Optical functional film, optical laminate, molded body, method for manufacturing optical member, optical member, virtual reality display device,
By using an optically functional film composed of polymeric liquid crystal compounds, which is shaped into a curved surface and then cured, the problems of phase difference variation and light leakage in virtual reality display devices are solved, and a pancake lens structure with high image quality and wide field of view is realized.
Patent Information
- Application Number
- CN202380033321.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-10-05
- Filing Date
- 2023-04-13
- Publication Date
- 2024-11-19
Smart Images

Figure CN118984958A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to an optical functional film, an optical laminate, a molded body, a method for manufacturing an optical component, an optical component, a virtual reality display device, an optical film, and a molding method. Background Art
[0002] A virtual reality display device is a display device that allows users to wear a dedicated headset on their head and visually recognize images displayed through a composite lens, thereby providing a sense of presence as if they have entered a virtual world.
[0003] A virtual reality display device generally includes an image display panel and a Fresnel lens. However, since the distance between the image display panel and the Fresnel lens is large, there is a problem that the headset becomes thicker and the wearability is poor.
[0004] Therefore, as described in Patent Documents 1 and 2, a lens structure of a composite lens called a Pancake Lens is proposed, which has an image display panel, a reflective polarizer and a half-reflective mirror. The overall thickness of the headset is reduced by allowing the light emitted from the image display panel to reciprocate between the reflective polarizer and the half-reflective mirror.
[0005] Here, the reflective polarizer is a polarizer having the function of reflecting one polarized light in the incident light and transmitting the other polarized light. The reflected light and the transmitted light generated by the reflective polarizer are in polarization states orthogonal to each other. Here, the polarization states orthogonal to each other refer to polarization states located at opposite diameters on the Poincaré sphere, for example, linear polarized light, right-handed circularly polarized light, and left-handed circularly polarized light orthogonal to each other correspond thereto.
[0006] As a reflective linear polarizer that converts transmitted light and reflected light into linearly polarized light, for example, a film obtained by stretching a dielectric multilayer film and a wire grid polarizer are known. Also, as a reflective circular polarizer that converts transmitted light and reflected light into circularly polarized light, for example, a cholesteric liquid crystal layer having a light reflecting layer in which a cholesteric liquid crystal phase is fixed is known.
[0007] Previous technical literature
[0008] Patent Literature
[0009] Patent Document 1: Japanese Patent Application No. 2020-519964
[0010] Patent Document 2: U.S. Patent 10394040B2 Summary of the invention
[0011] Technical issues to be solved by the invention
[0012] Patent Document 1 discloses a method of bonding an optical layered body to a spherical or aspherical curved surface of an optical lens in order to obtain a wide field of view, low chromatic aberration, low distortion, and excellent MTF (Modulation Transfer Function).
[0013] However, there is a problem that in order to bond an optical laminate including an optical anisotropic layer to a curved surface, the optical laminate needs to be formed into a three-dimensional shape including a curved surface, and at this time, the optical anisotropic layer is stretched, so that a phase difference appears in the optical anisotropic layer or the phase difference of the optical anisotropic layer changes. In addition, when the optical laminate is formed into a three-dimensional shape including a curved surface, there is also a problem that the amount of phase difference or the amount of change varies depending on the part because the optical laminate is stretched at different stretching ratios depending on the part.
[0014] When the optically anisotropic layer is a retardation layer such as a λ / 4 retardation layer, an undesirable retardation may occur, resulting in an undesirable retardation of the optically anisotropic layer. Furthermore, the orientation of the optical axis of the optically anisotropic layer may become undesirable.
[0015] Furthermore, even if the optically anisotropic layer is a layer that does not normally have a phase difference, such as a cholesteric liquid crystal layer, the optically anisotropic layer is stretched, which may cause a new phase difference. When a phase difference occurs in the cholesteric liquid crystal layer, the reflected polarized light may become elliptically polarized light instead of the expected circularly polarized light.
[0016] According to the research conducted by the present inventors, it is known that the occurrence and change of such undesirable phase difference disturbs the polarization of light emitted from the image display device in the pancake lens, thereby causing part of the light to leak, resulting in ghosting and reduced contrast.
[0017] Furthermore, Patent Document 1 discloses a composite lens of a pancake lens structure, which uses a reflective linear polarizer as a reflective polarizer and includes an image display panel, a reflective linear polarizer, and a half mirror in sequence. When the image display panel, the reflective polarizer, and the half mirror are included in sequence, the reflective polarizer needs to have a concave mirror effect for light incident from the half mirror side. In order to make the reflective linear polarizer have a concave mirror effect, a structure in which the reflective linear polarizer is formed into a curved shape is proposed.
[0018] In addition, Patent Document 2 discloses a composite lens of a pancake lens structure, which uses a reflective linear polarizer as a reflective polarizer and includes an image display panel, a half mirror, and a reflective linear polarizer in sequence. Patent Document 2 proposes a structure in which both the half mirror and the reflective polarizer are curved to improve the image curvature. In this case, the reflective polarizer needs to function as a convex mirror.
[0019] According to the research conducted by the inventors, it was found that when the reflective linear polarizer is formed into a curved shape, the phase difference of the phase difference film for converting circularly polarized light and linearly polarized light disposed between the reflective polarizer and the half mirror changes, and the incident light cannot be properly reflected or transmitted, resulting in increased light leakage. When the light leakage increases, double images are visually recognized.
[0020] The first embodiment of the present invention is completed in view of the above-mentioned facts. The problem to be solved by the first embodiment of the present invention is to provide an optical functional film that suppresses the occurrence of phase difference and the change of phase difference when formed into a three-dimensional shape including a curved surface, for example, when applied to a pancake lens type virtual reality display device, it can reduce light leakage. In addition, the problem to be solved by the first embodiment of the present invention is to provide an optical laminate, a molded body, a method for manufacturing an optical component, an optical component, and a virtual reality display device.
[0021] The second embodiment of the present invention has been made in view of the above-mentioned problems, and the problem to be solved by the second embodiment of the present invention is to provide an optical film that suppresses light leakage when applied to a pancake-type virtual reality display device.
[0022] Furthermore, a second embodiment of the present invention is also directed to providing a method for forming the optical film.
[0023] Means for solving technical problems
[0024] The present inventors have conducted intensive studies on the above-mentioned problems and have found that the above-mentioned problems can be solved by the following structure.
[0025] [1] An optically functional film, which is formed from a composition containing at least a liquid crystal compound having a polymerizable group, wherein:
[0026] The polymerization rate of the liquid crystal compound is 40% or less.
[0027] [2] The optically functional film according to [1], wherein
[0028] The liquid crystal compound is aligned in one direction.
[0029] [3] The optically functional film according to [1], wherein
[0030] The liquid crystal compound is helically oriented.
[0031] [4] An optical layered body comprising:
[0032] The optically functional film according to any one of [1] to [3]; and
[0033] A base film composed of a resin having a tan δ peak temperature of 170° C. or less.
[0034] [5] A molded body, wherein the optically functional film according to any one of [1] to [3], or an optically functional laminate having the optically functional film according to any one of [1] to [3] and a substrate film, is molded into a three-dimensional shape including a curved surface.
[0035] [6] A method for manufacturing an optical component, comprising:
[0036] The curing step is to subject the molded body described in [5] to at least one curing treatment selected from the group consisting of a heat treatment and ultraviolet irradiation, wherein the polymerization rate of the liquid crystal compound of the optical functional film becomes 50% or more through the curing treatment.
[0037] [7] The method for manufacturing an optical component according to [6], further comprising:
[0038] The alignment step is to heat the molded body to align the liquid crystal compound before the curing step.
[0039] [8] An optical component manufactured by the method for manufacturing an optical component described in [6] or [7].
[0040] [9] A virtual reality display device, comprising:
[0041] An image display device emitting polarized light; and
[0042] The optical component described in [8].
[0043] As a result of intensive research, the inventors found that a thin virtual reality display device with a pancake lens structure that can reduce light leakage can be realized by using an optical film with a non-planar shape, a curvature radius of 30 to 1000 mm, and an in-plane deviation of phase difference of less than 5%.
[0044] That is, it was found that the above-mentioned problems can be solved by the following configuration.
[0045]
[10] An optical film having a non-planar shape, a radius of curvature of 30 mm to 1000 mm, and an in-plane deviation of phase difference of less than 5%.
[0046]
[11] The optical film according to
[10] , wherein:
[0047] The radius of curvature is 30mm to 100mm.
[0048]
[12] The optical film according to
[10] or
[11] , wherein:
[0049] The in-plane deviation of the phase difference is less than 3%.
[0050]
[13] The optical film according to any one of
[10] to
[12] , wherein:
[0051] The in-plane deviation of the film thickness is less than 5%.
[0052]
[14] The optical film according to any one of
[10] to
[13] , wherein
[0053] The optical film is a phase difference film.
[0054]
[15] The optical film according to any one of
[10] to
[14] , wherein
[0055] The optical film is a phase difference film having an in-plane retardation in the range of 120 nm to 160 nm at a wavelength of 550 nm.
[0056]
[16] The optical film according to any one of
[10] to
[13] , wherein
[0057] The optical film is a laminated optical body including a phase difference film and a reflective polarizer.
[0058]
[17] A method for forming an optical film, comprising:
[0059] A step of heating an optical film having a planar shape;
[0060] A first forming step of pressing the optical film onto a first mold and deforming the optical film along the shape of the first mold; and
[0061] In the second molding step, the optical film obtained in the first molding step is pressed against a second mold to be deformed along the shape of the second mold.
[0062]
[18] The method for forming an optical film according to
[17] , wherein:
[0063] The shape of the first mold includes a convex curved surface portion, and the shape of the second mold includes a concave curved surface portion.
[0064]
[19] The method for forming an optical film according to
[17] or
[18] , wherein:
[0065] The radius of curvature of the first mold is greater than the radius of curvature of the second mold.
[0066]
[20] A method for forming an optical film, comprising:
[0067] A step of heating an optical film having a planar shape;
[0068] A step of pressing the optical film onto the mold and deforming the optical film along the shape of the mold; and
[0069] The process of cutting the deformed optical film.
[0070] The heating step is a step of heating the optical film by irradiating infrared rays.
[0071] The amount of infrared radiation has a distribution within the surface of the optical film.
[0072]
[21] The method for forming an optical film according to
[20] , wherein:
[0073] The mold is substantially a concave spherical shape. When the position of the optical film in the surface is projected onto the mold from the normal direction of the surface of the optical film,
[0074] The amount of infrared light irradiated onto the optical film located at the vertex of the concave spherical shape is smaller than the amount of infrared light irradiated onto the optical film located at the end of the concave spherical shape.
[0075]
[22] The method for forming an optical film according to
[20] or
[21] , wherein:
[0076] The mold is substantially a concave spherical shape. When the position of the optical film in the surface is projected onto the mold from the normal direction of the surface of the optical film,
[0077] The temperature of the optical film located at the vertex of the concave spherical shape is lower than the temperature of the optical film located at the end of the concave spherical shape.
[0078]
[23] A method for forming an optical film, which is a method for forming an optical film having a planar shape into a non-planar shape, wherein:
[0079] The in-plane deviation of the product of the stretch ratio in the radial direction and the stretch ratio in the circumferential direction is less than 5%.
[0080]
[24] The method for forming an optical film according to
[23] , wherein:
[0081] The in-plane deviation of the product of the stretch ratio in the radial direction and the stretch ratio in the circumferential direction is less than 3%.
[0082]
[25] The method for forming an optical film according to
[23] or
[24] , wherein:
[0083] The radial stretching ratio increases as it moves away from the center.
[0084] Effects of the Invention
[0085] According to the first embodiment of the present invention, an optical functional film can be provided, which suppresses the occurrence of phase difference and the change of phase difference when formed into a three-dimensional shape including a curved surface, for example, when applied to a pancake lens type virtual reality display device, it can reduce light leakage. In addition, according to the first embodiment of the present invention, an optical laminate, a molded body, a method for manufacturing an optical component, an optical component and a virtual reality display device can be provided.
[0086] According to the second embodiment of the present invention, it is possible to provide an optical film that can suppress the occurrence of light leakage when applied to a pancake-type virtual reality display device.
[0087] Furthermore, according to the second embodiment of the present invention, it is possible to provide a method for forming the optical film. BRIEF DESCRIPTION OF THE DRAWINGS
[0088] Figure 1 This is a schematic diagram showing an example of a virtual reality display device according to the first embodiment.
[0089] Figure 2 This is a schematic diagram showing another example of the virtual reality display device according to the first embodiment.
[0090] Figure 3 This is an example of a virtual reality display device using the stacked optical body according to the second embodiment of the present invention, and shows an example of light rays of a main image.
[0091] Figure 4 This is an example of a virtual reality display device using the laminated optical body according to the second embodiment of the present invention, and shows an example of double light.
[0092] Figure 5 This is a schematic diagram showing an example of a laminated optical body according to a second embodiment of the present invention.
[0093] Figure 6 This is a schematic diagram showing an example of a reflective circular polarizer according to a second embodiment of the present invention.
[0094] Figure 7 This is a schematic diagram showing an example of a laminated optical body according to a second embodiment of the present invention.
[0095] Figure 8 This is an example of a pattern drawn on the optical film in order to confirm the stretching ratios in the radial direction and the circumferential direction in the molding method according to the second embodiment of the present invention.
[0096] Fig. 9 This is a diagram for explaining the procedure for forming a film using a forming mold having a concave forming surface.
[0097] Fig.10 This is a diagram for explaining the procedure for forming a film using a forming mold having a concave forming surface.
[0098] Fig.11 is a top view of the membrane used in forming.
[0099] Fig.12 This is a diagram for explaining the procedure for forming a film using a forming mold having a convex forming surface.
[0100] Fig.13 This is a diagram for explaining the procedure for forming a film using a forming mold having a convex forming surface.
[0101] Fig.14 This is a diagram for explaining forming method 1.
[0102] Fig.15 This is a diagram for explaining forming method 1.
[0103] Fig.16 This is a diagram for explaining forming method 1.
[0104] Fig.17 This is a diagram for explaining forming method 2.
[0105] Fig.18 is a top view of a planar-shaped optical film used in Forming Method 2. DETAILED DESCRIPTION
[0106] Hereinafter, the present invention will be described in detail.
[0107] The description of the constituent elements described below is made based on representative embodiments of the present invention, but the present invention is not limited to these embodiments.
[0108] In addition, in this specification, the numerical range expressed using "to" means a range including the numerical values described before and after "to" as the lower limit and the upper limit.
[0109] Furthermore, in this specification, the liquid crystal composition and the liquid crystal compound are concepts that also include substances that no longer exhibit liquid crystallinity due to curing or the like.
[0110] Hereinafter, the present invention will be described in detail with reference to the accompanying drawings. The description of the constituent elements described below is sometimes completed based on representative embodiments and specific examples, but the present invention is not limited to such embodiments. In addition, in this specification, the numerical range represented by "to" refers to the range including the numerical values described before and after "to" as the lower limit and upper limit.
[0111] In this specification, "orthogonal" is set to mean 90°±10° (preferably 90°±5°), not 90° in a strict sense. Also, "parallel" is set to mean 0°±10° (preferably 0°±5°), not 0° in a strict sense. Furthermore, "45°" is set to mean 45°±10° (preferably 45°±5°), not 45° in a strict sense.
[0112] In this specification, the "absorption axis" refers to the polarization direction in which the absorbance in the plane becomes the maximum when incident linear polarized light. In addition, the "reflection axis" refers to the polarization direction in which the reflectivity in the plane becomes the maximum when incident linear polarized light. In addition, the "transmission axis" refers to the direction in the plane that is orthogonal to the absorption axis or the reflection axis. Furthermore, the "slow axis" refers to the direction in which the refractive index in the plane becomes the maximum.
[0113] In this specification, unless otherwise specified, phase difference refers to in-plane retardation and is recorded as Re(λ). Here, Re(λ) represents in-plane retardation at a wavelength λ, and unless otherwise specified, the wavelength λ is 550 nm.
[0114] In addition, the retardation in the thickness direction at the wavelength λ is described as Rth(λ) in this specification.
[0115] Re(λ) and Rth(λ) can use values measured at wavelength λ by AxoScan OPMF-1 (manufactured by OPTO SCIENCE, INC.) The following is calculated by inputting the average refractive index ((nx+ny+nz) / 3) and the film thickness (d (μm)) into AxoScan.
[0116] Slow axis direction (°)
[0117] Re(λ)=R0(λ)
[0118] Rth(λ)=((nx+ny) / 2-nz)×d.
[0119] In this specification, the polymerization rate of a liquid crystal compound having a polymerizable group refers to the ratio of the number of polymerizable groups that contribute to the polymerization reaction in a polymerization reaction in which the liquid crystal compound having a polymerizable group is polymerized by irradiation with active energy rays and / or heating. That is, (polymerization rate (%) = {the number of polymerizable groups that disappear due to the polymerization reaction / the number of polymerizable groups before the polymerization reaction} × 100).
[0120] Specifically, the polymerization rate of the liquid crystal compound having a polymerizable group can be obtained by measuring the ratio of the absorbance of the infrared absorption peak of the polymerizable group before and after the polymerization reaction. For example, when the polymerizable group is a methacrylate monomer, it is preferred that the ratio of the absorbance of the infrared absorption peak of the polymerizable group before and after the polymerization reaction be 810 cm-1 of the infrared absorption spectrum of the film or the like containing the polymerizable compound. -1 The absorption peak based on the polymerizable group (acryloyloxy or methacryloyloxy) is observed near the 986 cm-1 of the infrared absorption spectrum of the film or the like containing the polymerizable compound, and the above polymerization rate is calculated based on the absorbance of the observed absorption peak. -1An absorption peak based on the polymerizable group (oxetane group) is observed near 750 cm-1, and the above polymerization rate is calculated using the absorbance of the observed absorption peak. When the polymerizable compound is an epoxy compound, it is preferred that the polymerizable compound be able to absorb at 750 cm-1 of the infrared absorption spectrum of a film or the like containing the polymerizable compound. -1 An absorption peak based on the polymerizable group (epoxy group) is observed in the vicinity, and the above-mentioned polymerization rate is calculated|required from the absorbance of the observed absorption peak.
[0121] As a mechanism for measuring the infrared absorption spectrum of the optical functional film, a commercially available infrared spectrophotometer can be used, which can be either a transmission type or a reflection type, preferably appropriately selected according to the form of the sample. The infrared absorption spectrum of the optical functional film can be measured using, for example, an infrared spectrophotometer "FTS-6000" manufactured by Bio-Rad Laboratories, Inc.
[0122] A more specific method for determining the polymerization rate of the above-mentioned liquid crystal compound of the optical functional film is as follows. For example, when an optical functional film is formed using a composition containing a liquid crystal compound having a polymerizable group, before the coating film formed using the composition is irradiated with active energy rays and / or heated, the infrared absorption spectrum A of the above-mentioned coating film is measured by the ATR method (Attenuated Total Reflection), and then after irradiating and / or heating with active energy rays, the infrared absorption spectrum B of the formed film is measured by the ATR method. In these infrared absorption spectra A and B, absorption peaks based on the polymerizable groups possessed by the liquid crystal compound appear respectively. From the absorbance A of the absorption peak appearing in the infrared absorption spectrum A and the absorbance B of the absorption peak appearing in the infrared absorption spectrum B, the polymerization rate of the liquid crystal compound having a polymerizable group of the optical functional film can be calculated according to the following formula (1).
[0123] Polymerization rate (%) = {(absorbance A - absorbance B) / (absorbance A)} × 100 (1)
[0124] <Optical functional film>
[0125] The optically functional film of the first embodiment is formed of a composition containing a liquid crystal compound having a polymerizable group. Since the liquid crystal compound is easily oriented in an arbitrary direction by photo-alignment or the like, various optical functions can be imparted.
[0126] Furthermore, the polymerization rate of the liquid crystal compound having a polymerizable group in the optically functional film of the first embodiment is 40% or less.
[0127] Hereinafter, a liquid crystal compound having a polymerizable group may be simply referred to as a “liquid crystal compound”.
[0128] The liquid crystal compound conceptually includes substances that no longer exhibit liquid crystallinity due to curing or the like.
[0129] In the optical functional film, the liquid crystal compound may be aligned in one direction, for example. Such an optical functional film in which the liquid crystal compound is aligned in one direction can be used as a phase difference film.
[0130] Furthermore, an optically functional film including a liquid crystal compound aligned in one direction and further including a dichroic substance can be used as an absorbing linear polarizer.
[0131] Furthermore, in the optical functional film, the liquid crystal compound may be helically oriented. A helically oriented liquid crystal compound is also called a cholesteric liquid crystal, and the optical functional film including the helically oriented liquid crystal compound can be used as a reflective circular polarizer.
[0132] Any of the above-mentioned optically functional films can be used in pancake lens type virtual reality display devices and the like.
[0133] Here, a virtual reality display device manufactured using the optical functional film of the first embodiment will be described with reference to the drawings.
[0134] Figure 1 This is a schematic diagram showing an example of a virtual reality display device according to the first embodiment.
[0135] Figure 1 The virtual reality display device 10 shown in the figure has, from the right side of the figure, an image display device 72 composed of an image display panel 70, a λ / 4 phase difference layer 11, an absorption type linear polarizer 21, a λ / 4 phase difference layer 12 and an anti-reflection layer 50; a double convex lens 90 with an optical functional layer composed of a half mirror 30, a lens substrate 34 and an anti-reflection layer 51; and a plano-convex lens 80 with an optical functional layer composed of a reflective circular polarizer 40, a λ / 4 phase difference layer 13, an absorption type linear polarizer 22 and a lens substrate 36.
[0136] As described below, in Figure 1 In the virtual reality display device 10 shown, the λ / 4 phase difference layer 13, the absorbing linear polarizer 22 and the reflecting circular polarizer 40 can be films obtained by forming the optical functional film of the first embodiment into a three-dimensional shape including a curved surface (hereinafter also referred to as a "curved shape") and then performing a prescribed curing treatment.
[0137] As shown in the modified example of the virtual reality display device described later, the use form of the optical functional film of the first embodiment is not limited to Figure 1 The optical component included in the virtual reality display device 10 shown can also be used as an optical component bonded to a double convex lens, for example.
[0138] In the virtual reality display device 10, the lens substrate 34 is a biconvex lens, and a half mirror 30 formed into a curved surface is bonded to one side of the lens substrate 34, and an anti-reflection layer 51 formed into a curved surface is bonded to the other side. In addition, the bonding at this time can be performed by a known method such as a method using OCA (Optical Clear Adhesive). In this regard, the bonding described below is also the same.
[0139] Furthermore, the lens substrate 36 is a plano-convex lens, and the absorbing linear polarizer 22 , the λ / 4 phase difference plate 13 , and the reflective circular polarizer 40 , each formed into a curved shape, are sequentially bonded to the convex surface of the lens substrate 36 .
[0140] The lens base 34 and the lens base 36 are formed of a material that is transparent to visible light and has a small phase difference (preferably a material with no phase difference), such as glass and acrylic plate.
[0141] The image display panel 70 is, for example, a well-known image display panel such as an organic electroluminescent display panel.
[0142] In the example shown in the figure, the image display panel 70 emits a non-polarized image (image light). The non-polarized image emitted by the image display panel 70 passes through the λ / 4 phase difference layer 11, transmits the absorption type linear polarizer 21 and becomes linear polarized light, is converted into circular polarized light by the λ / 4 phase difference layer 12, and transmits the anti-reflection layer 50. Thus, left circularly polarized light is emitted from the image display device 72.
[0143] The absorbing linear polarizer 21 transmits linear polarized light perpendicular to the paper surface, for example. The λ / 4 phase difference layer 12 is provided, for example, in a slow axis direction to convert linear polarized light perpendicular to the paper surface into left circularly polarized light.
[0144] The anti-reflection layer 50 and the anti-reflection layer 51 are known anti-reflection layers (AR coatings) such as magnesium fluoride layers and silicon oxide layers. Alternatively, a known anti-reflection film may be bonded.
[0145] The left circularly polarized light having passed through the antireflection layer 50 is then incident on the half mirror 30 and half of it is transmitted. The left circularly polarized light having passed through the half mirror 30 passes through the lens base 34 and the antireflection layer 51 .
[0146] In addition, the left circularly polarized light reflected by the half mirror 30 is converted into right circularly polarized light by reflection, passes through the antireflection layer 50 , and enters the λ / 4 phase difference layer 12 .
[0147] The λ / 4 phase difference layer 12 converts linear polarization in a direction perpendicular to the paper surface into left circular polarization. Therefore, right circular polarization incident on the λ / 4 phase difference layer 12 is converted into linear polarization in a vertical direction on the paper surface and is incident on the absorbing linear polarizer 21 .
[0148] The absorbing linear polarizer 21 is an absorbing linear polarizer that transmits linear polarized light in a direction perpendicular to the paper surface. Therefore, the linear polarized light in the vertical direction of the paper surface is absorbed by the absorbing linear polarizer 21.
[0149] Regarding this point, the following Figure 2 The virtual reality display device 20 shown is also the same.
[0150] The reflective circular polarizer 40 is, for example, a reflective circular polarizer having a cholesteric liquid crystal layer, and is a reflective circular polarizer that reflects left circularly polarized light and transmits other light. Therefore, the left circularly polarized light incident on the reflective circular polarizer 40 is reflected by the reflective circular polarizer 40, transmits the anti-reflection layer 51 and the lens substrate 34, and is incident on the half mirror 30.
[0151] The reflective circular polarizer 40 may be a reflective circular polarizer obtained by forming the optically functional film of the first embodiment including a helically aligned liquid crystal compound into a curved shape and then subjecting the film to a predetermined curing treatment.
[0152] Half of the left circularly polarized light incident on the half mirror 30 is reflected by the half mirror 30. By this reflection, the left circularly polarized light is converted into right circularly polarized light.
[0153] The right circularly polarized light reflected by the half mirror 30 passes through the lens base 34 and the antireflection layer 51 and enters the reflective circular polarizer 40 .
[0154] As described above, the reflective circular polarizer 40 is a reflective circular polarizer (cholesteric liquid crystal layer) that reflects left circularly polarized light and transmits other light. Therefore, right circularly polarized light incident on the reflective circular polarizer 40 transmits the reflective circular polarizer 40 and enters the λ / 4 phase difference layer 13 .
[0155] The λ / 4 phase difference layer 13 is a λ / 4 phase difference layer configured to match the slow axis direction to convert right circular polarized light into linear polarized light in the vertical direction of the paper. In addition, the absorption type linear polarizer 22 is a linear polarizer configured to match the transmission axis to transmit linear polarized light in the vertical direction of the paper. Therefore, the right circular polarized light incident on the λ / 4 phase difference layer 13 is converted into linear polarized light in the vertical direction of the paper by the λ / 4 phase difference layer 13, then transmits the absorption type linear polarizer 22, further transmits the lens substrate 36, and is observed as a virtual reality image by the user of the virtual reality display device 10.
[0156] The λ / 4 phase difference layer 13 may be a reflective circular polarizer obtained by forming the optical functional film of the first embodiment including the liquid crystal compound oriented in one direction into a curved surface and then subjecting it to a predetermined curing treatment. Furthermore, the absorbing linear polarizer 22 may be a reflective circular polarizer obtained by forming the optical functional film of the first embodiment including the liquid crystal compound oriented in one direction and the dichroic substance into a curved surface and then subjecting it to a predetermined curing treatment.
[0157] The absorbing linear polarizer 22 shields light that has unnecessarily transmitted through the reflective circular polarizer 40 to prevent the light from leaking (ghosting) and being observed by the user of the virtual reality display device 10 .
[0158] That is, when the left circularly polarized light first enters the reflective circular polarizer 40 , there is also left circularly polarized light that is not reflected by the reflective circular polarizer 40 and unnecessarily transmits the reflective circular polarizer 40 .
[0159] However, the left circularly polarized light is converted into linearly polarized light in a direction perpendicular to the paper surface by the λ / 4 phase difference layer 13 that converts the right circularly polarized light into linearly polarized light in the vertical direction of the paper surface. Therefore, the linearly polarized light is absorbed by the absorptive linear polarizer 22, which is a linear polarizer configured to transmit linearly polarized light in the vertical direction of the paper surface with a transmission axis, and thus can be prevented from becoming leaked light and being observed by the user.
[0160] Here, in Figure 1 In the virtual reality display device 10 shown, the reflective circular polarizer 40, the λ / 4 phase difference layer 13, and the absorbing linear polarizer 22 are formed into a curved surface and bonded to the convex surface of the lens substrate 36 which is a plano-convex lens.
[0161] When an optical functional film is formed into a curved surface, residual stress is generated in the formed optical functional film due to stretching, and phase difference or phase difference changes due to the photoelastic effect. In addition, in the curved surface forming, the stretching ratio varies depending on the part, so the amount of phase difference and the amount of change may vary locally.
[0162] For example, in the λ / 4 phase difference layer 13 formed into a curved surface of the virtual reality display device 10, when the actual phase difference is at least partially different from the expected phase difference, the left circularly polarized light that has unnecessarily transmitted the reflective circular polarizer 40 is converted into light containing not only the component in the vertical direction of the paper surface but also the component in the vertical direction of the paper surface, depending on the position of the λ / 4 phase difference layer 13. This light is not completely absorbed by the absorptive linear polarizer 22, and thus becomes leakage light (ghost image) and is observed by the user of the virtual reality display device 10.
[0163] On the other hand, a cholesteric liquid crystal layer generally does not have a phase difference. However, in a cholesteric liquid crystal layer, a phase difference of different amounts may occur locally due to residual stress caused by stretching when the layer is formed into a curved shape.
[0164] For example, in Figure 1 In the virtual reality display device 10 shown, the reflected circularly polarized light becomes light including undesired circularly polarized light such as elliptically polarized light, depending on the portion of the reflective circular polarizer 40 having a cholesteric liquid crystal layer and formed into a curved surface. As a result, the amount of light that unnecessarily passes through the reflective circular polarizer 40 increases, which results in an increase in light leakage (ghosting) observed by the user of the virtual reality display device 10.
[0165] On the other hand, as described above, the optically functional film of the first embodiment is characterized in that it is a film formed of a composition containing a liquid crystal compound having a polymerizable group, and the polymerization rate of the liquid crystal compound having a polymerizable group is 40% or less.
[0166] The liquid crystal compound having a polymerizable group can be polymerized and fixed in its orientation direction by irradiation with active energy rays and heating, and the optical functional film can be given flexibility by setting the polymerization rate to 40% or less. Therefore, even if the optical functional film of the first embodiment is formed into a curved surface, the residual stress caused by stretching is reduced, and thus, by using the formed body obtained by forming the optical functional film of the first embodiment into a curved surface in the optical component of the virtual reality display device, the appearance and change of the (local) phase difference caused by the curved surface forming in the optical component can be reduced.
[0167] Therefore, when the optically functional film according to the first embodiment is applied to, for example, a pancake lens type virtual reality display device, it is possible to reduce light leakage and display a high-quality virtual reality image.
[0168] The structure of the virtual reality display device manufactured using the optical functional film of the first embodiment is not limited to Figure 1 The virtual reality display device 10 is shown.
[0169] Figure 2 Another example of the virtual reality display device according to the first embodiment is schematically shown.
[0170] Figure 2 The virtual reality display device 20 shown in the figure is generally used in the above-mentioned Figure 1 Therefore, in the following description, the same symbols are marked for the same components, and the Figure 1 The differences of the virtual reality display device 10 shown are described below.
[0171] Figure 2 The virtual reality display device 20 shown in the figure has, from the right side of the figure, an image display device 72 composed of an image display panel 70, a λ / 4 phase difference layer 11, an absorption type linear polarizer 21, a λ / 4 phase difference layer 12 and an anti-reflection layer 50; a double convex lens 92 with an optical functional layer composed of a half mirror 30, a lens substrate 34 and a λ / 4 phase difference layer 14; and a plano-convex lens 82 with an optical functional layer composed of an anti-reflection layer 52, a reflection type linear polarizer 42, an absorption type linear polarizer 22 and a lens substrate 36.
[0172] exist Figure 2 In the virtual reality display device 20 shown, the λ / 4 retardation layer 14 and the absorbing linear polarizer 22 may be films obtained by forming the optical functional film of the first embodiment into a curved shape and then subjecting it to a predetermined curing treatment.
[0173] In the biconvex lens 92 with an optical function layer, a half mirror 30 formed into a curved surface is bonded to one surface of a lens base 34 , and a λ / 4 phase difference layer 14 formed into a curved surface is bonded to the other surface.
[0174] In the plano-convex lens 92 with an optical function layer, the absorbing linear polarizer 22 , the reflecting circular polarizer 42 , and the antireflection layer 52 , each of which is formed into a curved shape, are sequentially bonded to the convex surface of the lens substrate 36 .
[0175] Similar to the above-mentioned antireflection layer 51 , the antireflection layer 52 may be a known antireflection layer (AR coating) or a known antireflection film.
[0176] and Figure 1 The virtual reality display device 10 shown in FIG. Figure 2 In the virtual reality display device 20 shown, the image emitted by the image display panel 70 is also converted into left circularly polarized light by the λ / 4 phase difference layer 11 and emitted from the image display device 72 .
[0177] The left circularly polarized light having passed through the antireflection layer 50 is then incident on the half mirror 30 and half of it is transmitted through it. The left circularly polarized light having passed through the half mirror 30 is transmitted through the lens base 34 and is incident on the λ / 4 phase difference layer 14 .
[0178] Here, as an example, the λ / 4 phase difference layer 14 is a λ / 4 phase difference layer that is configured in accordance with the slow axis direction to convert left circularly polarized light into linearly polarized light in a direction perpendicular to the paper surface. Therefore, the left circularly polarized light incident on the λ / 4 phase difference layer 14 is converted into linearly polarized light in a direction perpendicular to the paper surface.
[0179] The λ / 4 retardation layer 14 may be a reflective circular polarizer obtained by forming the optically functional film of the first embodiment including a liquid crystal compound aligned in one direction into a curved shape and then subjecting the curved surface to a predetermined curing treatment.
[0180] The linearly polarized light converted into a direction perpendicular to the paper surface by the λ / 4 phase difference layer 14 passes through the antireflection layer 52 and enters the reflective linear polarizer 42 .
[0181] As an example, the reflective linear polarizer 42 reflects linear polarized light in a direction perpendicular to the paper surface and transmits linear polarized light in a direction perpendicular to the paper surface. Therefore, the linear polarized light in a direction perpendicular to the paper surface incident on the reflective linear polarizer 42 is reflected by the reflective linear polarizer 42 and incident on the λ / 4 phase difference layer 14 again.
[0182] The λ / 4 phase difference layer 14 is a λ / 4 phase difference layer that converts left circularly polarized light into linearly polarized light in a direction perpendicular to the paper surface. Therefore, linearly polarized light in a direction perpendicular to the paper surface incident on the λ / 4 phase difference layer 14 is converted into left circularly polarized light by the λ / 4 phase difference layer 14.
[0183] The left circularly polarized light converted by the λ / 4 phase difference layer 14 transmits through the lens base 34 and enters the half mirror 30, and half of it is reflected by the half mirror 30. By this reflection, the left circularly polarized light is converted into right circularly polarized light.
[0184] The right circularly polarized light reflected by the half mirror 30 passes through the lens substrate 34 and is incident on the λ / 4 phase difference layer 14. The λ / 4 phase difference layer 14 is a λ / 4 phase difference layer that converts the left circularly polarized light into the linear polarized light in the direction perpendicular to the paper surface. Therefore, the right circularly polarized light is converted into the linear polarized light in the vertical direction of the paper surface by the λ / 4 phase difference layer 14, passes through the anti-reflection layer 52, and is incident on the reflective linear polarizer 42.
[0185] The reflective linear polarizer 42 reflects linear polarized light in a direction perpendicular to the paper surface and transmits linear polarized light in a vertical direction of the paper surface. Therefore, the linear polarized light in a vertical direction of the paper surface incident on the reflective linear polarizer 42 transmits the reflective linear polarizer 42 .
[0186] The linear polarized light in the vertical direction on the paper that has passed through the reflective linear polarizer 42 then passes through the absorbing linear polarizer 22 that transmits the linear polarized light in the vertical direction on the paper, and is observed as a virtual reality image by the user of the virtual reality display device 100 .
[0187] The absorptive linear polarizer 22 is used to shield light that has unnecessarily passed through the reflective linear polarizer 42 to prevent the light from leaking (ghosting) and being observed by the user of the virtual reality display device 100 .
[0188] That is, when linear polarized light in a direction perpendicular to the paper surface is first incident on the reflective linear polarizer 42 , there is also linear polarized light in a direction perpendicular to the paper surface that is not reflected by the reflective linear polarizer 42 and unnecessarily transmits the reflective linear polarizer 42 .
[0189] However, the linear polarized light in the direction perpendicular to the paper surface is absorbed by the absorbing linear polarizer 22 that transmits the linear polarized light in the vertical direction of the paper surface, and thus can be prevented from being observed as leakage light by the user.
[0190] Here, in Figure 2 In the virtual reality display device 20 shown, the λ / 4 phase difference layer 14 bonded to the convex surface of the lens substrate 34 as a double convex lens generates residual stress due to stretching when formed into a curved surface as described above, and a phase difference or a change in the phase difference occurs due to the photoelastic effect. In addition, in the curved surface forming, the stretching ratio varies depending on the part, so in the λ / 4 phase difference layer 14, the amount of phase difference that occurs and the amount of change may vary locally.
[0191] At this time, the left circularly polarized light initially incident cannot be converted into appropriate linearly polarized light in the λ / 4 phase difference layer 14, but is converted into light including elliptically polarized light, etc. A part of this light is not reflected by the reflective linear polarizer 42 but is transmitted through the reflective linear polarizer 42 and the absorptive linear polarizer 22, thereby causing light leakage (ghosting) and being observed by the user of the virtual reality display device 20.
[0192] In contrast, by using a film formed into a curved surface by forming the optical functional film of the first embodiment in which the polymerization rate of the liquid crystal compound is less than 40% as the λ / 4 phase difference layer 14, as described above, the appearance and change of the (local) phase difference caused by the curved surface forming in the optical component can be reduced, thereby reducing light leakage and displaying a high-quality virtual reality image.
[0193] Hereinafter, the optical functional film, the optical layered body, the molded body, the method for producing an optical component, the optical component, and the virtual reality display device according to the first embodiment will be described in detail.
[0194] The optical functional film of the first embodiment is an optical functional film formed by forming a composition containing a liquid crystal compound having a polymerizable group, and the polymerization rate of the liquid crystal compound having a polymerizable group is 40% or less. As described above, by setting the polymerization rate of the liquid crystal compound to 40% or less, the optical functional film has flexibility, and the residual stress generated when it is formed into a curved surface is reduced, and the occurrence and change of phase difference can be suppressed.
[0195] The polymerization rate of the liquid crystal compound of the optical functional film is preferably 20% or less, more preferably 10% or less. Furthermore, when the unpolymerized liquid crystal compound becomes a solid state at room temperature, it is preferred that all liquid crystal compounds are unpolymerized (i.e., the polymerization rate is 0%). That is, the above-mentioned polymerization rate can be 0%. When the polymerization rate is 20% or less (more preferably 10% or less, and further preferably 0%), after the optical functional film is formed into a curved surface, by heating the optical functional film, an orientation treatment for orienting the liquid crystal compound can be performed. Thus, the occurrence of phase difference caused by the curved surface forming and the change of phase difference can be further suppressed.
[0196] Furthermore, when an optically functional film composed of a polymer is used as an optically anisotropic layer, depending on the type of polymer, it may break when formed into a curved surface with a small radius of curvature. Therefore, the radius of curvature may have to be increased, which becomes a restriction in lens design, and it is impossible to obtain a lens with an optically functional layer having a wide field of view, low chromatic aberration, low distortion, and excellent MTF.
[0197] In contrast, the optical functional film of the first embodiment in which the polymerization rate of the liquid crystal compound is 40% or less (preferably 20% or less, more preferably 10% or less, and further preferably 0%) has flexibility, so when formed into a three-dimensional shape including a curved surface with a small radius of curvature, the breakage of the optical functional film can be suppressed. As a result, the degree of freedom in lens design is increased, and a lens with an optical functional layer having a wide field of view, low chromatic aberration, low distortion, and excellent MTF can be manufactured.
[0198] Furthermore, the reflection wavelength band of a cholesteric liquid crystal layer or a reflective linear polarizer may shift to the short wavelength side due to stretching. Due to this short wavelength shift, the pancake lens may not be able to properly reflect or transmit the wavelength region of a part of the light emitted from the image display device. In this case, part of the light becomes leak light, resulting in ghosting and reduced contrast, and causing changes in the color tone of the image.
[0199] In contrast, the first embodiment of the optical functional film in which the polymerization rate of the liquid crystal compound is 40% or less (preferably 20% or less, more preferably 10% or less, and further preferably 0%) can be subjected to an orientation treatment for orienting the liquid crystal compound by heating the optical functional film after the optical functional film is formed into a curved surface. Through this orientation treatment, the helical pitch of the cholesteric liquid crystal layer determined by the amount of the chiral agent changes, thereby suppressing the occurrence of short-wavelength shift caused by the curved surface formation. As a result, inappropriate reflection and transmission of light in a part of the wavelength region can be suppressed, and light leakage and changes in the color tone of the image can be suppressed.
[0200] The composition for forming the optically functional film of the first embodiment contains at least a liquid crystal compound having a polymerizable group.
[0201] As the liquid crystal compound having a polymerizable group, any of a rod-shaped liquid crystal compound having a polymerizable group and a disc-shaped liquid crystal compound having a polymerizable group can be used.
[0202] As described above, the optically functional film in which the liquid crystal compound is oriented in one direction can be used as a phase difference film (phase difference layer). When the optically functional film is a phase difference film, for example, it is also possible to refer to Japanese Patent Gazette No. 2020-084070, etc., by uniformly oriented and fixed rod-shaped liquid crystal compounds with abnormal dispersion to make a phase difference film with abnormal dispersion. Here, having abnormal dispersion means that as the wavelength becomes larger, the value of the phase difference at the wavelength becomes larger. When the optically functional film is a λ / 4 plate (λ / 4 phase difference layer), it is preferably at any wavelength in the visible range. There is a phase difference of about 1 / 4 wavelength.
[0203] As described above, the optically functional film may be an absorbing linear polarizer. The optically functional film as an absorbing linear polarizer can be produced, for example, by forming a coating film using a composition containing a liquid crystal compound and a dichroic substance and aligning the liquid crystal compound and the dichroic substance in one direction.
[0204] Furthermore, as described above, the optically functional film may be a reflective circular polarizer composed of a cholesteric liquid crystal layer containing a helically oriented liquid crystal compound. For example, a cholesteric liquid crystal layer may be prepared by forming a coating film using a composition containing a liquid crystal compound and a chiral agent and performing a heat treatment to helically align the film.
[0205] The heat treatment for helical orientation is preferably performed after forming into a curved surface. This can suppress the change of the helical pitch in the plane caused by the curved surface forming, and can make the helical pitch uniform in the plane.
[0206] As is known to all, the cholesteric liquid crystal layer has a spiral structure in which liquid crystal compounds are stacked by spiral rotation, and has a structure in which liquid crystal compounds are stacked by spiral rotation of one circle (360° rotation) as one spiral period (spiral period) and multiple periods of spirally rotated liquid crystal compounds are stacked.
[0207] The cholesteric liquid crystal layer reflects right circularly polarized light or left circularly polarized light in a specific wavelength range, depending on the length of the helical period and the handedness (sense) of the helix of the liquid crystal compound, and transmits other light.
[0208] Therefore, when the virtual reality display device displays a color image, the cholesteric liquid crystal layer can be, for example, a multilayer cholesteric liquid crystal layer having a central wavelength that selectively reflects red light, a cholesteric liquid crystal layer having a central wavelength that selectively reflects yellow light, a cholesteric liquid crystal layer having a central wavelength that selectively reflects green light, and a cholesteric liquid crystal layer having a central wavelength that selectively reflects blue light.
[0209] (Composition)
[0210] Hereinafter, the composition for forming the optically functional film of the first embodiment (hereinafter also referred to as “the present composition”) will be described in more detail.
[0211] The liquid crystal compound having a polymerizable group contained in the present composition may be a rod-shaped liquid crystal compound or a disc-shaped liquid crystal compound.
[0212] The liquid crystal compound having a polymerizable group may be of low molecular type or high molecular type. Here, high molecular means a substance having a polymerization degree of 100 or more (Polymer Physics and Phase Transition Dynamics, by Masao Doi, page 2, Iwanami Shoten, 1992).
[0213] As the liquid crystal compound, a rod-shaped liquid crystal compound is preferably used. In addition, the present composition may contain two or more liquid crystal compounds. As a combination of two or more liquid crystal compounds, it may be any one of a combination of two or more rod-shaped liquid crystal compounds, a combination of two or more disc-shaped liquid crystal compounds, and a combination of one or more rod-shaped liquid crystal compounds and one or more disc-shaped liquid crystal compounds.
[0214] The liquid crystal compound preferably has two or more polymerizable groups in one molecule. When the present composition contains two or more liquid crystal compounds, it is preferred that at least one liquid crystal compound has two or more polymerizable groups in one molecule.
[0215] In the present specification, in the optical functional film, a liquid crystal compound is fixed by polymerization, and even if it becomes a compound that does not show liquid crystallinity, it is referred to as a liquid crystal compound for convenience.
[0216] The type of the polymerizable group possessed by the liquid crystal compound is not particularly limited, and examples thereof include a radical polymerizable group and a cation polymerizable group.
[0217] Examples of free radical polymerizable groups include (meth)acryloyl, (meth)acryloyloxy, vinyl, styryl, and allyl. Here, (meth)acryloyl is a term for methacryloyl or acryloyl, and (meth)acryloyloxy is a term for methacryloyloxy or acryloyloxy. Examples of cation polymerizable groups include epoxy and oxetane.
[0218] As the polymerizable group possessed by the liquid crystal compound, a radical polymerizable group is preferred, and a (meth)acryloyl group is more preferred.
[0219] As the rod-shaped liquid crystal compound having a polymerizable group, for example, the liquid crystal compounds described in paragraphs
[0026] to
[0098] of Japanese Unexamined Patent Publication No. 11-513019 and Japanese Unexamined Patent Publication No. 2005-289980 can be cited. In addition, as the disc-shaped liquid crystal compound having a polymerizable group, for example, the liquid crystal compounds described in paragraphs
[0020] to
[0067] of Japanese Unexamined Patent Publication No. 2007-108732 and paragraphs
[0013] to
[0108] of Japanese Unexamined Patent Publication No. 2010-244038 can be cited. These descriptions are incorporated into this specification.
[0220] The present composition may contain a dichroic substance. By using the present composition containing a liquid crystal compound and a dichroic substance, an absorbing linear polarizer can be formed as the optically functional film of the first embodiment.
[0221] The dichroic substance is not particularly limited, and known dichroic substances (dichroic pigments) such as visible light absorbing substances (dichroic pigments), ultraviolet absorbing substances, infrared absorbing substances, nonlinear optical substances, carbon nanotubes, and inorganic substances (such as quantum rods) can be used.
[0222] The dichroic substance preferably has a crosslinkable group from the viewpoint of suppressing a decrease in polarization degree during stretching and molding. Examples of the crosslinkable group include a (meth)acryloyl group, an epoxy group, an oxetanyl group, and a styryl group.
[0223] The present compositions may comprise a chiral agent.
[0224] By using the present composition containing a liquid crystal compound and a chiral agent, a reflective circular polarizer composed of a cholesteric liquid crystal layer can be formed as the optically functional film of the first embodiment.
[0225] The chiral agent is a compound for adjusting the helical period of the cholesteric liquid crystal compound, and a known chiral agent can be used (for example, described in Liquid Crystal Device Handbook, Chapter 3, Item 4-3, Chiral Agents for TN and STN, page 199, edited by the 142nd Committee of the Japan Society for the Promotion of Science, 1989).
[0226] The chiral agent may have a polymerizable group. The polymerizable group of the chiral agent is preferably the same type of group as the polymerizable group of the liquid crystal compound. Furthermore, the chiral agent may be a liquid crystal compound.
[0227] The present composition preferably comprises a polymerization initiator.
[0228] The polymerization initiator is not particularly limited, but a photopolymerization initiator is preferred.
[0229] As the photopolymerization initiator, a known compound can be used. Examples of the photopolymerization initiator include α-carbonyl compounds (U.S. Patent No. 2367661 and U.S. Patent No. 2367670), acyloin ethers (U.S. Patent No. 2448828), α-hydrocarbon-substituted aromatic acyloin compounds (U.S. Patent No. 2722512), polynuclear quinone compounds (U.S. Patent No. 3046127 and U.S. Patent No. 2951758), combinations of triarylimidazole dimers and p-aminobenzophenones (U.S. Patent No. 3549367), and the like. ), acridine and phenazine compounds (Japanese Patent Publication No. 60-105667 and U.S. Patent No. 4239850), oxadiazole compounds (U.S. Patent No. 4212970), o-acyl oxime compounds (Japanese Patent Publication No. 2016-27384
[0065] ), and acylphosphine oxide compounds (Japanese Patent Publication No. 63-40799, Japanese Patent Publication No. 5-29234, Japanese Patent Publication No. 10-95788 and Japanese Patent Publication No. 10-29997), etc.
[0230] When the present composition contains a polymerization initiator, the content of the polymerization initiator is preferably 0.01 to 30 parts by mass based on 100 parts by mass of the total of the liquid crystal compound and the dichroic substance in the present composition.
[0231] From the viewpoint of workability and the like, the present composition preferably contains a solvent.
[0232] As the solvent, a known solvent used for forming an optically functional film can be used, and examples thereof include ketones, ethers, and amides.
[0233] When the present composition contains a solvent, the content of the solvent is preferably 80 to 99% by mass based on the total mass of the present composition.
[0234] (Method for forming optically functional film)
[0235] The method for forming the optical functional film of the first embodiment is not particularly limited as long as the polymerization rate of the liquid crystal compound in the formed film does not exceed 40%. For example, as the method for forming the optical functional film of the first embodiment, the following method can be cited: a coating film forming step comprising applying the composition on an orientation layer to form a coating film and an orientation step for orienting the liquid crystal compound in the coating film, and a curing step for curing a part of the liquid crystal compound as needed.
[0236] The coating film forming step is a step of forming a coating film on the alignment layer using the present composition.
[0237] By using the present composition containing the above-mentioned solvent or using a melt obtained by heating the present composition to be in a liquid state, the present composition can be easily applied to the alignment layer.
[0238] Specific examples of the coating method of the present composition include well-known methods such as roll coating, gravure printing, spin coating, wire bar coating, extrusion coating, direct gravure coating, reverse gravure coating, die coating, spray coating, and inkjet.
[0239] The alignment layer can use a known alignment layer (alignment film) having a function of orienting the liquid crystal compound on the alignment layer. As the alignment layer, for example, a rubbing treatment alignment layer formed by rubbing the surface of a resin substrate and a photo-alignment layer formed by irradiating a film composed of a composition containing a free radical polymerizable compound with light can be cited.
[0240] The alignment layer may be in a state of being laminated on the optically functional film, or may be peeled off from the optically functional film at any stage.
[0241] The alignment step is a step of aligning the liquid crystal compound contained in the coating film. In this way, an optically functional film can be obtained.
[0242] The orientation process may include a drying process. By drying, components such as the solvent can be removed from the coating film. The drying process may be performed by leaving the coating film at room temperature for a predetermined time (e.g., natural drying), or by heating and / or blowing air.
[0243] The liquid crystal compound contained in the present composition is sometimes oriented by the above-mentioned coating film forming step or drying treatment. For example, in the form of a coating liquid containing a solvent, the solvent is removed from the coating film by drying the coating film to obtain an optically functional film.
[0244] When the drying treatment is performed at a temperature higher than the transition temperature of the liquid crystal component contained in the coating film to the liquid crystal phase, the heating treatment described later may not be performed.
[0245] From the perspective of manufacturing suitability, the transition temperature of the liquid crystal compound contained in the coating film to the liquid crystal phase is preferably 10 to 250°C, and more preferably 25 to 190°C. If the above transition temperature is 10°C or more, there is no need for cooling treatment to reduce the temperature to the temperature range of the liquid crystal phase, so it is preferred. In addition, if the above transition temperature is 250°C or less, even if the temperature is set to be higher than the temperature range of the temporary liquid crystal phase, high temperature is not required, which can reduce heat energy waste, deformation and deterioration of the substrate, etc., so it is preferred.
[0246] The alignment step preferably includes a heat treatment. This allows the liquid crystal compound contained in the coating film to be aligned, so that the coating film after the heat treatment can be preferably used as an optical functional film.
[0247] From the viewpoint of production suitability, the heat treatment is preferably performed at 10 to 250° C., more preferably 25 to 190° C. The heating time is preferably 1 to 300 seconds, more preferably 1 to 60 seconds.
[0248] In the present embodiment, drying treatment and heating treatment are cited as methods for aligning the liquid crystal component included in the coating film, but the method is not limited thereto and can be implemented by a known alignment treatment.
[0249] After the alignment step, a curing step of curing the optically functional film may be performed within a range where the polymerization rate of the liquid crystal compound does not exceed 40%.
[0250] The curing step is performed, for example, by heating and / or light irradiation (exposure). Among them, the curing step is preferably performed by light irradiation.
[0251] As light that can be used for curing, various light such as infrared light, visible light and ultraviolet light can be mentioned, and ultraviolet light is preferred. In addition, during curing, ultraviolet light can be irradiated while heating, or ultraviolet light can be irradiated through a filter that transmits only a specific wavelength.
[0252] When light irradiation is performed simultaneously with heating, the heating temperature during light irradiation depends on the transition temperature of the liquid crystal compound to the liquid crystal phase, and is preferably 25 to 140°C.
[0253] <Optical laminate>
[0254] The optical layered body according to the first embodiment includes the above-mentioned optically functional film and a base film.
[0255] As the base film, a base film composed of a resin having a peak temperature of tan δ (loss coefficient) of 170° C. or less is preferred. Furthermore, the optically functional film may be laminated with a plurality of layers.
[0256] Examples of the resin having a tan δ peak temperature of 170° C. or less include polyacrylates, polymethacrylates, cyclic polyolefins, and polyolefins.
[0257] From the viewpoint that the optical laminate is easily formed into a curved surface, the peak temperature of tan δ of the resin constituting the substrate film is preferably 150° C. or less, more preferably 130° C. or less, and further preferably 120° C. or less. As resins having a peak temperature of tan δ of 120° C. or less, for example, polyacrylates and polymethacrylates can be cited. The lower limit is not particularly limited and may be 60° C. or more.
[0258] Here, the method for measuring tan δ is described.
[0259] Using a dynamic viscoelasticity measuring apparatus (DVA-200 manufactured by ITKDVA Co., Ltd.), a film sample that had been previously humidified in an Rh atmosphere at a temperature of 25°C and a humidity of 60% for more than 2 hours was measured under the following conditions: E" (loss modulus) and E' (storage modulus), which were used as the value for determining tanδ (=E" / E').
[0260] Device: DVA-200 manufactured by ITKDVA
[0261] Sample: 5mm, length 50mm (gap 20mm)
[0262] Measurement conditions: tensile mode
[0263] Measuring temperature: -150℃~220℃
[0264] Heating conditions: 5℃ / min
[0265] Frequency: 1Hz
[0266] In general optical applications, stretched resin substrates are often used, and the peak temperature of tan δ is often high due to the stretching process. For example, the peak temperature of tan δ of a triacetylcellulose (TAC) substrate (e.g., TG40 manufactured by FUJIFILM Corporation) is 180°C or higher.
[0267] The thickness of the substrate film is not particularly limited, but is preferably 5 to 300 μm, more preferably 5 to 100 μm, and even more preferably 5 to 30 μm.
[0268] The optical layered body of the first embodiment may have other layers other than the optically functional film and the base film. Examples of other layers include an orientation layer and an adhesive layer.
[0269] As the alignment layer, the above-mentioned alignment layers can be mentioned.
[0270] The optical laminate may have an adhesive layer at a position adjacent to the optical functional film or substrate film, such as between the optical functional film and the substrate film. The adhesive contained in the adhesive layer is not particularly limited as long as it exhibits adhesion through drying and reaction after lamination. As an adhesive, for example, a polyvinyl alcohol-based adhesive (PVA-based adhesive) exhibiting adhesion through drying and a curing adhesive exhibiting adhesion through reaction can be cited. As a curing adhesive, for example, active energy ray-curing adhesives such as (meth)acrylate-based adhesives and cationic polymerization curing adhesives having an epoxy group or an oxetane group can be cited.
[0271] <Molded body>
[0272] The molded article of the first embodiment is a member obtained by molding the optically functional film or an optical laminate having the optically functional film and a base film into a three-dimensional shape including a curved surface.
[0273] The molded body of the first embodiment is, for example, a molded body in which an optical functional film or an optical laminate (preferably an optical laminate having a base film made of a resin having a tan δ peak temperature of 170° C. or less) is laminated on the surface of a molded base. The optical functional film or optical laminate of the molded body has at least a curved surface.
[0274] As a method for forming the optical functional film or the optical laminate into a curved surface, for example, thermoforming and vacuum forming can be cited. More specifically, insert forming as described in Japanese Patent Publication No. 2004-322501, vacuum forming as described in International Publication No. 2010 / 001867 and Japanese Patent Publication No. 2012-116094, injection molding, pressure forming, decompression coating molding, in-mold transfer and mold stamping can be cited.
[0275] When the optical functional film or the optical laminate is formed into a curved surface, it is also preferable to perform a heat treatment. The temperature of the heat treatment is preferably 80 to 170°C, more preferably 100 to 150°C, and further preferably 110 to 140°C.
[0276] The molding substrate used for molding the molded body is not particularly limited. When the molded body having the molding substrate is used as an optical component, it is preferably composed of a transparent component. Examples of the transparent component include glass, acrylic resin, and polyolefin resin. Furthermore, when used as an optical component for a pancake lens, it is preferred that the molding substrate has no phase difference.
[0277] <Method for manufacturing optical component>
[0278] By subjecting the molded article of the first embodiment to a curing treatment, the optical component of the first embodiment can be obtained.
[0279] The curing treatment is carried out, for example, by heating and / or light irradiation (exposure). As light that can be used for curing, various lights such as infrared light, visible light and ultraviolet light can be cited, and ultraviolet light is preferred. In addition, during curing, ultraviolet light can be irradiated while heating, or ultraviolet light can be irradiated through a filter that transmits only a specific wavelength.
[0280] The manufacturing method of the optical component of the first embodiment preferably includes the following curing step: the molded body of the first embodiment is subjected to at least one curing treatment selected from the group consisting of heat treatment and ultraviolet irradiation to make the polymerization rate of the liquid crystal compound of the optical functional film become 50% or more. After being stacked into a curved surface, the curing treatment is performed, thereby fixing the orientation direction of the liquid crystal compound.
[0281] From the viewpoint of durability, the polymerization rate of the liquid crystal compound of the optical functional film of the optical component after curing is preferably 60% or more, more preferably 70% or more. The upper limit is not particularly limited and may be 100%.
[0282] When curing is performed by heating and light irradiation, the heating temperature during light irradiation depends on the transition temperature of the liquid crystal compound to the liquid crystal phase and is preferably 25 to 140° C., and the heating time is preferably 0.1 to 60 seconds. In addition, when curing is performed only by heating, the heating temperature is preferably 100 to 140° C., and the heating time is preferably more than 5 minutes and less than 30 minutes.
[0283] The manufacturing method of the optical component of the first embodiment may further include an orientation process of heating the molded body before the above-mentioned curing process to orient the liquid crystal compound contained in the optical functional film, preferably including the above-mentioned orientation process. When the polymerization rate of the liquid crystal compound is sufficiently small, the liquid crystal compound can be oriented by an orientation process of heating the optical functional film. The molded body is subjected to an orientation process, and then the above-mentioned curing process (preferably a curing process based on ultraviolet irradiation) is performed, thereby, even after being formed into a curved surface, the liquid crystal compound can be fixed in an arbitrary orientation state.
[0284] The heating temperature in the orientation step is, for example, 10 to 250° C., or preferably 25 to 190° C. The heating time is, for example, 1 to 300 seconds, or preferably 1 to 60 seconds.
[0285] In order to make the liquid crystal compound into an arbitrary orientation state in the orientation step, the molded body preferably has an orientation layer adjacent to the optical functional film. As the orientation layer, the above-mentioned orientation layers can be mentioned, and among them, a photo-alignment layer can be preferably used.
[0286] When the optically functional film is a cholesteric liquid crystal layer, it is preferred to add a chiral agent in advance to the present composition containing a liquid crystal compound having a polymerizable group.
[0287] (Optical Components)
[0288] The optical component of the first embodiment can be obtained by the above-mentioned method for producing the optical component of the first embodiment. That is, the optical component of the first embodiment is a component obtained by subjecting the molded body of the first embodiment to the above-mentioned curing treatment.
[0289] When the optical component of the first embodiment is used in a pancake lens type virtual reality display device, it is possible to design and manufacture an optical component with an appropriate shape having a curved surface to obtain a wide field of view, low chromatic aberration, low distortion, and excellent MTF.
[0290] <Virtual reality display device>
[0291] The virtual reality display device of the first embodiment includes an image display device that emits at least polarized light and the optical component of the first embodiment. In addition to the image display device and the optical component, the virtual reality display device may also include additional optical components such as a half mirror and a diopter adjustment lens.
[0292] As an image display device that emits polarized light, a known image display device can be used, for example, an organic electroluminescent display device (OLED: Organic Light Emitting Diode), an LED (Light Emitting Diode: Light Emitting Diode) display device, and a micro-LED display device, etc., which are display devices in which self-luminous fine light-emitting bodies are arranged on a transparent substrate. These self-luminous display devices usually have a (circular) polarizer attached to the display surface to prevent reflection from the display surface. Therefore, the emitted light is polarized. In addition, as another image display device, a liquid crystal display device is exemplified. The liquid crystal display device also has a polarizer on the surface, so the emitted light is polarized.
[0293] <Optical film>
[0294] The optical film according to the second embodiment of the present invention has a non-planar shape.
[0295] The non-planar shape refers to a shape other than a planar shape, and an example thereof includes a curved surface shape.
[0296] The curved surface shape is a shape with a curvature greater than 0, including a developable curved surface and a three-dimensional curved surface. A developable curved surface is a surface whose parts can be developed in a planar manner without stretching or shrinking.
[0297] As for the curved surface shape as a developable curved surface, for example, a surface equivalent to a cylindrical surface, an elliptical cylindrical surface, a conical surface, and an elliptical conical surface can be cited, and it can be a convex curved surface or a concave curved surface. A three-dimensional curved surface refers to a curved surface that cannot be formed by plane deformation, that is, a curved surface that is not a developable curved surface. As a three-dimensional curved surface, a surface equivalent to a spherical surface and a rotating ellipsoid surface and a surface equivalent to a curved surface with a cross section of a parabola or a hyperbola (for example, a rotating parabola) can be cited, and it can be a convex curved surface or a concave curved surface.
[0298] The curved surface shape is preferably a lens shape. Examples of the curved surface shape of the lens shape include a spherical surface shape and a rotational ellipsoidal surface shape, and the curved surface shape may be a convex lens shape or a concave lens shape.
[0299] The non-planar shape of the optical film is preferably a spherical shape, a rotational ellipsoid shape, or a rotational parabola shape.
[0300] As described above, the optical film has a non-planar shape and exhibits a predetermined curvature radius. That is, the portion of the optical film having a non-planar shape (non-planar shape portion, preferably a curved shape portion) exhibits a predetermined curvature radius.
[0301] The radius of curvature is 30 to 1000 mm, and preferably 30 to 100 mm from the perspective of further suppressing light leakage when the optical film of the second embodiment of the present invention is applied to a pancake-type virtual reality display device (hereinafter also referred to as "an aspect in which the effect of the present invention is more excellent").
[0302] The radius of curvature may be constant at any position of the optical film, or may be different.
[0303] The in-plane deviation of the phase difference of the optical film is less than 5%. From the viewpoint of more excellent effects of the present invention, it is preferably less than 3%, and more preferably less than 1%. The lower limit is not particularly limited, and 0% is an example.
[0304] The in-plane deviation of the phase difference of the optical film is calculated by the following method. In this specification, the following method is also referred to as "Specific Method 1". In addition, the in-plane deviation of the phase difference is calculated using the measured value of the in-plane retardation at a wavelength of 550 nm at each position of the optical film.
[0305] First, the optical film is observed from above in the normal direction of the output surface of the image display panel when the optical film is applied to a virtual reality display device, and the intersection of the axis extending in the above-mentioned normal direction through the center of the output surface and the optical film observed from above is taken as the center of the optical film.
[0306] Next, in the projection image obtained by looking down at the optical film, a straight line passing through the above-mentioned center and extending in one direction in the in-plane direction is set as the first straight line, a straight line passing through the above-mentioned center and rotated 45° clockwise from the first straight line is set as the second straight line, a straight line passing through the above-mentioned center and rotated 45° clockwise from the second straight line is set as the third straight line, and a straight line passing through the above-mentioned center and rotated 45° clockwise from the third straight line is set as the fourth straight line.
[0307] Next, a circle is drawn that is located in the projection image obtained by looking down at the optical film and has the center of the optical film as its center. At this time, the inscribed circle with the maximum radius that can be drawn is the first circle, and the circle with half the radius of the first circle is the second circle.
[0308] Next, the in-plane retardation of the position of the optical film corresponding to the center of the optical film in the plan view, the in-plane retardation of the position of the optical film corresponding to the two intersections of the first straight line and the first circle, the in-plane retardation of the position of the optical film corresponding to the two intersections of the first straight line and the second circle, the in-plane retardation of the position of the optical film corresponding to the two intersections of the second straight line and the first circle, the in-plane retardation of the position of the optical film corresponding to the two intersections of the third straight line and the first circle, the in-plane retardation of the position of the optical film corresponding to the two intersections of the third straight line and the second circle, the in-plane retardation of the position of the optical film corresponding to the two intersections of the fourth straight line and the first circle, and the in-plane retardation of the position of the optical film corresponding to the two intersections of the fourth straight line and the first circle, and the in-plane retardation of the position of the optical film corresponding to the two intersections of the fourth straight line and the second circle. In addition, the position of the optical film corresponding to the center of the optical film in the plan view corresponds to the intersection of the axis extending in the normal direction of the projection image and the optical film. That is, the center position in the projection image is reflected to the position of the optical film, and the in-plane retardation of the position of the optical film is calculated. Furthermore, the position of the optical film corresponding to the above-mentioned intersection is equivalent to the intersection of the axis extending along the normal direction of the projection image and the optical film at the position of the selected intersection in the projection image obtained by looking down at the optical film. That is, the intersection position in the projection image is reflected to the position of the optical film, and the in-plane retardation of the position of the optical film is calculated. In the above order, the in-plane retardation of the optical film is measured at 17 locations.
[0309] Next, the maximum value, the minimum value, and the average value were determined from the obtained measured values, and the in-plane deviation (%) of the phase difference was calculated by the following formula.
[0310] Formula: In-plane deviation (%) = {(maximum value - minimum value) / average value} × 100
[0311] The shape of the outer peripheral edge of the optical film according to the second embodiment of the present invention is not particularly limited, and for example, a perfect circle, an ellipse, or an irregular shape can be used.
[0312] The shape of the outer peripheral end refers to the shape of the outer peripheral end of the optical film when the optical film is observed from the normal direction of the light emission surface of the image display panel when the optical film is applied to a virtual reality display device.
[0313] The in-plane variation of the film thickness of the optical film of the second embodiment of the present invention is not particularly limited, but is preferably less than 5%, more preferably less than 3%, from the viewpoint of more excellent effects of the present invention. The lower limit is not particularly limited, and may be 0%.
[0314] As a method for measuring the in-plane deviation of the above-mentioned film thickness, the film thickness at 17 locations where the in-plane delay was measured when calculating the in-plane deviation of the above-mentioned phase difference was measured, and the maximum value, minimum value and average value were respectively found from the measured values obtained, and the in-plane deviation (%) of the phase difference was calculated by the following formula.
[0315] Formula: In-plane deviation (%) = {(maximum value - minimum value) / average value} × 100
[0316] The film thickness at each location was measured by cutting the optical film with a microtome to expose a cross section, and observing the cross section with a scanning electron microscope (SEM) at an appropriate magnification (20,000 to 50,000 times) to determine the film thickness of the optical film.
[0317] In addition, the measurement sample may be subjected to appropriate treatment such as carbon deposition and etching to facilitate cross-section observation. The acceleration voltage is preferably optimized under the condition of 1 to 10 kV.
[0318] In this specification, the method for measuring the in-plane variation of the film thickness described above is also referred to as “specific method 2”.
[0319] As the optical film of the second embodiment of the present invention, for example, a laminated optical body composed of a combination of a retardation film, a cholesteric liquid crystal layer, a polarizer, a reflective polarizer, an antireflection film, a transparent film, and a part thereof is used.
[0320] That is, the optical film of the second embodiment of the present invention may be a film of a single-layer structure or a film of a multi-layer structure. For example, the optical film of the second embodiment of the present invention may be composed of only a phase difference film, or the optical film of the second embodiment of the present invention may be a laminated optical body composed of a phase difference film and a reflective polarizer.
[0321] The optical film of the second embodiment of the present invention preferably includes at least a retardation film. That is, the optical film of the second embodiment of the present invention preferably consists of a single-layer retardation film or is a laminated optical body including a retardation film.
[0322] Hereinafter, first, the retardation film will be described in detail.
[0323] <Phase difference film (hereinafter also referred to as "phase difference layer")>
[0324] The phase difference layer has the function of converting the outgoing light into approximately linear polarized light when circularly polarized light is incident. For example, a phase difference layer whose Re is approximately 1 / 4 wavelength at any wavelength in the visible range can be used. In this case, the in-plane retardation Re (550) at a wavelength of 550 nm is preferably 120 nm to 150 nm, more preferably 125 nm to 145 nm, and further preferably 135 nm to 140 nm.
[0325] Furthermore, a retardation layer having Re of approximately 3 / 4 wavelength or approximately 5 / 4 wavelength is also preferred because it can convert linearly polarized light into circularly polarized light.
[0326] Furthermore, the phase difference layer preferably has anomalous dispersion with respect to wavelength. If it has anomalous dispersion, it can convert circularly polarized light into linearly polarized light in a wavelength range wide in the visible range, so it is preferred. Here, having anomalous dispersion with respect to wavelength means that as the wavelength becomes larger, the phase difference value at the wavelength becomes larger.
[0327] The phase difference layer having anomalous dispersion can be produced by uniaxially stretching a polymer film such as a modified polycarbonate resin film having anomalous dispersion, for example, with reference to Japanese Patent Application Laid-Open No. 2017-049574.
[0328] Furthermore, the phase difference layer having anomalous dispersion only needs to have anomalous dispersion in substance. For example, as disclosed in Japanese Patent Gazette No. 06259925, it can also be produced by stacking a phase difference layer having Re of about 1 / 4 wavelength and a phase difference layer having Re of about 1 / 2 wavelength so that their slow axes form an angle of about 60° with each other. It is known that in this case, even if the 1 / 4 wavelength phase difference layer and the 1 / 2 wavelength phase difference layer have normal dispersion (as the wavelength increases, the phase difference value at the wavelength decreases), circularly polarized light can be converted into linearly polarized light within a wide wavelength range of the visible range, and it can be regarded as having anomalous dispersion in substance.
[0329] Furthermore, the phase difference layer also preferably has a layer formed by fixing the uniformly oriented liquid crystal compound. For example, a layer obtained by uniformly aligning a rod-shaped liquid crystal compound horizontally with the in-plane direction and a layer obtained by uniformly aligning a disc-shaped liquid crystal compound vertically with the in-plane direction can be used. Furthermore, for example, it is also possible to make a phase difference layer with abnormal dispersion by uniformly aligning and fixing a rod-shaped liquid crystal compound with abnormal dispersion, with reference to Japanese Patent Publication No. 2020-084070.
[0330] Furthermore, the phase difference layer also preferably has a layer formed by fixing a liquid crystal compound twisted and oriented with the thickness direction as the helical axis. For example, as disclosed in Japanese Patent No. 5753922 and Japanese Patent No. 5960743, a phase difference layer having a layer formed by fixing a rod-shaped liquid crystal compound or a disc-shaped liquid crystal compound twisted and oriented with the thickness direction as the helical axis can also be used. In this case, the phase difference layer can be regarded as having anomalous dispersion in essence, and is therefore preferred.
[0331] The thickness of the retardation layer is not particularly limited, but is preferably 0.1 to 8 μm, more preferably 0.3 to 5 μm, from the viewpoint of thinning.
[0332] Furthermore, in order to minimize the impact on various sensors that use near-infrared light as a light source, such as eye tracking, expression recognition, and iris authentication, which are incorporated into optical systems such as virtual reality display devices and electronic viewfinders, the phase difference layer preferably has near-infrared light transmittance.
[0333] <Laminated optical body>
[0334] One form of a laminated optical body includes at least a cholesteric liquid crystal layer and a phase difference layer for mutually converting circularly polarized light and linearly polarized light.
[0335] One form of a laminated optical body includes at least a cholesteric liquid crystal layer, a phase difference layer for mutually converting circularly polarized light and linearly polarized light, and a linear polarizer in this order.
[0336] One embodiment of a laminated optical body includes at least a linearly polarized light reflective polarizer and a phase difference layer for converting circularly polarized light and linearly polarized light into each other.
[0337] One embodiment of a laminated optical body includes at least a phase difference layer for mutually converting circularly polarized light and linearly polarized light, a linearly polarized light type reflective polarizer, and a linear polarizer in this order.
[0338] The phase difference layer included in the laminated optical body is as described above.
[0339] Other components that may be included in the laminated optical body will be described in detail below.
[0340] [Cholesteric liquid crystal layer]
[0341] The cholesteric liquid crystal layer is an optical component that separates incident light into right-handed circularly polarized light and left-handed circularly polarized light and reflects one circularly polarized light and transmits the other circularly polarized light. For example, it is possible to refer to Japanese Patent Gazette No. 2020-060627, etc., and use a cholesteric liquid crystal layer formed by fixing the cholesteric liquid crystal phase. The film formed by fixing the cholesteric liquid crystal phase is a thin film, and the transmitted light has a high degree of polarization, so it is preferred. From the viewpoint of suppressing the reduction of polarization degree and / or polarization axis distortion when stretching or forming into a three-dimensional shape, it is preferred to use a cholesteric liquid crystal layer as a film for curved surface forming. In addition, the reduction of polarization degree caused by polarization axis distortion is not easy to occur.
[0342] The cholesteric liquid crystal layer preferably has a blue light reflection layer with a reflectivity of 40% or more at a wavelength of 460nm, a green light reflection layer with a reflectivity of 40% or more at a wavelength of 550nm, a yellow light reflection layer with a reflectivity of 40% or more at a wavelength of 600nm, and a red light reflection layer with a reflectivity of 40% or more at a wavelength of 650nm. If such a structure is adopted, high reflectivity can be exhibited in a wavelength range with a wide visible range, so it is preferred. In addition, the above-mentioned reflectivity is the reflectivity when non-polarized light is incident on the cholesteric liquid crystal layer at each wavelength.
[0343] Furthermore, the blue light reflecting layer, the green light reflecting layer, the yellow light reflecting layer, and the red light reflecting layer formed by fixing the cholesteric liquid crystal phase may have a pitch gradient layer that continuously changes the helical pitch of the cholesteric liquid crystal phase in the thickness direction. For example, the green light reflecting layer and the yellow light reflecting layer can be continuously produced with reference to Japanese Patent Publication No. 2020-060627.
[0344] Furthermore, the cholesteric liquid crystal layer also preferably includes a light reflecting layer formed by fixing a cholesteric liquid crystal phase containing a rod-shaped liquid crystal compound and a light reflecting layer formed by fixing a cholesteric liquid crystal phase containing a disc-shaped liquid crystal compound. With such a structure, the cholesteric liquid crystal phase containing the rod-shaped liquid crystal compound has a positive RtH, while the cholesteric liquid crystal phase containing the disc-shaped liquid crystal compound has a negative RtH, so that the Rths of each other are canceled, and the occurrence of ghosting can be suppressed even for incident light from an oblique direction, so it is preferred.
[0345] If the situation where Rth is offset is expressed by a formula, it is as follows. In an optical laminate film having n light reflecting layers, when the light reflecting layers are named L1, L2, L3, ..., Ln in order from the light source side, the sum of the Rth of each layer from the light reflecting layer L1 to the light reflecting layer Li is taken as SRthi. Specifically, it is the following formula.
[0346] SRth1=Rth1
[0347] SRth2=Rth1+Rth2
[0348] …
[0349] SRthi=Rth1+Rth2……+Rthi
[0350] …
[0351] SRthn=Rth1+Rth2……+Rthi……+Rthn
[0352] The absolute value of all these SRthi (SRth1 to SRthn) is preferably 0.3 μm or less, more preferably 0.2 μm or less, and further preferably 0.1 μm or less. Rthi of each layer in the above formula is obtained by the above formula for calculating Rth.
[0353] The thickness of the cholesteric liquid crystal layer is not particularly limited, but is preferably 30 μm or less, and more preferably 15 μm or less, from the viewpoint of thinning.
[0354] Furthermore, when the cholesteric liquid crystal layer is stretched or formed, the reflection wavelength region of the cholesteric liquid crystal layer may be displaced sometimes, so it is preferable to select the reflection wavelength region by assuming the displacement of the wavelength in advance. For example, when an optical film formed by fixing the cholesteric liquid crystal phase is used as the cholesteric liquid crystal layer, the film is elongated due to stretching or forming, which sometimes causes the helical pitch of the cholesteric liquid crystal phase to become smaller, so it is preferable to pre-set the helical pitch of the cholesteric liquid crystal phase to be larger. Furthermore, assuming the short-wave displacement of the reflection wavelength region caused by stretching or forming, the cholesteric liquid crystal layer also preferably has an infrared light reflection layer with a reflectivity of 40% or more at a wavelength of 800nm.
[0355] Furthermore, when the stretching ratio during stretching or forming is not uniform in the plane, a suitable reflection wavelength region can be selected at each part in the plane according to the wavelength shift caused by stretching. That is, there may be regions with different reflection wavelength regions in the plane. In addition, it is also preferred to set the reflection wavelength region wider than the desired wavelength region in advance, assuming that the stretching ratio at each part in the plane is different.
[0356] (Method for producing a cholesteric liquid crystal layer)
[0357] The cholesteric liquid crystal layer can be formed by applying a liquid crystal composition obtained by dissolving a liquid crystal compound, a chiral agent, a polymerization initiator, and a surfactant added as needed in a solvent on a support or a base layer formed on a support and drying the coating film, orienting the liquid crystal compound in the coating film, and irradiating the coating film with active light to cure the liquid crystal composition. In this way, a cholesteric liquid crystal layer having a cholesteric liquid crystal structure with fixed cholesteric regularity can be formed.
[0358] 〔Coating method〕
[0359] In addition, as a coating method for the liquid crystal composition, for example, known methods such as roll coating, gravure printing, spin coating, wire bar coating, extrusion coating, direct gravure coating, reverse gravure coating, die coating, spray coating and inkjet coating can be cited.
[0360] [Method of providing in-plane distribution of the helical pitch]
[0361] As a method for imparting an in-plane distribution to the helical pitch of the cholesteric liquid crystal layer, for example, there is a method of using a chiral reagent that is changed by photoisomerization of HTP.
[0362] The following is a detailed description. A cholesteric liquid crystal layer obtained by coating (and then heating, depending on the situation) a liquid crystal composition containing a chiral agent whose HTP changes due to photoisomerization and aligning it is subjected to light irradiation corresponding to the photoisomerization, whereby the HTP of the chiral agent changes, and as a result, the helical pitch of the cholesteric liquid crystal layer can be changed and the reflection wavelength can be changed. Utilizing this property, an exposure mask or the like is used to irradiate the oriented cholesteric liquid crystal layer in a patterned manner to make it photoisomerized, thereby obtaining a pattern that changes the reflection wavelength only in the area irradiated with light. After obtaining the pattern, the entire cholesteric liquid crystal layer is exposed to cure the liquid crystal composition, and the liquid crystal composition is polymerized, thereby finally being able to obtain a cholesteric liquid crystal layer (patterned cholesteric liquid crystal layer) having an in-plane distribution of the helical pitch. Photoisomerization no longer occurs in the patterned cholesteric liquid crystal layer after curing, and it has stable properties.
[0363] In order to efficiently form a pattern, it is preferable to separate the light irradiation for photoisomerization and the light irradiation for curing. In other words, when one of photoisomerization and curing is being performed, the other should not be performed as much as possible. As a method for separating the two, for example, separation based on oxygen concentration, separation based on exposure wavelength, etc. can be cited.
[0364] First, regarding oxygen concentration, photoisomerization is not easily affected by oxygen concentration, but curing (depending on the initiator used) is less likely to occur as the oxygen concentration increases. Therefore, photoisomerization is performed under conditions with high oxygen concentration, such as in the atmosphere, and curing is performed under conditions with low oxygen concentration, such as using a nitrogen atmosphere at an oxygen concentration of 300 volume ppm or less, thereby making it easy to separate photoisomerization from curing.
[0365] In addition, regarding the exposure wavelength, the photoisomerization of the chiral agent is likely to proceed at the absorption wavelength of the chiral agent, and the curing is likely to proceed at the absorption wavelength of the photopolymerization initiator. Therefore, if the chiral agent and the photopolymerization initiator are selected so that the absorption wavelengths of the chiral agent and the photopolymerization initiator are different, the photoisomerization and curing based on the exposure wavelength can be separated.
[0366] In addition, one or both of photoisomerization and curing may be performed under heating as needed. The temperature during heating is preferably 25 to 140°C, more preferably 30 to 100°C.
[0367] As another method of using a chiral reagent that changes due to photoisomerization of HTP, there is also a method as follows: first, curing is performed in a pattern, and then the uncured area is isomerized. That is, for the oriented cholesteric liquid crystal phase, first, an exposure mask or the like is used to irradiate the curing light in a pattern. By then performing light irradiation for overall photoisomerization (since the area that was first cured is unlikely to undergo a pitch change caused by photoisomerization), a pitch change caused by photoisomerization and a change in the reflection wavelength only occur in the area that was not first cured. At this time, after obtaining the pattern, the entire cholesteric liquid crystal layer is exposed to cure the liquid crystal composition, and the liquid crystal composition is polymerized, thereby obtaining the final patterned cholesteric liquid crystal layer.
[0368] [Direct coating of each layer]
[0369] It is preferred to directly form adjacent layers between the light reflecting layers of the cholesteric liquid crystal layer without an adhesive layer. When forming the layers, the adhesive layer can be omitted by directly coating on the adjacent layers that have been formed. Furthermore, in order to reduce the refractive index difference in all directions within the plane, it is preferred to configure the orientation direction (slow axis direction) of the liquid crystal compound to change continuously at the interface. For example, when a light reflecting layer formed using a rod-shaped liquid crystal compound is formed on a light reflecting layer formed using a disc-shaped liquid crystal compound, a coating liquid containing a rod-shaped liquid crystal compound is directly coated, and the light reflecting layer containing the disc-shaped liquid crystal compound can also be oriented so that the slow axis direction is continuous at the interface by the orientation restriction force of the disc-shaped liquid crystal compound.
[0370] [Method of bonding each layer]
[0371] The cholesteric liquid crystal layer is preferably a laminate composed of a plurality of light reflecting layers. The layers can be bonded together by any bonding method, for example, a bonding agent or an adhesive can be used.
[0372] As the adhesive, any commercially available adhesive can be used. Among them, from the viewpoint of thinning and reducing the surface roughness Ra of the laminated optical body, the thickness of the adhesive layer is preferably 25 μm or less, more preferably 15 μm or less, and most preferably 6 μm or less. In addition, an adhesive that does not easily produce outgassing is preferred. In particular, when stretching or forming, vacuum treatment or heat treatment may be required, and it is also preferred that outgassing does not occur under these conditions.
[0373] As the adhesive, any commercially available adhesive or the like can be used, and for example, an epoxy resin adhesive or an acrylic resin adhesive can be used.
[0374] From the perspective of thinning and reducing the surface roughness Ra of the cholesteric liquid crystal layer, the thickness of the adhesive layer is preferably 25 μm or less, more preferably 5 μm or less, and most preferably 1 μm or less. In addition, from the perspective of thinning the adhesive layer and applying the adhesive to the adherend with a uniform thickness, the viscosity of the adhesive is preferably 300 cP or less, and more preferably 100 cP or less.
[0375] Furthermore, when the adherend has a surface concavo-convex, from the viewpoint of reducing the surface roughness Ra of the cholesteric liquid crystal layer, the adhesive and the bonding agent can also select a suitable viscoelasticity or thickness so as to be able to embed the surface concavo-convex of the bonding layer. From the viewpoint of embedding the surface concavo-convex, the viscosity of the adhesive and the bonding agent is preferably 50 cP or more. Furthermore, the thickness is preferably thicker than the height of the surface concavo-convex.
[0376] As a method for adjusting the viscosity of the adhesive, for example, a method of using an adhesive containing a solvent can be cited. At this time, the viscosity of the adhesive can be adjusted according to the ratio of the solvent. In addition, by applying the adhesive to the adherend and then drying the solvent, the thickness of the adhesive can be further reduced.
[0377] In the cholesteric liquid crystal layer, from the viewpoint of reducing unnecessary reflection and suppressing the decrease in the polarization degree of transmitted light, the adhesive or bonding agent used to bond each layer preferably has a small refractive index difference with the adjacent layer. Since the liquid crystal layer has birefringence and the refractive index in the fast axis direction is different from the refractive index in the slow axis direction, when the value obtained by adding the refractive index in the fast axis direction and the refractive index in the slow axis direction and dividing by 2 is set as the average refractive index nave of the liquid crystal layer, the difference between the refractive index of the adjacent adhesive layer or bonding layer and nave is preferably 0.075 or less, more preferably 0.05 or less, and further preferably 0.025 or less. The refractive index of the adhesive or bonding agent can be adjusted by, for example, mixing titanium oxide particles or zirconium oxide particles.
[0378] Furthermore, although the cholesteric liquid crystal layer, phase difference layer and linear polarizer have in-plane refractive index anisotropy, the refractive index difference with adjacent layers in all directions in the plane is preferably 0.10 or less. Therefore, the adhesive and pressure-sensitive adhesive may have in-plane refractive index anisotropy.
[0379] Furthermore, between the cholesteric liquid crystal layer and the adhesive or between the cholesteric liquid crystal layer and the adhesive, there may be a refractive index adjustment layer whose difference between the refractive index in the fast axis direction and the refractive index in the slow axis direction is smaller than that of the cholesteric liquid crystal layer. In this case, the refractive index adjustment layer preferably has a cholesteric liquid crystal layer. By having a refractive index adjustment layer, it is possible to further suppress interface reflection and further suppress the generation of ghosting. Furthermore, the average refractive index of the refractive index adjustment layer is more preferably smaller than the average refractive index of the cholesteric liquid crystal layer. Furthermore, the central wavelength of the reflected light of the refractive index adjustment layer may be less than 430 nm or greater than 670 nm, more preferably less than 430 nm.
[0380] Furthermore, it is also preferred that the thickness of the adhesive layer between each layer is less than 100nm. If the thickness of the adhesive layer is less than 100nm, the refractive index difference is not easily perceived by light in the visible range, and unnecessary reflection can be suppressed. The thickness of the adhesive layer is more preferably less than 50nm, and further preferably less than 30nm. As a method for forming an adhesive layer with a thickness of less than 100nm, for example, a method of vapor-depositing a ceramic adhesive such as silicon oxide (SiOx layer) on the bonding surface can be cited. The bonding surface of the bonding component can be subjected to surface modification treatments such as plasma treatment, corona treatment and saponification treatment or given a primer layer before bonding. Furthermore, when there are multiple bonding surfaces, the type or thickness of the adhesive layer can be adjusted according to the bonding surface. Specifically, for example, an adhesive layer with a thickness of less than 100nm can be provided in the order shown in the following (1) to (3).
[0381] (1) The laminated layers are bonded to a dummy support made of a glass substrate.
[0382] (2) A SiOx layer having a thickness of 100 nm or less is formed on both the surface of the stacked layer and the surface of the stacked layer by vapor deposition or the like. The vapor deposition can be performed using SiOx powder as a vapor deposition source, for example, using a vapor deposition device (model ULEYES) manufactured by ULVAC, Inc. In addition, it is preferred that a plasma treatment be performed in advance on the surface of the formed SiOx layer.
[0383] (3) After the formed SiOx layers are bonded together, the dummy support is peeled off. The bonding is preferably performed at a temperature of 120°C, for example.
[0384] The coating, bonding or lamination of each layer can be performed in a roll-to-roll manner or in a single wafer manner.
[0385] From the viewpoint of improving productivity and reducing axial deviation of each layer, a roll-to-roll method is preferred.
[0386] On the other hand, the single wafer method is preferred in terms of suitability for small-volume and high-variety production or the ability to select a special bonding method such as the above-mentioned bonding layer having a thickness of 100 nm or less.
[0387] In addition, as a method for applying the adhesive to the adherend, for example, known methods such as roll coating, gravure printing, spin coating, wire bar coating, extrusion coating, direct gravure coating, reverse gravure coating, die coating, spray coating and inkjet coating can be cited.
[0388] Furthermore, in order to minimize the influence on various sensors that use near-infrared light as a light source, such as eye tracking, expression recognition, and iris authentication incorporated into optical systems such as virtual reality display devices and electronic viewfinders, the cholesteric liquid crystal layer preferably has near-infrared light transmittance.
[0389] <Linear Polarizer>
[0390] The linear polarizer is an absorption type polarizer, which absorbs linear polarized light in the absorption axis direction of incident light and transmits linear polarized light in the transmission axis direction. As the linear polarizer, a general polarizer can be used, for example, a polarizer obtained by dyeing polyvinyl alcohol or other polymer resin with a dichroic substance and stretching it, or a polarizer obtained by aligning a dichroic substance by using the orientation of a liquid crystal compound. From the viewpoint of availability and the viewpoint of improving the degree of polarization, a polarizer obtained by dyeing polyvinyl alcohol with iodine and stretching it is preferred.
[0391] The thickness of the linear polarizer is preferably 10 μm or less, more preferably 7 μm or less, and further preferably 5 μm or less. When the linear polarizer is thin, cracks or breaks in the film can be prevented when the laminated optical body is stretched or formed.
[0392] Furthermore, the single plate transmittance of the linear polarizer is preferably 40% or more, more preferably 42% or more. Furthermore, the polarization degree is preferably 90% or more, more preferably 95% or more, and further preferably 99% or more. In addition, in this specification, the single plate transmittance and polarization degree of the linear polarizer are measured using an automatic polarization film measuring device: VAP-7070 (manufactured by JASCO Corporation).
[0393] Furthermore, the transmission axis of the linear polarizer is preferably aligned with the polarization axis of the light converted into linear polarized light by the phase difference layer. For example, when the phase difference layer is a layer having a phase difference of 1 / 4 wavelength, the angle between the transmission axis of the linear polarizer and the slow axis of the phase difference layer is preferably about 45°.
[0394] The linear polarizer is also preferably a light absorption anisotropic layer containing a liquid crystal compound and a dichroic substance. The linear polarizer containing a liquid crystal compound and a dichroic substance can be made thinner, and even if stretched or formed, it is still difficult to crack or break, so it is preferred. The thickness of the light absorption anisotropic layer is not particularly limited, but from the viewpoint of thinning, it is preferably 0.1 to 8 μm, and more preferably 0.3 to 5 μm.
[0395] A linear polarizer including a liquid crystal compound and a dichroic substance can be produced with reference to Japanese Patent Application Laid-Open No. 2020-023153, for example.
[0396] From the viewpoint of improving the polarization degree of the linear polarizer, the orientation degree of the dichroic substance in the light absorption anisotropic layer is preferably 0.95 or more, more preferably 0.97 or more.
[0397] Furthermore, in order to minimize the influence on various sensors that use near-infrared light as a light source, such as eye tracking, expression recognition, and iris authentication, which are incorporated into optical systems such as virtual reality display devices and electronic viewfinders, the linear polarizer preferably has transmissivity to near-infrared light.
[0398] <Other functional layers>
[0399] The laminated optical body may have other functional layers in addition to the above-mentioned cholesteric liquid crystal layer, phase difference layer and linear polarizer.
[0400] Furthermore, in order to minimize the impact on various sensors that use near-infrared light as a light source, such as eye tracking, expression recognition, and iris authentication, which are incorporated into optical systems such as virtual reality display devices and electronic viewfinders, the other functional layers are preferably transmissive to near-infrared light.
[0401] <Positive C plate>
[0402] The laminated optical body also preferably further has a positive C plate. Here, the positive C plate refers to a phase difference layer in which Re is substantially zero and Rth has a negative value. The positive C plate can be obtained, for example, by vertically aligning a rod-like liquid crystal compound. For details of the manufacturing method of the positive C plate, for example, reference can be made to the records in Japanese Patent Publication No. 2017-187732, Japanese Patent Publication No. 2016-053709, and Japanese Patent Publication No. 2015-200861.
[0403] The positive C plate functions as an optical compensation layer for increasing the polarization degree of the transmitted light for the light incident from an oblique direction. The positive C plate can be provided at any position of the laminated optical body, and a plurality of positive C plates can be provided.
[0404] The positive C plate can be arranged adjacent to the cholesteric liquid crystal layer, or arranged inside the cholesteric liquid crystal layer. As the cholesteric liquid crystal layer, for example, when a light reflecting layer formed by fixing a cholesteric liquid crystal phase containing a rod-shaped liquid crystal compound is used, the light reflecting layer has a positive Rth. At this time, when light is incident from an oblique direction relative to the cholesteric liquid crystal layer, the polarization state of the reflected light and the transmitted light changes due to the effect of Rth, and sometimes the polarization degree of the transmitted light decreases. If there is a positive C plate inside or near the cholesteric liquid crystal layer, the change in the polarization state of the oblique incident light can be suppressed, and the decrease in the polarization degree of the transmitted light can be suppressed, so it is preferred. The positive C plate is preferably arranged on the opposite side of the green reflecting layer relative to the blue light reflecting layer, but it can also be arranged at other locations. At this time, the Re of the positive C plate is preferably less than about 10nm, and the Rth is preferably -600 to -100nm, and more preferably -400 to -200nm.
[0405] Furthermore, the positive C plate can be arranged adjacent to the phase difference layer or arranged inside the phase difference layer. As the phase difference layer, for example, when a layer formed by fixing a rod-like liquid crystal compound is used, the phase difference layer has a positive Rth. At this time, when light is incident from an oblique direction relative to the phase difference layer, the polarization state of the transmitted light changes due to the action of Rth, and sometimes the polarization degree of the transmitted light decreases. If there is a positive C plate inside or near the phase difference layer, the change in the polarization state of the oblique incident light can be suppressed, and the reduction in the polarization degree of the transmitted light can be suppressed, so it is preferred. The positive C plate is preferably arranged on the opposite side of the linear polarizer relative to the phase difference layer, but can also be arranged at other locations. At this time, the Re of the positive C plate is preferably less than about 10nm, and the Rth is preferably -90 to -40nm.
[0406] <Anti-reflection layer>
[0407] The laminated optical body also preferably has an anti-reflection layer on the surface. The laminated optical body has the function of reflecting specific circularly polarized light and transmitting circularly polarized light orthogonal thereto. The reflection on the surface of the laminated optical body usually includes the reflection of undesired polarized light, thereby reducing the polarization degree of the transmitted light. Therefore, the laminated optical body preferably has an anti-reflection layer on the surface. The anti-reflection layer can be provided on one surface of the laminated optical body, or on both surfaces.
[0408] The type of anti-reflection layer is not particularly limited, but from the viewpoint of further reducing the reflectivity, moth-eye film and AR film are preferred. Furthermore, when the laminated optical body is stretched or formed, even if the film thickness changes due to stretching, high anti-reflection performance can be maintained, so moth-eye film is preferred. Furthermore, when the anti-reflection layer includes a support and is stretched or formed, from the viewpoint of easy stretching or forming, the peak temperature of Tg of the support is preferably 170°C or less, more preferably 130°C or less. Specifically, for example, PMMA film is preferred.
[0409] <Second phase difference layer>
[0410] The laminated optical body also preferably further has a second retardation layer different from the retardation layer. For example, the laminated optical body may include a cholesteric liquid crystal layer, a retardation layer, a linear polarizer, and a second retardation layer in this order.
[0411] The second retardation layer preferably converts linearly polarized light into circularly polarized light, and for example, preferably has Re of 1 / 4 wavelength. The reason for this is described below.
[0412] Light incident on the stacked optical body from the cholesteric liquid crystal layer side and transmitting the cholesteric liquid crystal layer, the phase difference layer and the linear polarizer is linearly polarized light, a portion of which is reflected on the outermost surface on the linear polarizer side and emitted again from the surface on the cholesteric liquid crystal layer side. This light is unnecessary reflected light and may become a factor in reducing the polarization degree of the reflected light, so it is preferred to reduce it. Therefore, in order to suppress the reflection on the outermost surface on the linear polarizer side, there is also a method of stacking an anti-reflection layer, but when the stacked optical body is bonded to a medium such as glass and plastic for use, even if there is an anti-reflection layer on the bonding surface of the stacked optical body, the reflection on the surface of the medium cannot be suppressed, so the anti-reflection effect cannot be obtained.
[0413] On the other hand, when a second phase difference layer is provided to convert linear polarized light into circular polarized light, light reaching the outermost surface on one side of the linear polarizer becomes circular polarized light, and is converted into orthogonal circular polarized light when reflected at the outermost surface of the medium. After that, the light passes through the second phase difference layer again, and when it reaches the linear polarizer, the light becomes linear polarized light in the absorption axis orientation of the linear polarizer, and is absorbed by the linear polarizer. Therefore, unnecessary reflection can be prevented.
[0414] From the viewpoint of more effectively suppressing unnecessary reflection, the second retardation layer preferably has substantially anomalous dispersion properties.
[0415] <Support body>
[0416] The laminated optical body may further include a support. The support can be provided at any position, and for example, when the cholesteric liquid crystal layer, the phase difference layer, or the linear polarizer is a film transferred from a dummy support, the support can be used as the transfer destination.
[0417] The type of the support is not particularly limited, but is preferably transparent. For example, films such as cellulose acylate, polycarbonate, polysulfone, polyethersulfone, polyacrylate, polymethacrylate, cyclic polyolefin, polyolefin, polyamide, polystyrene, and polyester can be used. Among them, cellulose acylate films, cyclic polyolefin films, polyacrylate films, and polymethacrylate films are preferred. In addition, commercially available cellulose acetate films (e.g., "TD80U" and "Z-TAC" manufactured by FUJIFILM Corporation, etc.) can also be used.
[0418] Furthermore, from the viewpoint of suppressing the adverse effect on the polarization degree of transmitted light and facilitating optical inspection of the laminated optical body, the phase difference of the support is preferably small. Specifically, the size of Re is preferably less than 10 nm, and the absolute value of the size of Rth is preferably less than 50 nm.
[0419] When the laminated optical body is stretched or molded, the support preferably has a tan δ peak temperature of 170° C. or less. From the viewpoint of enabling molding at low temperatures, the tan δ peak temperature is preferably 150° C. or less, more preferably 130° C. or less.
[0420] Here, the method for measuring tanδ is described. Using a dynamic viscoelasticity measuring device (DVA-200 manufactured by ITKDVA), a film sample that has been humidified in an Rh atmosphere at a temperature of 25°C and a humidity of 60% for more than 2 hours is measured under the following conditions: E" (loss elastic modulus) and E' (storage elastic modulus), which are used as the value for calculating tanδ (=E" / E').
[0421] Device: DVA-200 manufactured by ITKDVA
[0422] Sample: 5mm, length 50mm (gap 20mm)
[0423] Measurement conditions: tensile mode
[0424] Measuring temperature: -150℃~220℃
[0425] Heating conditions: 5℃ / min
[0426] Frequency: 1Hz
[0427] In general optical applications, stretched resin substrates are often used, and the peak temperature of tan δ often becomes high due to the stretching process. For example, the peak temperature of tan δ of a TAC (triacetylcellulose) substrate (TG40, manufactured by FUJIFILM Corporation) is 180° C. or higher.
[0428] The support having a peak temperature of tanδ of 170°C or less is not particularly limited, and various resin substrates can be used. For example, polyolefins such as polyethylene, polypropylene, and norbornene polymers; cyclic olefin resins; polyvinyl alcohol; polyethylene terephthalate; acrylic resins such as polymethacrylate and polyacrylate; polyethylene naphthalate; polycarbonate; polysulfone; polyethersulfone; polyetherketone; polyphenylene sulfide and polyphenylene ether. Among them, cyclic olefin resins, polyethylene terephthalate, or acrylic resins are preferred from the viewpoint of easy market availability or excellent transparency, and cyclic olefin resins or polymethacrylates are particularly preferred.
[0429] Examples of commercially available resin substrates include TECHNOLLOY S001G, TECHNOLLOY S014G, TECHNOLLOY S000, TECHNOLLOY C001, TECHNOLLOY C000 (SUMIKA ACRYL CO., LTD.), Lumirror U type, Lumirror FX10, Lumirror SF20 (TORAY INDUSTRIE S, INC.), HK-53A (Higashiyama Film Co., Ltd.), Teflex FT3 (Teijin DuPont Films), "ESUSHINA" and SCA40 (SEKISUI CHEMICAL CO., LTD.), Zeonor Film (OPTES Corporation), and Arton Film (JSR Corporation).
[0430] The thickness of the support is not particularly limited, but is preferably 5 to 300 μm, more preferably 5 to 100 μm, and even more preferably 5 to 30 μm.
[0431] <Method of bonding each layer>
[0432] The laminated optical body is a laminated body composed of a plurality of layers. Each layer can be bonded by any bonding method, for example, a bonding agent or an adhesive can be used.
[0433] As the adhesive, any commercially available adhesive can be used. From the viewpoint of thinning and reducing the surface roughness Ra of the laminated optical body, the thickness of the adhesive layer is preferably 25 μm or less, more preferably 15 μm or less, and further preferably 6 μm or less. In addition, an adhesive that does not easily release gas is preferably used. In particular, when stretching or forming, vacuum treatment or heat treatment is sometimes required, and it is also preferable that no release gas is generated under these conditions.
[0434] As the adhesive, any commercially available adhesive or the like can be used, and for example, an epoxy resin adhesive and an acrylic resin adhesive can be used.
[0435] From the viewpoint of thinning and reducing the surface roughness Ra of the laminated optical body, the thickness of the adhesive layer is preferably 25 μm or less, more preferably 5 μm or less, and further preferably 1 μm or less. In addition, from the viewpoint of thinning the adhesive layer and applying the adhesive to the adherend with a uniform thickness, the viscosity of the adhesive is preferably 300 cP or less, more preferably 100 cP or less, and further preferably 10 cP or less.
[0436] Furthermore, when the adherend has a surface concavo-convex, from the viewpoint of reducing the surface roughness Ra of the laminated optical body, the adhesive and the bonding agent can also select suitable viscoelasticity or thickness so as to be able to embed the surface concavo-convex of the adherend layer. From the viewpoint of embedding the surface concavo-convex, the viscosity of the preferred adhesive and the bonding agent is more than 50cP. Furthermore, the preferred thickness is thicker than the height of the surface concavo-convex.
[0437] As a method for adjusting the viscosity of the adhesive, for example, a method of using an adhesive containing a solvent can be cited. At this time, the viscosity of the adhesive can be adjusted according to the ratio of the solvent. In addition, by applying the adhesive to the adherend and then drying the solvent, the thickness of the adhesive can be further reduced.
[0438] In the laminated optical body, from the viewpoint of reducing unnecessary reflection and suppressing the decrease in the polarization degree of transmitted light and reflected light, the adhesive or bonding agent used to bond each layer preferably has a small refractive index difference with the adjacent layer. Specifically, the refractive index difference between adjacent layers is preferably 0.1 or less, more preferably 0.05 or less, and further preferably 0.01 or less. The refractive index of the adhesive or bonding agent can be adjusted by mixing, for example, titanium oxide particles or zirconium oxide particles.
[0439] Furthermore, although the cholesteric liquid crystal layer, phase difference layer and linear polarizer have in-plane refractive index anisotropy, the refractive index difference with adjacent layers in all directions in the plane is preferably 0.05 or less. Therefore, the adhesive or pressure-sensitive adhesive may have in-plane refractive index anisotropy.
[0440] Furthermore, it is also preferred that the thickness of the adhesive layer between each layer is less than 100nm. If the thickness of the adhesive layer is less than 100nm, the refractive index difference is not easily perceived by light in the visible range, and unnecessary reflection can be suppressed. The thickness of the adhesive layer is more preferably less than 50nm. As a method for forming an adhesive layer with a thickness of less than 100nm, for example, a method of vapor-depositing a ceramic adhesive such as silicon oxide (SiOx layer) on the bonding surface can be cited. The bonding surface of the bonding component can be subjected to surface modification treatments such as plasma treatment, corona treatment, and saponification treatment and a primer layer can be given before bonding. Furthermore, when there are multiple bonding surfaces, the type or thickness of the adhesive layer can be adjusted according to the bonding surface. Specifically, for example, an adhesive layer with a thickness of less than 100nm can be provided in the order shown in the following (1) to (3).
[0441] (1) The laminated layers are bonded to a dummy support made of a glass substrate.
[0442] (2) A SiOx layer having a thickness of 100 nm or less is formed on both the surface of the stacked layer and the surface of the stacked layer by vapor deposition or the like. The vapor deposition can be performed using SiOx powder as a vapor deposition source, for example, using a vapor deposition device (model ULEYES) manufactured by ULVAC, Inc. In addition, it is preferred that a plasma treatment be performed in advance on the surface of the formed SiOx layer.
[0443] (3) After the formed SiOx layers are bonded together, the dummy support is peeled off. The bonding is preferably performed at a temperature of 120°C, for example.
[0444] The coating, bonding or lamination of each layer may be performed by a roll-to-roll method or a single wafer method. The roll-to-roll method is preferred from the viewpoint of improving productivity or reducing axial deviation of each layer.
[0445] On the other hand, the single wafer method is preferred in terms of suitability for small-volume and high-variety production or the ability to select a special bonding method such as the above-mentioned bonding layer having a thickness of 100 nm or less.
[0446] In addition, as a method for applying the adhesive to the adherend, for example, known methods such as roll coating, gravure printing, spin coating, wire bar coating, extrusion coating, direct gravure coating, reverse gravure coating, die coating, spray coating and inkjet coating can be cited.
[0447] <Direct coating of each layer>
[0448] It is also preferred that there is no adhesive layer between the layers of the laminated optical body. When forming the layers, the adhesive layer can be omitted by directly coating on the adjacent layers that have already been formed. Furthermore, when one or both of the adjacent layers are layers containing liquid crystal compounds, in order to reduce the refractive index difference in all directions in the plane, it is preferred to set the orientation direction of the liquid crystal compounds to change continuously at the interface. For example, a phase difference layer containing a liquid crystal compound is directly coated on a linear polarizer containing a liquid crystal compound and a dichroic substance. Through the orientation restriction force of the linear polarizer based on the liquid crystal compound, the liquid crystal compound can also be oriented so that the liquid crystal compound of the phase difference layer is continuous at the interface.
[0449] <Layer stacking order>
[0450] The laminated optical body is composed of a plurality of layers, but the order of the steps of laminating these layers is not particularly limited and can be arbitrarily selected.
[0451] For example, when transferring the functional layer from a film composed of a dummy support and a functional layer, the stacking order is adjusted so that the thickness of the film to be transferred becomes 10 μm or more, thereby preventing wrinkles and cracks during transfer.
[0452] Furthermore, from the viewpoint of reducing the surface roughness Ra of the laminated optical body, when another layer is laminated on a layer with large surface roughness, the surface roughness may be further amplified. Therefore, it is preferable to laminate in order from the layer with the smallest surface roughness Ra.
[0453] Furthermore, the order of stacking can be selected from the perspective of quality evaluation in the manufacturing process of the stacked optical body. For example, after stacking layers other than the cholesteric liquid crystal layer and performing quality evaluation based on the transmission optical system, the cholesteric liquid crystal layer can be stacked and the quality evaluation can be performed using the reflection optical system.
[0454] Furthermore, the order of stacking can be selected from the viewpoint of improving the manufacturing yield of the stacked optical body or reducing the cost.
[0455] As a preferred use example of the retardation film used in the second embodiment of the present invention, the stacked optical body including the retardation film, and the composite lens including the retardation film, a virtual reality display device using the stacked optical body is cited, and the function of the stacked optical body is described in detail.
[0456] Figure 3 It is a virtual reality display device using a stacked optical body. Figure 3As shown, the light 1000 emitted from the image display panel 500 passes through the circular polarizer 400 and becomes circularly polarized light, and then passes through the half mirror 300. Then, it passes through the lens 200, is incident on the stacked optical body 100 and is reflected, and after passing through the lens 200 again, it is reflected again in the half mirror 300, and then passes through the lens 200 again and is incident on the stacked optical body 100. At this time, the circularly polarized light state of the light 1000 does not change when it is reflected in the stacked optical body 100, but when it is reflected in the half mirror, it becomes a circularly polarized light orthogonal to the circularly polarized light when it is incident on the stacked optical body 100. Therefore, the light 1000 passes through the stacked optical body 100 and is visually recognized by the user. Furthermore, when the light 1000 is reflected in the half mirror 300, since the shape of the half mirror is a concave mirror, the image is magnified, and the user can visually recognize the magnified virtual image. The above-mentioned mechanism is called a reciprocating optical system or a folding optical system, etc.
[0457] on the other hand, Figure 4 This is a schematic diagram showing a situation where light 2000 is not reflected but transmitted as light leakage when it first enters the laminated optical body 100. As can be seen from the figure, at this time, the user visually recognizes an unmagnified image. This image is called a ghost image, etc., and it is required to be reduced.
[0458] The stacked optical body 100 satisfies the requirements of the second embodiment of the present invention, and thus can reduce leakage of transmitted light (ie, ghosting) when light first enters the stacked optical body 100 .
[0459] Furthermore, the stacked optical body 100 satisfies the requirements of the second embodiment of the present invention, and thus can improve the transmittance of light when it is incident on the stacked optical body 100 for the second time, increase the brightness of the virtual image, and further suppress the coloration of the virtual image.
[0460] like Figure 3 and Figure 4 As shown, the stacked optical body 100 is sometimes formed on a curved surface such as a lens. This can suppress the curvature of the image plane and improve pupil swimming. In addition, effects such as reducing chromatic aberration and expanding the viewing angle can be obtained.
[0461] For example, in a laminated optical body formed by laminating a reflective circular polarizer and a phase difference layer having a phase difference of 1 / 4 wavelength, the cholesteric liquid crystal layer does not have an optical axis and thus is less likely to be degraded in polarization due to stretching or forming.
[0462] A layer structure of a laminated optical body (100) is shown in Figure 5 In addition, Figure 5 In the figure, the non-planar shape of the stacked optical body as the optical film is not shown, but is simplified as a planar shape.
[0463] A cholesteric liquid crystal layer (101), a positive C plate (102), a phase difference layer (103), a linear polarizer (104), a phase difference layer (105), and an anti-reflection film (106) are sequentially arranged. In addition, when the stacked optical body is stretched or formed, the slow axis of the phase difference layer or the absorption axis of the linear polarizer may be distorted, but as described above, the cholesteric liquid crystal layer still maintains a high degree of polarization even after stretching or forming, and the amount of light leakage from the cholesteric liquid crystal layer is small, so the increase in leakage light can be suppressed to a small amount.
[0464] Furthermore, an example of the layer structure of the cholesteric liquid crystal layer (101) used in the second embodiment of the present invention is shown in FIG. Figure 6 A first light reflecting layer (131), a second light reflecting layer (132), a third light reflecting layer (133), and a fourth light reflecting layer (134) are sequentially arranged. Figure 6 In the figure, the non-planar shape of the cholesteric liquid crystal layer that the optical film may include is not shown, but is simplified as a planar shape.
[0465] Another embodiment of the laminated optical body (100B) having a different layer structure is shown in Figure 7 In addition, Figure 7 In the figure, the non-planar shape of the stacked optical body as the optical film is not shown, but is simplified as a planar shape.
[0466] In the stacked optical body (100B), a positive C plate (111), a phase difference layer (112), a linear polarized light type reflective polarizer (113), a linear polarizer (114), a phase difference layer (115) and an anti-reflection film (116) are arranged in sequence.
[0467] Furthermore, the surface roughness Ra of the stacked optical body is preferably less than 100 nm. If Ra is small, it is preferred because the clarity of the image can be improved when the stacked optical body is applied to a virtual reality display device, etc. The inventors of the present invention speculate that when light is reflected in the stacked optical body, if there are bumps, it will cause angular distortion of the reflected light, distortion or blurring of the image. The Ra of the stacked optical body is preferably less than 50 nm, more preferably less than 30 nm, and further preferably less than 10 nm.
[0468] Furthermore, the laminated optical body is made by laminating a plurality of layers. When another layer is laminated on a layer having concavoconvexity, the concavoconvexity is sometimes magnified. Therefore, in the laminated optical body, it is preferred that the Ra of all layers is small. The Ra of each layer of the laminated optical body is preferably 50 nm or less, more preferably 30 nm or less, and further preferably 10 nm or less.
[0469] Furthermore, from the viewpoint of improving the image clarity of a reflected image, it is particularly preferred that the Ra of the cholesteric liquid crystal layer is small.
[0470] The surface roughness Ra can be measured, for example, using a non-contact surface / layer cross-section shape measuring system VertScan (manufactured by Mitsubishi Chemical Systems, Inc.). Since Vertscan is a surface shape measuring method that uses the phase of the reflected light from the sample, when measuring a cholesteric liquid crystal layer composed of a light reflecting layer formed by a fixed cholesteric liquid crystal phase, sometimes the reflected light from the inside of the film overlaps and the surface shape cannot be accurately measured. At this time, in order to increase the reflectivity of the surface to further suppress the reflection from the inside, a metal layer can be formed on the surface of the sample. As the main method for forming a metal layer on the surface of the sample, a sputtering method is used. As sputtering materials, Au, Al, Pt, etc. are used.
[0471] The number of point defects per unit area of the stacked optical body is preferably small. Since the stacked optical body is made by stacking a plurality of layers, in order to reduce the number of point defects of the stacked optical body as a whole, the number of point defects in each layer is also preferably small. Specifically, the number of point defects in each layer is preferably 20 or less per square meter, more preferably 10 or less, and further preferably 1 or less. As for the stacked optical body as a whole, the number of point defects is preferably 100 or less per square meter, more preferably 50 or less, and further preferably 5 or less.
[0472] Point defects may lead to a decrease in the polarization degree of transmitted light or a decrease in image clarity, and therefore, the fewer the point defects, the better.
[0473] Here, the point defects include foreign matter, scratches, dirt, film thickness variation, and poor orientation of liquid crystal compounds.
[0474] Furthermore, regarding the number of the point defects, it is preferred that the number of point defects having a size of preferably 100 μm or more (more preferably 30 μm or more, and most preferably 10 μm or more) be counted.
[0475] Furthermore, in order to minimize the impact on various sensors that use near-infrared light as a light source, such as eye tracking, expression recognition, and iris authentication, which are incorporated into optical systems such as virtual reality display devices and electronic viewfinders, the laminated optical body is preferably transmissive to near-infrared light.
[0476] <Compound lens>
[0477] One form of the composite lens includes a lens and an optical film of the second embodiment of the present invention. A half-reflecting mirror can be formed on one side of the lens. As the lens, a convex lens and a concave lens can be used. As the convex lens, a biconvex lens, a plano-convex lens and a convex meniscus lens can be used. As the concave lens, a biconcave lens, a plano-concave lens and a concave meniscus lens can be used.
[0478] As a lens used for a virtual reality display device, in order to expand the viewing angle, a convex meniscus lens or a concave meniscus lens is preferred, and from the viewpoint of further suppressing chromatic aberration, a concave meniscus lens is more preferred.
[0479] As the lens material, materials transparent to visible light such as glass, crystal, and plastic can be used. Since the birefringence of the lens may cause rainbow spots or light leakage, it is preferred to have a small birefringence, and a material with zero birefringence is more preferred.
[0480] <Virtual reality display device>
[0481] One form of a virtual reality display device includes at least an image display device that emits polarized light and a composite lens including the optical film of the second embodiment of the present invention, and may also include additional optical components such as a half mirror or a diopter adjustment lens.
[0482] <Image display device>
[0483] As an image display device used in the second embodiment of the present invention, a known image display device can be used. For example, an organic electroluminescent display device, an LED (Light Emitting Diode) display device, and a micro-LED display device, etc., in which self-luminous fine light-emitting bodies are arranged on a transparent substrate, can be exemplified. These self-luminous display devices usually have a (circular) polarizer attached to the display surface to prevent reflection of the display surface. Therefore, the outgoing light is polarized. In addition, a liquid crystal display device is exemplified as another image display device. The liquid crystal display device also has a polarizer on the surface, so the outgoing light is polarized. In the following description, the organic electroluminescent display device is also referred to as an OLED. OLED is the abbreviation of "Organic Light Emitting Diode".
[0484] <Molding method>
[0485] The method for manufacturing the optical film having a non-planar shape is not particularly limited.
[0486] Among them, the optical film forming method of the second embodiment of the present invention preferably includes: a step of heating an optical film having a planar shape; a step of pressing the heated optical film against a mold to deform it along the shape of the mold; and a step of cutting the optical film.
[0487] Hereinafter, each step will be described in detail.
[0488] (Step of heating the optical film having a planar shape)
[0489] The optical film used in this step has a planar shape. As described below, a predetermined shape is transferred to the optical film having a planar shape to obtain the optical film having a non-planar shape.
[0490] The optical film having a planar shape includes various components that the optical film having a non-planar shape may have (for example, a phase difference film, etc.). Among them, the various components included in the optical film having a planar shape have a planar shape.
[0491] Methods for heating an optical film having a planar shape include heating based on contact with a heated solid, heating based on contact with a heated liquid, heating based on contact with a heated gas, heating based on irradiation of infrared rays, and heating based on irradiation of microwaves. Heating based on irradiation of infrared rays that can be remotely heated immediately before forming is preferred.
[0492] The wavelength of the infrared light used for heating is preferably 1.0 μm to 30.0 μm, more preferably 1.5 μm to 5 μm.
[0493] As an IR light source, a near-infrared lamp heater formed by sealing a tungsten filament in a quartz tube or a wavelength control heater as a mechanism of multiplexing a quartz tube and cooling a part of the quartz tubes with air can be used. In addition, by imparting an infrared irradiation amount distribution on the optical film, the physical property value during molding can be controlled according to the purpose. As a method of imparting an intensity distribution, a method of setting a density of the configuration density of the IR light source and a method of configuring a filter that patterns the transmittance of infrared light between the IR light source and the optical film can be used. As a filter that patterns the transmittance, a filter that evaporates metal on glass, a filter that infraredizes the reflection band of a cholesteric liquid crystal layer, a filter that infraredizes the reflection band in a dielectric multilayer film, and a filter coated with an infrared absorbing ink are used. Regarding the temperature control of the optical film, it is controlled by the intensity of the infrared irradiation, and it is controlled by the infrared irradiation time or the illuminance of the infrared irradiation. The temperature of the optical film can be monitored using a non-contact radiation thermometer or a thermocouple, and can be molded at a target temperature.
[0494] (Step of pressing the optical film against the mold and deforming it along the shape of the mold)
[0495] As a method of pressing the heated optical film against the mold and deforming it along the shape of the mold, a method of reducing pressure and / or increasing pressure in the molding space can be used. Alternatively, a method of pressing the film into the mold can be used.
[0496] In one form of the forming device used in this process, it is composed of a mold box 1 having an opening in the upper direction and a mold box 2 having an opening in the lower direction. In order to form a forming space, the opening of the mold box 1 is directly or via other fixtures to splice the opening of the mold box 2, thereby forming a closed forming space. A mold (also called an adherend) of a shape to be formed and a formed film to be formed are arranged in the forming space. The formed film serves as a partition to divide the forming space composed of the mold box 1 and the mold box 2 into two spaces. The mold is arranged on the side of the mold box 1 on the lower side of the formed film. The vacuum forming device is further dispersedly configured with a plurality of heating elements for heating the formed film. The heating element can be arranged in the forming space, or it can be arranged outside the forming space and heat and irradiate the formed film through a transparent window.
[0497] (Optical film cutting process)
[0498] As a method of cutting the formed optical film into an arbitrary shape, a cutter, scissors, a plotter, a laser cutter, or the like can be used.
[0499] <Concept of the molding method that does not generate phase difference distribution>
[0500] In order to form an optical film having a planar shape to obtain the above-mentioned optical film having a non-planar shape and an in-plane deviation of the phase difference of less than 5%, it is preferred that the in-plane distribution of the phase difference is not generated during the forming. Hereinafter, the concept of the forming method without generating the phase difference distribution is described in detail, taking the phase difference film included in the optical film as an example.
[0501] As described above, it is preferable that when the retardation film is formed into a curved surface, no in-plane distribution of the retardation occurs. Thus, even when a retardation film formed into a curved surface is used in a pancake lens in a virtual reality display device, the occurrence of ghosting can be suppressed.
[0502] The reason why the phase difference of the phase difference film is distributed in the plane is that the film thickness d after forming is different according to the position, so the product of the birefringence Δn and the film thickness d, that is, the phase difference Re, has an in-plane distribution. The reason why the film thickness d has an in-plane distribution is that the stretching ratio during forming (the product of the stretching ratios of the two orthogonal directions) will be different according to the position. Therefore, in order to suppress this situation, it is necessary to deform it into the shape of the curved surface of the mold while making the product of the stretching ratios of the two orthogonal directions constant. As two orthogonal directions, for example, the center of gravity position of the mold shape during curved surface forming is set to point O, and when a circular coordinate system centered on point O is assumed, the product of the radial (direction in which the straight line connecting the position of each point to point O extends) stretching ratio of each point and the circumferential (direction orthogonal to the radial) stretching ratio is preferably constant. Here, constant means that when the in-plane deviation (%) is expressed as {(maximum value-minimum value) / average value}×100, it is preferably less than 5%, more preferably less than 3%, and further preferably less than 1%. The lower limit is not particularly limited, and 0% is exemplified.
[0503] In addition, the calculation method of the stretching ratio in the radial direction and the stretching ratio in the circumferential direction will be described later.
[0504] By setting the deviation of the product of the radial stretch ratio and the circumferential stretch ratio to less than 5%, the film thickness unevenness can be suppressed to less than 5%, thereby suppressing the phase difference unevenness to less than 5%.
[0505] Furthermore, by setting the deviation of the product of the radial stretch ratio and the circumferential stretch ratio to less than 3%, the film thickness unevenness can be suppressed to less than 3%, thereby suppressing the phase difference unevenness to less than 3%.
[0506] Furthermore, by setting the deviation of the product of the radial stretch ratio and the circumferential stretch ratio to less than 1%, the film thickness unevenness can be suppressed to less than 1%, thereby suppressing the phase difference unevenness to less than 1%.
[0507] As a specific stretching property for achieving this, it is preferred that the stretching ratio in the radial direction increases as the distance from the point O increases. More preferably, when the distance from the point O is set to x, the stretching ratio in the radial direction satisfies the following formula.
[0508] Radial stretch ratio = p*x / R / sqrt(1-(1-p*x 2 / 2 / R 2 ) 2 )
[0509] Here, * represents a product, sqrt represents a square root, p represents a product of a radial stretching ratio and a circumferential stretching ratio, and R represents a radius of curvature of a mold.
[0510] <How to set up the mold>
[0511] There is no particular limitation on the method of setting the mold in the forming device. For example, a horizontally movable mounting table with a top plate can be set in the mold box 1 at the lower side of the above-mentioned forming device, and the mold can be set on the mounting table. In this case, after the inside of the forming device is evacuated, the movable mounting table is raised, so that the mold can be pressed against the film to be formed.
[0512] Furthermore, the mold provided on the mounting table may be one or more. From the viewpoint of improving productivity, a plurality of molds may be provided to simultaneously produce a plurality of molded bodies by using a film to be formed whose area is larger than the mold area.
[0513] <Jig for holding the mold>
[0514] And, also preferably, in order to prevent the mold from moving on the stage, use a fixture having a groove that can be embedded in the mold to hold the mold. By processing like this, the mold can be fixed so that it does not move on the stage.
[0515] Furthermore, the fixture for holding the mold preferably covers the surface other than the forming surface of the mold (the surface to which the formed film is attached). When the formed film is intended to cover the forming surface of the mold and the end surface of the mold other than the forming surface, the formed film will be greatly stretched, which may sometimes cause significant unevenness in the film thickness or optical properties of the film. Therefore, it is preferred to use a fixture that covers the surface other than the forming surface of the mold to prevent the formed film from contacting the surface other than the forming surface.
[0516] And, the fixture preferably has the same height as the forming surface of the mold and has a horizontal plane at the part where the mold does not exist. By processing in this way, the part of the formed film outside the forming surface of the mold can be suppressed from being stretched, and the uniformity of the film thickness or optical properties of the film can be improved.
[0517] Furthermore, when the film to be formed is formed in the mold, it is preferred that the movable mounting table on which the clamp and the mold are installed is raised until the position of the molding surface of the mold is approximately equal to the height of the film to be formed. By doing so, it is possible to prevent the film to be formed from contacting the end surface of the clamp and being greatly stretched.
[0518] The clamp may be integrated with the mounting table.
[0519] <Method of bonding optical film to adherend>
[0520] The method of bonding the optical film to the adherend is not particularly limited. For example, after the optical film is formed into a curved shape by any of the above methods, it can be bonded to an adherend such as a lens using an adhesive or the like.
[0521] Furthermore, from the viewpoint of simplifying the process, it is preferred that a pressure-sensitive adhesive sheet is previously bonded to the surface of the optical film that contacts the mold, and the film is bonded to the curved surface of the mold while being formed into a curved shape.
[0522] <Evaluation method of stretch ratio>
[0523] In order to evaluate the stretching ratio at each location of the forming method, for example, Figure 8 The pattern shown is drawn on the film before forming. As an example of this pattern, circles (for example, Figure 8 The radius of the inscribed circle represented by the solid line is 20 mm, and the circles represented by the dotted lines with a radius of 5 mm are drawn. In the azimuth direction, straight lines with equal intervals of 45 degrees are drawn ( Figure 8 The straight line in the circle is the straight line of the film). In addition, the center of the circle is equivalent to the center of gravity of the film. Moreover, the straight lines mentioned above are all straight lines passing through the center of the circle. The coordinates of the intersections of the pattern are measured before and after forming, and the rate of change between adjacent intersections is obtained, thereby being able to evaluate the radial stretch ratio. More specifically, when the distance between the two points located in the radial direction and before forming is set to L0, and the distance between the two points after forming is set to L1, the stretch ratio can be obtained by calculating L1 / L0. According to the above order, 32 L1 / L0 are calculated as the radial stretch ratio of each point.
[0524] Furthermore, by using the coordinates of each intersection relative to the center of the circle, the circumferential stretch ratio can be evaluated. More specifically, the distance from the center before forming is set to r0, and the distance between the center and the intersection when projected onto a plane parallel to the tangent plane of the center after forming is set to r1. The circumference of the circle depicted by this distance changes from 2πr0 to 2πr1, so the circumferential stretch ratio can be calculated as r1 / r0. r0 and r1 can be obtained from the xyz coordinates of each point (the center is the origin 0,0,0), by r0=sqrt(x0 2 +y0 2 )、r1=sqrt(x1 2 +y1 2 According to the above procedure, r0 is appropriately changed, and r1 / r0 of the 32 points of the radial stretching ratio is calculated as the stretching ratio of each point in the circumferential direction.
[0525] The product of the stretch ratio in the radial direction and the stretch ratio in the circumferential direction (direction perpendicular to the radial direction) at each of the 32 points calculated as above is calculated, and the maximum value, minimum value and average value are obtained to calculate the above-mentioned in-plane deviation (%).
[0526] <Molding method 1 that does not generate phase difference distribution>
[0527] As an example of a forming method that does not produce a phase difference distribution, there can be cited a forming method for an optical film, which includes: a heating step of heating an optical film having a planar shape; a first forming step of pressing the heated optical film onto a first mold and deforming it along the shape of the first mold; and a second forming step of pressing the optical film formed in the first forming step onto a second mold and deforming it along the shape of the second mold.
[0528] In the above-mentioned forming method, preferably, the shape of the first mold includes a convex curved surface portion, and the shape of the second mold includes a concave curved surface portion.
[0529] Furthermore, in the above-mentioned forming method, it is preferred that the radius of curvature of the first mold is larger than the radius of curvature of the second mold.
[0530] This can provide a molding characteristic in which the radial stretch ratio increases as the distance from the center increases. As a result, it is possible to suppress the deviation of the product of the radial stretch ratio and the circumferential ratio, the uneven film thickness, and the uneven phase difference.
[0531] Hereinafter, preferred aspects of the above method will be described in more detail.
[0532] First, refer to Figures 9-11 , the phenomenon that occurs when a film is formed using a forming mold having a concave forming surface is described. Fig. 9 and 10 The following is a sequence for forming a film using a forming die having a concave forming surface. Fig.11 The film used for forming is shown.
[0533] like Fig. 9 As shown, a circular film 222 is arranged on a forming mold 220 having a concave forming surface, as shown in FIG. Fig.10 As shown, the film 222 is deformed along the molding surface of the molding die 220, thereby obtaining a film 224 to which the concave shape is transferred.
[0534] Usually, when this concave surface is formed, the surrounding Fig. 9 and 11 The central portion 222C of the film 222 shown and the peripheral portion 222R of the central portion 222C have different stretching ratios. More specifically, the central portion 222C of the film 222 is more easily stretched than the peripheral portion 222R of the film 222. As a result, in the film 224 to which the concave shape is transferred, the film thickness of the central portion 224C is thinner than the film thickness of the peripheral portion 224R.
[0535] Next, refer to Figures 11 to 13 , the phenomenon that occurs when a film is formed using a forming mold having a convex forming surface is described. Fig.12 and 13The following is a sequence for forming a film using a forming die having a convex forming surface. Fig.11 The film used for forming is shown.
[0536] like Fig.12 As shown, a circular film 222 is arranged on a forming die 226 having a convex forming surface, as shown in FIG. Fig.13 As shown, the film 222 is deformed along the molding surface of the molding die 226, thereby obtaining a film 228 to which a convex shape is transferred.
[0537] Usually, in this convex surface forming, Fig.11 and 12 The central portion 222C and the peripheral portion 222R of the film 222 shown in the figure have different stretching ratios. More specifically, the peripheral portion 222R of the film 222 is more easily stretched than the central portion 222C of the film 222. As a result, in the film 228 to which the convex shape is transferred, the film thickness of the peripheral portion 228R is thinner than the film thickness of the central portion 228C.
[0538] As described above, when the concave surface is formed, the film thickness in the center portion of the obtained film is thinner than the film thickness in the peripheral portion, and when the convex surface is formed, the film thickness in the peripheral portion of the obtained film is thinner than the film thickness in the center portion.
[0539] Therefore, as described above, as a preferred form of the above-mentioned forming method 1, there can be cited a manufacturing method comprising the following steps: step 1A, using a forming mold having a convex-shaped forming surface to deform a planar-shaped optical film along the forming surface of the forming mold; and step 2A, using a forming mold having a concave-shaped forming surface with a curvature radius smaller than the curvature radius of the above-mentioned convex-shaped forming surface, using the surface of the optical film to which the convex shape obtained by the step 1A is transferred, which is opposite to the surface contacting the forming mold of the step 1A, as the forming surface side of the above-mentioned forming mold, to deform the optical film to which the convex shape is transferred along the above-mentioned concave-shaped forming surface.
[0540] Hereinafter, a preferred embodiment of the above-mentioned forming method 1 will be described with reference to the drawings.
[0541] In a preferred embodiment of the molding method 1, first, a step 1A is performed in which a molding die having a convex molding surface is used to deform a planar optical film along the molding surface of the molding die. By performing this step, Fig.14 As shown, an optical film 232 having a convex shape transferred to a molding die 230 having a convex shape molding surface can be obtained. In the optical film 232, as shown in the above Fig.12 and 13 As described above, the film thickness of the peripheral portion 232R of the optical film 232 is thinner than the film thickness of the central portion 232C.
[0542] Next, a step 2A is performed in which a molding die having a concave-shaped molding surface having a smaller curvature radius than the convex-shaped molding surface is used, and the surface of the optical film having the convex shape transferred thereto obtained in step 1A is opposite to the surface in contact with the molding die in step 1A, and the optical film having the convex shape transferred thereto is deformed along the concave-shaped molding surface. The molding die 234 having a concave-shaped molding surface used in step 2A has a smaller curvature radius than the molding die 230 having a convex-shaped molding surface used in step 1A. In step 2A, first, as Fig.15 As shown in FIG. 1 , the optical film 232 obtained in step 1A is arranged on a molding die 234 having a molding surface with a smaller curvature radius than the molding die 230 used in step 1A. When the optical film 232 is arranged on the molding die 234, the surface of the optical film 232 opposite to the surface in contact with the molding die 230 is arranged on the molding surface side of the molding die 234. Next, as shown in FIG. Fig.16 As shown, by deforming the optical film 232 along the molding surface of the molding die 234, an optical film 236 having a curved surface can be obtained.
[0543] As reference Fig. 9 and 10 As described above, during concave surface forming, the film thickness at the center portion is usually thinner than that at the peripheral portion. Therefore, during step 2A, the thickness reduction at the center portion 232C of the optical film 232 is greater than that at the peripheral portion 232R.
[0544] That is, in process 1A, the reduction in film thickness at the peripheral portion of the optical film is greater than the reduction in film thickness at the central portion, and in process 2A, the reduction in film thickness at the central portion of the optical film is greater than the reduction in film thickness at the peripheral portion. Therefore, when performing process 1A and process 2A, the reduction in film thickness at the central portion and the peripheral portion is approximately the same. As a result, in-plane deviation of film thickness can be suppressed in the obtained optical film 236.
[0545] As described above, the curvature radius of the molding surface of the molding die used in step 2A is smaller than the curvature radius of the molding surface of the molding die used in step 1A.
[0546] The ratio (CA2 / CA1) of the radius of curvature (CA2) of the molding surface of the molding mold used in step 2A to the radius of curvature (CA1) of the molding surface of the molding mold used in step 1A is selected to be an optimal value according to the optical film to be manufactured, preferably 0.6 to 0.9, and more preferably 0.7 to 0.85.
[0547] When the radius of curvature varies depending on the position of the molding surface of the molding die used in step 1A, the smallest radius of curvature is defined as the "radius of curvature of the molding surface of the molding die used in step 1A".
[0548] When the radius of curvature varies depending on the position of the molding surface of the molding die used in step 2A, the smallest radius of curvature is defined as the "radius of curvature of the molding surface of the molding die used in step 2A".
[0549] [Molding method 2 that does not generate phase difference distribution]
[0550] As another example of a forming method that does not produce a phase difference distribution, there is a forming method for an optical film, which includes: a process of heating an optical film having a planar shape; a process of pressing the heated optical film onto a mold and deforming it along the shape of the mold; and a process of cutting the deformed optical film, wherein the heating process is a process of heating the optical film by irradiating infrared rays, and the amount of infrared rays irradiated is distributed within the surface of the optical film.
[0551] Among them, in the above-mentioned molding method, it is preferred that the mold is essentially a concave spherical shape, and when the position of the optical film within the surface is projected onto the mold from the normal direction of the surface of the optical film, the amount of infrared light irradiated on the optical film located at the vertex of the concave sphere is less than the amount of infrared light irradiated on the optical film located at the end of the concave sphere.
[0552] Furthermore, in the above-mentioned molding method, preferably, the mold is substantially in the shape of a concave sphere, and when the position within the surface of the optical film is projected onto the mold from the normal direction of the surface of the optical film, the temperature of the optical film located at the vertex of the concave sphere is lower than the temperature of the optical film located at the end of the concave sphere.
[0553] This can provide a molding characteristic in which the radial stretch ratio increases as the distance from the center increases. As a result, it is possible to suppress the deviation of the product of the radial stretch ratio and the circumferential ratio, the uneven film thickness, and the uneven phase difference.
[0554] Hereinafter, preferred aspects of the above method will be described in more detail.
[0555] As described above, when a molding die having a concave molding surface is used, the film thickness in the center portion of the film tends to be thinner than the film thickness in the peripheral portion.
[0556] Therefore, in the preferred embodiment of the above-mentioned forming method 2, as Fig.17 and 18As shown in the figure, by making the heating temperature of the peripheral portion 242R of the planar optical film 242 disposed on the forming mold 240 having a concave forming surface higher than the heating temperature of the central portion 242C based on infrared irradiation, the peripheral portion 242R is easily stretched when the optical film 242 is deformed along the forming surface. That is, as described above, in general, in the forming using the forming mold having a concave forming surface, the reduction amount of the film thickness of the central portion is greater than the reduction amount of the film thickness of the peripheral portion. In contrast, by changing the heating conditions of the central portion and the peripheral portion, the central portion is made more difficult to stretch, the peripheral portion is made easier to stretch, the reduction amount of the film thickness of the central portion is suppressed, and the reduction amount of the film thickness of the peripheral portion is increased. As a result, in the deformed optical film, the in-plane deviation of the film thickness can be suppressed.
[0557] In the present invention, the first embodiment and the second embodiment can be used in combination.
[0558] For example, the optical functional film of the first embodiment and the optical film forming method of the second embodiment may be used in combination. As an example, the optical functional film of the first embodiment may be formed by the forming method 1 or the forming method 2 of the second embodiment to produce an optical film having a non-planar shape.
[0559] The above is an example of the combination of the first embodiment and the second embodiment, and the present invention is not limited to the above combination.
[0560] Example
[0561] Below, give embodiment, feature of the present invention is described in more detail.In addition, material, usage, ratio, processing content and processing sequence etc. shown below, as long as do not depart from the gist of the present invention, then can be appropriately changed.And, as long as do not depart from the gist of the present invention, also can adopt the structure other than the structure shown below.
[0562] <<First embodiment>>
[0563] [Preparation of phase difference layer 1]
[0564] Referring to the method described in paragraphs 0151 to 0163 of Japanese Patent Application No. 2020-084070, a phase difference layer 1 with abnormal dispersion was prepared on a pseudo support composed of a cellulose acylate film using a phase difference layer forming coating liquid A1 containing a liquid crystal compound having a polymerizable group. The irradiation amount of ultraviolet rays when irradiating the coating film of the coating liquid A1 with ultraviolet rays in order to polymerize the liquid crystal compound was reduced from 300 mJ / cm 2 Changed to 50mJ / cm 2 .
[0565] The phase difference of the obtained phase difference layer 1 was Re=146 nm and Rth=73 nm. The polymerization rate of the liquid crystal compound in the phase difference layer 1 was 26%. In the phase difference layer 1, the liquid crystal compound was aligned in one direction.
[0566] In addition, in this embodiment, the phase difference of each optical functional film or each layer was measured by the above method using AxoScan OPMF-1 (manufactured by OPTO SCIENCE, INC.). In addition, the polymerization rate of the liquid crystal compound of each optical functional film or each layer was measured by the above method of observing the absorption peak based on the polymerizable group using an infrared spectrophotometer ("FTS-6000" manufactured by Bio-Rad Laboratories, Inc.).
[0567] When the virtual reality display devices of Examples 1 and 2 were produced, the phase difference layer 1 produced in this way was used as an optical functional film.
[0568] [Production of phase difference layer 2]
[0569] The irradiation amount of ultraviolet rays irradiated to the coating film of the coating liquid A1 for polymerizing the liquid crystal compound was changed to 300 mJ / cm 2 , except for this, the phase difference layer 2 was produced by the same method as the phase difference layer 1.
[0570] The phase difference of the obtained phase difference layer 2 was Re = 145 nm, Rth = 72 nm. The polymerization rate of the liquid crystal compound contained in the phase difference layer 2 was 73%, and the liquid crystal compound was aligned in one direction in the phase difference layer 2.
[0571] When the virtual reality display device of Comparative Example 1 was produced, the phase difference layer 2 produced in this way was used as an optical functional film.
[0572] [Preparation of coating liquid for cholesteric liquid crystal layer]
[0573] (Coating liquid for cholesteric liquid crystal layer R-1)
[0574] The composition shown below was stirred and dissolved in a container maintained at a temperature of 70° C., thereby preparing a coating liquid R-1 for a cholesteric liquid crystal layer. Here, R represents a coating liquid containing a rod-like liquid crystal compound.
[0575]
[0576]
[0577] (Coating liquid for cholesteric liquid crystal layer R-2)
[0578] A cholesteric liquid crystal layer coating liquid R-2 was prepared in the same manner as the cholesteric liquid crystal layer coating liquid R-1 except that the addition amount of the chiral agent A was changed as shown in the following table.
[0579] Table 1. Amount of chiral agent in coating solution containing rod-shaped liquid crystal compound [Table 1]
[0580]
[0581] Mixture of rod-like liquid crystal compounds
[0582] [Chemical formula 1]
[0583]
[0584] In the above mixture, the numerical values are mass %, and R is a group bonded to an oxygen atom. Furthermore, the rod-shaped liquid crystal compound has an average molar absorption coefficient of 140 / mol·cm at a wavelength of 300 to 400 nm.
[0585] Chiral Reagent A
[0586] [Chemical formula 2]
[0587]
[0588] Surfactant F1
[0589] [Chemical formula 3]
[0590]
[0591] Surfactant F2
[0592] [Chemical formula 4]
[0593]
[0594] Photopolymerization initiator B
[0595] [Chemical formula 5]
[0596]
[0597] Chiral reagent A is a chiral reagent whose helical twisting power (HTP: Helical Twisting Power) decreases due to light.
[0598] (Coating liquid for cholesteric liquid crystal layer D-1)
[0599] The composition shown below was stirred and dissolved in a container maintained at a temperature of 50° C. to prepare a coating liquid D-1 for a cholesteric liquid crystal layer. Here, D represents a coating liquid containing a discotic liquid crystal compound.
[0600]
[0601]
[0602] (Coating liquid for cholesteric liquid crystal layer D-2)
[0603] A cholesteric liquid crystal layer coating liquid D-2 was prepared in the same manner as the cholesteric liquid crystal layer coating liquid D-1, except that the addition amount of the chiral agent A was changed as shown in Table 2 below.
[0604] Table 2. Amount of chiral agent in coating solution containing discotic liquid crystal compound [Table 2]
[0605]
[0606] Discotic liquid crystal compound (A)
[0607] [Chemical formula 6]
[0608]
[0609] Discotic liquid crystal compound (B)
[0610] [Chemical formula 7]
[0611]
[0612] Polymerizable monomer E1
[0613] [Chemical formula 8]
[0614]
[0615] Surfactant F4
[0616] [Chemical formula 9]
[0617]
[0618] [Preparation of Cholesteric Liquid Crystal Layer 1]
[0619] As a pseudo support, a PET (polyethylene terephthalate) film (A4100 manufactured by TOYOBO CO., LTD.) having a thickness of 50 μm was prepared. The PET film had an easy-adhesion layer on one side.
[0620] The surface without the easy-adhesive layer of the PET film was rubbed, and the above-prepared cholesteric liquid crystal layer coating liquid R-1 was applied using a wire bar coater, and then dried at 110°C for 120 seconds. Thereafter, the surface was irradiated at 100°C with an illumination of 40 mW / cm2 in a low oxygen atmosphere (less than 100 ppm).2 、Irradiation 50mJ / cm 2 The coating was cured by light from a metal halide lamp, thereby forming a red light reflecting cholesteric liquid crystal layer composed of a cholesteric liquid crystal layer. The light irradiation was performed from the cholesteric liquid crystal layer side. At this time, the coating thickness was adjusted so that the film thickness of the red light reflecting cholesteric liquid crystal layer after curing became 4.5 μm.
[0621] The polymerization rate of the liquid crystal compound of the obtained red light reflecting cholesteric liquid crystal layer was 17%.
[0622] Next, the discharge rate was 150W·min / m 2 After the surface of the red light reflecting cholesteric liquid crystal layer was subjected to corona treatment, the cholesteric liquid crystal layer coating liquid D-1 was applied to the corona treated surface using a wire bar coater. Next, the coating film was dried at 70°C for 2 minutes to vaporize the solvent, and then heated and aged at 115°C for 3 minutes to obtain a uniform orientation state. Thereafter, the coating film was irradiated with ultraviolet rays (irradiation amount: 50 mJ / cm2) using a metal halide lamp in a nitrogen atmosphere while maintaining the temperature at 45°C. 2 ) to cure, thereby forming a yellow light reflecting cholesteric liquid crystal layer on the red light reflecting cholesteric liquid crystal layer. The light irradiation is performed from the cholesteric liquid crystal layer side. At this time, the coating thickness is adjusted so that the film thickness of the yellow light reflecting cholesteric liquid crystal layer after curing becomes 3.3 μm.
[0623] The polymerization rate of the liquid crystal compound of the obtained yellow light reflecting cholesteric liquid crystal layer was 21%.
[0624] Next, the coating liquid R-2 for the cholesteric liquid crystal layer was applied onto the yellow light reflecting cholesteric liquid crystal layer using a wire bar coater and then dried at 110°C for 120 seconds. Thereafter, the coating liquid R-2 was irradiated at 100°C with an illumination of 40 mW and an irradiation amount of 50 mJ / cm in a low oxygen atmosphere (less than 100 ppm). 2 The green light reflecting cholesteric liquid crystal layer was formed on the yellow light reflecting cholesteric liquid crystal layer by curing with the light of a metal halide lamp. The light irradiation was performed from the cholesteric liquid crystal layer side. At this time, the coating thickness was adjusted so that the film thickness of the green light reflecting cholesteric liquid crystal layer after curing became 2.7 μm.
[0625] The polymerization rate of the liquid crystal compound of the obtained green light reflecting cholesteric liquid crystal layer was 19%.
[0626] Next, the discharge rate was 150W·min / m 2After the surface of the green light reflecting cholesteric liquid crystal layer was subjected to corona treatment, the cholesteric liquid crystal layer coating liquid D-2 was applied to the corona treated surface using a wire bar coater. Next, the coating film was dried at 70°C for 2 minutes to vaporize the solvent, and then heated and aged at 115°C for 3 minutes to obtain a uniform orientation state. Thereafter, the coating film was irradiated with ultraviolet rays (irradiation amount: 50 mJ / cm2) using a metal halide lamp in a nitrogen atmosphere while maintaining the temperature at 45°C. 2 ) to cure, thereby forming a blue light reflecting cholesteric liquid crystal layer on the green light reflecting cholesteric liquid crystal layer. The light irradiation is performed from the cholesteric liquid crystal layer side. At this time, the coating thickness is adjusted so that the film thickness of the blue light reflecting cholesteric liquid crystal layer after curing becomes 2.5 μm.
[0627] The polymerization rate of the liquid crystal compound of the obtained blue light reflecting cholesteric liquid crystal layer was 24%.
[0628] In this way, a cholesteric liquid crystal layer 1 (optically functional film) in which the red light reflecting cholesteric liquid crystal layer, the yellow light reflecting cholesteric liquid crystal layer, the green light reflecting cholesteric liquid crystal layer, and the blue light reflecting cholesteric liquid crystal layer were sequentially stacked was obtained.
[0629] [Production of optical layered body 1]
[0630] A PMMA film "TECHNOLLOY S001 (thickness 75 μm)" manufactured by SUMIKA ACRYL CO., LTD. was prepared as a substrate, and the above-mentioned phase difference layer 1 with a pseudo support was bonded to the substrate using an ultraviolet curing adhesive. Next, the cellulose acylate film used as a pseudo support was peeled off from the phase difference layer 1. In this way, an optical laminate 1 having the phase difference layer 1 and the substrate was obtained.
[0631] Furthermore, as a result of measurement by the above-mentioned tan δ measurement method, the peak temperature of tan δ of the resin constituting the above-mentioned base material was 100°C.
[0632] [Production of optical layered body 2]
[0633] An optical layered body 2 was obtained by the same method as the method for producing the optical layered body 1 except that the phase difference layer 1 was changed to the phase difference layer 2.
[0634] [Production of optical layered body 3]
[0635] An optical layered body 3 was obtained by the same method as the method for producing the optical layered body 1 except that the phase difference layer 1 was changed to the cholesteric liquid crystal layer 1 .
[0636] [Example 1]
[0637] The virtual reality display device "VIVE FLOW" manufactured by HTC was disassembled and the optical lens was removed from the lens barrel. In addition, "VIVE FLOW" is a virtual reality display device that uses a pancake lens, and as an image display device, a liquid crystal display device that emits circularly polarized light from a polarizing plate attached to the surface is used.
[0638] The optical lenses taken out were two: a biconvex lens having a half mirror coating formed on one surface and a plano-convex lens having an optical laminate bonded on a flat surface.
[0639] Of the two optical lenses taken out, the optical laminate 1 was formed by vacuum forming on the surface of the biconvex lens opposite to the surface on which the half-mirror coating was formed, thereby obtaining a molded body formed into a three-dimensional shape including a curved surface. In addition, as an adhesive for attaching the optical laminate 1 to the biconvex lens, an adhesive "NCF-D695" manufactured by LINTEC Corporation was used to form an adhesive layer with a thickness of 5 μm. Next, when using the vacuum forming method, the optical film was attached to the curved surface using the adhesive "NCF-D695" manufactured by LINTEC Corporation.
[0640] At 300mJ / cm 2 The molded body thus obtained was irradiated with ultraviolet rays at an intensity of , thereby obtaining an optical component 1 having a phase difference layer 1 (λ / 4 phase difference layer), a double convex lens and a half mirror coating in sequence. In the optical component 1, the polymerization rate of the liquid crystal compound of the phase difference layer 1 was 78%.
[0641] Next, the optical laminate was peeled off from the plane of the taken out plano-convex lens, and an absorbing polarizer, a reflective linear polarizer "APF" manufactured by 3M Company, and an antireflection film "AR100" manufactured by Dexerials Corporation were sequentially attached instead, thereby obtaining a plano-convex lens A with an optical laminate.
[0642] Instead of the biconvex lens and plano-convex lens taken out as described above, the obtained optical component 1 and the plano-convex lens A with an optical laminate were respectively assembled into the lens barrel of "VIVE FLOW" to produce the virtual reality display device of Example 1.
[0643] [Example 2]
[0644] The virtual reality display device "VIVE FLOW" manufactured by HTC was disassembled and the two optical lenses mentioned above were taken out.
[0645] Of the two optical lenses taken out, a plano-convex lens 1 having a radius of curvature of 65 mm, a diameter of 50 mm, and a focal length of 125 mm on the convex side was prepared as an optical lens to be bonded instead of the plano-convex lens to which the optical laminate was bonded. On the convex side of the plano-convex lens 1, an absorbing polarizer, the optical laminate 1, and the optical laminate 3 were sequentially formed and bonded simultaneously by a vacuum forming method, thereby obtaining a molded body molded into a three-dimensional shape including a curved surface.
[0646] Next, the obtained molded body was heated at 110° C. for 30 seconds to perform an alignment treatment for aligning the liquid crystal compounds contained in the retardation layer 1 and the cholesteric liquid crystal layer, and then further heated at 300 mJ / cm 2 The phase difference layer 1 and the cholesteric liquid crystal layer were irradiated with ultraviolet rays at an intensity of 1000 nm, thereby obtaining an optical component 2. The obtained optical component 2 sequentially comprises a plano-convex lens, an absorption polarizer, a phase difference layer 1 (λ / 4 phase difference layer) and a cholesteric liquid crystal layer 1 (reflection circular polarizer). A portion of the optical laminate 1 was peeled off from the optical component 2 to measure the polymerization rate of the liquid crystal compound of the phase difference layer 1 of the optical component 2, and the result was 73%. Similarly, the polymerization rate of the liquid crystal compound of the cholesteric liquid crystal layer 1 was 65%.
[0647] The obtained optical component 2 is assembled into the lens barrel of "VIVE FLOW" instead of the plano-convex lens taken out as mentioned above, and the biconvex lens taken out as mentioned above is assembled into the lens barrel of "VIVE FLOW" again to produce the virtual reality display device of Example 2.
[0648] [Comparative Example 1]
[0649] The virtual reality display device "VIVE FLOW" manufactured by HTC was disassembled and the two optical lenses mentioned above were taken out.
[0650] Of the two optical lenses taken out, the optical layered body 2 is formed by vacuum forming on the surface of the biconvex lens opposite to the surface on which the half mirror coating is formed, and the optical layered body 2 is attached to the surface, thereby obtaining a molded body formed into a three-dimensional shape including a curved surface. The molded body obtained in this way is used as an optical component 3. In the optical component 3, a part of the phase difference layer 2 is broken.
[0651] Next, the optical laminate was peeled off from the plane of the taken out plano-convex lens, and an absorbing polarizer, a reflective linear polarizer "APF" manufactured by 3M Company, and an antireflection film "AR100" manufactured by Dexerials Corporation were sequentially attached instead, thereby obtaining a plano-convex lens A with an optical laminate.
[0652] Instead of the biconvex lens and plano-convex lens taken out as described above, the obtained optical component 3 and the plano-convex lens A with an optical laminate were respectively assembled into the lens barrel of "VIVE FLOW", thereby producing a virtual reality display device of Comparative Example 1.
[0653] [evaluate]
[0654] <Evaluation of Phase Difference of Optical Laminated Body>
[0655] The phase difference of the optical components of Examples 1 to 2 and Comparative Example 1 was measured using AxoScan OPMF-1 (manufactured by OPTO SCIENCE, INC.). The phase difference was measured at each azimuth angle of 45° from the center of the optical lens (biconvex lens or planoconvex lens) possessed by each optical component to a position with a radius of 15 mm, and the maximum value of the deviation of Re from the phase difference of the above-mentioned phase difference layer 1 or phase difference layer 2 was recorded. In addition, for the optical component 2 of Example 2, the phase difference was measured at a wavelength of 500 nm at which the cholesteric liquid crystal layer 1 used for the optical laminate 3 has no reflectivity. The phase difference of other optical laminates was measured at a wavelength of 550 nm.
[0656] Table 1 shows the measurement results of the phase difference of each optical component.
[0657] <Evaluation of light leakage>
[0658] In the virtual reality display devices of Examples 1 to 2 and Comparative Example 1, a black and white checkered pattern was displayed on the image display device, and the degree of light leakage was visually evaluated according to the following three stages. If light leakage exists, double images are visually recognized, and the contrast of the corresponding part is reduced.
[0659] A: Ghosting is barely visible.
[0660] B: Slight double vision is visible, but it is not a big deal.
[0661] C; The ghost image is clearly visible.
[0662] Table 1 shows the evaluation results of light leakage.
[0663] <Evaluation of display uniformity>
[0664] In the virtual reality display devices of Examples 1 and 2 and Comparative Example 1 thus produced, a black and white checkered pattern was displayed on an image display device, and display uniformity was visually evaluated in the following three stages.
[0665] A: The overall display is uniform.
[0666] B; A portion of the image is distorted unevenly.
[0667] C; Most of the image is distorted.
[0668] Table 3 shows the evaluation results of display uniformity.
[0669] Table 3. Evaluation results of virtual reality display devices of Examples and Comparative Examples [Table 3]
[0670]
[0671] It can be confirmed from Table 3 that in the optical components of Examples 1 and 2, the deviation of Re of the phase difference layer 1 within the plane is suppressed to be small. Therefore, the virtual reality display device of the first embodiment effectively reduces light leakage and suppresses the occurrence of ghosting and contrast reduction compared with the comparative example.
[0672] Furthermore, the image display of the virtual reality display device using the optical components of Examples 1 and 2 is uniform overall, but the virtual reality display device using the optical components of Comparative Example 1 has most of the images distorted due to the breakage of the phase difference layer 1 of the optical components.
[0673] As mentioned above, the virtual reality display device according to the first embodiment of the present invention has been described in detail, but the present invention is not limited to the above example, and various improvements and changes can be made without departing from the gist of the present invention.
[0674] <<Second embodiment>>
[0675] <Production of Phase Difference Film 11>
[0676] With reference to the method described in paragraphs 0151 to 0163 of Japanese Patent Gazette No. 2020-084070, a phase difference film 11 with abnormal dispersion was prepared using a coating liquid for forming a phase difference layer containing a liquid crystal compound having a polymerizable group. The phase difference of the phase difference film 11 is Re=146nm, Rth=73nm. In addition, AxoScan OPMF-1 (manufactured by OPTO SCIENCE, INC.) was used in the evaluation of the phase difference. And, the in-plane deviation of Re is 0.7%. The film thickness of the coating of the phase difference film 11 is 2.5μm. And, the in-plane deviation of the film thickness of the coating is 0.7%. Here, SEM is used in the evaluation of the film thickness of the coating. And, in the phase difference film 11, the above-mentioned liquid crystal compound is oriented in one direction.
[0677] In addition, the in-plane variation of Re and the in-plane variation of film thickness were measured as follows.
[0678] First, a circle with the center of the phase difference film 11 (equivalent to the center of gravity) as the center is drawn. At this time, the inscribed circle with the maximum radius that can be drawn is set as the first circle, and the circle with half the radius of the first circle is set as the second circle. In addition, a straight line passing through the center of the phase difference film 11 and extending in one direction in the in-plane direction is set as the first straight line, a straight line passing through the center and rotating the first straight line 45° clockwise is set as the second straight line, a straight line passing through the center and rotating the second straight line 45° clockwise is set as the third straight line, and a straight line passing through the center and rotating the third straight line 45° clockwise is set as the fourth straight line.
[0679] Next, the film thickness and in-plane delay at the center of the phase difference film 11, the film thickness and in-plane delay at the two intersections of the first straight line and the first circle, the film thickness and in-plane delay at the two intersections of the first straight line and the second circle, the film thickness and in-plane delay at the two intersections of the second straight line and the first circle, the film thickness and in-plane delay at the two intersections of the second straight line and the second circle, the film thickness and in-plane delay at the two intersections of the third straight line and the first circle, the film thickness and in-plane delay at the two intersections of the third straight line and the second circle, the film thickness and in-plane delay at the two intersections of the fourth straight line and the first circle, and the film thickness and in-plane delay at the two intersections of the fourth straight line and the second circle. Based on the average, maximum, and minimum values of the measured values at these 17 points, the in-plane deviation (in-plane deviation of Re and in-plane deviation of film thickness) was calculated. Specifically, the maximum value, the minimum value, and the average value were determined from the obtained measured values, and the in-plane variation (%) of Re and the in-plane variation (%) of the film thickness were calculated by the following formulae.
[0680] Formula: In-plane deviation (%) = {(maximum value - minimum value) / average value} × 100
[0681] For example, when calculating the in-plane variation of the film thickness, the average value, the maximum value, and the minimum value of the measured values of the film thickness at 17 points are calculated, and each value is substituted into the above formula.
[0682] <Production of Phase Difference Film 12>
[0683] Referring to the method described in paragraphs 0151 to 0163 of Japanese Patent Application No. 2020-084070, a phase difference film 12 with abnormal dispersion was prepared using a phase difference layer forming coating liquid containing a liquid crystal compound having a polymerizable group. When curing the liquid crystal compound, the irradiation amount of ultraviolet light was increased from 300 mJ / cm 2 Changed to 50mJ / cm 2 Furthermore, in the phase difference film 12 , the liquid crystal compound is aligned in one direction.
[0684] In the obtained phase difference film 12, Re=146nm, Rth=73nm. And the in-plane deviation of Re is 0.7%. The film thickness of the coating of the phase difference film 12 is 2.5μm. And the in-plane deviation of the film thickness of the coating is 0.7%. Here, SEM is used in the film thickness evaluation of the coating. And the polymerization rate of the liquid crystal compound is 26%.
[0685] The in-plane variation (%) of Re and the in-plane variation (%) of film thickness were calculated in the same procedure as the above-mentioned [Production of Phase Difference Film 1].
[0686] The polymerization rate was measured by the method described in the above-mentioned first embodiment.
[0687] <Production of Reflective Circular Polarizer 11>
[0688] [Reflective layer coating liquid R-1]
[0689] The composition shown below was stirred and dissolved in a container maintained at a temperature of 70° C., to prepare a reflective layer coating liquid R-1. Here, R represents a coating liquid using a rod-like liquid crystal compound.
[0690]
[0691]
[0692] Mixture of rod-like liquid crystal compounds
[0693] [Chemical formula 10]
[0694]
[0695] In the above mixture, the numerical values are mass %, and R is a group bonded to an oxygen atom. Furthermore, the average molar absorption coefficient of the above rod-shaped liquid crystal at a wavelength of 300 to 400 nm is 140 / mol·cm.
[0696] Chiral Reagent A
[0697] [Chemical formula 11]
[0698]
[0699] Surfactant F1
[0700] [Chemical formula 12]
[0701]
[0702] Surfactant F2
[0703] [Chemical formula 13]
[0704]
[0705] Photopolymerization initiator B
[0706] [Chemical formula 14]
[0707]
[0708] Chiral reagent A is a chiral reagent whose helical twisting power (HTP: Helical Twisting Power) decreases due to light.
[0709] [Reflective layer coating liquid R-2]
[0710] The reflective layer coating liquid R-1 was prepared in the same manner as in the above-mentioned method except that the amount of the chiral agent A added was changed as shown in Table 4 below.
[0711] Table 4. Amount of chiral agent in coating solution containing rod-shaped liquid crystal compound [Table 4]
[0712]
[0713] [Reflective layer coating liquid D-1]
[0714] The composition shown below was stirred and dissolved in a container maintained at a temperature of 50° C., to prepare a reflective layer coating liquid D-1. Here, D represents a coating liquid using a discotic liquid crystal.
[0715]
[0716]
[0717] Discotic liquid crystal compound (A)
[0718] [Chemical formula 15]
[0719]
[0720] Discotic liquid crystal compound (B)
[0721] [Chemical formula 16]
[0722]
[0723] Polymerizable monomer E1
[0724] [Chemical formula 17]
[0725]
[0726] Surfactant F4
[0727] [Chemical formula 18]
[0728]
[0729] [Reflective layer coating liquid D-2]
[0730] Except that the addition amount of the chiral agent A was changed as shown in the following Table 5, the reflective layer coating liquid D-1 was prepared in the same manner as that of the reflective layer coating liquid D-1.
[0731] Table 5. Amount of chiral agent in coating solution containing discotic liquid crystal compound [Table 5]
[0732]
[0733] [Manufacturing of Reflective Circular Polarizer 11]
[0734] As a pseudo support, a PET (polyethylene terephthalate) film (A4100 manufactured by TOYOBO CO., LTD.) having a thickness of 50 μm was prepared. The PET film had an easy-adhesion layer on one side.
[0735] The surface without the easy-adhesive layer of the PET film was rubbed, and the reflective layer coating liquid R-1 prepared above was applied using a wire bar coater, and then dried at 110°C for 120 seconds. Thereafter, the surface was irradiated at 100°C with an illumination of 80 mW / cm2 in a low oxygen atmosphere (less than 100 ppm). 2 、Irradiation 500mJ / cm 2 The yellow light reflecting layer (first light reflecting layer) composed of a cholesteric liquid crystal layer was cured by light from a metal halide lamp. The light irradiation was performed from the cholesteric liquid crystal layer side. At this time, the coating thickness was adjusted so that the film thickness of the yellow light reflecting layer after curing became 2.5 μm.
[0736] Next, the discharge rate was 150W·min / m 2 After the yellow light reflecting layer was subjected to corona treatment, the reflecting layer coating liquid D-1 was applied to the corona treated surface using a wire bar coater. Next, the coating film was dried at 70°C for 2 minutes to vaporize the solvent, and then heated and aged at 115°C for 3 minutes to obtain a uniform orientation state. Thereafter, the coating film was maintained at 45°C and irradiated with ultraviolet light (300 mJ / cm 2 ) was cured, thereby forming a green light reflecting layer (second light reflecting layer) on the yellow light reflecting layer. The light irradiation was performed from the cholesteric liquid crystal layer side. At this time, the coating thickness was adjusted so that the film thickness of the green light reflecting layer after curing became 2.4 μm.
[0737] Next, the green light reflecting layer was coated with the reflective layer coating liquid R-2 using a wire bar coater and dried at 110°C for 120 seconds. Thereafter, the green light reflecting layer was irradiated at 100°C with an illumination of 80 mW and an irradiation amount of 500 mJ / cm in a low oxygen atmosphere (less than 100 ppm). 2 The red light reflecting layer (third light reflecting layer) was formed on the green light reflecting layer by curing with the light of a metal halide lamp. The light irradiation was performed from the cholesteric liquid crystal layer side. At this time, the coating thickness was adjusted so that the film thickness of the red light reflecting layer after curing became 2.4 μm.
[0738] Next, the discharge rate was 150W·min / m 2 After the red light reflecting layer was subjected to corona treatment, the reflective layer coating liquid D-2 was applied to the corona treated surface using a wire bar coater. Next, the coating film was dried at 70°C for 2 minutes to vaporize the solvent, and then heated and aged at 115°C for 3 minutes to obtain a uniform orientation state. Thereafter, the coating film was maintained at 45°C and irradiated with ultraviolet light (300 mJ / cm 2 ) to cure, thereby forming a blue light reflecting layer (fourth light reflecting layer) on the red light reflecting layer. The light irradiation is performed from the cholesteric liquid crystal layer side. At this time, the coating thickness is adjusted so that the film thickness of the blue light reflecting layer after curing becomes 2.6 μm.
[0739] In this way, the reflective circular polarizer 11 was produced. Table 6 shows the reflective layer coating liquid used when producing the reflective circular polarizer 11, the reflection center wavelength, and the film thickness.
[0740] [Table 6]
[0741]
[0742] <Production of positive C plate 11>
[0743] The film thickness was adjusted with reference to the method described in paragraphs 0132 to 0134 of Japanese Patent Application Laid-Open No. 2016-053709 to produce the positive C plate 11. In the positive C plate 11, Re=0.2 nm, Rth=-310 nm.
[0744] <Production of Phase Difference Layer 11>
[0745] Referring to the method described in paragraphs 0151 to 0163 of Japanese Patent Gazette No. 2020-084070, a phase difference layer 11 with abnormal dispersion was prepared using a phase difference layer forming coating liquid containing a liquid crystal compound having a polymerizable group. In the phase difference layer 11, Re=146nm, Rth=73nm. The phase difference of the phase difference layer 11 is Re=146nm, Rth=73nm. In addition, AxoScan OPMF-1 (manufactured by OPTO SCIENCE, INC.) was used in the evaluation of the phase difference. And, the in-plane deviation of Re is 0.7%. The film thickness of the phase difference layer 11 is 2.5μm. In addition, in the phase difference layer 1, the above-mentioned liquid crystal compound is oriented in one direction. And, the in-plane deviation of the film thickness is 0.7%. Here, SEM is used in the film thickness evaluation.
[0746] The in-plane variation (%) of Re and the in-plane variation (%) of film thickness were calculated in the same procedure as the above-mentioned [Production of Phase Difference Film 11].
[0747] <Production of Phase Difference Layer 12>
[0748] Referring to the method described in paragraphs 0151 to 0163 of Japanese Patent Application No. 2020-084070, a phase difference layer 12 with abnormal dispersion was prepared using a phase difference layer forming coating liquid containing a liquid crystal compound having a polymerizable group. When curing the liquid crystal compound, the irradiation amount of ultraviolet light was increased from 300 mJ / cm 2 Changed to 50mJ / cm 2 Furthermore, in the phase difference layer 12, the liquid crystal compound is aligned in one direction.
[0749] In the obtained phase difference layer 12, Re=146nm, Rth=73nm. And the in-plane deviation of Re is 0.7%. The film thickness of the phase difference layer 12 is 2.5μm. And the in-plane deviation of the film thickness of the coating is 0.7%. Here, SEM is used in the film thickness evaluation of the coating. And the polymerization rate of the liquid crystal compound is 26%.
[0750] The in-plane variation (%) of Re and the in-plane variation (%) of film thickness were calculated in the same procedure as the above-mentioned [Production of Phase Difference Film 11].
[0751] The polymerization rate was measured by the method described in the above-mentioned first embodiment.
[0752] <Production of linear polarizer>
[0753] (Production of Cellulose Acylate Film 11)
[0754] The following composition was placed in a mixing tank and stirred to dissolve the components, thereby preparing a cellulose acetate solution to be used as a doping agent for the cellulose acylate in the core layer.
[0755]
[0756] Compound F
[0757] [Chemical formula 19]
[0758]
[0759] To 90 parts by mass of the core layer cellulose acylate doping agent was added 10 parts by mass of the following matting agent solution to prepare a cellulose acetate solution as an outer layer cellulose acylate doping agent.
[0760]
[0761] After filtering the core layer cellulose acylate dopant and the outer layer cellulose acylate dopant using filter paper with an average pore size of 34 μm and a sintered metal filter with an average pore size of 10 μm, a total of three layers of the core layer cellulose acylate dopant and the outer layer cellulose acylate dopant on both sides thereof are simultaneously cast from a casting port onto a drum at 20° C. (belt casting machine).
[0762] Next, the film was peeled at a solvent content of about 20% by mass, and both ends of the film in the width direction were clamped by a tenter clip, stretched in the transverse direction at a stretching ratio of 1.1 times, and dried.
[0763] Thereafter, the film was carried between rollers of a heat treatment device and further dried to produce an optical film having a thickness of 40 μm, which was referred to as a cellulose acylate film 11. The in-plane retardation of the obtained cellulose acylate film 11 was 0 nm.
[0764] (Formation of Photo-Alignment Layer PA1)
[0765] The coating liquid S-PA-1 for forming an alignment layer described later was continuously coated on the cellulose acylate film 11 using a wire bar. The support with the coating film was dried with warm air at 140° C. for 120 seconds, and then the coating film was irradiated with polarized ultraviolet rays (10 mJ / cm 2 , using an ultra-high pressure mercury lamp), thereby forming a photo-alignment layer PA1 with a film thickness of 0.3 μm.
[0766]
[0767]
[0768] Polymer M-PA-1
[0769] [Chemical formula 20]
[0770]
[0771] Acid Generator PAG-1
[0772] [Chemical formula 21]
[0773]
[0774] Acid Generator CPI-110F
[0775] [Chemical formula 22]
[0776]
[0777] (Formation of Light Absorption Anisotropic Layer P1)
[0778] The following coating liquid SP-1 for forming an anisotropic light absorbing layer was continuously coated on the obtained orientation layer PA1 using a wire bar. Next, the coating layer P1 was heated at 140°C for 30 seconds and cooled to room temperature (23°C). Next, it was heated at 90°C for 60 seconds and cooled to room temperature again. Thereafter, an LED lamp (central wavelength 365nm) was used at an illumination of 200mW / cm 2 The light absorption anisotropic layer P1 was formed on the alignment layer PA1 under the irradiation condition of 2 seconds. The film thickness was 1.6 μm.
[0779]
[0780] Dichroic substance D-1
[0781] [Chemical formula 23]
[0782]
[0783] Dichroic substance D-2
[0784] [Chemical formula 24]
[0785]
[0786] Dichroic substance D-3
[0787] [Chemical formula 25]
[0788]
[0789] Polymer liquid crystal compound MP-1
[0790] [Chemical formula 26]
[0791]
[0792] Low molecular weight liquid crystal compound M-1
[0793] [Chemical formula 27]
[0794]
[0795] Surfactant F-1
[0796] [Chemical formula 28]
[0797]
[0798] <Production of Laminated Optical Body 11>
[0799] The transfer of the reflective circular polarizer 11 is performed in the following order. The obtained reflective circular polarizer 11 is transferred to the support side of the obtained positive C plate 11. At this time, in order to make the layer on the pseudo support side of the reflective circular polarizer 11 (the first light reflecting layer) be located on the positive C plate 11 side, the pseudo support temporarily transferred to the adhesive layer is exposed and then bonded to the positive C plate 11. After bonding, the pseudo support of the reflective circular polarizer 11 is peeled off and removed. The obtained phase difference layer 11 is bonded to the side of the obtained positive C plate 11 opposite to the support. Next, the light absorption anisotropic layer P1 is transferred. At this time, the transfer is performed in such a way that the layer on the side of the light absorption anisotropic layer P1 opposite to the pseudo support is located on the phase difference layer 11 side. After transfer, the pseudo support of the light absorption anisotropic layer P1 is peeled off and removed. The transfer of the light absorption anisotropic layer P1 is performed in the following order.
[0800] (1) Using a wire bar coater, UV adhesive Chemiseal U2084B (manufactured by CHEMITECH INC., with a refractive index of n: 1.60 after curing) was applied to the support side of the positive C plate 11 to a thickness of 2 μm. The light absorption anisotropic layer P1 was laminated thereon using a laminator so that the side opposite to the dummy support contacted the UV adhesive.
[0801] (2) After nitrogen flushing in a flushing box until the oxygen concentration becomes 100 ppm or less, the light absorption anisotropic layer P1 is cured by irradiating with ultraviolet light from a high pressure mercury lamp from the dummy support side. The illuminance is 25 mW / cm 2 , the irradiation dose is 1000mJ / cm 2 .
[0802] (3) Finally, the dummy support of the light absorption anisotropic layer P1 is peeled off.
[0803] The phase difference layer 11 was laminated so that the slow axis and the absorption axis of the light absorption anisotropic layer P1 formed a 45° angle. Finally, the support of the positive C plate 11 was peeled off. Next, the phase difference layer 11 and the anti-reflection film were sequentially laminated on the light absorption anisotropic layer P1. In this way, a laminated optical body 1 using the reflective circular polarizer 11 as a circularly polarized light reflective polarizer was obtained.
[0804] <Production of Laminated Optical Body 12>
[0805] As a linear polarization type reflective polarizer, a broadband dielectric multilayer film (3M Company, trade name APF) was used. A phase difference layer 11 and a positive C plate 11 were sequentially laminated on one surface of the APF. In addition, a light absorption anisotropic layer P1 was transferred to the opposite surface in the same order as the above-mentioned laminated optical body 11. Next, a phase difference layer 11 and an anti-reflection film were laminated on the light absorption anisotropic layer P1. In this way, a laminated optical body 2 using a linear polarization type reflective polarizer was manufactured.
[0806] <Production of Laminated Optical Body 13>
[0807] As a linear polarization type reflective polarizer, a broadband dielectric multilayer film (3M Company, trade name APF) was used. In the same order as the above-mentioned laminated optical body 11, the light absorption anisotropic layer P1 was transferred to one side of the APF. Then, the phase difference layer 11 and the anti-reflection film were attached to the light absorption anisotropic layer P1. In this way, a laminated optical body 13 using a linear polarization type reflective polarizer was produced. In addition, on the opposite side, the phase difference layer 12 and the positive C plate 11 were attached in sequence via the adhesive sheet "NCF-D692 (5)" manufactured by LINTEC Corporation.
[0808] <Forming a half mirror on a lens>
[0809] Aluminum was vapor-deposited on the convex surface of a lens (convex meniscus lens LE1076-A (2-inch diameter, focal length 100 mm) manufactured by Thorlabs, Inc.) until the reflectivity reached 40%, thereby forming a half mirror.
[0810] <Examples 11 and 12>
[0811] (Forming method 1)
[0812] The phase difference film 11 is bonded to the PMMA film via the adhesive sheet "NCF-D692 (5)" manufactured by LINTEC Corporation and is set in a molding device. At this time, it is configured in a manner that the PMMA film side is on the lower side. The molding space in the molding device is composed of a mold box 1 and a mold box 2 separated by the phase difference film 11. On the mold box 1 located on the lower side of the phase difference film 11, a mold #32-974 (a convex lens with a diameter of 2 inches and a radius of curvature of 78 mm) manufactured by Edmund Optics, Inc. is configured with the convex surface facing upward. In addition, in the mold box 2 located on the upper side of the phase difference film 11, a transparent window is provided at the upper part, and an IR light source for heating the phase difference film 11 is provided on the outer side thereof. Then, the inside of the mold box 1 and the mold box 2 are evacuated with a vacuum pump until they are respectively below 0.1 atmospheres. Next, as a process for heating the phase difference film 11, infrared rays are irradiated and heated until the temperature of the phase difference film 11 reaches 108°C. The glass transition temperature Tg of the PMMA film used as a support is 105°C, so the goal is to make the film easily stretched during molding. Next, as a process of pressing the phase difference film 11 on the mold and deforming it along the shape of the mold, gas is flowed from the cylinder into the mold box 2 and pressurized to 300 kPa to press the phase difference film 11 onto the mold. Finally, the phase difference film 11 is removed from the lens serving as the mold. Thus, a phase difference film 11 formed into a non-planar shape is obtained.
[0813] Next, the non-planar phase difference film 11 formed into a non-planar shape is inverted in the opposite direction to the initial forming, and is placed in a forming device in a manner such that the PMMA film side is on the upper side. At this time, the non-planar region formed in the phase difference film 11 based on the initial forming protrudes downward. Directly below the non-planar region formed in the phase difference film 11, a convex meniscus lens LE1076-A (2 inches in diameter, focal length 100 mm, radius of curvature 65 mm on the concave side) manufactured by Thorlabs, Inc., which has been aluminum evaporated on the convex side, is arranged as a mold with the concave surface facing upward. Next, a vacuum pump is used to evacuate the inside of the mold box 1 and the inside of the mold box 2 until they are respectively below 0.1 atmospheres. Next, as a process for heating the phase difference film 11, infrared rays are irradiated and heated until the temperature of the phase difference film 11 reaches 108°C. Next, as a process of pressing the phase difference film 11 against the mold and deforming it along the shape of the mold, gas was flowed from the cylinder into the mold box 2 and pressurized to 300 kPa, and the phase difference film 11 was pressed against the mold. Finally, the phase difference film 11 was removed from the lens serving as the mold. Thus, the phase difference film 11 formed into a curved surface by the forming method 1 was obtained as Example 11.
[0814] (Forming method 2)
[0815] The phase difference film 11 is bonded to the PMMA film via an adhesive sheet "NCF-D692 (5)" manufactured by LINTEC Corporation and is set in a molding device. The molding space in the molding device is composed of a mold box 1 and a mold box 2 separated by the phase difference film 11. On the mold box 1 located on the lower side of the phase difference film 11, a convex meniscus lens LE1076-A (2 inches in diameter, focal length 100 mm, radius of curvature 65 mm on the concave side) manufactured by Thorlabs, Inc., which has aluminum vapor deposition on the convex side, is arranged as a mold with the concave side facing upward. In addition, in the mold box 2 located on the upper side of the phase difference film 11, a transparent window is set at the top, and an IR light source for heating the phase difference film 11 is set on the outside. A circular pattern infrared reflection filter is arranged between the IR light source and the phase difference film 11. It is obtained by cutting a cholesteric liquid crystal layer that reflects infrared rays with a wavelength of 2.2μm to 3.0μm at a reflectivity of about 50% into a circular shape with a diameter of 1 inch. At this time, it is arranged so that the center of the pattern infrared reflection filter is located at the center of the mold when viewed from directly above. Next, the inside of the mold box 1 and the inside of the mold box 2 are evacuated with a vacuum pump until they become less than 0.1 atmospheres respectively. Next, as a process for heating the phase difference film 11, infrared rays are irradiated and heated until the center of the phase difference film 11 reaches 99°C and the end reaches 108°C. The glass transition temperature Tg of the PMMA film used as a support is 105°C, so the goal is to achieve a state in which the center is not easy to stretch and the end is easy to stretch during molding. Next, as a process of pressing the phase difference film 11 against the mold and deforming it along the shape of the mold, gas was flowed from the cylinder into the mold box 2 and pressurized to 300 kPa, and the phase difference film 11 was pressed against the mold. Finally, the phase difference film 11 was removed from the lens serving as the mold. Thus, the phase difference film 11 formed into a curved surface by the forming method 2 was obtained as Example 12.
[0816] In the above-mentioned forming method 2, the stretching ratio in the radial direction increases as the distance from the center increases.
[0817] <Examples 15 and 16>
[0818] (Forming method 3)
[0819] The phase difference film 12 is bonded to the PMMA film via the adhesive sheet "NCF-D692 (5)" manufactured by LINTEC Corporation and is set in a molding device. At this time, it is configured in a manner that the PMMA film side is on the lower side. The molding space in the molding device is composed of a mold box 1 and a mold box 2 separated by the phase difference film 12. On the mold box 1 located on the lower side of the phase difference film 12, a mold #32-974 (a convex lens with a diameter of 2 inches and a radius of curvature of 78 mm) manufactured by Edmund Optics, Inc. is configured with the convex surface facing upward. In addition, in the mold box 2 located on the upper side of the phase difference film 12, a transparent window is provided at the upper part, and an IR light source for heating the phase difference film 12 is provided on the outer side thereof. Then, the inside of the mold box 1 and the mold box 2 are evacuated with a vacuum pump until they are respectively below 0.1 atmospheres. Next, as a process for heating the phase difference film 12, infrared rays are irradiated and heated until the temperature of the phase difference film 12 reaches 108°C. The glass transition temperature Tg of the PMMA film used as a support is 105°C, so the goal is to make the film easily stretched during molding. Next, as a process of pressing the phase difference film 12 on the mold and deforming it along the shape of the mold, gas is flowed from the cylinder into the mold box 2 and pressurized to 300 kPa to press the phase difference film 12 onto the mold. Finally, the phase difference film 12 is removed from the lens serving as the mold. Thus, a phase difference film 12 formed into a non-planar shape is obtained.
[0820] Next, the non-planar phase difference film 12 formed into a non-planar shape is inverted in the opposite direction to the initial forming, and is placed in a forming device in a manner such that the PMMA film side is on the upper side. At this time, the non-planar region formed in the phase difference film 12 based on the initial forming protrudes downward. Directly below the non-planar region formed in the phase difference film 12, a convex meniscus lens LE1076-A (2 inches in diameter, focal length 100 mm, radius of curvature 65 mm on the concave side) manufactured by Thorlabs, Inc., which has been aluminum evaporated on the convex side, is arranged as a mold with the concave surface facing upward. Next, a vacuum pump is used to evacuate the inside of the mold box 1 and the inside of the mold box 2 until they are respectively below 0.1 atmospheric pressure. Next, as a process for heating the phase difference film 12, infrared rays are irradiated and heated until the temperature of the phase difference film 12 reaches 108°C. Next, as a step of pressing the retardation film 12 against the mold and deforming it along the shape of the mold, gas was flowed from the cylinder into the mold box 2 and pressurized to 300 kPa to press the retardation film 12 against the mold. Next, the mold to which the retardation film 12 was pressed was heated at 110°C for 30 seconds for orientation treatment, and further heated at 300 mJ / cm 2The phase difference film 12 was cured by irradiating ultraviolet light with an intensity of 1000 nm. The polymerization rate of the liquid crystal layer of the phase difference film 12 was measured by the ATR method, and the polymerization rate was 78%. Finally, the phase difference film 12 was removed from the lens as a mold. Thus, the phase difference film 12 formed into a curved surface by the forming method 3 was obtained as Example 15.
[0821] (Forming method 4)
[0822] The phase difference film 12 is bonded to the PMMA film via an adhesive sheet "NCF-D692 (5)" manufactured by LINTEC Corporation and is set in a molding device. The molding space in the molding device is composed of a mold box 1 and a mold box 2 separated by the phase difference film 12. On the mold box 1 located on the lower side of the phase difference film 12, a convex meniscus lens LE1076-A (2 inches in diameter, focal length 100 mm, radius of curvature 65 mm on the concave side) manufactured by Thorlabs, Inc., which has aluminum vapor deposition on the convex side, is arranged as a mold with the concave side facing upward. In addition, in the mold box 2 located on the upper side of the phase difference film 12, a transparent window is set at the top, and an IR light source for heating the phase difference film 12 is set on the outside thereof. A circular pattern infrared reflection filter is arranged between the IR light source and the phase difference film 12. It is obtained by cutting a cholesteric liquid crystal layer that reflects infrared rays with a wavelength of 2.2μm to 3.0μm at a reflectivity of about 50% into a circular shape with a diameter of 1 inch. At this time, it is arranged so that the center of the pattern infrared reflection filter is located at the center of the mold when viewed from directly above. Next, the inside of mold box 1 and mold box 2 are evacuated with a vacuum pump until they become less than 0.1 atmospheres respectively. Next, as a process for heating the phase difference film 12, infrared rays are irradiated and heated until the center of the phase difference film 12 reaches 99°C and the ends reach 108°C. The glass transition temperature Tg of the PMMA film used as a support is 105°C, so the goal is to achieve a state in which the center is not easy to stretch and the ends are easy to stretch during molding. Next, as a step of pressing the retardation film 12 against the mold and deforming it along the shape of the mold, gas was flowed from the cylinder into the mold box 2 and pressurized to 300 kPa to press the retardation film 12 against the mold. Next, the mold to which the retardation film 12 was pressed was heated at 110°C for 30 seconds for orientation treatment, and further heated at 300 mJ / cm 2 The phase difference film 12 was cured by irradiating ultraviolet rays with an intensity of 1000 nm. The polymerization rate of the liquid crystal layer of the phase difference film 12 was measured by the ATR method, and the polymerization rate was 78%. Finally, the phase difference film 12 was removed from the lens as a mold. Thus, the phase difference film 12 formed into a curved surface by the forming method 4 was obtained as Example 16.
[0823] <Evaluation of the formed phase difference film>
[0824] The phase difference of the phase difference film 11 formed into a curved surface of Example 11 is Re = 140nm, Rth = 70nm. And the in-plane deviation of Re is 2.7%. The film thickness of the phase difference film 11 formed into a curved surface of Example 11 is 2.4μm. And the in-plane deviation of the film thickness is 3.0%. Therefore, it is confirmed that the phase difference and in-plane deviation of the film thickness of the phase difference film 11 formed into a curved surface by forming method 11 are increased by about 2%.
[0825] The in-plane deviation of the product of the stretch ratio in the radial direction and the stretch ratio in the circumferential direction (direction orthogonal to the radial direction) of the retardation film 11 formed into a curved surface of Example 11 was 2.1%.
[0826] The in-plane variation of Re and the in-plane variation of the film thickness were measured by the above-mentioned methods (the above-mentioned specific method 1 and the above-mentioned specific method 2).
[0827] The phase difference of the phase difference film 11 formed into a curved surface of Example 12 is Re = 140nm, Rth = 70nm. In addition, the in-plane deviation of Re is 3.3%. The film thickness of the phase difference film 11 formed into a curved surface of Example 12 is 2.4μm. In addition, the in-plane deviation of the film thickness is 3.2%. Therefore, it is confirmed that the phase difference and in-plane deviation of the film thickness of the phase difference film 11 formed into a curved surface by forming method 2 are increased by about 2.5%.
[0828] The in-plane deviation of the product of the stretch ratio in the radial direction and the stretch ratio in the circumferential direction (direction orthogonal to the radial direction) of the retardation film 11 formed into a curved surface of Example 12 was 2.5%.
[0829] The in-plane variation of Re and the in-plane variation of the film thickness were measured by the above-mentioned methods (the above-mentioned specific method 1 and the above-mentioned specific method 2).
[0830] The phase difference of the phase difference film 12 formed into a curved surface of Example 15 is Re = 140nm, Rth = 70nm. In addition, the in-plane deviation of Re is 2.5%. The film thickness of the phase difference film 12 formed into a curved surface of Example 15 is 2.4μm. In addition, the in-plane deviation of the film thickness is 3.2%. Therefore, it is confirmed that the in-plane deviation of the phase difference of the phase difference film 12 formed into a curved surface by forming method 3 increases by about 1.8%. In addition, it is confirmed that the in-plane deviation of the film thickness increases by about 2.5%.
[0831] The in-plane deviation of the product of the stretch ratio in the radial direction and the stretch ratio in the circumferential direction (direction orthogonal to the radial direction) of the retardation film 12 formed into a curved surface of Example 15 was 2.5%.
[0832] The phase difference of the phase difference film 12 formed into a curved surface of Example 16 is Re = 140nm, Rth = 70nm. In addition, the in-plane deviation of Re is 2.5%. The film thickness of the phase difference film 12 formed into a curved surface of Example 16 is 2.4μm. In addition, the in-plane deviation of the film thickness is 3.2%. Therefore, it is confirmed that the in-plane deviation of the phase difference of the phase difference film 12 formed into a curved surface by forming method 4 increases by about 1.8%. In addition, it is confirmed that the in-plane deviation of the film thickness increases by about 2.5%.
[0833] The in-plane deviation of the product of the stretch ratio in the radial direction and the stretch ratio in the circumferential direction (direction orthogonal to the radial direction) of the retardation film 12 formed into a curved surface of Example 16 was 2.5%.
[0834] <Examples 13 and 14>
[0835] The laminated optical body 11 is molded in the same order as the molding method 1. In addition, the laminated optical body 11 is attached to the mold via an adhesive sheet, and finally the portion of the laminated optical body 11 protruding from the lens serving as the mold is cut out, thereby obtaining a composite lens 11 in which the laminated optical body 11 molded into a curved surface is attached to the lens.
[0836] The laminated optical body 12 is formed in the same order as the forming method 1. In addition, the laminated optical body 12 is attached to the mold via an adhesive sheet, and finally the portion of the laminated optical body 12 protruding from the lens serving as the mold is cut out, thereby obtaining a composite lens 12 in which the laminated optical body 12 formed into a curved surface is attached to the lens.
[0837] <Examples 17 and 18>
[0838] The laminated optical body 13 is formed in the same order as the forming method 3. In addition, the laminated optical body 13 is attached to the mold via an adhesive sheet, and finally the portion of the laminated optical body 13 protruding from the lens serving as the mold is cut out, thereby obtaining a composite lens 13 in which the laminated optical body 13 formed into a curved surface is attached to the lens.
[0839] The laminated optical body 13 is formed in the same order as the forming method 4. In addition, the laminated optical body 13 is attached to the mold via an adhesive sheet, and finally the portion of the laminated optical body 13 protruding from the lens serving as the mold is cut out, thereby obtaining a composite lens 14 in which the laminated optical body 13 formed into a curved surface is attached to the lens.
[0840] <Production of virtual reality display device>
[0841] A virtual reality display device "Huawei VR Glass" manufactured by Huawei Technologies Co., Ltd., which uses a reciprocating optical system, was disassembled and all the composite lenses were removed. Instead, the composite lens 11 bonded to the laminated optical body 11 was assembled to the main body, and the light absorption anisotropic layer P1 side of the laminated optical body was further arranged between the composite lens 11 and the eye to be located on the eye side, thereby producing a virtual reality display device of Example 13. In the produced virtual reality display device, a black and white checkered pattern was displayed on the image display panel, and the ghosting visual recognition was visually evaluated according to the following four stages.
[0842] (Evaluation of Ghosting)
[0843] AA; barely visible.
[0844] A: Slightly visible, but not serious.
[0845] B; Weak ghosting is visible.
[0846] C; Slightly stronger double images can be seen.
[0847] D; strong ghosting is visible.
[0848] Furthermore, virtual reality display devices of Examples 14, 17, and 18 were produced in the same procedure, and the ghosting visibility was evaluated. The molding methods and types of optical films used in each Example are shown in Table 7. The evaluation results are shown in Table 8.
[0849] As a result, in the virtual reality display devices of Examples 13, 14, 17, and 18, the double image was good in the entire field of view. In addition, the color change of the white part of the black and white checkered pattern was not a problem.
[0850] Table 7. Forming methods and types of optical films used in Examples [Table 7]
[0851]
[0852] Table 8. Evaluation results of the examples [Table 8]
[0853]
[0854] Explanation of symbols
[0855] 10, 20-virtual reality display device, 11, 12, 13, 14-λ / 4 phase difference layer, 21, 22-absorption type linear polarizer, 30-half mirror, 34, 36-lens substrate, 40-reflection type circular polarizer, 42-reflection type linear polarizer, 50, 51, 52-anti-reflection layer, 70-image display panel, 72-image display device, 80, 82-plano-convex lens with optical functional layer, 90, 92-double convex lens with optical functional layer, 100, 100B-laminated optical body, 101-cholesteric liquid crystal layer, 102-positive C plate, 103-phase difference layer, 104-linear polarizer, 105-phase difference layer, 106-anti-reflection film, 111-positive C plate, 112-phase difference layer, 113-linear polarized light type reflective polarizer , 114-linear polarizer, 115-phase difference layer, 116-anti-reflection film, 131-first light reflecting layer, 132-second light reflecting layer, 133-third light reflecting layer, 134-fourth light reflecting layer, 200-lens, 220, 234, 240-molding mold having a concave shape molding surface, 222-film, 224-film with a concave shape transferred, 226, 230-molding mold having a convex shape molding surface, 228-film with a convex shape transferred, 232-optical film with a convex shape transferred, 236-optical film with a curved shape portion, 242-optical film with a flat shape, 300-half-mirror, 400-reflective circular polarizer, 500-image display panel, 1000-light that forms a virtual image, 2000-light that forms a double image.
Claims
1. An optically functional film, which is an optically functional film obtained by forming a composition containing at least a liquid crystal compound having a polymerizable group, wherein: The polymerization rate of the liquid crystal compound is 40% or less.
2. The optically functional film according to claim 1, wherein The liquid crystal compound is aligned in one direction.
3. The optically functional film according to claim 1, wherein The liquid crystal compound is helically oriented.
4. An optical laminate, comprising: The optically functional film according to any one of claims 1 to 3; and A base film composed of a resin having a tan δ peak temperature of 170° C. or less. 5 . A molded body, wherein the optical functional film according to claim 1 or an optical laminate comprising the optical functional film according to claim 1 and a substrate film is molded into a three-dimensional shape including a curved surface.
6. A method for manufacturing an optical component, comprising a curing step of subjecting the molded article according to claim 5 to at least one curing treatment selected from the group consisting of a heat treatment and ultraviolet irradiation, Through the curing treatment, the polymerization rate of the liquid crystal compound in the optically functional film becomes 50% or more.
7. The method for manufacturing an optical component according to claim 6, wherein: The method further includes an alignment step of heating the molded body to align the liquid crystal compound before the curing step. 8 . An optical component manufactured by the method for manufacturing an optical component according to claim 6 .
9. A virtual reality display device, comprising: An image display device emitting polarized light; and The optical component according to claim 8.
10. An optical film having a non-planar shape, a curvature radius of 30 mm to 1000 mm, and an in-plane deviation of phase difference of less than 5%.
11. The optical film according to claim 10, wherein: The radius of curvature is 30mm to 100mm.
12. The optical film according to claim 10 or 11, wherein: The in-plane deviation of the phase difference is less than 3%.
13. The optical film according to claim 10 or 11, wherein: The in-plane deviation of the film thickness is less than 5%.
14. The optical film according to claim 10 or 11, wherein: The optical film is a phase difference film.
15. The optical film according to claim 10 or 11, wherein: The optical film is a phase difference film having an in-plane retardation in the range of 120 nm to 160 nm at a wavelength of 550 nm.
16. The optical film according to claim 10 or 11, wherein: The optical film is a laminated optical body including a phase difference film and a reflective polarizer.
17. A method for forming an optical film, comprising: A step of heating an optical film having a planar shape; A first forming step of pressing the optical film onto a first mold and deforming the optical film along the shape of the first mold; and In the second molding step, the optical film obtained in the first molding step is pressed against a second mold to deform the optical film along the shape of the second mold.
18. The method for forming an optical film according to claim 17, wherein: The shape of the first mold includes a convex curved surface portion, and the shape of the second mold includes a concave curved surface portion.
19. The method for forming an optical film according to claim 17 or 18, wherein: The curvature radius of the first mold is greater than the curvature radius of the second mold.
20. A method for forming an optical film, comprising: A step of heating an optical film having a planar shape; The step of pressing the optical film onto a mold and deforming the optical film along the shape of the mold; and a step of cutting the deformed optical film, The heating step is a step of heating the optical film by irradiating infrared rays. The irradiation amount of the infrared rays has a distribution within the surface of the optical film.
21. The method for forming an optical film according to claim 20, wherein: The mold is substantially in the shape of a concave sphere, and when the position in the surface of the optical film is projected onto the mold from the normal direction of the surface of the optical film, The amount of infrared light irradiated onto the optical film located at the vertex of the concave spherical shape is smaller than the amount of infrared light irradiated onto the optical film located at the end of the concave spherical shape.
22. The method for forming an optical film according to claim 20 or 21, wherein: The mold is substantially in the shape of a concave sphere, and when the position in the surface of the optical film is projected onto the mold from the normal direction of the surface of the optical film, The temperature of the optical film located at the vertex of the concave spherical shape is lower than the temperature of the optical film located at the end of the concave spherical shape.
23. A method for forming an optical film, which is a method for forming an optical film having a planar shape into a non-planar shape, wherein: The in-plane deviation of the product of the stretch ratio in the radial direction and the stretch ratio in the circumferential direction is less than 5%.
24. The method for forming an optical film according to claim 23, wherein: The in-plane deviation of the product of the radial stretch ratio and the circumferential stretch ratio is less than 3%.
25. The method for forming an optical film according to claim 23 or 24, wherein: The stretching ratio in the radial direction increases as it moves away from the center.
Citation Information
Patent Citations
Shell separation supplying device for cassette case
JP1994259925A
polymerizable liquid crystal compound
JP1999513019A
Molding method of decorating molded article and equipment therefor
JP2004322501A
Liquid crystal compound, liquid crystyal composition, polymer, retardation plate, and elliptical polarization plate
JP2005289980A
Polarizing plate and liquid crystal display device
JP2007108732A