resin composition containing sliding carbon fibers, the sliding carbon fibers being carbon fibers blended into a sliding resin composition for use in making a sliding part by a predetermined process, wherein the 5 wt% reduction temperature based on thermogravimetric measurement is set to a value within the range of 400 to 550° C., the sliding resin composition having the following blended components (a) to (c) or blended components (a), (b), (d), or blended components (a) to (d).
[0327] (a) Resin component: 100 parts by weight
[0328] (b) 5 wt% uncarbonized carbon fibers with a reduction temperature of 400 to 550°C: 10 to 400 parts by weight
[0329] (c) Inorganic materials: 10 to 80 parts by weight
[0330] (d) Lubricating additive: 10 to 80 parts by weight
[0331] 4. Characteristic 1 (Linear Expansion Coefficient)
[0332] The linear expansion coefficient of the sliding member when the sliding resin composition as the compounding component (c) contains a predetermined amount of an inorganic material and when substantially containing no inorganic material can be measured using a thermomechanical analyzer (TMA) under the following predetermined conditions.
[0333] That is, a square test piece with a thickness of 3 mm and a single piece length of 5 mm was produced by molding, and the temperature of the square test piece was raised from 25°C to 100°C at 5°C / min using TMA. The change in the length of the square test piece was measured, and the linear expansion coefficient of the resin in the thickness direction (MD) at 35 to 80°C was calculated as the linear expansion coefficient.
[0334] In addition, it is usually preferred that the linear expansion coefficient is 10×10 -5 / ℃ below.
[0335] The reason is that if the linear expansion coefficient is greater than 10×10 -5 / °C, the desired dimensional accuracy may not be maintained due to sliding heat, and the sliding properties and durability of the sliding parts may be significantly reduced.
[0336] However, if the linear expansion coefficient becomes too small, the types, forms, and blending amounts of selectable resin components, inorganic materials, sliding carbon fibers, and the like may be excessively limited.
[0337] Therefore, it is more preferable to set the linear expansion coefficient of the sliding member to 1×10 -5 / ℃~5×10 -5 / °C, and more preferably 2×10 -5 / ℃~4.5×10 -5 / ℃ range.
[0338] Here again, refer to Figure 1 (a) The relationship between the sintering temperature of carbon fibers (including carbon fibers for sliding and other carbon fibers) and the linear expansion coefficient when processed into a predetermined sliding member is described.
[0339] Right now, Figure 1 The horizontal axis of (a) represents the calcination temperature of the carbon fiber (°C), and the vertical axis represents the linear expansion coefficient (1×10 -5 / ℃) relationship.
[0340] Moreover, as described later, Figure 1 The data of the characteristic curve (a) are based on the linear expansion coefficient of the carbon fibers used in Examples 1 to 3 and Comparative Examples 1 and 2, in which the types and amounts of the compounding components (a) to (d) are the same and only the calcination temperature of the carbon fibers is different.
[0341] According to the Figure 1 From the characteristic curve shown in (a), it can be seen that the sintering temperature (°C) of the carbon fiber has no significant influence on the linear expansion coefficient of the predetermined sliding member.
[0342] 5. Characteristic 2 (friction coefficient)
[0343] The friction coefficient of the sliding resin composition as a sliding member when it contains a predetermined amount of an inorganic material as the compounding component (c) and when it contains substantially no inorganic material can be measured under the following conditions using a thrust unidirectional rotation method in accordance with JIS K 7218:1986.
[0344] Sliding speed: 90m / min
[0345] Load (surface pressure): 10kg / cm 2
[0346] Test time: 20 hours
[0347] Test piece: Rectangular plate of 30 mm (horizontal width) × 30 mm (vertical width) × 3 mm (thickness)
[0348] Target material: Hollow cylindrical (SUS 304, inner diameter 20mm, outer diameter 25.6mm, length 15mm, surface roughness Ra 0.1)
[0349] Lubrication conditions: No lubrication
[0350] Furthermore, it is usually preferred that the friction coefficient be a value of 0.4 or less.
[0351] The reason for this is that if the friction coefficient exceeds 0.4, the sliding properties and durability of the sliding member may be significantly reduced.
[0352] However, depending on the purpose, form, etc. of the sliding member, the friction coefficient is more preferably a value within the range of 0.01 to 0.2, and further preferably a value within the range of 0.03 to 0.1.
[0353] in addition, Figure 1 (b) is a diagram for explaining the relationship between the sintering temperature of carbon fibers (including carbon fibers for sliding and other carbon fibers) and the friction coefficient when processed into sliding parts.
[0354] Right now, Figure 1 The horizontal axis of (b) represents the calcination temperature (°C) of the carbon fibers, and the vertical axis represents the friction coefficient (-) obtained when a sliding resin composition prepared by blending carbon fibers calcined at a predetermined temperature is processed into a sliding part.
[0355] Moreover, as described later, Figure 1 The data of the characteristic curve (b) are based on the results of the friction coefficient of the carbon fibers used in Examples 1 to 3 and Comparative Examples 1 and 2, which have the same types and amounts of the compounding components (a) to (d) but different only in the firing temperatures.
[0356] From this Figure 1 It can be understood from the characteristic curve (b) that the lower the sintering temperature of the carbon fiber is, the smaller the friction coefficient of the predetermined sliding member tends to be.
[0357] More specifically, it can be understood that if the sintering temperature of the carbon fiber is about 1250°C, the friction coefficient of the predetermined sliding component can be adjusted to a value below 0.4, and if the sintering temperature of the carbon fiber is about 800°C, the friction coefficient can be adjusted to a value below 0.1.
[0358] 6. Characteristic 3 (Durability)
[0359] In addition, the endurance time which is a standard of the sliding property of the sliding member can be measured using the above-mentioned thrust unidirectional rotation method.
[0360] Furthermore, generally, as a criterion for good sliding properties, the durability time of the sliding member is preferably 10 hours or more.
[0361] However, depending on the purpose, form, etc. of the sliding component, the durability time is more preferably 15 hours or more, and further preferably 20 hours or more.
[0362] 7. Characteristic 4 (wear amount)
[0363] In addition, the wear amount which is another reference|standard of the sliding property of a sliding member can be measured using the above-mentioned thrust one-way rotation method.
[0364] That is, the thrust unidirectional rotation method was performed for a predetermined time (20 hours), and the thickness change of the test piece composed of the sliding member from the initial value after the lapse of 20 hours was calculated as the wear amount.
[0365] Furthermore, generally, as a criterion for good sliding properties, the wear amount of the test piece is preferably 100 μm or less.
[0366] However, depending on the purpose, form, etc. of the sliding component, the wear amount of the test piece is more preferably 80 μm or less, and further preferably 50 μm or less.
[0367] If melting was observed on the test piece before 20 hours had passed, the test by the thrust unidirectional rotation method was terminated at that time, and the thickness change from the initial value of the test piece composed of the sliding member was calculated as the wear amount.
[0368] in addition, Figure 1 (c) is a diagram for explaining the relationship between the sintering temperature of carbon fibers (including carbon fibers for sliding and other carbon fibers) and the wear amount under predetermined conditions when processed into a sliding part including the carbon fibers.
[0369] Right now, Figure 1 The horizontal axis of (c) represents the calcination temperature (°C) of the carbon fibers, and the vertical axis represents the relationship between the wear loss (μm) under the above measurement conditions when a sliding resin composition prepared by mixing carbon fibers calcined at a predetermined temperature is processed into a sliding part.
[0370] Moreover, as described later, Figure 1 The data of the characteristic curve (c) are the wear amounts of Examples 1 to 3 and Comparative Examples 1 and 2, in which the types and amounts of the compounding components (a) to (d) are the same and only the sintering temperatures of the carbon fibers are different.
[0371] By Figure 1 From the characteristic curve (c), it can be seen that as the sintering temperature (°C) of the carbon fiber increases, the wear amount temporarily decreases and then tends to increase.
[0372] More specifically, when the sintering temperature (°C) of the carbon fiber is lower than 600°C, the wear loss becomes a value larger than 100 μm, but becomes 100 μm or less at 600°C, and becomes larger than 100 μm again at higher than 800°C.
[0373] Therefore, if we consider Figure 1 From the results of the characteristic curves shown in (a) to (c), it can be said that by adjusting the sintering temperature (°C) of the carbon fiber to a specified range (below 800°C, especially 600 to 800°C), when processed into sliding parts, the friction coefficient and wear amount as sliding properties can be kept below the specified values while maintaining the linear expansion coefficient low.
[0374] [Example]
[0375] Hereinafter, the present invention will be described in detail based on examples, but the scope of rights of the present invention will not be narrowed by the description of the examples unless there is a particular reason.
[0376] In addition, the resin as the compounding component (a), the carbon fiber for sliding as the compounding component (b), the inorganic material as the compounding component (c), and the lubricating additive as the compounding component (d) used in the examples are as follows.
[0377] (A) Compounding ingredients (a)
[0378] (A-1) Polyphenylene sulfide resin (PPS resin) (manufactured by Polyplastics Co., Ltd., trade name “DURAFIDE”, type of PPS resin: linear type)
[0379] (A-2) Polyetheretherketone resin (PEEK resin) (manufactured by Solvay Specialty Polymers Co., Ltd., trade name "KETASPIRE")
[0380] (A-3) Polyethersulfone resin (PES resin) (manufactured by Sumitomo Chemical Co., Ltd., trade name "SUMIKAEXCEL"
[0381] (B) Compounding ingredients (b)
[0382] (B-1) Isotropic pitch-based uncarbonized carbon fiber 1 (sintering temperature: 700° C., sintering time: 30 minutes, average diameter: 15 μm, average length: 200 μm, saturated moisture content: 5.8 wt %)
[0383] (B-2) Isotropic pitch-based uncarbonized carbon fibers 2 (sintering temperature: 650° C., sintering time: 30 minutes, average diameter: 15 μm, average length: 200 μm, saturated moisture content: 5.5 wt %)
[0384] (B-3) Isotropic pitch-based uncarbonized carbon fibers 3 (sintering temperature: 750° C., sintering time: 30 minutes, average diameter: 15 μm, average length: 200 μm, saturated moisture content: 6.5 wt %)
[0385] (B') corresponds to carbon fiber of compounding component (b)
[0386] (B′-1) Isotropic pitch-based carbon fiber 1 (sintering temperature: 450° C., sintering time: 30 minutes, average diameter: 15 μm, average length: 200 μm, saturated moisture content: 8.5 wt %)
[0387] (B′-2) Isotropic pitch-based carbon fiber 2 (sintering temperature: 1300° C., sintering time: 30 minutes, average diameter: 15 μm, average length: 200 μm, saturated moisture content: 0.5 wt %)
[0388] (C) Compounding ingredients (c)
[0389] (C-1) Talc (manufactured by Nippon Talc Co., Ltd., trade name "MS-P", average particle size: 14 μm)
[0390] (C-2) Mica (manufactured by Yamaguchi Mica Co., Ltd., trade name "J-31M", average particle size: 23 μm)
[0391] (D) Compounding ingredients (d)
[0392] (D-1) Polytetrafluoroethylene (PTFE) (manufactured by AGC Corporation, trade name “FLUON (registered trademark) PTFE”, average particle size: 5 μm)
[0393] (D-2) Perfluoroalkoxyalkane (PFA) (manufactured by Daikin Industries, Ltd., trade name “NEOFLON”, average particle size: 5 μm)
[0394] (D-3) Ethylene-tetrafluoroethylene copolymer (ETFE) (manufactured by AGC Corporation, trade name "FLUON (registered trademark) ETFE", average particle size: 5 μm)
[0395] [Example 1]
[0396] 1. Preparation of sliding resin composition and evaluation parts
[0397] (1) Preparation of sliding resin composition
[0398] In a predetermined container equipped with a stirrer, as shown in Table 1, with respect to 100 parts by weight of the PPS resin A-1 as the resin component of the compounding component (a), 100 parts by weight of B-1 as the sliding carbon fiber of the compounding component (b), 30 parts by weight of the inorganic material C-1 as the compounding component (c), and 30 parts by weight of D-1 as the lubricating additive of the compounding component (d) are weighed and accommodated.
[0399] As shown in Table 2, it was confirmed by TGA that TG5 was 450°C only for the carbon fiber for sliding of the blending component (b).
[0400] Furthermore, the amount of carbon on the surface of the sliding carbon fibers as the blended component (b) was separately confirmed to be 93% by weight by XPS elemental analysis.
[0401] Next, a 20-L mixer was used as a stirrer to stir the components (a) to (d) uniformly at a rotation speed of 400 rpm for 90 seconds to prepare a sliding resin composition.
[0402] Next, the obtained sliding resin composition was dried using a heating furnace heated to 130° C. in the air to prepare a sliding resin composition (in powder form) having a water content of 0.01% by weight or less.
[0403] Next, the obtained sliding resin composition (powdered form) was melt-kneaded using a twin-screw extruder to prepare a pelletized composition.
[0404] (2) Preparation of evaluation parts
[0405] After the obtained sliding resin composition (pellet form) is filled into a specified mold using an injection molding device, the evaluation component A is press-molded into a plate-shaped evaluation component A of 5 mm (lateral width) × 5 mm (vertical width) × 3 mm (thickness) and the evaluation component B is press-molded into a plate-shaped evaluation component B of 30 mm (lateral width) × 30 mm (vertical width) × 3 mm (thickness) under specified pressurizing conditions (e.g., 10 to 200 MPa).
[0406] The evaluation parts are substitute parts for evaluating various properties of sliding parts obtained by processing the sliding resin composition. Among the evaluation parts, evaluation part A is used in evaluation 6 (linear expansion coefficient) described later, and evaluation part B is used in evaluation 7 (friction coefficient), evaluation 8 (durability time) and evaluation 9 (wear amount) described later.
[0407] 2. Evaluation of sliding resin composition and sliding parts
[0408] (1) Evaluation 1 (firing temperature)
[0409] The calcination temperature of the carbon fibers was evaluated according to the following evaluation criteria. The results are shown in Table 2.
[0410] ◎: Temperature of 650 to 750°C.
[0411] 0: A temperature of 600 to less than 650°C or a temperature of more than 750 to 800°C.
[0412] △: A temperature of 500 to less than 600°C or a temperature of 800 to 1000°C.
[0413] ×: Temperature lower than 500°C or temperature higher than 1000°C.
[0414] (2) Evaluation 2 (tensile elastic modulus)
[0415] The tensile modulus of carbon fiber was measured in accordance with JIS R7606:2000 and evaluated according to the following evaluation criteria.
[0416] ◎:15~25GPa.
[0417] 0: less than 10-15 GPa or greater than 25-35 GPa.
[0418] △: less than 1~10GPa or greater than 35~50GPa.
[0419] ×: less than 1 GPa or greater than 50 GPa.
[0420] (3) Evaluation 3 (tensile elongation)
[0421] The tensile elongation of carbon fibers was measured in accordance with JIS R7606:2000 and evaluated according to the following evaluation criteria.
[0422] ◎:2.3~4%.
[0423] ○: less than 2-2.3% or greater than 4-5%.
[0424] △: 1.5 to less than 2% or greater than 5 to 6%.
[0425] ×: less than 1.5% or more than 6%.
[0426] (4) Evaluation 4 (Volume Resistivity)
[0427] The volume resistivity of the carbon fibers was measured by a four-terminal method using a digital voltmeter, and evaluated according to the following evaluation criteria.
[0428] ◎:5×10 0 ~1×10 3 Ω·cm.
[0429] 0:1×10 0 ~5×10 0 Ω·cm or greater than 1×10 3 ~1×10 4 Ω·cm.
[0430] △: 1×10 -1 ~1×10 0 Ω·cm or greater than 1×10 4 ~1×10 5 Ω·cm.
[0431] ×: less than 1×10 -1 Ω·cm or greater than 1×10 5 Ω·cm.
[0432] (5) Rating 5 (TG5)
[0433] The TG5 (5 wt% reduction temperature) of the carbon fiber was measured using TGA (manufactured by Mettler-Toledo, product name "TGA / SDTA 851e") at an air flow rate of 100 ml / min and a heating rate of 5°C / min, and the evaluation was performed according to the following evaluation criteria. The results are shown in Table 2.
[0434] ◎:430~500℃.
[0435] 0: 400 to less than 430°C or 500 to 550°C.
[0436] △: 350~less than 400℃ or 550~600℃.
[0437] ×: less than 350°C or more than 600°C.
[0438] (6) Evaluation 6 (Linear Expansion Coefficient)
[0439] The linear expansion coefficient of the resin molded product as the sliding part was measured using a thermomechanical analyzer (manufactured by Mettler-Toledo, product name "TMA / SDTA 841e") for evaluation member A, and evaluated according to the following evaluation criteria.
[0440] ◎:4.5×10 -5 / ℃ below.
[0441] 0: 5×10 -5 / ℃ below.
[0442] △: 1×10 -4 / ℃ below.
[0443] ×: greater than 1×10 -4 / ℃.
[0444] (7) Evaluation 7 (friction coefficient)
[0445] The friction coefficient, which is one of the criteria for the sliding properties of sliding parts, was measured using the thrust unidirectional rotation method described above under the above-described prescribed conditions in accordance with JIS K 7218:1986 using the evaluation part B as the object, and then evaluated according to the following evaluation criteria.
[0446] ◎: 0.05 or less.
[0447] 〇: 0.1 or less.
[0448] △: 0.4 or less.
[0449] ×: greater than 0.4.
[0450] (8) Rating 8 (Durability)
[0451] The durability time, which is one of the criteria for the sliding properties of sliding parts, was evaluated using the evaluation member B according to JIS K 7218:1986 using the thrust unidirectional rotation method described above and the following evaluation criteria.
[0452] ◎: No melting phenomenon was observed in 20 hours.
[0453] ○: No melting phenomenon was observed for more than 10 hours.
[0454] △: No melting phenomenon was observed for more than 1 hour.
[0455] ×: Melting phenomenon was observed in less than 1 hour.
[0456] (9) Evaluation 9 (wear loss)
[0457] The evaluation member B was used as an object, and the wear amount, which is one of the criteria for sliding properties of sliding members, was measured after 20 hours using the thrust unidirectional rotation method according to JIS K 7218:1986, and the wear amount was evaluated according to the following evaluation criteria.
[0458] If melting was observed in the evaluation member before 20 hours had passed, the test by the thrust unidirectional rotation method was terminated at that time, and the thickness change from the initial value of the evaluation member was calculated as the wear amount.
[0459] ◎: 50 μm or less.
[0460] 0: 80 μm or less.
[0461] △: 100 μm or less.
[0462] ×: larger than 100 μm.
[0463] [Examples 2-3]
[0464] In Examples 2 and 3, except that B-2 and B-3 were used as uncarbonized carbon fibers of the compounding component (b), a sliding resin composition and an evaluation member were prepared in the same manner as in Example 1, and each evaluation was performed. The evaluation results are shown in Tables 1 and 2.
[0465] As shown in Table 2, TG5 was separately confirmed to be 440° C. and 460° C. by TGA only for the uncarbonized carbon fibers of the blended component (b).
[0466] Furthermore, the carbon amounts on the surfaces of the uncarbonized carbon fibers of the blended component (b) were separately confirmed to be 90 wt % and 95 wt % by XPS elemental analysis.
[0467] [Examples 4 to 5]
[0468] In Examples 4 and 5, the amount of the uncarbonized carbon fiber of the compounding component (b) was changed to 50 parts by weight and 150 parts by weight, respectively, relative to 100 parts by weight of the resin component as the compounding component (a). In addition, the sliding resin composition and the evaluation component were prepared in the same manner as in Example 1, and each evaluation was performed. The evaluation results obtained are shown in Tables 1 and 2.
[0469] [Examples 6-7]
[0470] In Examples 6 and 7, except that the types of the resin components of the formulation component (a) were changed to A-2 and A-3, respectively, the sliding resin compositions and evaluation parts were prepared in the same manner as in Example 1, and each evaluation was performed. The evaluation results obtained are shown in Tables 1 and 2.
[0471] [Examples 8 to 9]
[0472] In Examples 8 and 9, except that the type of inorganic material of the blending component (c) was changed to C-2 and a mixture of C-1 / C-2 (mixing weight ratio: 80 / 20), the sliding resin composition and the evaluation member were prepared in the same manner as in Example 1, and each evaluation was performed. The obtained evaluation results are shown in Tables 1 and 2.
[0473] [Examples 10-11]
[0474] In Examples 10 and 11, the amount of the inorganic material of the formulation component (c) was changed to 60 parts by weight and 0 parts by weight, respectively, relative to 100 parts by weight of the resin component of the formulation component (a). The sliding resin composition and the evaluation member were prepared in the same manner as in Example 1, and each evaluation was performed. The evaluation results obtained are shown in Tables 1 and 2.
[0475] [Examples 12-13]
[0476] In Examples 12 and 13, the amount of the lubricating additive of the formulation component (d) was changed to 60 parts by weight and 0 parts by weight, respectively, relative to 100 parts by weight of the resin component of the formulation component (a). The sliding resin composition and the evaluation member were prepared in the same manner as in Example 1, and each evaluation was performed. The obtained evaluation results are shown in Tables 1 and 2.
[0477] [Examples 14-15]
[0478] In Examples 14 and 15, except that the type of lubricating additive was changed to D-2 or D-3 as the compounding component (d), the sliding resin composition and the evaluation member were prepared in the same manner as in Example 1, and each evaluation was performed. The obtained evaluation results are shown in Tables 1 and 2.
[0479] [Comparative Examples 1-2]
[0480] In Comparative Examples 1 and 2, except that the carbon fiber corresponding to the compounding component (b) was changed to B'-1 and B'-2, respectively, a sliding resin composition and a sliding part were prepared in the same manner as in Example 1, and each evaluation was performed. The obtained evaluation results are shown in Tables 1 and 2.
[0481] As shown in Table 2, only the carbon fibers corresponding to the blended component (b) were separately confirmed to have TG5 of 390° C. and 560° C. using TGA.
[0482] Furthermore, the amounts of carbon on the surface of the carbon fibers corresponding to the blended component (b) were separately confirmed to be 84% by weight and 97% by weight according to XPS elemental analysis.
[0483] [Comparative Examples 3-4]
[0484] In Comparative Examples 3 and 4, the amount of uncarbonized carbon fiber of the blending component (b) was changed to 5 parts by weight and 450 parts by weight, respectively, relative to 100 parts by weight of the resin component of the blending component (a). The sliding resin composition and the evaluation member were prepared in the same manner as in Example 1, and each evaluation was performed. The evaluation results obtained are shown in Tables 1 and 2.
[0485] [Table 1]
[0486]
[0487] [Table 2]
[0488]
[0489] [Industrial Availability]
[0490] As described above, when the resin component is combined with the sliding carbon fiber of the present invention and processed into a sliding part through the sliding resin composition, the friction coefficient and wear amount are reduced without damaging the mating parts, and a sliding part with excellent sliding properties can be provided.
[0491] In particular, the sliding resin composition prepared by blending the sliding carbon fiber or the like of the present invention contains a predetermined amount of a predetermined inorganic material, and when processed into a sliding part, a sliding part having excellent sliding properties or the like can be provided.
[0492] On the other hand, even when the sliding resin composition prepared by blending the sliding carbon fiber of the present invention does not substantially contain the prescribed inorganic material, when it is processed into a sliding part, although it also depends on the type of the counterpart material, etc., the friction coefficient becomes relatively low, and a sliding part with excellent sliding properties and durability can be provided.
[0493] Therefore, the carbon fiber for sliding of the present invention can be used in a wide range of fields as a mechanical part including the carbon fiber for sliding, such as a sliding part for a submersible pump having excellent low friction and wear resistance, through a resin composition for sliding containing the carbon fiber.
[0494] That is, it is expected to be widely used as a sliding part of a submersible pump for circulating cooling water, chemical liquid, solvent, oil, beverage, etc. for automobile engines, inverters, batteries or fuel cells, etc., circulating hot water for water heaters, floor heating equipment, etc., or other liquid pumps.
[0495] For example, in the case of bearings for submersible pumps, if there is sufficient water on the sliding surface, it will be close to a fluid lubrication state and good sliding properties can be obtained. However, in the early stage of pump operation, the bearing and the counterpart shaft will rub in a dry state, so good sliding properties are required even under dry conditions.
[0496] In this regard, the sliding bearing of the water pump in the prior art Patent Document 1 contains at least one of polytetrafluoroethylene resin and graphite as a lubricant, but it is not sufficient to obtain sliding properties. That is, if the proportion of the lubricant is increased in order to obtain good low friction properties under dry conditions, the strength of the bearing itself is reduced, which deteriorates the wear resistance.
[0497] On the other hand, if the blending ratio of carbon fibers is increased in order to improve wear resistance, low friction cannot be achieved, and problems such as damage to the counterpart material may occur.
[0498] However, in the case of a sliding part made from the sliding resin composition of the present invention, the above-mentioned problems peculiar to submersible pump bearings can be effectively suppressed even when the blending ratio of the carbon fibers is relatively increased.
[0499] Therefore, the sliding resin composition of the present invention and the sliding parts made from such a sliding resin composition are particularly suitable for use in bearings for submersible pumps among a wide range of uses.
Claims
1. A sliding carbon fiber for use in combination with a sliding resin composition to be made into a sliding part through a predetermined process, characterized in that: The 5% weight reduction temperature by thermogravimetric measurement is set to a value within the range of 400 to 550°C.
2. The sliding carbon fiber according to claim 1, characterized in that The tensile modulus measured in accordance with JIS R7606:2000 is a value within a range of 10 to 35 GPa.
3. The sliding carbon fiber according to claim 1 or 2, characterized in that: The tensile elongation measured in accordance with JIS R7606:2000 is a value within the range of 2 to 5%.
4. The sliding carbon fiber according to any one of claims 1 to 3, characterized in that The saturated water content measured in accordance with JIS K 7209:2000 is set to a value within the range of 1 to 8% by weight.
5. The sliding carbon fiber according to any one of claims 1 to 4, characterized in that The carbon content of the surface determined by XPS elemental analysis was within a range of 85 to 96% by weight relative to the total amount.
6. The sliding carbon fiber according to any one of claims 1 to 5, characterized in that The volume resistivity is 1×10 0 ~1×10 4 The value is within the range of Ω·cm.
7. The sliding carbon fiber according to any one of claims 1 to 6, characterized in that The resin component in the sliding resin composition is at least one selected from polyphenylene sulfide resin, polyethersulfone resin, polyetheretherketone resin, polyimide resin, polyamide resin, polyacetal resin, polytetrafluoroethylene resin, polyketone resin, thermosetting phenolic resin, epoxy resin, melamine resin, diallyl phthalate resin and unsaturated polyester resin.
8. A method for producing a sliding carbon fiber, which is a method for producing a sliding carbon fiber to be blended with a sliding resin composition, characterized in that: The method comprises the following steps (1) to (2): (1) A process for preparing raw material fibers of carbon fibers; (2) In a calcining step, the raw material fibers of the carbon fibers are calcined at a calcining temperature in the range of 600 to 800° C., and the 5 wt % reduction temperature of the obtained sliding carbon fibers based on thermogravimetric measurement is in the range of 400 to 550° C.
Citation Information
Patent Citations
Sliding member
JP1991237062A