Optical member, and AR glasses and head-mounted display using same

By introducing a porous layer and an adhesive layer into the optical waveguide, combined with concave and convex optical elements and an anti-reflective layer, the existing problems of heavy optical components and light leakage are solved, achieving thin, lightweight and highly transparent effects, which is suitable for AR glasses and HMD.

CN118742830APending Publication Date: 2024-10-01NITTO DENKO CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380021801.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-02-24
Filing Date
2023-02-27
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

The optical components in existing AR glasses and head-mounted displays have problems of being thick, dim, and leaking light, making it difficult to achieve thin, lightweight, and highly transparent results.

Method used

Adopting an optical waveguide structure with a porous layer and an adhesive layer, combined with concave and convex optical elements and an anti-reflection layer, the low refractive index of the porous layer and the elastic modulus of the adhesive layer achieve thinness, lightweight and high transparency. , using both a protective layer and a hard coating to enhance mechanical strength and protection.

Benefits of technology

A thin, lightweight, bright, and light-leak-suppressed optical component has been realized, which is suitable for AR glasses and HMDs. It significantly reduces thickness and weight while improving transparency and mechanical strength.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118742830A_ABST
    Figure CN118742830A_ABST
Patent Text Reader

Abstract

The invention provides an AR optical member which is thin, light, bright and capable of suppressing light leakage. An optical member according to an embodiment of the present invention comprises: an optical waveguide having a first main surface and a second main surface; an optical element provided on at least one of the first main surface and the second main surface of the optical waveguide, the optical element having an uneven structure; a porous layer that is provided at least on the main surface of the optical waveguide on which the optical element is provided; and an adhesive layer that is provided on the side of the porous layer opposite the optical waveguide and has a thickness of 3 [mu] m or more.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to an optical component and AR glasses and a head-mounted display using the optical component. Background Art

[0002] In recent years, the so-called AR (Augmented Reality) technology has attracted attention. Typically, AR "virtually enhances" the world in front of you by superimposing virtual visual information on the actual scenery. With the development of AR, the development of AR glasses and head-mounted displays (Head Mounted Display: HMD) for AR is underway. AR glasses and HMD typically use optical components including waveguides. However, such optical components are thick, heavy, dark, and prone to light leakage due to water or dirt, etc., leaving various research issues for practical application.

[0003] Prior art literature

[0004] Patent Literature

[0005] Patent Document 1: U.S. Patent Application Publication No. 2017 / 0131545

[0006] Patent Document 2: U.S. Patent Application Publication No. 2020 / 0379184 Summary of the invention

[0007] Problems to be solved by the invention

[0008] The present invention has been made to solve the above-mentioned conventional problems, and a main object of the present invention is to provide an optical member for AR which is thin, lightweight, bright, and has suppressed light leakage.

[0009] Solutions for solving problems

[0010] An optical component of an embodiment of the present invention comprises: an optical waveguide having a first principal surface and a second principal surface; an optical element, which is provided on at least one principal surface of the first principal surface and the second principal surface and has a concave-convex structure; a porous layer, which is provided on at least the principal surface of the optical waveguide on which the optical element is provided; and an adhesive layer, which is provided on the side of the porous layer opposite to the optical waveguide and has a thickness of 3 μm or more.

[0011] In one embodiment, the refractive index of the porous layer is 1.20 or less.

[0012] In one embodiment, the thickness of the porous layer is 5 μm or less.

[0013] In one embodiment, the porous layer has a haze of less than 5%.

[0014] In one embodiment, the storage elastic modulus of the adhesive layer is 0.2×10 5 (Pa) or above.

[0015] In one embodiment, the optical member further includes a protective layer composed of a resin film having a thickness of 20 μm or more on the outside of the pressure-sensitive adhesive layer.

[0016] In one embodiment, the Young's modulus of the protective layer is 2 GPa or more.

[0017] In one embodiment, the optical member further includes a hard coating layer on the outer side of the protective layer.

[0018] In one embodiment, the optical member further includes an antireflection layer on the outer side of the hard coat layer.

[0019] According to another aspect of the present invention, there is provided an AR pair of glasses, which includes the above-mentioned optical component.

[0020] According to another aspect of the present invention, a head-mounted display is provided, which includes the above-mentioned optical component.

[0021] Effects of the Invention

[0022] According to the embodiment of the present invention, it is possible to realize an optical member for AR that is thin, lightweight, bright, and has suppressed light leakage. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 This is a schematic cross-sectional view of an optical member according to one embodiment of the present invention.

[0024] Figure 2 This is a schematic cross-sectional view of an optical member according to another embodiment of the present invention.

[0025] Figure 3 This is a schematic cross-sectional view of an optical member according to still another embodiment of the present invention. DETAILED DESCRIPTION

[0026] The following will describe the embodiments of the present invention, but the present invention is not limited to these embodiments. It should be noted that, for ease of observation, the drawings are schematically shown, and the thickness, size, and thickness ratios of the components of the optical components in the drawings are different from the actual ones.

[0027] A. Overall composition of optical components

[0028] Figure 1It is a schematic cross-sectional view of an optical component according to an embodiment of the present invention. The optical component 100 shown in the figure has an optical waveguide 10, optical elements 20a and 20b, a porous layer 30 and an adhesive layer 40. The optical waveguide 10 has a first principal surface 10a and a second principal surface 10b. The optical elements 20a and 20b have concave-convex structures respectively (hereinafter, the optical elements 20a and 20b are sometimes referred to as concave-convex optical elements, respectively). The concave-convex optical element 20a typically functions as an incident optical element of the optical waveguide, and the concave-convex optical element 20b typically functions as an emitting optical element of the optical waveguide. The concave-convex optical elements 20a and 20b are provided on at least one principal surface of the first principal surface 10a and the second principal surface 10b of the optical waveguide 10. The concave-convex optical elements 20a and 20b may be provided on the same principal surface of the optical waveguide, or may be provided on principal surfaces different from each other. In the example shown in the figure, the concave-convex optical elements 20a and 20b are provided on the first principal surface 10a of the optical waveguide 10. The porous layer 30 is provided at least on the principal surface of the optical waveguide 10 on which the concave-convex optical elements 20a and 20b are provided (the first principal surface 10a in the example shown in the figure). The porous layer 30 is typically provided in a manner covering the concave-convex optical elements 20a and 20b, and in one embodiment, is provided on substantially the entire principal surface of the optical waveguide 10 on which the concave-convex optical elements 20a and 20b are provided (the first principal surface 10a in the example shown in the figure). The adhesive layer 40 is provided on the side of the porous layer 30 opposite to the optical waveguide 10 (i.e., the outer surface of the porous layer). The thickness of the adhesive layer is 3 μm or more. According to such a structure, a thin, lightweight, bright optical component for AR with suppressed light leakage can be realized.

[0029] As required, a protective layer 50, a hard coating layer 60 and / or an anti-reflection layer 70 may be provided on the outside of the adhesive layer 40 (on the side opposite to the porous layer 30). In the illustrated example, a protective layer 50, a hard coating layer 60 and an anti-reflection layer 70 are provided in sequence from the adhesive layer 40 side. Depending on the purpose and the desired configuration, at least one of the protective layer 50, the hard coating layer 60 and the anti-reflection layer 70 may be omitted. In the case where a protective layer, a hard coating layer and an anti-reflection layer are not provided, it is preferred that a release liner (not shown) is temporarily attached to the surface of the adhesive layer 40 until the optical member is provided for use. By temporarily attaching a release liner, a roll of an optical film can be formed while protecting the adhesive layer.

[0030] Figure 21 is a schematic cross-sectional view of an optical component according to another embodiment of the present invention. In the optical component 101 shown in the example, in addition to the main surface (the first main surface 10a in the example shown) of the optical waveguide 10 on which the concave-convex optical elements 20a and 20b are provided, a porous layer 30 and an adhesive layer 40 are also provided on the main surface (the second main surface 10b in the example shown) on which the concave-convex optical elements are not provided. In the example shown in the example shown, protective layers 50, 50, hard coating layers 60, 60 and anti-reflection layers 70, 70 are provided in order from the adhesive layer side on the outside of the adhesive layers 40, 40, but unlike Figure 1 Similarly, some or all of them may be omitted.

[0031] Figure 3 1 is a schematic cross-sectional view of an optical component according to another embodiment of the present invention. In the optical component 102 shown in the figure, in addition to the first principal surface 10a of the optical waveguide 10, a concave-convex optical element 20b is also provided on the second principal surface 10b. Figure 2 The implementation method is the same.

[0032] The total light transmittance of the optical component is preferably 60% or more and 99% or less, more preferably 70% or more and 98% or less, and further preferably 80% or more and 97% or less. In addition, the haze of the optical component is preferably 0.1% or more and 3% or less, more preferably 0.2% or more and 2.5% or less, and further preferably 0.3% or more and 2% or less. According to an embodiment of the present invention, excellent transparency can be achieved as an optical component as a whole. As a result, the optical component can be suitable for AR glasses and HMD (hereinafter, AR glasses and HMD are sometimes collectively referred to as "AR glasses, etc.").

[0033] The thickness of the optical component is preferably 0.35 mm to 4.8 mm, more preferably 0.55 mm to 3.8 mm, and even more preferably 0.75 mm to 2.8 mm. According to an embodiment of the present invention, the optical component can be formed without using a thick glass cover, so the thickness can be reduced to about one-fifth compared to the conventional optical component for AR glasses using a glass cover. As a result, the weight can also be reduced to about one-third. As a result, the optical component can be suitably used in AR glasses, etc. In this specification, the "thickness of the optical component" refers to the total thickness from the outermost layer on one side of the optical component to the outermost layer on the other side. For example, in Figure 1 In an embodiment of the present invention, the thickness of the optical member is the thickness from the outer surface of the antireflection layer to the second main surface of the optical waveguide; in addition, for example, Figure 2 and Figure 3 In an embodiment of the present invention, the thickness of the optical member is a thickness from an outer surface of one anti-reflection layer to an outer surface of another anti-reflection layer.

[0034] The above-mentioned embodiments can be appropriately combined or modified. Figure 1 and Figure 2 In the embodiment shown, either the concave-convex optical element 20a or 20b can be provided on the second main surface 10b of the optical waveguide; Figure 3 In the embodiment shown, the concave-convex optical element 20a can be provided on the second main surface 10b of the optical waveguide; Figure 1 to Figure 3 In the illustrated embodiment, the concavoconvex optical element 20a may be provided on both the first principal surface 10a and the second principal surface 10b of the optical waveguide.

[0035] Hereinafter, the components of the optical member will be described in detail.

[0036] B. Optical waveguide

[0037] The optical waveguide 10 is typically configured so that the light incident on the optical waveguide propagates in the optical waveguide by total reflection and is emitted in a specified direction at a specified position. As described above, the optical waveguide 10 has a first principal surface 10a and a second principal surface 10b. In the case where the optical component is used for AR glasses, etc., light from an image source (not shown) (representatively, the projection light of the image) is incident on the optical waveguide through an incident optical element (the concave-convex optical element 20a in the example shown in the figure) provided on the first principal surface and / or the second principal surface. The incident light propagates in the optical waveguide by total reflection, is emitted through an emitting optical element (the concave-convex optical element 20b in the example shown in the figure) provided on the first principal surface and / or the second principal surface, and is visually recognized by the user of the AR glasses, etc. By appropriately constructing the concave-convex optical elements 20a and 20b, the light from the image source is emitted while maintaining the image information. As a result, the image from the image source can be visually recognized by the user of the AR glasses, etc.

[0038] The optical waveguide may be made of glass or plastic. The refractive index of the optical waveguide is preferably 1.4 to 2.5, more preferably 1.6 to 2.4, and further preferably 2.0 to 2.3. If the refractive index is within such a range, good light incidence from the outside, good light emission to the outside, and good total reflection inside the optical waveguide can be achieved. The Abbe number of the optical waveguide is preferably greater than 10 and less than 80, more preferably greater than 15 and less than 70.

[0039] The thickness variation (TTV: total thickness variation) of the optical waveguide (first main surface and second main surface) is preferably 5 μm or less, more preferably 3 μm or less, and further preferably 1 μm or less. The smaller the thickness variation, the better, and it can be zero, for example. If the thickness variation of the optical waveguide is within such a range, the strain of the optical path in the optical waveguide can be reduced.

[0040] The surface roughness Ra of the optical waveguide (the first main surface and the second main surface) is preferably 10 nm or less, more preferably 5 nm or less, and further preferably 1 nm or less. If the surface roughness Ra is in such a range, the haze can be reduced. Such a surface roughness Ra can be achieved, for example, by grinding the first main surface and the second main surface of the optical waveguide. On the other hand, the surface roughness Ra can be, for example, 0.1 nm or more. It should be noted that Ra refers to the arithmetic mean roughness based on JIS B 0601.

[0041] The optical waveguide can be used alone or in a stack of two or more sheets (e.g., two, three, or four sheets). The thickness of the optical waveguide can be, for example, 0.3 mm to 4.0 mm. The thickness of the optical waveguide can be, for example, 0.3 mm to 1.3 mm, and can also be, for example, 0.4 mm to 1.2 mm, and can also be, for example, 0.5 mm to 1.1 mm. Alternatively, the thickness of the optical waveguide can be, for example, 1.3 mm to 2.0 mm, and can also be, for example, 1.4 mm to 1.9 mm, and can also be, for example, 1.5 mm to 1.8 mm. Alternatively, the thickness of the optical waveguide can be, for example, 2.0 mm to 4.0 mm, and can also be, for example, 2.2 mm to 3.8 mm, and can also be, for example, 2.4 mm to 3.6 mm.

[0042] C. Optical components

[0043] The concave-convex optical element 20a is configured to guide the light incident on the optical waveguide from the image source in the direction of the waveguide, and the concave-convex optical element 20b is configured to emit the light propagating in the optical waveguide in a direction that can be visually recognized. Hereinafter, the concave-convex optical elements 20a and 20b are sometimes collectively referred to as concave-convex optical elements. In the case where it is necessary to distinguish the concave-convex optical element 20a from the concave-convex optical element 20b, their respective figure marks are indicated. However, even in the case where the concave-convex optical elements 20a and 20b are unified as concave-convex optical elements, the concave-convex optical elements 20a and 20b may be respectively the same structure or may be different structures from each other.

[0044] As the concave-convex structure of the concave-convex optical element, any appropriate fine concave-convex shape that can exhibit light direction conversion functions such as light diffusion, light scattering, light reflection, and light diffraction can be adopted. As representative examples of concave-convex optical elements, diffraction gratings, holographic elements, and metasurfaces can be listed. The following is an example of a diffraction grating.

[0045] The diffraction grating is typically formed of a diffraction pattern of grooves or slits. The diffraction pattern can be appropriately set according to the purpose. The diffraction pattern can be a one-dimensional diffraction pattern that is striped when viewed from above, or a two-dimensional diffraction pattern that is lattice-shaped when viewed from above. The one-dimensional diffraction pattern is typically formed alternately with convex portions and slits extending in one direction respectively. The cross-sectional shape of the convex portion observed from the direction in which the convex portion extends can be a rectangle, a parallelogram (inclined type), or a trapezoid. The one-dimensional diffraction pattern can also have a concave-convex shape extending in one direction with a cross-sectional waveform. The direction in which the stripes of the one-dimensional diffraction pattern extend can be parallel to the waveguide direction of the light, or a direction orthogonal to the waveguide direction of the light, or an inclined direction at a specified angle relative to the waveguide direction of the light. The two-dimensional diffraction pattern can be provided with slits in a manner that forms a convex portion of a rectangle when viewed from above, or it can be provided with slits in a manner that forms a convex portion of a parallelogram when viewed from above. The above-mentioned diffraction patterns can also be appropriately combined. For example, two one-dimensional diffraction patterns having fringes extending in different directions (for example, the fringes extending in directions orthogonal to each other) may be combined, or three diffraction patterns of two such one-dimensional diffraction patterns and a two-dimensional diffraction pattern may be combined.

[0046] The pitch Λ of the concavoconvex is preferably 30nm to 700nm, more preferably 40nm to 600nm, and further preferably 50nm to 500nm. The width of the convex portion and the slit (concave portion) may be 1 / 2 of the pitch, or may not be 1 / 2 of the pitch (they may each have any appropriate width corresponding to the purpose). The height h of the concavoconvex is preferably 10nm to 800nm, more preferably 20nm to 700nm, further preferably 30nm to 600nm, and particularly preferably 40nm to 500nm.

[0047] The concave-convex optical element can be integrally formed with the optical waveguide or formed separately from the optical waveguide. In the case where the concave-convex optical element is integrally formed with the optical waveguide, the concave-convex optical element can be formed, for example, by cutting the optical waveguide. In addition, for example, it can also be formed by nanoimprinting in a plastic optical waveguide. In the case where the concave-convex optical element is formed separately from the optical waveguide, the concave-convex optical element can be representatively composed of a dielectric or a resin. Specific examples of dielectrics include aluminum oxide, titanium dioxide, and silicon. The refractive index of the dielectric is preferably 1.6 to 4.0, and more preferably 2.0 to 3.5. In the case where the concave-convex optical element is composed of a dielectric, the concave-convex optical element can be formed, for example, by sputtering. Specific examples of resins include thermosetting resins and UV curable resins. The refractive index of such a resin is preferably 1.5 to 1.9. In the case where the concave-convex optical element is composed of a resin, the concave-convex optical element can be formed, for example, by coating the resin on the optical waveguide and performing nanoimprinting. When the concave-convex optical element is a metasurface, the concave-convex optical element can be formed by the method described in the following document, for example: “Supplementary Section 2. Details of experiments” in the Supplementary Information of A broadband achromatic metalens in the visible (Nature Nanotechnology volume 13, pages 227-232 (2018)).

[0048] D. Porous layer

[0049] The porous layer 30 typically has voids inside. The porosity of the porous layer is preferably 35% by volume or more, more preferably 38% by volume or more, and particularly preferably 40% by volume or more. If the porosity is in such a range, a porous layer with a particularly low refractive index can be formed. The upper limit of the porosity of the low refractive index layer is, for example, 90% by volume or less, preferably 75% by volume or less. If the porosity is in such a range, a porous layer with excellent strength can be formed. The porosity is a value of the porosity calculated by Lorentz-Lorenz's formula based on the value of the refractive index measured by an ellipsometer.

[0050] The refractive index of the porous layer is preferably less than 1.20, more preferably less than 1.18, further preferably less than 1.16, and particularly preferably less than 1.14. On the other hand, the refractive index of the porous layer is preferably greater than 1.05, more preferably greater than 1.08, and further preferably greater than 1.10. By providing a porous layer having such a refractive index on the main surface of the optical waveguide provided with a concave-convex optical element, light leakage can be suppressed without substantially affecting the optical properties of the optical waveguide and the concave-convex optical element. Furthermore, as described later, the porous layer can be very thin, and thus can contribute to the thinning and lightening of the optical component (resulting in AR glasses). In addition, if the refractive index of the porous layer is in the above-mentioned range, the prescribed mechanical strength can be ensured and breakage can be suppressed. Unless otherwise specified, the refractive index refers to the refractive index measured at a wavelength of 550 nm. The refractive index is a value measured by the method described in "(1) Refractive index of porous layer" of the embodiment described later.

[0051] The total light transmittance of the porous layer is preferably 85% to 99%, more preferably 87% to 98%, and further preferably 89% to 97%. By providing a porous layer having such a refractive index on the main surface of the optical waveguide provided with the concave-convex optical element, it is possible to exhibit the effect of the above-mentioned refractive index while ensuring excellent transparency. As a result, the optical component can be suitably used in AR glasses and the like.

[0052] The haze of the porous layer is, for example, less than 5%, preferably less than 3%. On the other hand, the haze is, for example, 0.1% or more, preferably 0.2% or more. By providing a porous layer having such a haze on the main surface of the optical waveguide provided with the concave-convex optical element, the effect brought about by the above-mentioned refractive index can be exhibited, and excellent transparency can be ensured. As a result, the optical component can be suitably used in AR glasses, etc. The haze can be measured, for example, by the following method.

[0053] The void layer (porous layer) was cut into a size of 50 mm×50 mm and placed in a haze meter (HM-150 manufactured by Murakami Color Research Laboratory Co., Ltd.) to measure the haze. The haze value was calculated by the following formula.

[0054] Haze (%) = [diffuse transmittance (%) / total transmittance (%)] × 100 (%)

[0055] The thickness of the porous layer is preferably 5 μm or less, more preferably 4 μm or less, further preferably 3 μm or less, particularly preferably 2 μm or less, and particularly preferably 1.5 μm or less. On the other hand, the thickness of the porous layer is preferably 300 nm or more, more preferably 400 nm or more, and further preferably 500 nm or more. If the thickness of the porous layer is within such a range, excellent transparency can be ensured and light leakage can be well suppressed.

[0056] As long as the porous layer has the above-mentioned desired characteristics, any appropriate structure can be adopted. The porous layer can be preferably formed by coating or printing. As the material constituting the porous layer, for example, the materials described in International Publication No. 2004 / 113966, Japanese Patent Publication No. 2013-254183 and Japanese Patent Publication No. 2012-189802 can be used. As a representative example, silicon compounds can be cited. As silicon compounds, for example: silicon dioxide compounds; hydrolyzable silanes, and their partial hydrolyzates and dehydrated condensates; silicon compounds containing silanol groups; active silica obtained by contacting silicates with acids and ion exchange resins. Also listed are: organic polymers; polymerizable monomers (such as (meth) acrylic monomers and styrene monomers); curable resins (such as (meth) acrylic resins, fluorine-containing resins and urethane resins). These materials can be used alone or in combination. The porous layer can be formed by coating or printing a solution or dispersion of such a material.

[0057] The size of the void (pore) in the porous layer refers to the diameter of the long axis of the void (pore) and the diameter of the short axis. The size of the void (pore) is, for example, 2nm to 500nm. The size of the void (pore) is, for example, more than 2nm, preferably more than 5nm, more preferably more than 10nm, and further preferably more than 20nm. On the other hand, the size of the void (pore) is, for example, less than 500nm, preferably less than 200nm, and more preferably less than 100nm. The range of the size of the void (pore) is, for example, 2nm to 500nm, preferably 5nm to 500nm, more preferably 10nm to 200nm, and further preferably 20nm to 100nm. The size of the void (pore) can be adjusted to the desired size according to the purpose and use. The size of the void (pore) can be quantified by the BET test method.

[0058] The size of the voids (pores) can be quantified by the BET test method. Specifically, after 0.1 g of sample (formed void layer) is put into the capillary of the specific surface area measuring device (made by Micromeritics: ASAP 2020), it is dried under reduced pressure at room temperature for 24 hours to degas the gas in the void structure. Then, the adsorption isotherm is drawn by adsorbing nitrogen on the above sample to obtain the pore distribution. Thus, the void size can be evaluated.

[0059] Examples of the porous layer having voids therein include a porous layer and / or a porous layer having an air layer at least in a portion thereof. The porous layer typically includes aerogels and / or particles (e.g., hollow microparticles and / or porous particles). The porous layer may preferably be a nanoporous layer (specifically, a layer in which 90% or more of the micropores have a diameter of 10-1 nm~10 3 nm range).

[0060] As the above-mentioned particles, any appropriate particles can be used. The particles are typically composed of a silica-based compound. As the shape of the particles, for example, spherical, plate-like, needle-like, linear and grape-like shapes can be listed. As linear particles, for example, particles in which a plurality of particles having a spherical, plate-like or needle-like shape are connected to form a rosary, short-fiber particles (for example, short-fiber particles described in Japanese Patent Gazette No. 2001-188104), and combinations thereof can be listed. Linear particles can be straight-chain or branched. As grape-like particles, for example, particles in which a plurality of spherical, plate-like and needle-like particles are agglomerated to form grape-like particles can be listed. The shape of the particles can be confirmed, for example, by observation with a transmission electron microscope.

[0061] An example of a specific composition of the porous layer is described below. The porous layer of this embodiment is composed of one or more structural units that form a fine void structure, and the structural units are chemically bonded to each other via catalysis. As the shape of the structural unit, for example, there can be listed: particle-shaped, fibrous, rod-shaped, and flat-plate-shaped. The structural unit can have only one shape, or it can be combined to have more than two shapes. Below, the porous layer is mainly described as a void layer of a porous body in which the above-mentioned fine pore particles are chemically bonded to each other.

[0062] Such a void layer can be formed by chemically bonding, for example, microporous particles to each other in the void layer forming process. It should be noted that, in the embodiment of the present invention, the shape of the "particles" (such as the above-mentioned microporous particles) is not particularly limited, for example, it can be spherical or other shapes. In addition, in the embodiment of the present invention, the above-mentioned microporous particles can be, for example, sol-gel beaded particles, nanoparticles (hollow nano-silica / nanosphere particles), nanofibers, etc. The microporous particles typically include inorganic substances. As specific examples of inorganic substances, silicon (Si), magnesium (Mg), aluminum (Al), titanium (Ti), zinc (Zn), and zirconium (Zr) can be listed. They can be used alone or in combination of two or more. In one embodiment, the above-mentioned microporous particles are, for example, microporous particles of silicon compounds, and the above-mentioned porous body is, for example, an organosilicon porous body. The microporous particles of the above-mentioned silicon compound, for example, include a pulverized body of a gel-like silica compound. In addition, as other forms of porous layers and / or porous layers having an air layer in at least a portion, there are, for example, void layers composed of fibrous materials such as nanofibers, which are entangled with each other to form voids to form layers. The method for manufacturing such a void layer is not particularly limited, for example, it is the same as the case of the void layer of a porous body in which the above-mentioned microporous particles are chemically bonded to each other. As another scheme, void layers using hollow nanoparticles and nanoclays, and void layers formed using hollow nanospheres and magnesium fluoride can be listed. The void layer can be a void layer composed of a single constituent material, or it can be a void layer composed of multiple constituent materials. The void layer can be composed of a single above-mentioned method, or it can be composed of multiple above-mentioned methods.

[0063] In the present embodiment, the porous structure of the porous body can be, for example, a continuous bubble structure with a continuous pore structure. The continuous bubble structure refers to, for example, in the above-mentioned organosilicon porous body, the pore structure is three-dimensionally connected, and it can also be said that the internal voids of the pore structure are continuous. The porous body has a continuous bubble structure, which can increase the porosity. However, in the case of using single bubble particles (particles having pore structures respectively) such as hollow silica, a continuous bubble structure cannot be formed. On the other hand, for example, in the case of using silica sol particles (a crushed product of a gel-like silicon compound forming a sol), since the particles have a three-dimensional tree structure, the tree-like particles settle and accumulate in the coating film (a coating film of a sol containing a crushed product of a gel-like silicon compound), so that a continuous bubble structure can be easily formed. The porous layer more preferably has a monolithic structure in which the continuous bubble structure includes a plurality of pore distributions. The monolithic structure, for example, refers to a hierarchical structure of a continuous bubble structure composed of a structure containing fine voids of nanometer size and a collection of nanovoids. When a monolithic structure is formed, for example, the membrane strength can be imparted by fine voids, and the high porosity can be imparted by coarse interconnected voids, thereby achieving both membrane strength and high porosity. Such a monolithic structure can be preferably formed by controlling the pore distribution of the void structure generated in the gel (gel-like silicon compound) at the previous stage of pulverization into silica sol particles. In addition, for example, when pulverizing the gel-like silicon compound, the particle size distribution of the pulverized silica sol particles is controlled to a desired size to form a monolithic structure.

[0064] The porous layer contains, for example, a pulverized product of a gel-like compound as described above, and the pulverized products are chemically bonded to each other. The form of chemical bonding (chemical bonding) between the pulverized products in the porous layer is not particularly limited, and examples thereof include cross-linking, covalent bonding, and hydrogen bonding.

[0065] The volume average particle size of the above-mentioned pulverized material in the porous layer is, for example, 0.10 μm or more, preferably 0.20 μm or more, and more preferably 0.40 μm or more. On the other hand, the volume average particle size is, for example, 2.00 μm or less, preferably 1.50 μm or less, and more preferably 1.00 μm or less. The range of the volume average particle size is, for example, 0.10 μm to 2.00 μm, preferably 0.20 μm to 1.50 μm, and more preferably 0.40 μm to 1.00 μm. The particle size distribution can be measured, for example, by a particle size distribution evaluation device such as a dynamic light scattering method and a laser diffraction method, and an electron microscope such as a scanning electron microscope (SEM) and a transmission electron microscope (TEM). It should be noted that the volume average particle size is an indicator of the particle size deviation of the pulverized material.

[0066] The type of the gel-like compound is not particularly limited. Examples of the gel-like compound include gel-like silicon compounds.

[0067] In addition, in the porous layer (void layer), for example, the silicon atoms contained therein are preferably siloxane-bonded. As a specific example, the proportion of unbonded silicon atoms (i.e., residual silanol) among all silicon atoms contained in the void layer is, for example, less than 50%, preferably less than 30%, and more preferably less than 15%.

[0068] An example of a method for forming such a porous layer will be described below.

[0069] The method typically includes: a precursor forming step, forming a void structure as a precursor of a porous layer (void layer) on the optical waveguide; and a cross-linking reaction step, in which a cross-linking reaction occurs inside the precursor after the precursor forming step. The method also includes a liquid preparation step of preparing a liquid containing microporous particles (hereinafter sometimes referred to as "microporous particle-containing liquid" or simply "containing liquid"), and a drying step of drying the liquid. In the precursor forming step, the microporous particles in the dried body are chemically bonded to each other to form a precursor. The containing liquid is not particularly limited, and is, for example, a suspension containing microporous particles. It should be noted that the following mainly describes the case where the microporous particles are a pulverized product of a gel-like compound and the void layer is a porous body (preferably a silicone porous body) containing a pulverized product of a gel-like compound. However, the porous layer can also be formed in the same manner in the case where the microporous particles are other than a pulverized product of a gel-like compound.

[0070] According to the above method, for example, a porous layer (void layer) having a very low refractive index is formed. The reason for this is, for example, presumed as follows. However, this presumption does not limit the method for forming the porous layer.

[0071] The above-mentioned crushed material is obtained by crushing a gel-like silicon compound, so the three-dimensional structure of the gel-like silicon compound before crushing is in a state of being dispersed in the three-dimensional basic structure. Furthermore, in the above-mentioned method, the crushed material of the gel-like silicon compound is applied to a resin film to form a precursor of a porous structure based on the three-dimensional basic structure. That is, according to the above-mentioned method, a new porous structure (three-dimensional basic structure) based on the coating of the crushed material, which is different from the three-dimensional structure of the gel-like silicon compound, is formed. Therefore, in the finally obtained void layer, for example, a low refractive index that functions to the same extent as an air layer can be achieved. Furthermore, in the above-mentioned method, in order to chemically bond the crushed materials to each other, the three-dimensional basic structure is fixed. Therefore, the finally obtained void layer can maintain sufficient strength and flexibility despite being a structure with voids.

[0072] The specific structure and formation method of the porous layer are described in detail in, for example, International Publication No. 2019 / 151073. The description of this publication is incorporated herein by reference.

[0073] E. Adhesive layer

[0074] The adhesive layer 40 has a hardness such that the adhesive constituting the adhesive layer does not penetrate into the voids of the porous layer under normal conditions. Therefore, the storage elastic modulus of the adhesive layer at 23° C. is preferably 0.2×10 5 (Pa) or more, more preferably 0.4×10 5 (Pa) or more, more preferably 0.6×10 5 (Pa) or more, particularly preferably 0.8×10 5 (Pa) or more, particularly preferably 1.0×10 5 On the other hand, considering the durability of the adhesive layer, the storage elastic modulus of the adhesive layer at 23°C is preferably 5.0×10 7 (Pa) or less, more preferably 4.0×10 7 (Pa) or less, more preferably 3.0×10 7 (Pa) or less, particularly preferably 2.0×10 7 (Pa) or less, particularly preferably 1.0×10 7 (Pa) or less. In addition, for example, the storage elastic modulus of the adhesive layer at 23°C may be 1.0×10 6 (Pa) or less. Such an adhesive layer has a buffering function (shock absorption function) against external forces and has flexibility that can suppress damage to the porous layer. The storage elastic modulus is obtained by reading the value at 23°C when measuring at a temperature increase rate of 5°C / min in the range of -50°C to 150°C under a frequency of 1 Hz according to the method described in JIS K 7244-1 "Plastics - Test methods for dynamic mechanical properties".

[0075] As the adhesive constituting the adhesive layer, any appropriate adhesive can be used as long as it has the characteristics as described above. As the adhesive, an acrylic adhesive (acrylic adhesive composition) can be cited as a representative example. The acrylic adhesive composition typically contains a (meth)acrylic polymer as a main component (base polymer). In the solid content of the adhesive composition, the (meth)acrylic polymer can be contained in the adhesive composition in a ratio of, for example, 50% by weight or more, preferably 70% by weight or more, and more preferably 90% by weight or more. The (meth)acrylic polymer contains an alkyl (meth)acrylate as a main component in terms of monomer units. It should be noted that (meth)acrylate refers to acrylate and / or methacrylate. As the alkyl group of the alkyl (meth)acrylate, for example, a linear or branched alkyl group having 1 to 18 carbon atoms can be cited. The average number of carbon atoms of the alkyl group is preferably 3 to 9. As monomers constituting (meth)acrylic polymers, in addition to (meth)acrylic acid alkyl esters, comonomers such as carboxyl-containing monomers, hydroxyl-containing monomers, amide-containing monomers, aromatic ring-containing (meth)acrylates, and heterocyclic (meth)acrylates can also be listed. The comonomer is preferably a hydroxyl-containing monomer and / or a heterocyclic (meth)acrylate, and more preferably N-acryloylmorpholine. The acrylic adhesive composition may preferably contain a silane coupling agent and / or a crosslinking agent. As a silane coupling agent, for example, epoxy-containing silane coupling agents can be listed. As a crosslinking agent, for example, isocyanate crosslinking agents and peroxide crosslinking agents can be listed. The details of such an adhesive layer or acrylic adhesive composition are described, for example, in Japanese Patent No. 4140736, and the description of the patent gazette is cited as a reference in this specification.

[0076] As described above, the thickness of the adhesive layer is 3 μm or more, preferably 10 μm or more, more preferably 25 μm or more, further preferably 30 μm or more, and particularly preferably 40 μm or more. When the thickness of the adhesive layer is within such a range, the damage of the porous layer can be well suppressed. As a result, the optical properties of the optical waveguide and the concave-convex optical element can be well maintained, and light leakage can be well suppressed. When the thickness of the adhesive layer is 15 μm or more, the above-mentioned effect can be obtained, so there is no upper limit on the thickness. However, from the perspective of thinness, lightness and cost, the thickness of the adhesive layer can be, for example, 200 μm or less, and further, for example, 150 μm or less, and further, for example, 120 μm or less.

[0077] F. Protective layer

[0078] The thickness of the protective layer 50 is preferably 20 μm or more, more preferably 25 μm or more, and further preferably 30 μm or more. On the other hand, the thickness of the protective layer is preferably 200 μm or less, more preferably 150 μm or less, and further preferably 120 μm or less. When the thickness of the protective layer is within such a range, when the optical component is applied to AR glasses, etc., it is possible to impart excellent surface protection performance and suppress damage to the porous layer.

[0079] The Young's modulus of the protective layer 50 is preferably 2 GPa or more, more preferably 2.5 GPa or more, and further preferably 3 GPa or more. On the other hand, the Young's modulus of the protective layer is preferably 10 GPa or less, more preferably 9 GPa or less, and further preferably 8 GPa or less. When the Young's modulus of the protective layer is within such a range, when the optical component is applied to AR glasses, etc., it is possible to impart excellent surface protection performance and suppress damage to the porous layer.

[0080] The protective layer 50 is composed of any appropriate resin film. Examples of the material for forming the resin film include: (meth) acrylic resin; cellulose resins such as diacetyl cellulose and triacetyl cellulose; cycloolefin resins such as norbornene resins; olefin resins such as polypropylene; ester resins such as polyethylene terephthalate resins; polyamide resins; polycarbonate resins; and copolymer resins thereof. It should be noted that "(meth) acrylic resin" refers to acrylic resin and / or methacrylic resin.

[0081] The moisture permeability of the protective layer 50 is preferably 0.1 g / m 2 / 24hr~1000g / m 2 / 24hr, more preferably 0.5g / m 2 / 24hr~800g / m 2 / 24hr, more preferably 1g / m 2 / 24hr~500g / m 2 When the moisture permeability of the protective layer is within such a range, damage to the porous layer can be further suppressed.

[0082] G.Hard coating

[0083] The hard coating layer 60 preferably has a pencil hardness of H or more, more preferably 2H or more, and further preferably 3H or more. On the other hand, the pencil hardness of the hard coating layer is preferably 6H or less, more preferably 5H or less. When the pencil hardness of the hard coating layer is within such a range, when the optical component is applied to AR glasses, etc., it is possible to impart excellent surface protection performance and suppress damage to the porous layer. The pencil hardness can be measured based on the "pencil hardness test" of JIS K 5400.

[0084] The thickness of the hard coating layer may be, for example, 0.5 μm to 30 μm, 1 μm to 20 μm, or 2 μm to 15 μm. When the thickness of the hard coating layer is within such a range, when the optical component is applied to AR glasses, etc., excellent surface protection performance can be imparted and damage to the porous layer can be suppressed.

[0085] As long as the hard coat layer satisfies the above-mentioned characteristics, it can be composed of any appropriate material. The hard coat layer is, for example, a cured layer of a thermosetting resin or an ionizing radiation (e.g., visible light, ultraviolet light) curable resin. The hard coat layer can be, for example, a cured layer of a thermosetting resin or an ionizing radiation (e.g., visible light, ultraviolet light) curable resin. Ultraviolet curable resins are preferred. This is because the hard coat layer can be formed with simple operation and high efficiency. As specific examples of ultraviolet curable resins, polyester, (meth) acrylic, carbamate, amide, silicone, epoxy, and unsaturated polyester ultraviolet curable resins can be listed. (Meth) acrylic ultraviolet curable resins include carbamate (meth) acrylates, polyester (meth) acrylates, and epoxy (meth) acrylates. Ultraviolet curable resins can include ultraviolet curable monomers, oligomers, and polymers. As preferred ultraviolet curable resins, resin compositions containing monomer components or oligomer components of acrylics having preferably 2 or more, more preferably 3 to 6 ultraviolet polymerizable functional groups can be listed. Typically, a photopolymerization initiator is blended into the ultraviolet curable resin.

[0086] The hard coat layer can be formed by any appropriate method. The hard coat layer can be preferably formed by applying a hard coat layer-forming resin composition on the protective layer, drying the composition, and curing the dried coating film by irradiating ultraviolet rays.

[0087] The details of the hard coat layer are described in, for example, Japanese Patent Application Laid-Open No. 2011-237789 and Japanese Patent Application Laid-Open No. 2016-224443. The descriptions of these publications are incorporated herein by reference.

[0088] H. Anti-reflection layer

[0089] Any appropriate structure can be adopted as the structure of the antireflection layer 70. Representative structures of the antireflection layer include: (1) a single layer of a low refractive index layer having an optical film thickness of 120 nm to 140 nm and a refractive index of about 1.35 to 1.55; (2) a laminate having a medium refractive index layer, a high refractive index layer, and a low refractive index layer in order from the optical waveguide side; (3) a laminate having a plurality of layers of high refractive index layers and low refractive index layers alternately.

[0090] As materials that can form a low refractive index layer, for example, silicon oxide (SiO2) and magnesium fluoride (MgF2) can be listed. The refractive index of the low refractive index layer is typically about 1.35 to 1.55. As materials that can form a high refractive index layer, for example, titanium oxide (TiO2), niobium oxide (Nb2O3 or Nb2O5), tin-doped indium oxide (ITO), antimony-doped tin oxide (ATO), and ZrO2-TiO2 can be listed. The refractive index of the high refractive index layer is typically about 1.60 to 2.20. As materials that can form a medium refractive index layer, for example, titanium oxide (TiO2), a mixture of a material that can form a low refractive index layer and a material that can form a high refractive index layer (for example, a mixture of titanium oxide and silicon oxide) can be listed. The refractive index of the medium refractive index layer is typically about 1.50 to 1.85. The thickness of the low refractive index layer, the medium refractive index layer, and the high refractive index layer can be set in a manner to achieve an appropriate optical film thickness corresponding to the layer structure of the anti-reflection layer, the desired anti-reflection performance, etc.

[0091] The above-mentioned anti-reflection layer is typically formed by a dry process. As specific examples of the dry process, PVD (Physical Vapor Deposition) method and CVD (Chemical Vapor Deposition) method can be listed. As the PVD method, vacuum evaporation method, reactive evaporation method, ion beam assisted method, sputtering method, and ion plating method can be listed. As the CVD method, plasma CVD method can be listed. Sputtering method is preferred. This is because it can achieve more uniform film formation with less uneven film thickness.

[0092] The thickness of the antireflection layer is, for example, approximately 20 nm to 300 nm.

[0093] The anti-reflection layer 70 can be a cured layer of an ionizing radiation curable resin composition. The ionizing radiation curable resin composition contains an ionizing radiation curable resin. As ionizing radiation curable resins, representative examples include thermosetting resins, ultraviolet curable resins, light (visible light) curable resins, and electron beam curable resins. For example, as ionizing radiation curable resins, silicone resins, polyester resins, polyether resins, epoxy resins, urethane resins, alkyd resins, spiroacetal resins, polybutadiene resins, and polythiol polyene resins can be listed. In addition, for example, ionizing radiation curable resins can be curable compounds having acrylate groups and / or methacrylate groups that are cured by heat, light (ultraviolet rays, etc.) or electron beams, etc. As specific examples, oligomers or prepolymers such as acrylates and / or methacrylates of multifunctional compounds such as polyols can be listed. Ionizing radiation curable resins can be used alone or in combination of two or more. Depending on the purpose, the ionizing radiation curable resin composition may further contain a reactive diluent, an additive containing a fluorine element, hollow particles and / or solid particles. The anti-reflection layer of the present embodiment can be formed representatively by the following manufacturing method: coating an anti-reflection layer-forming coating liquid obtained by diluting the ionizing radiation curable resin composition with a diluent solvent; drying the coating film; and curing the dried coating film. The thickness of the anti-reflection layer of the present embodiment can be, for example, 0.1 μm to 50 μm, and can also be, for example, 0.3 μm to 40 μm, and can also be, for example, 0.5 μm to 30 μm, and can also be, for example, 1.0 μm to 20 μm, and can also be, for example, 2.0 μm to 10 μm.

[0094] Example

[0095] The present invention is specifically described below by way of examples, but the present invention is not limited to these examples. In addition, the measuring methods of various properties are as follows. In addition, unless otherwise specified, "%" and "part" in the examples are weight references.

[0096] (1) Refractive index of porous layer

[0097] After forming a porous layer on the optical waveguide, it was cut into a size of 50 mm × 50 mm and attached to the surface of a glass plate (thickness: 3 mm) via an adhesive layer. The central part of the back of the above-mentioned glass plate (about 20 mm in diameter) was painted with a black marker to prepare a sample that was not reflected on the back of the glass plate. The above-mentioned sample was placed in an ellipsometer (manufactured by JA Woollam Japan: VASE) and the refractive index was measured under the conditions of a wavelength of 550 nm and an incident angle of 50 to 80 degrees.

[0098] (2) Optical waveguide protection

[0099] (2-1) Pencil hardness

[0100] The measurement was conducted in accordance with the “pencil hardness test” of JIS K 5400 except that the load was 500 g.

[0101] (2-2) Image whitening

[0102] A predetermined image was incident and emitted through the optical members obtained in Examples and Comparative Examples, and the emitted image was visually observed. The observed image was compared with the emitted image from the optical waveguide alone of Reference Example 1, and evaluated according to the following criteria.

[0103] ○ (good): No whitening was observed.

[0104] × (bad): Whitening was observed.

[0105] (2-3) Surface pollution resistance

[0106] A 0.1 ml water droplet was dropped onto the surface of the optical member obtained in the example and the comparative example, and the output image was visually observed in the same manner as in (2-2), and evaluated based on the following criteria.

[0107] ○ (good): No disturbance of the image and no light leakage were observed.

[0108] × (poor): Disturbance of the image and / or light leakage were observed.

[0109] [Manufacturing Example 1] Preparation of a coating liquid for forming a porous layer

[0110] (1) Gelation of Silicon Compounds

[0111] 0.95 g of methyltrimethoxysilane (MTMS), which is a precursor of a silicon compound, was dissolved in 2.2 g of dimethyl sulfoxide (DMSO) to prepare a mixed solution A. 0.5 g of a 0.01 mol / L aqueous oxalic acid solution was added to the mixed solution A, and the mixture was stirred at room temperature for 30 minutes to hydrolyze MTMS, thereby generating a mixed solution B containing tri(hydroxy)methylsilane.

[0112] After adding 0.38 g of 28 wt % ammonia water and 0.2 g of pure water to 5.5 g of DMSO, the mixed solution B was further added and stirred at room temperature for 15 minutes to gel the tri(hydroxy)methylsilane, thereby obtaining a mixed solution C containing a gel-like silicon compound.

[0113] (2) Aging treatment

[0114] The mixed solution C containing the gel-like silicon compound prepared as described above was incubated at 40° C. for 20 hours for aging treatment.

[0115] (3) Crushing

[0116] Next, use a spatula to crush the gel-like silicon compound that has been aged as described above into particles with a size of several mm to several cm. Next, add 40 g of isopropyl alcohol (IPA) to the mixed solution C, stir gently, and let it stand at room temperature for 6 hours to decant the solvent and catalyst in the gel. By performing the same decantation treatment three times, the solvent is replaced to obtain a mixed solution D. Next, the gel-like silicon compound in the mixed solution D is subjected to a pulverization treatment (high-pressure medium-free pulverization). The pulverization treatment (high-pressure medium-free pulverization) is performed using a homogenizer (manufactured by SMT, trade name "UH-50"). After weighing 1.85 g of the gel-like compound and 1.15 g of IPA in the mixed solution D in a 5 cc threaded bottle, the mixture is pulverized at 50 W and 20 kHz for 2 minutes.

[0117] By this pulverization treatment, the gel-like silicon compound in the mixed solution D was pulverized, and the mixed solution D became a sol solution E of the pulverized product. The volume average particle size indicating the particle size deviation of the pulverized product contained in the sol solution E was confirmed by a dynamic light scattering type Nanotrac particle size analyzer (manufactured by Nikkiso Co., Ltd., UPA-EX 150 model), and the result was 0.50 to 0.70. Furthermore, 0.062 g of a 1.5 wt% MEK (methyl ethyl ketone) solution of a photobase generator (Wako Pure Chemical Industries, Ltd.: trade name WPBG266) and 0.036 g of a 5% MEK solution of bis(trimethoxysilyl)ethane were added to 0.75 g of the sol solution E at a ratio of the above solutions to obtain a coating solution for forming a porous layer.

[0118] [Manufacturing Example 2] Preparation of Adhesive Constituting Adhesive Layer

[0119] In a four-necked flask equipped with a stirring blade, a thermometer, a nitrogen inlet tube, and a condenser, 90.7 parts of butyl acrylate, 6 parts of N-acryloylmorpholine, 3 parts of acrylic acid, 0.3 parts of 2-hydroxybutyl acrylate, and 0.1 parts by weight of 2,2'-azobisisobutyronitrile as a polymerization initiator were added together with 100 g of ethyl acetate, and nitrogen was introduced while slowly stirring to replace the atmosphere with nitrogen. Then, the liquid temperature in the flask was maintained at about 55°C and a polymerization reaction was performed for 8 hours to prepare an acrylic polymer solution. With respect to 100 parts of the solid content of the obtained acrylic polymer solution, 0.2 parts of an isocyanate crosslinking agent (CORONATE L manufactured by Nippon Polyurethane Industries, Ltd., an adduct of trimethylolpropane and toluene diisocyanate), 0.3 parts of benzoyl peroxide (NYPER BMT manufactured by NOF Corporation), and 0.2 parts of γ-glycidoxypropylmethoxysilane (KBM-403 manufactured by Shin-Etsu Chemical Co., Ltd.) were added to prepare an acrylic adhesive solution. Next, the acrylic adhesive solution was applied to one side of a silicone-treated polyethylene terephthalate (PET) film (manufactured by Mitsubishi Chemical Polyester Film Co., Ltd., thickness: 38 μm) so that the adhesive layer after drying had a thickness of 20 μm, and dried at 150° C. for 3 minutes to form an adhesive layer. The storage elastic modulus of the obtained adhesive was 1.0×10 5 (Pa).

[0120] [Example 1]

[0121] An optical waveguide was taken out from a commercially available AR glasses (manufactured by Vuzix, product name "M 4000"). The thickness of the optical waveguide was 1.05 mm. Furthermore, a diffraction grating (concave-convex optical element) was formed on the optical waveguide. The coating liquid for forming a porous layer prepared in Manufacturing Example 1 was applied to both sides of the optical waveguide. The coated film was treated at a temperature of 100°C for 1 minute and dried to form a porous layer (thickness 1.2 μm). The obtained porous layer had a porosity of 60% by volume and a refractive index of 1.18. Next, the adhesive layer (thickness 10 μm, storage elastic modulus 1.3×10 5 Pa). Furthermore, a PET film (manufactured by Mitsubishi Chemical Polyester Film Co., Ltd., thickness 50 μm, elastic modulus 4.0 GPa) was laminated as a protective layer on the surface of each adhesive layer. In this way, an optical component was produced. The obtained optical component was subjected to the above evaluation. The results are shown in Table 1.

[0122] [Example 2]

[0123] Optical members were prepared in the same manner as in Example 1 except that triacetylcellulose (TAC) films (thickness 80 μm, elastic modulus 3.0 GPa) were used as the protective layers instead of the PET films. The obtained optical members were evaluated in the same manner as in Example 1. The results are shown in Table 1.

[0124] [Comparative Example 1]

[0125] An optical member was produced in the same manner as in Example 1 except that the pressure-sensitive adhesive layer and the protective layer were not formed. The obtained optical member was subjected to the same evaluation as in Example 1. The results are shown in Table 1.

[0126] [Comparative Example 2]

[0127] An optical member was produced in the same manner as in Example 1 except that the porous layer was not formed. The obtained optical member was subjected to the same evaluation as in Example 1. The results are shown in Table 1.

[0128] [Reference Example 1]

[0129] The optical waveguide itself was used as an optical member and subjected to the same evaluation as in Example 1. Table 1 shows the results.

[0130] [Examples 3 to 7]

[0131] An optical member was produced in the same manner as in Example 1 except that the thickness of the pressure-sensitive adhesive layer, the thickness of the protective layer, and the Young's modulus of the protective layer were changed as shown in Table 1. The obtained optical member was subjected to the same evaluation as in Example 1. The results are shown in Table 1.

[0132] [Table 1]

[0133]

[0134] As can be seen from Table 1, according to the embodiment of the present invention, an optical component capable of realizing an output image with suppressed surface contamination, whitening and light leakage can be obtained. Furthermore, the total thickness of the optical component of the embodiment is about 1.2 mm, achieving significant thinning (resulting in significant weight reduction).

[0135] Possibility of Industrial Application

[0136] The optical member according to the embodiment of the present invention can be suitably used for AR glasses and HMD.

[0137] Description of Reference Numerals

[0138] 10: optical waveguide; 10a: first main surface; 10b: second main surface; 20a: concave-convex optical element; 20b: concave-convex optical element; 30: porous layer; 40: adhesive layer; 50: protective layer; 60: hard coating layer; 70: antireflection layer; 100: optical component; 101: optical component; 102: optical component.

Claims

1. An optical component comprising: An optical waveguide having a first main surface and a second main surface; an optical element, provided on at least one of the first main surface and the second main surface, the optical element having a concave-convex structure; a porous layer provided at least on a main surface of the optical waveguide on which the optical element is provided; as well as The adhesive layer is provided on the side of the porous layer opposite to the optical waveguide, and the thickness of the adhesive layer is 3 μm or more.

2. The optical component according to claim 1, in, The refractive index of the porous layer is 1.20 or less.

3. The optical component according to claim 1 or 2, in, The porous layer has a thickness of 5 μm or less.

4. The optical component according to any one of claims 1 to 3, in, The porous layer has a haze of less than 5%.

5. The optical component according to any one of claims 1 to 4, in, The storage elastic modulus of the adhesive layer is 0.2×10 5 Pa or above.

6. The optical component according to any one of claims 1 to 5, in, A protective layer composed of a resin film having a thickness of 20 μm or more is further provided on the outer side of the adhesive layer.

7. The optical component according to claim 6, in, The Young's modulus of the protective layer is greater than or equal to 2 GPa.

8. The optical component according to claim 6 or 7, in, A hard coating layer is further provided on the outer side of the protective layer.

9. The optical component according to claim 8, in, An antireflection layer is further provided on the outer side of the hard coat layer. 10 . AR glasses comprising the optical component according to claim 1 . 11 . A head-mounted display comprising the optical member according to claim 1 .