Laminated film

By forming a laminated film structure of a porous layer and an adhesive layer on the first main surface of the optical functional layer, the problem of functional degradation of the optical functional layer when protective measures are used is solved, and the light direction changing function is maintained and transparent. sexual enhancement.

CN118742833APending Publication Date: 2024-10-01NITTO DENKO CORP
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202380022750.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-02-28
Filing Date
2023-01-19
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

In the prior art, when protective measures are used for the optical functional layer with the function of changing the direction of light, the function is easily reduced or eliminated, and the existing protective structure will affect the performance of the optical functional layer.

Method used

A laminated film structure with a porous layer is adopted, in which the porous layer is composed of a silicon compound, has a refractive index of 1.15 to 1.30, a void ratio of 20 to 60 volume %, and a thickness of 30 nm to 5 μm, and is directly formed on the first main surface of the optical functional layer , and an adhesive layer is provided on the opposite side of the porous layer to protect the optical functional layer and inhibit functional degradation.

Benefits of technology

It is possible to protect the optical functional layer while maintaining its light direction changing function, ensuring the transparency and visual recognition of the laminated film, expanding the scope of application, and avoiding functional degradation caused by the adhesive layer.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118742833A_ABST
    Figure CN118742833A_ABST
Patent Text Reader

Abstract

Provided is a laminated film which is provided with an optical functional layer that has a function of changing the direction of light and an adhesive layer that protects the optical functional layer, and in which a reduction in the function of the optical functional layer due to the adhesive layer is suppressed. A laminated film according to an embodiment of the present invention comprises: an optical functional layer having a first main surface and a second main surface, the first main surface having a concavo-convex structure, the height of the concavo-convex being 10 nm to 100 [mu] m; a porous layer provided on the first main surface of the optically functional layer; and an adhesive layer provided on the porous layer on the opposite side from the optically functional layer. The optical functional layer is a reflective holographic film, a micro-lens array film or a prism film, and the refractive index of the porous layer is 1.15-1.30.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to laminated films. Background Art

[0002] As a means of improving the design of various products, decorative films have been used. Depending on the purpose, the decorative film sometimes has an optical functional layer (e.g., holographic, microlens array film, prism film) with a function of changing the direction of light (e.g., patent documents 1 and 2). The optical functional layer with the function of changing the direction of light typically has a concave-convex structure on the surface. If such an optical functional layer is arranged on the outermost surface, sometimes the surface (substantially a concave-convex structure) is damaged, and the function of the optical functional layer is reduced or disappears. On the other hand, even if you want to protect the surface of the optical functional layer (substantially a concave-convex structure) using, for example, an adhesive, the function of the optical functional layer is sometimes reduced or disappears due to the protective structure.

[0003] Prior art literature

[0004] Patent Literature

[0005] Patent Document 1: Japanese Patent Application Publication No. 2020-028981

[0006] Patent Document 2: Japanese Patent Application Publication No. 2020-104467 Summary of the invention

[0007] Problems to be solved by the invention

[0008] The present invention has been made to solve the above-mentioned conventional problems, and its main object is to provide a laminated film comprising an optical functional layer having a function of redirecting light and an adhesive layer for protecting the optical functional layer, wherein degradation of the function of the optical functional layer caused by the adhesive layer is suppressed.

[0009] Solutions to the problem

[0010] The laminated film of an embodiment of the present invention comprises: an optical functional layer having a first main surface and a second main surface, the first main surface having a concave-convex structure, and the height of the concave-convex is 10nm to 100μm; a porous layer arranged on the first main surface of the optical functional layer; and an adhesive layer arranged on the side of the porous layer opposite to the optical functional layer, the optical functional layer is a reflective holographic film, a microlens array film or a prismatic film, and the refractive index of the porous layer is 1.15 to 1.30.

[0011] In one embodiment, the porous layer includes a silicon compound.

[0012] In one embodiment, the porosity of the porous layer is 20 volume % to 60 volume %.

[0013] In one embodiment, the porous layer has a thickness of 30 nm to 5 μm.

[0014] In one embodiment, the porous layer comprises one or more constituent units forming a fine void structure, and the constituent units are chemically bonded together by a catalyst.

[0015] In one embodiment, the constituent units of the porous layer are constituent units in at least one shape selected from the group consisting of particles, fibers, rods, and plates.

[0016] In one embodiment, the bonding between the constituent units of the porous layer includes hydrogen bonds or covalent bonds.

[0017] In one embodiment, the porous layer is formed directly on the first main surface of the optical function layer.

[0018] Effects of the Invention

[0019] According to the embodiment of the present invention, a laminated film can be provided which includes an optical function layer having a function of converting the direction of light and a pressure-sensitive adhesive layer for protecting the optical function layer, and in which degradation of the function of the optical function layer caused by the pressure-sensitive adhesive layer is suppressed. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 It is a schematic cross-sectional view of a laminated film according to one embodiment of the present invention.

[0021] Figure 2 It is a schematic cross-sectional view of a laminated film according to another embodiment of the present invention.

[0022] Figure 3 It is a schematic cross-sectional view of a laminated film according to still another embodiment of the present invention.

[0023] Figure 4 It is a schematic cross-sectional view of a laminated film according to still another embodiment of the present invention.

[0024] Figure 5 It is a schematic cross-sectional view of a laminated film according to still another embodiment of the present invention.

[0025] Explanation of symbols

[0026] 10Optical functional layer

[0027] 10a 1st main side

[0028] 10b 2nd main side

[0029] 20 porous layers

[0030] 30 1st adhesive layer

[0031] 40 2nd adhesive layer

[0032] 100 layers of laminated film DETAILED DESCRIPTION

[0033] Hereinafter, embodiments of the present invention will be described, but the present invention is not limited to these embodiments.

[0034] A. Overall structure of laminated film

[0035] Figure 1 It is a cross-sectional schematic diagram of a laminated film of an embodiment of the present invention. The laminated film 100 shown in the figure has an optical functional layer 10, a porous layer 20 and an adhesive layer 30. The optical functional layer 10 has a first main surface 10a and a second main surface 10b, and the first main surface 10a has a concavo-convex structure. The porous layer 20 is arranged on the first main surface 10a of the optical functional layer 10. The adhesive layer 30 is arranged on the opposite side of the porous layer 20 to the optical functional layer 10. As required, another adhesive layer 40 can be provided as the outermost layer on the second main surface 10b side of the optical functional layer 10. For convenience, the adhesive layer 30 is sometimes referred to as the first adhesive layer, and the other adhesive layer 40 is referred to as the second adhesive layer. When actually used, it is preferred that a release liner (not shown) is temporarily pasted on the surface of the first adhesive layer and the second adhesive layer respectively until the laminated film is used. By temporarily pasting the release liner, a roll of the laminated film can be formed while protecting the first adhesive layer and the second adhesive layer.

[0036] In an embodiment of the present invention, the optical functional layer 10 typically has a function of changing the direction of light. A laminated film comprising such an optical functional layer can achieve the following effects depending on the type of the optical functional layer: (1) various products can be surface decorated to improve their design or appearance design; (2) the color of the displayed image can be changed due to the visual recognition angle; and (3) different images due to the visual recognition angle can be displayed. Therefore, the laminated film of an embodiment of the present invention can also be referred to as a decorative film, an optical laminate, etc. Representative examples of optical functional layers include reflective holographic films, microlens array films, and prism films. Figure 1 and Figure 2 They are schematic cross-sectional views of a laminated film having a reflective holographic film as an optical functional layer; Figure 3 is a schematic cross-sectional view of a laminated film having an additional reflective holographic film as an optical functional layer; Figure 4 is a schematic cross-sectional view of a laminated film having a microlens array film as an optical functional layer; Figure 5It is a schematic cross-sectional view of a laminated film having a prism film as an optical functional layer. According to an embodiment of the present invention, even when the first adhesive layer is arranged on the first principal surface (concave-convex surface) side of the optical functional layer to protect the optical functional layer, the functional reduction of the optical functional layer caused by the first adhesive layer can be suppressed. In addition, when the optical functional layer is a holographic film (representatively a reflective holographic film), the function of the optical functional layer can be well exhibited without providing a metal layer or a metal oxide layer on the first principal surface (concave-convex surface). As a result, the effect of the optical functional layer can be obtained while ensuring transparency. Therefore, even when a holographic film is used as the optical functional layer, the application range of the laminated film can be significantly expanded. It should be noted that the composition of the reflective holographic film, the microlens array film and the prism film will be described in the following items B-1 to B-3, respectively.

[0037] The height and shape of the concavoconvex of the first main surface 10a of the optical functional layer 10 can be appropriately set according to the purpose (therefore, the type of optical functional layer). In an embodiment of the present invention, the height of the concavoconvex of the first main surface is 200nm to 100μm. In the case where the optical functional layer is a reflective holographic film, the height of the concavoconvex can be representatively less than a few μm or nanometer level. In the case where the optical functional layer is a microlens array film or a prism film, the height of the concavoconvex can be representatively micrometer level (a few μm to about 100μm). In this specification, "the height of the concavoconvex" refers to the distance from the peak (or top) to the valley (or flat end) of one concavoconvex part, and in the case where the concavoconvex is an irregular structure, it refers to the average distance from the peak (or top) to the valley (or flat end) of each concavoconvex part. In addition, "the spacing of the concavoconvex" refers to the distance from adjacent peaks (or tops) to peaks (or tops), and in the case where the concavoconvex is an irregular structure, it refers to the average distance from each adjacent peak (or top) to peak (or top). The details of the height and shape of the concavo-convexity of the first main surface will be described later in Sections B-1 to B-3 together with the configurations of the reflective holographic film, the microlens array film, and the prism film.

[0038] As described in item C below, the porous layer 20 preferably has a very low refractive index and a very high transparency. By using such a porous layer, appropriate reflection can be achieved at the interface with the optical functional layer, and the transparency of the entire laminate film can be ensured. As a result, the light direction conversion function brought by the optical functional layer can be fully exerted, and the visual recognizability of the product structure, image, etc. on the side opposite to the visible side of the optical functional layer can be ensured. The porous layer 20 can be formed on the first main surface 10a of the optical functional layer 10 via an adhesive layer, or it can be formed directly on the first main surface. Preferably, the porous layer is formed directly on the first main surface. If it is constructed in this way, it is possible to avoid adverse effects caused by the refractive index of the adhesive layer. Such direct formation can be achieved, for example, by coating or printing a porous layer forming liquid as described later. As for the porous layer 20, it can be as follows Figure 1 As shown in the figure, the surface of the first adhesive layer 30 side is uneven (it can follow the unevenness of the first main surface 10a of the optical function layer 10), or it can be as shown in the figure. Figure 2 As shown, the surface on the first adhesive layer 30 side is flat. Figure 2 The configuration in which the surface on the first adhesive layer side is flat as shown can be achieved, for example, by increasing the thickness of the porous layer so as to fill the recessed portion.

[0039] The transmittance difference ΔY of the laminated film is preferably -5 to +2, more preferably -5 to +1, and further preferably -5 to 0. According to an embodiment of the present invention, the laminated film can achieve excellent transparency as a whole. As a result, when the laminated film is applied to various products, the visual recognizability of the product structure, image, etc. on the opposite side of the visible side of the optical functional layer can be ensured. It should be noted that the transmittance difference ΔY can be calculated as described below. The transmittance of the laminated film is measured, and the Y value in the XYZ color system is calculated based on the transmission spectrum, which is used as the Ya value. On the other hand, the Y value of the film with the same structure except that the porous layer is not included is similarly calculated, and it is used as the Yb value. The transmittance difference ΔY is calculated by ΔY=Yb-Ya. The transmittance difference ΔY can be used as an indicator of the transparency of the laminated film.

[0040] The haze difference ΔH of the laminated film is preferably 0.1% to 1.0%, more preferably 0.1% to 0.8%, and further preferably 0.1% to 0.5%. According to an embodiment of the present invention, the haze of the laminated film as a whole can be reduced. As a result, when the laminated film is applied to various products, the visual recognizability of the product structure, image, etc. on the opposite side of the optical functional layer to the visible side can be ensured. It should be noted that the haze difference ΔH can be calculated as described below. The haze of the laminated film is measured and taken as the Ha value. On the other hand, the haze of a film of the same structure except that the porous layer is not included is similarly measured and taken as the Hb value. The haze difference ΔH is calculated by ΔH=Ha-Hb. The transmittance difference ΔY can be used as an indicator of the transparency of the laminated film.

[0041] The above embodiments may be combined appropriately. For example, the porous layer may follow Figure 3 to Figure 5 The optical function layer is formed by the unevenness of the first main surface.

[0042] Hereinafter, the constituent elements of the laminated film will be described in detail.

[0043] B. Optical functional layer

[0044] In the embodiment of the present invention, as described above, the optical functional layer 10 can be a reflective holographic film, a microlens array film or a prism film. It should be noted that they can be made of materials known in the industry and methods known in the industry, respectively, and therefore, the description of the constituent materials and manufacturing methods is omitted.

[0045] B-1. Reflective holographic film

[0046] In an embodiment of the present invention, a porous layer is formed on the first main surface (concave-convex surface) of a reflective holographic film, so that a holographic function can be exhibited without forming a metal reflective layer on the reflective holographic film. As a reflective holographic film, any appropriate structure can be adopted. As the concave-convex shape of the reflective holographic film, any appropriate fine concave-convex shape that can exhibit functions such as light diffusion, light scattering, light reflection, and light diffraction can be adopted. As representative examples, Fourier transform structure, double convex lens, light diffraction pattern, moth eye structure can be cited. In addition, it can also be a concave-convex shape such as a fine line pattern, a matte pattern, a parallel line pattern, and an interference pattern that has no light diffraction function but can exhibit a specific brightness. In one embodiment, the reflective holographic film is capable of converting reflected light into diffracted light.

[0047] In one embodiment, if Figure 1As shown, the reflective holographic film can have a concave-convex shape with a corrugated cross section and extending in one direction. The direction in which the concave-convex extends can be appropriately set according to the purpose. In this case, the spacing between the concave-convex is preferably 100nm to 900nm, more preferably 200nm to 800nm, further preferably 300nm to 700nm, and particularly preferably 400nm to 600nm. The height of the concave-convex is, for example, 10nm to 100μm, preferably 50nm to 100μm, more preferably 100nm to 2000nm, further preferably 200nm to 700nm, particularly preferably 220nm to 600nm, particularly preferably 240nm to 500nm, and most preferably 260nm to 350nm. In another embodiment, as Figure 3 As shown, the reflective holographic film may have a concave-convex shape (stripes in top view, so-called line & space) with convex portions having rectangular cross sections and extending in one direction at certain intervals. The direction in which the concave-convex portions extend may be appropriately set according to the purpose. The width of the convex portions may be, for example, 50nm to 350nm, or 100nm to 300nm, or 150nm to 250nm. In this case, the spacing of the concave-convex portions may be, for example, 50nm to 350nm, or 100nm to 300nm, or 150nm to 250nm; the height of the concave-convex portions may be the same as that of the concave-convex shape having a corrugated cross section and extending in one direction, and may be, for example, 50nm to 350nm, or 100nm to 300nm, or 150nm to 250nm. In the reflective holographic film having a concave-convex shape as shown in FIG. Figure 3 In the case of the structure shown, the width of the convex portion can be, for example, 500nm to 1500nm (1.5μm), and can be, for example, 700nm to 1300nm (1.3μm), and can be, for example, 900nm to 1100nm (1.1μm). In this case, the pitch of the concave and convex can be, for example, 500nm to 1500nm (1.5μm), and can be, for example, 700nm to 1300nm (1.3μm), and can be, for example, 900nm to 1100nm (1.1μm); the height of the concave and convex can also be the same as the case of the concave and convex shape having a cross-sectional waveform and extending in one direction, and can be, for example, 500nm to 4000nm (4.0μm), and can be, for example, 1000nm (1.0μm) to 3000nm (3.0μm), and can be, for example, 1500nm (1.5μm) to 2500nm (2.5μm). When the reflective holographic film has any of the above-mentioned structures, as long as the height and pitch of the concavo-convex portions are within the above-mentioned ranges, the light direction conversion function can be well maintained.

[0048] B-2. Microlens array film

[0049] Microlens array film Figure 4 As shown in FIG. 1 , the optical fiber has a flat base and a lens portion disposed on one side of the base. The lens portion is composed of a plurality of lenses. The lenses constituting the lens portion are typically convex lenses, and may have, for example, Figure 4 The lens can be as Figure 4 The patterns can be arranged in rows and columns (matrix), in a given pattern (e.g., stripes), or randomly. Figure 4 In the embodiment, the spacing of the concave and convex (lens) is preferably 50μm to 500μm, more preferably 70μm to 400μm, further preferably 100μm to 300μm, and particularly preferably 150μm to 250μm. The height of the concave and convex (lens) is preferably 2μm to 25μm, more preferably 4μm to 20μm, further preferably 6μm to 15μm, and particularly preferably 8μm to 12μm. In this case, the diameter of the lens (the diameter of the connection surface with the base portion, i.e., the bottom of the lens) is preferably 20μm to 200μm, more preferably 40μm to 180μm, further preferably 60μm to 150μm, and particularly preferably 80μm to 120μm. In the case where the optical functional layer is a microlens array film, when the spacing, height and diameter of the lens are in such a range, the light direction conversion function can be well maintained.

[0050] B-3. ​​Prism film

[0051] Prismatic film Figure 5 As shown, it has a flat base portion and a prism portion. The prism portion is typically composed of a plurality of unit prisms with a convex cross-section triangular shape arranged on the opposite side of the base portion and extending in one direction. The direction in which the unit prism extends (the direction of the ridgeline of the unit prism) can be appropriately set according to the purpose. Figure 5 In the embodiment, the pitch of the concave-convex (unit prism) is preferably 5μm to 25μm, more preferably 8μm to 20μm, further preferably 10μm to 18μm, and particularly preferably 12μm to 16μm. The height of the concave-convex (unit prism) is preferably 2μm to 25μm, more preferably 4μm to 20μm, further preferably 6μm to 15μm, and particularly preferably 8μm to 12μm. The length of the base of the unit prism is preferably 5μm to 25μm, more preferably 8μm to 20μm, further preferably 10μm to 18μm, and particularly preferably 12μm to 16μm. When the optical functional layer is a prism film, when the pitch, height and base length of the unit prism are in such a range, the light direction conversion function can be well maintained.

[0052] C. Porous layer

[0053] The porous layer typically has voids inside. The porosity of the porous layer is preferably 20% to 60% by volume, more preferably 25% to 55% by volume, further preferably 30% to 50% by volume, and particularly preferably 35% to 45% by volume. When the porosity is in such a range, the refractive index of the porous layer can be brought into an appropriate range, and a given mechanical strength can be ensured. The porosity is a value obtained by calculating the porosity using the Lorentz-Lorenz's formula based on the value of the refractive index measured using an ellipsometer.

[0054] The refractive index of the porous layer is preferably 1.15 to 1.30, more preferably 1.17 to 1.28, further preferably 1.18 to 1.26, and particularly preferably 1.19 to 1.24. By providing a porous layer having such a refractive index on the first main surface (concave-convex surface) of the optical functional layer, appropriate reflection can be achieved at the interface with the optical functional layer. As a result, the function of changing the direction of light brought by the optical functional layer can be fully utilized. Unless otherwise specified, the refractive index refers to the refractive index measured at a wavelength of 550 nm. The refractive index is a value measured by the method described in "(1) Refractive index of porous layer" of the embodiments described later.

[0055] The total light transmittance of the porous layer is preferably 85% to 99%, more preferably 87% to 98%, and further preferably 89% to 97%. By providing a porous layer having such a total light transmittance on the first main surface (concave-convex surface) of the optical functional layer, the laminated film can achieve excellent transparency as a whole. As a result, when the laminated film is applied to various products, the visual recognizability of the product structure, image, etc. on the opposite side of the optical functional layer to the visible side can be ensured.

[0056] The haze of the porous layer is, for example, less than 5%, preferably less than 3%. On the other hand, the haze is, for example, more than 0.1%, preferably more than 0.2%. By arranging the porous layer with such a haze on the first main surface (concave-convex surface) of the optical functional layer, the laminated film can achieve excellent transparency as a whole. As a result, when the laminated film is applied to various products, the visual recognition of the product structure, image, etc. on the opposite side of the optical functional layer to the visible side can be ensured. The haze can be measured, for example, by the method described below.

[0057] The void layer (porous layer) was cut into a size of 50 mm×50 mm, and the haze was measured by using a haze meter (HM-150 manufactured by Murakami Color Research Laboratory Co., Ltd.). The haze value was calculated by the following formula.

[0058] Haze (%) = [diffuse transmittance (%) / total light transmittance (%)] × 100 (%)

[0059] The thickness of the porous layer is preferably 30 nm to 5 μm, more preferably 200 nm to 4 μm, further preferably 400 nm to 2 μm, and particularly preferably 600 nm to 1 μm. When the thickness of the porous layer is within such a range, the light direction conversion function can be well maintained. Figure 2 to Figure 5 When the surface on the first adhesive layer 30 side has a flat structure as shown, the thickness of the porous layer refers to the maximum thickness.

[0060] As long as the porous layer has the above-mentioned desired characteristics, any appropriate structure can be adopted. The porous layer can be preferably formed by coating or printing. As the material constituting the porous layer, for example, the materials described in International Publication No. 2004 / 113966, Japanese Patent Publication No. 2013-254183, and Japanese Patent Publication No. 2012-189802 can be used. As a representative example, silicon compounds can be cited. As silicon compounds, for example, silicon dioxide compounds; hydrolyzable silanes, and their partial hydrolyzates and dehydrated condensates; silicon compounds containing silanol groups; active silica obtained by contacting silicates with acids and ion exchange resins. Also exemplified are: organic polymers; polymerizable monomers (for example, (meth) acrylic monomers, and styrene monomers); curable resins (for example, (meth) acrylic resins, fluorine-containing resins, and urethane resins). These materials can be used alone or in combination. The porous layer can be formed by applying or printing a solution or dispersion of such a material.

[0061] The size of the void (pore) in the porous layer refers to the diameter of the major axis of the void (pore) and the diameter of the minor axis. The size of the void (pore) is, for example, 2nm to 500nm. The size of the void (pore) is, for example, more than 2nm, preferably more than 5nm, more preferably more than 10nm, and further preferably more than 20nm. On the other hand, the size of the void (pore) is, for example, less than 500nm, preferably less than 200nm, and more preferably less than 100nm. The range of the size of the void (pore) is, for example, 2nm to 500nm, preferably 5nm to 500nm, more preferably 10nm to 200nm, and further preferably 20nm to 100nm. The size of the void (pore) can be adjusted to the desired size according to the purpose and use. The size of the void (pore) can be quantified by the BET test method.

[0062] The size of the voids (pores) can be quantified by the BET test method. Specifically, after 0.1 g of the sample (the void layer formed) is put into the capillary of the specific surface area measuring device (manufactured by McMeretic: ASAP2020), it is dried under reduced pressure at room temperature for 24 hours to degas the gas in the void structure. Then, by adsorbing nitrogen on the above sample to draw an adsorption isotherm, the pore distribution is obtained. In this way, the void size can be evaluated.

[0063] As the porous layer having voids inside, for example, a porous layer having a porous layer and / or an air layer in at least a portion thereof can be cited. The porous layer typically includes aerogels and / or particles (e.g., hollow microparticles and / or porous particles). The porous layer can be preferably a nanoporous layer (specifically, 90% or more of the micropores have a diameter of 10 -1 nm~10 3 nm range).

[0064] As the above-mentioned particles, any appropriate particles can be used. The particles are typically formed of a silicon dioxide compound. As the shape of the particles, for example, spherical, plate-like, needle-like, rope-like, and grape-like. As rope-like particles, for example, a plurality of particles having a spherical, plate-like, or needle-like shape are connected to form a rosary-like particle; short fiber-like particles (for example, short fiber-like particles described in Japanese Patent Gazette No. 2001-188104), and combinations thereof can be listed. Rope-like particles can be straight-chain or branched. As grape-like particles, for example, a plurality of spherical, plate-like, and needle-like particles are condensed to form grape-like particles. The shape of the particles can be confirmed by observation using, for example, a transmission electron microscope.

[0065] An example of a specific composition of the porous layer is described below. The porous layer of this embodiment contains one or more structural units that form a fine void structure, and the structural units are chemically bonded together by catalysis. As the shape of the structural unit, for example: particle-shaped, fibrous, rod-shaped, and flat-plate-shaped can be listed. The structural unit can have only one shape, or it can have a combination of two or more shapes. The following mainly describes the case where the porous layer is a porous layer of a porous body in which the above-mentioned fine pore particles are chemically bonded together.

[0066] Such a void layer can be formed by, for example, chemically bonding microporous particles to each other in the void layer forming process. It should be noted that, in an embodiment of the present invention, the shape of the "particles" (for example, the above-mentioned microporous particles) is not particularly limited, for example, it can be spherical or other shapes. In addition, in an embodiment of the present invention, the above-mentioned microporous particles can be, for example, sol-gel beaded particles, nanoparticles (hollow nano-silica / nano hollow sphere particles), nanofibers, etc. The microporous particles typically include inorganic substances. As specific examples of inorganic substances, silicon (Si), magnesium (Mg), aluminum (Al), titanium (Ti), zinc (Zn), and zirconium (Zr) can be cited. They can be used alone or in combination of two or more. In one embodiment, the above-mentioned microporous particles are, for example, microporous particles of silicon compounds, and the above-mentioned porous body is, for example, an organosilicon porous body. The microporous particles of the above-mentioned silicon compound, for example, include a pulverized body of a gel-like silica compound. In addition, as other forms of porous layers having a porous layer and / or an air layer in at least a portion, there are, for example, void layers formed by fibrous materials such as nanofibers, in which the fibrous materials are entangled with each other to form voids and form a layer. The method for manufacturing such a void layer is not particularly limited, for example, it is the same as the case of the void layer of a porous body in which the above-mentioned microporous particles are chemically bonded to each other. In addition, as other forms, void layers using hollow nanoparticles and nanoclays, void layers formed using hollow nano hollow spheres and magnesium fluoride can be listed. The void layer can be a void layer formed by a single constituent substance, or it can be a void layer formed by multiple constituent substances. The void layer can be composed of a single form mentioned above, or it can be composed of multiple forms mentioned above.

[0067] In the present embodiment, the porous structure of the porous body can be, for example, a continuous bubble structure formed by a continuous pore structure. As for the continuous bubble structure, for example, in the above-mentioned organic silicon porous body, it refers to the state in which the pore structure is three-dimensionally connected, and it can also be said that the internal voids of the pore structure are continuous. By making the porous body have a continuous bubble structure, the porosity can be increased. However, in the case of using single bubble particles (particles each having a pore structure) such as hollow silica, a continuous bubble structure cannot be formed. On the other hand, in the case of using, for example, silica gel particles (a crushed product of a gel-like silicon compound forming a sol), since the particles have a three-dimensional tree-like structure, the tree-like particles will settle and precipitate in the coating film (a coating film of a sol containing a crushed product of a gel-like silicon compound), thereby easily forming a continuous bubble structure. The porous layer is more preferably a monolithic structure in which the continuous bubble structure includes a plurality of pore distributions. The monolithic structure represents a hierarchical structure, which includes, for example, a structure in which nano-sized fine voids exist, and a continuous bubble structure formed by the aggregation of such nano-voids. In the case of forming a monolithic structure, for example, fine voids can be used to impart membrane strength, and coarse interconnected voids can be used to impart high porosity, thereby achieving both membrane strength and high porosity. Such a monolithic structure can preferably be formed by controlling the pore distribution of the void structure generated in the gel (gel-like silicon compound) at the pre-stage of crushing into silica gel particles. In addition, for example, when crushing the gel-like silicon compound, the particle size distribution of the crushed silica gel particles is controlled to a desired size, so that a monolithic structure can be formed.

[0068] The porous layer contains, for example, pulverized products of the gel-like compound as described above, and the pulverized products are chemically bonded together. The form of chemical bonding (chemical bond) between the pulverized products in the porous layer is not particularly limited, and examples thereof include cross-linking, covalent bonding, and hydrogen bonding.

[0069] The volume average particle size of the above-mentioned pulverized material in the porous layer is, for example, 0.10 μm or more, preferably 0.20 μm or more, and more preferably 0.40 μm or more. On the other hand, the volume average particle size is, for example, 2.00 μm or less, preferably 1.50 μm or less, and more preferably 1.00 μm or less. The range of the volume average particle size is, for example, 0.10 μm to 2.00 μm, preferably 0.20 μm to 1.50 μm, and more preferably 0.40 μm to 1.00 μm. The particle size distribution can be measured by a particle size distribution evaluation device such as a dynamic light scattering method and a laser diffraction method, and an electron microscope such as a scanning electron microscope (SEM) and a transmission electron microscope (TEM). It should be noted that the volume average particle size is an indicator of the deviation of the particle size of the pulverized material.

[0070] The type of the gel-like compound is not particularly limited. Examples of the gel-like compound include gel-like silicon compounds.

[0071] In addition, in the porous layer (void layer), for example, the silicon atoms contained preferably form siloxane bonds. As a specific example, the proportion of unbonded silicon atoms (i.e., residual silanol) among all silicon atoms contained in the void layer is, for example, less than 50%, preferably less than 30%, and more preferably less than 15%.

[0072] An example of a method for forming such a porous layer will be described below.

[0073] Typically, the method includes: a precursor forming step of forming a void structure as a precursor of a porous layer (void layer) on a resin film; and a cross-linking reaction step of inducing a cross-linking reaction inside the precursor after the precursor forming step. The method further includes: a liquid containing liquid (hereinafter sometimes referred to as "microporous particle containing liquid" or simply "containing liquid") containing microporous particles; and a drying step of drying the containing liquid, in which the microporous particles in the dried body are chemically bonded to each other to form a precursor. The containing liquid is not particularly limited, and is, for example, a suspension containing microporous particles. It should be noted that the following mainly describes the case where the microporous particles are a pulverized product of a gel-like compound and the void layer contains a porous body (preferably a silicone porous body) of the pulverized product of the gel-like compound. It should be noted that in the case where the microporous particles are other than the pulverized product of the gel-like compound, the porous layer can also be formed in the same manner.

[0074] According to the above method, for example, a porous layer (void layer) having a very low refractive index can be formed. The reason for this can be speculated as follows, for example. However, this speculation does not limit the method for forming the porous layer.

[0075] The above-mentioned pulverized material is obtained by pulverizing a gel-like silicon compound, and therefore, the three-dimensional structure of the gel-like silicon compound before pulverization is formed in a state dispersed in the three-dimensional basic structure. Furthermore, in the above-mentioned method, by coating the pulverized material of the gel-like silicon compound on a resin film, a precursor of a porous structure based on the three-dimensional basic structure can be formed. That is, according to the above-mentioned method, a new porous structure (three-dimensional basic structure) based on the coating of the pulverized material, which is different from the three-dimensional structure of the gel-like silicon compound, can be formed. Therefore, in the void layer finally obtained, for example, a low refractive index that functions to the same extent as an air layer can be achieved. In addition, in the above-mentioned method, chemical bonds are formed between the pulverized materials, and therefore, the three-dimensional basic structure can be fixed. Therefore, although the void layer finally obtained is a structure with voids, sufficient strength and flexibility can be maintained.

[0076] The specific structure and formation method of the porous layer are described in detail in, for example, International Publication No. 2019 / 151073. The description of this publication is incorporated herein by reference.

[0077] D. 1st adhesive layer

[0078] The first adhesive layer has a hardness that is not permeable to the voids in the porous layer under normal conditions. The storage modulus of the first adhesive layer at 23° C. is typically 1.0×10 5 (Pa)~1.0×10 7 (Pa). For example, 1.1×10 5 (Pa) or more, 1.2×10 5 (Pa) or more, 1.3×10 5 (Pa) or more, 1.4×10 5 (Pa) or more, 1.5×10 5 (Pa) or more, 1.6×10 5 (Pa) or more, 1.7×10 5 (Pa) or more, 1.8×10 5 (Pa) or more, 1.9×10 5 (Pa) or above or 2.0×10 5 (Pa) or more, and 1.0×10 7 (Pa) or less, 5.0×10 6 (Pa) or less, 1.0×10 6 (Pa) or less or 5.0×10 5 (Pa) or less. Preferably 1.3×10 5 (Pa)~1.0×10 6 (Pa), more preferably 1.5×10 5 (Pa)~5.0×10 5 The storage modulus can be determined by the method described in JIS K 7244-1 "Plastics - Test methods for dynamic mechanical properties", by measuring at a frequency of 1 Hz in a range of -50°C to 150°C at a heating rate of 5°C / min and reading the value at 23°C.

[0079] As the adhesive constituting the first adhesive layer, any appropriate adhesive can be used as long as it has the characteristics as described above. As the adhesive, an acrylic adhesive (acrylic adhesive composition) can be cited as a representative example. The acrylic adhesive composition typically contains a (meth) acrylic polymer as a main component (base polymer). In the solid content of the adhesive composition, for example, the (meth) acrylic polymer can be contained in the adhesive composition at a ratio of more than 50% by weight, preferably more than 70% by weight, and more preferably more than 90% by weight. The (meth) acrylic polymer contains an alkyl (meth) acrylate as a monomer unit as a main component. It should be noted that (meth) acrylate refers to acrylate and / or methacrylate. As the alkyl group of the alkyl (meth) acrylate, for example, a straight-chain or branched alkyl group having 1 to 18 carbon atoms can be cited. The average number of carbon atoms of the alkyl group is preferably 3 to 9. As monomers constituting (meth) acrylic polymers, in addition to (meth) alkyl acrylates, comonomers such as carboxyl-containing monomers, hydroxyl-containing monomers, amide-containing monomers, aromatic ring-containing (meth) acrylates, and heterocyclic (meth) acrylates can be cited. The comonomer is preferably a hydroxyl-containing monomer and / or a heterocyclic (meth) acrylate, more preferably N-acryloylmorpholine. The acrylic adhesive composition may preferably contain a silane coupling agent and / or a crosslinking agent. As a silane coupling agent, for example, an epoxy-containing silane coupling agent can be cited. As a crosslinking agent, for example, an isocyanate crosslinking agent and a peroxide crosslinking agent can be cited. The details of such an adhesive layer or acrylic adhesive composition are, for example, recorded in Japanese Patent No. 4140736, and the records of the gazette are cited in this specification as a reference.

[0080] The thickness of the first pressure-sensitive adhesive layer is preferably 3 μm to 30 μm, more preferably 5 μm to 10 μm. When the thickness of the first pressure-sensitive adhesive layer is within such a range, there are advantages in that sufficient adhesion is obtained and the influence on the optical function layer is small.

[0081] E. Second adhesive layer

[0082] The second adhesive layer is formed of any appropriate adhesive. In one embodiment, the second adhesive layer is formed of an adhesive having flexibility that can absorb the propagation of vibration and suppress damage to the porous layer. The storage modulus of the second adhesive layer at 23° C. is, for example, 1.0×10 5 (Pa) or less, for example, 1.0×10 5 (Pa) or less, 9.5×10 4 (Pa) or less, 9.0×10 4 (Pa) or less, 8.5×10 4 (Pa) or less, 8.0×10 4 (Pa) or less, 7.5×104 (Pa) or less, or 7.0×10 4 (Pa) or less, and 1.0×10 3 (Pa) or more, 5.0×10 3 (Pa) or more, 1.0×10 4 (Pa) or above, or 5.0×10 4 (Pa) or more. Preferably 5.0×10 3 (Pa)~9.0×10 4 (Pa) or less, more preferably 1.0×10 4 (Pa)~8.5×10 4 (Pa).

[0083] As the adhesive constituting the second adhesive layer, any appropriate adhesive can be used as long as it has the characteristics as described above. As the adhesive, an acrylic adhesive (acrylic adhesive composition) can be representatively mentioned. As the acrylic adhesive composition, it is as described in the above-mentioned item D. However, the adhesive constituting the second adhesive layer preferably does not contain a heterocyclic (meth)acrylate as a comonomer. In addition, the weight-average molecular weight Mw of the base polymer in the adhesive composition is preferably 2,000,000 or less, more preferably 5,000 to 1,600,000. The details of the second adhesive layer or the acrylic adhesive composition constituting the second adhesive layer are described, for example, in Japanese Patent Publication No. 2016-190996, and the description of the publication is cited in this specification as a reference.

[0084] The thickness of the second adhesive layer is preferably 5 μm to 300 μm, more preferably 10 μm to 200 μm. When the thickness of the second adhesive layer is within such a range, the impact can be mitigated and damage to the porous layer can be reduced, particularly during lateral vibration.

[0085] F. Usage of laminated film

[0086] As described above, the laminated film can be used as a decorative film or a logo. For example, the laminated film can be attached to an image display device (representatively a smart phone, a tablet terminal) and used as a logo. In addition, for example, the laminated film can be attached to the back of a smart phone and used as a decorative film.

[0087] Example

[0088] Hereinafter, the present invention will be specifically described in conjunction with the examples, but the present invention is not limited to these examples. It should be noted that the measuring methods of each characteristic are as follows. In addition, as long as there is no particular clear description, the "%" and "part" in the examples are weight references.

[0089] (1) Refractive index of porous layer

[0090] After forming a porous layer on the acrylic film, it was cut into a size of 25 mm × 50 mm and attached to the surface of a glass plate (thickness: 3 mm) via an adhesive. The central part of the back of the above-mentioned glass plate (about 20 mm in diameter) was filled with a black marker pen to obtain a sample that does not reflect on the back of the glass plate. The above-mentioned sample was placed in an ellipsometer (manufactured by JA Woollam Japan: VASE), and the refractive index was measured under the conditions of a wavelength of 550 nm and an incident angle of 50 to 80 degrees.

[0091] (2) Peel test

[0092] The laminated film obtained in the embodiment and the comparative example was cut into 25 mm × 50 mm pieces as test samples. For the test sample, a 180° peeling test was performed to peel the porous layer from the optical functional layer using a tensile testing machine (trade name: TCM-1kNB, manufactured by MINEBEA Co., Ltd.), and the interlayer adhesion (180° peeling adhesion) (N / 25mm) between the optical functional layer and the porous layer was measured and evaluated according to the following criteria. The measurement was performed in an atmosphere of 23°C and 50% RH at a peeling angle of 180° and a tensile speed of 300 mm / min.

[0093] ○ (good): Adhesion strength is 0.5 (N / 25mm) or more

[0094] ×(bad): Adhesion strength is less than 0.5(N / 25mm)

[0095] (3) Fixedness

[0096] The measurement was performed according to JIS K 5600. Specifically, a transparent resin film was arranged on the outermost layer of the first main surface (concave-convex surface) side of the optical functional layer of the laminated film obtained in the examples and comparative examples, and whether the resin film moved was confirmed by steel wool #0000, load 250g, and stroke 25mm, and the evaluation was performed according to the following criteria. It should be noted that, with respect to comparative example 5, the obtained laminated film was directly provided for the test.

[0097] ○ (good): Film migration

[0098] × (bad): The film did not move

[0099] (4) Changes in visual recognition due to angle

[0100] A transparent resin film is disposed as the outermost layer on the first principal surface (concave-convex surface) side of the optical functional layer of the laminated film obtained in the embodiments and comparative examples to prepare a test sample. It should be noted that, with respect to comparative example 5, the obtained laminated film is directly used as a test sample. A light source is disposed in the normal direction of the transparent resin film side of the test sample, and a point image with a diameter of 5 mm and a spacing of 15 mm is disposed on the opposite side of the test sample from the transparent resin film. The image is observed through the test sample from the normal direction and the direction at a polar angle of 45° relative to the normal direction, and evaluated according to the following benchmarks.

[0101] ○ (Good): The image (size, shape, and color of dots) changes as a whole in the normal direction and 45° direction.

[0102] △ (middle): In the normal direction and 45° direction, the image (size, shape, color of the dots) changes in some areas.

[0103] × (bad): The image (dot size, shape, color) does not change in the normal direction and 45° direction.

[0104] (5) Transmittance difference ΔY

[0105] The transmittance of the laminated film obtained in the examples and comparative examples was measured using a spectrophotometer (manufactured by Hitachi, Ltd., "U-4100"). The Y value in the XYZ color system was calculated from the transmission spectrum and was taken as the Ya value. On the other hand, the Y value of the film having the same structure except that the porous layer was not included was similarly calculated and taken as the Yb value. The transmittance difference ΔY was calculated by ΔY=Yb-Ya and evaluated according to the following criteria. It should be noted that the transmittance difference ΔY is an indicator of transparency.

[0106] ○ (good): ΔY less than 2.0

[0107] × (bad): ΔY is 2.0 or more

[0108] [Manufacturing Example 1] Preparation of a coating liquid for forming a porous layer

[0109] (1) Gelation of Silicon Compounds

[0110] 0.95 g of methyltrimethoxysilane (MTMS), a precursor of a silicon compound, was dissolved in 2.2 g of dimethyl sulfoxide (DMSO) to prepare a mixed solution A. 0.5 g of a 0.01 mol / L aqueous oxalic acid solution was added to the mixed solution A, and the mixture was stirred at room temperature for 30 minutes to hydrolyze MTMS, thereby generating a mixed solution B containing tri(hydroxy)methylsilane.

[0111] To 5.5 g of DMSO were added 0.38 g of 28 wt % ammonia water and 0.2 g of pure water, and the mixed solution B was further added, followed by stirring at room temperature for 15 minutes to gel tri(hydroxy)methylsilane, thereby obtaining a mixed solution C containing a gel-like silicon compound.

[0112] (2) Aging treatment

[0113] The mixed solution C containing the gel-like silicon compound prepared as described above was aged at 40° C. for 20 hours as it was, thereby performing an aging treatment.

[0114] (3) Crushing

[0115] Next, the gel-like silicon compound that has been aged as described above is crushed into particles of several mm to several cm in size using a spatula. Next, 40 g of isopropyl alcohol (IPA) is added to the mixed solution C, and after slight stirring, it is allowed to stand at room temperature for 6 hours to decant the solvent and catalyst in the gel. The same decantation treatment is performed three times to replace the solvent and obtain a mixed solution D. Next, the gel-like silicon compound in the mixed solution D is subjected to a pulverization treatment (high-pressure medium-free pulverization). The pulverization treatment (high-pressure medium-free pulverization) is performed using a homogenizer (manufactured by SMT Co., Ltd., trade name "UH-50"). After weighing 1.85 g of the gel-like compound and 1.15 g of IPA in the mixed solution D in a 5 cc screw-capped bottle, the mixture is pulverized for 2 minutes at 50 W and 20 kHz.

[0116] By this pulverization treatment, the gel-like silicon compound in the mixed solution D was pulverized, and the mixed solution D became a sol solution E of the pulverized product. The volume average particle size indicating the particle size deviation of the pulverized product contained in the sol solution E was confirmed by a dynamic light scattering nano-tracking particle size analyzer (manufactured by Nikkiso Co., Ltd., UPA-EX150 model), and the result was 0.50 to 0.70. Furthermore, 0.062 g of a 1.5 wt% MEK (methyl ethyl ketone) solution of a photobase generator (Wako Pure Chemical Industries, Ltd.: trade name WPBG266) and 0.036 g of a 5% MEK solution of bis(trimethoxysilyl)ethane were added to 0.75 g of the sol solution E to obtain a coating solution for forming a porous layer.

[0117] [Manufacturing Example 2] Preparation of Adhesive Constituting the First Adhesive Layer

[0118] In a four-necked flask equipped with a stirring blade, a thermometer, a nitrogen inlet tube, and a condenser, 90.7 parts of butyl acrylate, 6 parts of N-acryloylmorpholine, 3 parts of acrylic acid, 0.3 parts of 2-hydroxybutyl acrylate, 0.1 parts by weight of 2,2'-azobisisobutyronitrile as a polymerization initiator, and 100 g of ethyl acetate were added, and nitrogen was introduced while slowly stirring to replace the atmosphere with nitrogen. Then, a polymerization reaction was carried out for 8 hours while maintaining the liquid temperature in the flask at approximately 55°C, thereby preparing an acrylic polymer solution. An acrylic adhesive solution was prepared by mixing 0.2 parts of an isocyanate crosslinking agent (CORONATA L manufactured by Nippon Polyurethane Industries, Ltd., an adduct of trimethylolpropane and toluene diisocyanate), 0.3 parts of benzoyl peroxide (NYPER BMT manufactured by NOF Corporation), and 0.2 parts of γ-glycidoxypropylmethoxysilane (KBM-403 manufactured by Shin-Etsu Chemical Co., Ltd.) with respect to 100 parts of the solid content of the obtained acrylic polymer solution. Next, the acrylic adhesive solution was applied to one side of a polyethylene terephthalate (PET) film (manufactured by Mitsubishi Chemical Polyester Film Co., Ltd., thickness: 38 μm) treated with silicone so that the thickness of the adhesive layer after drying reached 20 μm, and dried at 150°C for 3 minutes to form an adhesive layer. The storage modulus of the obtained adhesive was 1.3×10 5 (Pa).

[0119] [Manufacturing Example 3] Preparation of Adhesive Constituting Second Adhesive Layer

[0120] In a four-necked flask equipped with a stirring blade, a thermometer, a nitrogen inlet tube, and a condenser, 99 parts of butyl acrylate, 1 part of 4-hydroxybutyl acrylate, 0.1 part of 2,2'-azobisisobutyronitrile as a polymerization initiator, and 100 parts of ethyl acetate were added, and nitrogen was introduced while slowly stirring to replace the atmosphere with nitrogen. Then, the liquid temperature in the flask was maintained at around 55°C and a polymerization reaction was performed for 8 hours to prepare an acrylic polymer solution. To 100 parts of the solid content of the obtained acrylic polymer solution, 0.1 part of an isocyanate crosslinking agent (TAKENATED 110N manufactured by Mitsui Takeda Chemical Co., Ltd., trimethylolpropane benzyl diisocyanate), 0.1 part of benzoyl peroxide (NYPER BMT manufactured by NOF Corporation), and 0.2 part of γ-glycidoxypropylmethoxysilane (KBM-403 manufactured by Shin-Etsu Chemical Co., Ltd.) were added to prepare a solution of an acrylic adhesive composition. Next, the solution of the acrylic adhesive composition was applied to one side of a polyethylene terephthalate film (separator: manufactured by Mitsubishi Chemical Polyester Film Co., Ltd., MRF38) treated with a silicone release agent, and dried at 150°C for 3 minutes to form a 20 μm thick adhesive layer on the surface of the separator. The storage modulus of the obtained adhesive was 8.2×10 4 (Pa).

[0121] [Example 1]

[0122] As an optical functional layer, a transparent reflective holographic film (manufactured by HOLOGRAM SUPPLY, "SP-3T") having a corrugated concave and convex shape in cross section was used. The concave and convex height of "SP-3T" is 350nm. The coating liquid for forming a porous layer prepared in Manufacturing Example 1 was applied to the concave and convex surface of the holographic film. The coated film was treated at a temperature of 100°C for 1 minute to dry it, and a porous layer (thickness 30nm) was formed on the holographic film (optical functional layer). The porosity of the obtained porous layer was 60% and the refractive index was 1.15. Next, a first adhesive layer (thickness 10μm) composed of the adhesive prepared in Manufacturing Example 2 was formed on the surface of the porous layer, and a second adhesive layer (thickness 28μm) composed of the adhesive prepared in Manufacturing Example 3 was further formed on the surface of the substrate. In this way, a laminated film having the structure of the first adhesive layer / porous layer / optical functional layer / second adhesive layer was produced. The obtained laminated film was subjected to the evaluations of (2) to (5) above. The results are shown in Table 1.

[0123] [Example 2]

[0124] A laminated film was produced in the same manner as in Example 1 except that the thickness of the porous layer was 800 nm. The obtained laminated film was subjected to the same evaluation as in Example 1. The results are shown in Table 1.

[0125] [Example 3]

[0126] A laminated film was produced in the same manner as in Example 1 except that the thickness of the porous layer was set to 800 nm and the refractive index of the porous layer was set to 1.20. The obtained laminated film was subjected to the same evaluation as in Example 1. The results are shown in Table 1. It should be noted that the refractive index of the porous layer was adjusted by adjusting the amounts of bis(trimethoxysilyl)ethane and the photobase generator in the porous layer-forming coating liquid of Production Example 1.

[0127] [Example 4]

[0128] A laminated film was produced in the same manner as in Example 1 except that the thickness of the porous layer was set to 5 μm (5000 nm) and the refractive index of the porous layer was set to 1.20. The obtained laminated film was subjected to the same evaluation as in Example 1. The results are shown in Table 1. It should be noted that the refractive index of the porous layer was adjusted by adjusting the amounts of bis(trimethoxysilyl)ethane and the photobase generator in the porous layer-forming coating liquid of Production Example 1.

[0129] [Example 5]

[0130] A laminated film was produced in the same manner as in Example 1 except that the thickness of the porous layer was set to 800 nm and the refractive index of the porous layer was set to 1.30. The obtained laminated film was subjected to the same evaluation as in Example 1. The results are shown in Table 1. It should be noted that the refractive index of the porous layer was adjusted by adjusting the amounts of bis(trimethoxysilyl)ethane and the photobase generator in the porous layer-forming coating liquid of Production Example 1.

[0131] [Example 6]

[0132] As the optical functional layer, a transparent reflective holographic film (manufactured by Scivax, "FCLS / 200-4×4") having a concave-convex surface in a top-view stripe shape (lines and spaces) was used instead of "SP-3T", and a laminated film was prepared in the same manner as in Example 3. The concave-convex height of "FCLS" was 200 nm. The obtained laminated film was subjected to the same evaluation as in Example 1. The results are shown in Table 1.

[0133] [Example 7]

[0134] As an optical functional layer, a transparent reflective holographic film having a concave-convex surface with a top-view stripe shape (lines and gaps) (manufactured by Scivax, "FTLS / 1000 / 2000 / 2000-100×100") was used instead of "SP-3T". A laminated film was prepared in the same manner as in Example 3. The concave-convex height of "FTLS" was 2 μm (2000 nm). The obtained laminated film was subjected to the same evaluation as in Example 1. The results are shown in Table 1.

[0135] [Example 8]

[0136] As the optical functional layer, a microlens array film (manufactured by Grapac Japan, "HALS") was used instead of "SP-3T", and a laminated film was prepared in the same manner as in Example 3. The concavo-convex height of the microlens array film was 10 μm (10000 nm). The obtained laminated film was subjected to the same evaluation as in Example 1. The results are shown in Table 1.

[0137] [Example 9]

[0138] A laminated film was prepared in the same manner as in Example 3 except that a prism film was used instead of "SP-3T" as the optical functional layer. The prism film had a concavo-convex height of 10 μm (10000 nm). The obtained laminated film was evaluated in the same manner as in Example 1. The results are shown in Table 1.

[0139] [Comparative Example 1]

[0140] The first adhesive layer was directly formed at both ends of the concavo-convex surface of the optical function layer. In addition, a laminated film having the structure of the first adhesive layer (end only) / optical function layer / second adhesive layer was prepared in the same manner as in Example 1. In the laminated film obtained, an air layer (gap portion) was formed on the upper part of the concavo-convex surface of the optical function layer. The laminated film obtained was provided for the same evaluation as in Example 1. The results are shown in Table 1.

[0141] [Comparative Example 2]

[0142] A laminated film was produced in the same manner as in Example 1 except that the thickness of the porous layer was set to 700 nm and the refractive index of the porous layer was set to 1.10. The obtained laminated film was subjected to the same evaluation as in Example 1. The results are shown in Table 1. It should be noted that the refractive index of the porous layer was adjusted by adjusting the amounts of bis(trimethoxysilyl)ethane and the photobase generator in the porous layer-forming coating liquid of Production Example 1.

[0143] [Comparative Example 3]

[0144] A laminated film was produced in the same manner as in Example 1 except that a ZrO2 layer (refractive index 2.05, thickness 50 nm) was formed by sputtering instead of the porous layer. The obtained laminated film was subjected to the same evaluation as in Example 1. The results are shown in Table 1.

[0145] [Comparative Example 4]

[0146] A laminated film was produced in the same manner as in Example 1 except that a SiO2 layer (refractive index 1.47, thickness 50 nm) was formed by sputtering instead of the porous layer. The obtained laminated film was subjected to the same evaluation as in Example 1. The results are shown in Table 1.

[0147] [Comparative Example 5]

[0148] A laminated film having a structure of transparent resin film / water / optical functional layer / second adhesive layer was prepared in the same manner as in Example 1, except that a transparent resin film was laminated on the concavoconvex surface of the optical functional layer while the surface was wetted with water. The obtained laminated film was subjected to the same evaluation as in Example 1. The results are shown in Table 1.

[0149] [Comparative Example 6]

[0150] A laminated film having a structure of first adhesive layer / optical functional layer / second adhesive layer was prepared in the same manner as in Example 1, except that the first adhesive layer was directly formed on the concavo-convex surface of the optical functional layer. The obtained laminated film was subjected to the same evaluation as in Example 1. The results are shown in Table 1.

[0151]

[0152] It is clear from Table 1 that according to an embodiment of the present invention, the direction conversion function of light brought by the optical functional layer can be fully exerted, and the transparency of the laminated film as a whole can be ensured. In particular, even if the optical functional layer is a holographic film, it is not necessary to provide a metal layer (reflective layer) to perform the function well. In addition, according to an embodiment of the present invention, the optical functional layer has a large adhesive force with the porous layer, and therefore, the integrity of the laminated film is also good.

[0153] Industrial Applicability

[0154] The laminated film according to the embodiment of the present invention can be suitably used as a decorative film.

Claims

1. A laminated film comprising: An optical functional layer having a first main surface and a second main surface, wherein the first main surface has a concavo-convex structure, and the height of the concavo-convex is 10 nm to 100 μm; A porous layer disposed on the first main surface of the optical functional layer; and an adhesive layer provided on the side of the porous layer opposite to the optical functional layer, The optical functional layer is a reflective holographic film, a microlens array film or a prism film. The refractive index of the porous layer is 1.15 to 1.

30.

2. The laminated film according to claim 1, wherein The porous layer includes a silicon compound.

3. The laminated film according to claim 1 or 2, wherein The porosity of the porous layer is 20 volume % to 60 volume %.

4. The laminated film according to any one of claims 1 to 3, wherein The thickness of the porous layer is 30 nm to 5 μm.

5. The laminated film according to any one of claims 1 to 4, wherein The porous layer includes one or more constituent units forming a fine void structure, and the constituent units are chemically bonded together by a catalyst.

6. The laminated film according to claim 5, wherein The constituent units of the porous layer are constituent units in at least one shape selected from the group consisting of a particle shape, a fiber shape, a rod shape, and a plate shape.

7. The laminated film according to claim 5 or 6, wherein The bonding between the constituent units of the porous layer includes hydrogen bonding or covalent bonding.

8. The laminated film according to any one of claims 1 to 7, wherein The porous layer is formed directly on the first main surface of the optical function layer.

Citation Information

Patent Citations

  • Antireflection film, polarizer and display device

    JP2012189802A

  • Antireflection film, manufacturing method thereof, polarizer, and image display device

    JP2013254183A

  • Decoration film and method for producing the same

    JP2020028981A

  • Decorative film

    JP2020104467A

  • Antireflective film

    WO2004113966A1