Solid electrolyte material and battery using same

By adding specific oxide materials to solid electrolyte materials to form a composite to absorb hydrogen halide gas, the problem of hydrogen halide gas generation in battery manufacturing is solved, enabling battery manufacturing at higher dew point temperatures and lower manufacturing costs. It also improves lithium-ion conductivity and battery performance.

CN118742974AInactive Publication Date: 2024-10-01PANASONIC INTELLECTUAL PROPERTY MANAGEMENT CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202280092430.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-11
Filing Date
2022-11-30
Publication Date
2024-10-01
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing solid electrolyte materials produce hydrogen halide gas when manufacturing batteries, leading to increased manufacturing costs and environmental pollution, and it is difficult to reduce the amount of gas generated.

Method used

A solid electrolyte material containing Li, M, O, and X is used, where M is Nb, Ta, and Zr, and The mass ratio of the solid electrolyte is 1% or more and 50% or less to absorb and reduce the generation of hydrogen halide gas.

Benefits of technology

It effectively reduces the generation of hydrogen halide gas, allows batteries to be manufactured at higher dew point temperatures, reduces manufacturing costs, and improves lithium ion conductivity and battery charge and discharge characteristics.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118742974A_ABST
    Figure CN118742974A_ABST
Patent Text Reader

Abstract

The solid electrolyte material of the present disclosure includes a solid electrolyte and an oxide material. The solid electrolyte contains Li, M, O and X. M is at least one selected from the group consisting of Nb, Ta, and Zr. And X is at least one selected from the group consisting of F, Cl, Br and I. The oxide material contains at least one selected from the group consisting of oxides of divalent metal elements and oxides of trivalent metal elements. The mass ratio of the oxide material to the solid electrolyte is from 1% to 50% (inclusive). A battery (1000) according to the present disclosure is provided with a positive electrode (201), a negative electrode (203), and a solid electrolyte layer (202) provided between the positive electrode (201) and the negative electrode (203). At least one selected from the group consisting of the positive electrode (201), the negative electrode (203), and the electrolyte layer (202) contains the solid electrolyte material according to the present disclosure.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to a solid electrolyte material and a battery using the same. Background Art

[0002] Patent Document 1 discloses a solid electrolyte material containing Li, M, O, and X. M is at least one element selected from Nb and Ta, and X is at least one element selected from Cl, Br, and I.

[0003] Prior art literature

[0004] Patent Literature

[0005] Patent Document 1: International Publication No. 2020 / 137153 Summary of the invention

[0006] Problems to be solved by the invention

[0007] An object of the present disclosure is to provide a solid electrolyte material having a reduced amount of hydrogen halide gas generated.

[0008] Means for solving problems

[0009] The solid electrolyte material disclosed herein comprises a solid electrolyte and an oxide material, wherein:

[0010] The solid electrolyte contains Li, M, О and X,

[0011] M is at least one selected from Nb, Ta and Zr,

[0012] X is at least one selected from F, Cl, Br and I,

[0013] The oxide material contains at least one selected from the group consisting of an oxide of a divalent metal element and an oxide of a trivalent metal element,

[0014] The mass ratio of the oxide material to the solid electrolyte is 1% or more and 50% or less.

[0015] Effects of the Invention

[0016] The present disclosure provides a solid electrolyte material that reduces the amount of hydrogen halide gas generated. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 A cross-sectional view showing a battery 1000 according to a second embodiment.

[0018] Figure 2 A cross-sectional view showing an electrode material 1100 according to the second embodiment.

[0019] Figure 3A schematic diagram showing a press mold 300 for evaluating the ion conductivity of a solid electrolyte material. DETAILED DESCRIPTION

[0020] Hereinafter, embodiments of the present disclosure will be described with reference to the drawings.

[0021] (First embodiment)

[0022] The solid electrolyte material of the first embodiment includes a solid electrolyte and an oxide material. The solid electrolyte contains Li, M, О and X. M is at least one selected from Nb, Ta and Zr. X is at least one selected from F, Cl, Br and I. The oxide material contains at least one selected from an oxide of a divalent metal element and an oxide of a trivalent metal element. The mass ratio of the oxide material to the solid electrolyte is 1% or more and 50% or less.

[0023] The solid electrolyte material of the first embodiment can reduce the amount of hydrogen halide gas generated. In addition, the solid electrolyte material of the first embodiment can have, for example, a practical ion conductivity (for example, a practical ion conductivity that can be used in a battery). In addition, the solid electrolyte material of the first embodiment can have, for example, a high lithium ion conductivity. Here, the so-called high lithium ion conductivity is, for example, 1 mS / cm or more.

[0024] When manufacturing batteries in a dry room, the moisture in the dry room atmosphere reacts with the solid electrolyte, and sometimes gas is generated from the solid electrolyte. In the case of a sulfide solid electrolyte, hydrogen sulfide may be generated. In order to reduce the amount of gas generated, it is necessary to suppress the amount of moisture in the dry room to a low level, that is, it is necessary to build a dry room with a low dew point temperature. For this purpose, an expensive dehumidification device is required, which leads to an increase in battery manufacturing costs.

[0025] The inventors of the present invention have found that in a solid electrolyte containing halogen and oxygen, hydrogen halide gas is generated when a battery is manufactured. The solid electrolyte material of the first embodiment can reduce the amount of hydrogen halide gas generated. Therefore, a battery using the solid electrolyte material of the first embodiment can be manufactured at a higher dew point temperature, thereby reducing manufacturing costs.

[0026] The solid electrolyte material of the first embodiment may also be a mixture of the above-mentioned solid electrolyte and the above-mentioned oxide material. In order to reduce the amount of hydrogen halide gas generated, in the solid electrolyte material of the first embodiment, the above-mentioned solid electrolyte may also form a composite with the above-mentioned oxide material. By forming a composite, the oxide material can efficiently absorb the hydrogen halide gas generated from the solid electrolyte. Thus, the amount of hydrogen halide gas discharged into the environment can be reduced. For example, the hydrogen halide gas absorbed by the oxide material can also generate halides of the metals constituting the oxide and water by reacting with the oxide material.

[0027] In addition, the oxide contained in the oxide material is, for example, an oxide different from the positive electrode active material. In other words, the oxide material contained in the solid electrolyte material of the first embodiment is, for example, an oxide other than the positive electrode active material.

[0028] The oxide material may contain at least one selected from ZnO, CaO, MgO, La2O3 and Fe2O3. According to the above configuration, the amount of hydrogen halide gas can be further reduced.

[0029] In order to further reduce hydrogen halide gas, the oxide material may also contain ZnO.

[0030] In order to further reduce the hydrogen halide gas, in the solid electrolyte material of the first embodiment, the mass ratio of the oxide material to the solid electrolyte may be 1.6% to 39.0%.

[0031] In order to further reduce the hydrogen halide gas, in the solid electrolyte material of the first embodiment, the mass ratio of the oxide material to the solid electrolyte may be 25% or less.

[0032] When the oxide material is in the form of particles (eg, spheres), the oxide material may have a median particle size of 1 μm or less, or may have a median particle size of 0.1 μm or less.

[0033] The median particle size of particles refers to the particle size (d50) when the cumulative volume in the volume-based particle size distribution corresponds to 50%. The volume-based particle size distribution can be measured by a laser diffraction measuring device or an image analysis device.

[0034] The smaller the particle size of the oxide material, the better. When the particle size of the oxide material is small, the surface area per unit mass of the particle increases. As a result, more hydrogen halide gas can be absorbed.

[0035] In order to improve the ion conductivity of the solid electrolyte material, the solid electrolyte may be substantially composed of Li, M, O and X. Here, the so-called "solid electrolyte is substantially composed of Li, M, O and X" means that the molar ratio of the total amount of Li, M, O and X constituting the solid electrolyte to the total amount of all elements is 90% or more. As an example, the molar ratio may also be 95% or more.

[0036] In order to improve the ion conductivity of the solid electrolyte material, the solid electrolyte may be composed of Li, M, O and X only.

[0037] The solid electrolyte may have a composition represented by the following composition formula (1).

[0038] Li a MO b X c (1)

[0039] Among them, 0.1≤a≤7.0, 0.4≤b≤1.9 and 1.0≤c≤11 are satisfied.

[0040] In the composition formula (1), 0.3≤a≤5.0, 0.6≤b≤1.6, and 2.0≤c≤9.0 may be satisfied, and 0.6≤a≤3.0, 0.7≤b≤1.2, and 3.0≤c≤7.0 may be satisfied.

[0041] In order to improve the ion conductivity of the solid electrolyte material, X may also contain Cl in the solid electrolyte. X may also be Cl.

[0042] In order to improve the ion conductivity of the solid electrolyte material, the molar ratio of Li to M in the solid electrolyte may be 0.6 to 3.0.

[0043] The shape of the solid electrolyte is not limited. Examples of the shape are needle-shaped, spherical, and ellipsoidal. The solid electrolyte may also be a particle. The solid electrolyte may also be formed in a pellet or plate shape.

[0044] When the solid electrolyte material is in the form of particles (eg, spheres), the solid electrolyte may have a median particle size of 0.1 μm to 100 μm, or 0.5 μm to 10 μm, so that the solid electrolyte and other materials can be well dispersed.

[0045] <Method for producing solid electrolyte>

[0046] The solid electrolyte can be produced as follows.

[0047] A raw material powder is prepared so as to have a target composition. Examples of the raw material powder are oxides, hydroxides, halides or acid halides.

[0048] As an example, in a solid electrolyte composed of Li, M, O and X, M is Ta, X is Cl, and when the molar ratio Li / M and the molar ratio O / X when the raw materials are mixed are 1.0 and 0.2 respectively, Li2O2 and TaCl5 are mixed at a molar ratio of Li2O2:TaCl5=1:2.

[0049] The raw material powders are selected to determine M and X. The molar ratios of Li / M and O / X can be adjusted by appropriately selecting the mixing ratio of the raw material powders.

[0050] The reactant is obtained by calcining a mixture of raw material powders. In order to suppress the evaporation of raw materials caused by calcination, the mixture of raw material powders can also be sealed in an airtight container formed of quartz glass or borosilicate glass for calcination under vacuum or inert gas atmosphere. The inert atmosphere is, for example, an argon atmosphere or a nitrogen atmosphere. Alternatively, a reactant can be obtained by reacting the mixture of raw material powders with each other in a mechanochemical manner (i.e., by using a mechanochemical grinding method) in a mixing device such as a planetary ball mill. By these methods, the solid electrolyte contained in the solid electrolyte material of the first embodiment can be obtained.

[0051] By calcining the solid electrolyte, a part of M or a part of X may evaporate. As a result, the molar ratio Li / M and the molar ratio O / X of the obtained solid electrolyte can be greater than the values ​​calculated from the molar ratio of the prepared raw material powder. Specifically, the molar ratio Li / M can be increased by about 20% to 70%, and the molar ratio O / X can be increased by about 40% to 75%.

[0052] The composition of the solid electrolyte can be determined by, for example, ICP emission spectrometry, ion chromatography, inert gas fusion-infrared absorption, or EPMA (Electron Probe Micro Analyzer) method.

[0053] <Method for producing solid electrolyte material>

[0054] By mixing the solid electrolyte with an oxide material, a solid electrolyte material can be obtained.

[0055] The mixing method may be a mechanochemical grinding method or a mortar mixing method. The mortar mixing method is a method in which the powder material is placed in an agate mortar and stirred using the mortar and pestle.

[0056] It is sufficient for the two powders to be blended with each other, preferably evenly.

[0057] (Second embodiment)

[0058] Hereinafter, the second embodiment will be described, and matters described in the first embodiment will be appropriately omitted.

[0059] The battery of the second embodiment includes a positive electrode, an electrolyte layer, and a negative electrode. The electrolyte layer is disposed between the positive electrode and the negative electrode. At least one selected from the positive electrode, the electrolyte layer, and the negative electrode contains the solid electrolyte material of the first embodiment.

[0060] The battery of the second embodiment has excellent charge and discharge characteristics.

[0061] Figure 1 A cross-sectional view showing a battery 1000 according to a second embodiment.

[0062] The battery 1000 includes a positive electrode 201 , an electrolyte layer 202 , and a negative electrode 203 . The electrolyte layer 202 is disposed between the positive electrode 201 and the negative electrode 203 .

[0063] The positive electrode 201 includes positive electrode active material particles 204 , solid electrolyte particles 100 , and oxide particles 102 .

[0064] The electrolyte layer 202 contains an electrolyte material. The electrolyte material may be, for example, the solid electrolyte material of the first embodiment. When the electrolyte layer 202 contains the solid electrolyte material of the first embodiment, the electrolyte layer 202 may be Figure 1 As shown, solid electrolyte particles 100 and oxide particles 102 are included.

[0065] The negative electrode 203 includes negative electrode active material particles 205 , solid electrolyte particles 100 , and oxide particles 102 .

[0066] The solid electrolyte particle 100 is a particle containing the solid electrolyte contained in the solid electrolyte material of the first embodiment. The solid electrolyte particle 100 may also be a particle containing the solid electrolyte contained in the solid electrolyte material of the first embodiment as a main component. The so-called particle containing the solid electrolyte contained in the solid electrolyte material of the first embodiment as a main component refers to a particle containing the solid electrolyte contained in the solid electrolyte material of the first embodiment as the largest component. The solid electrolyte particle 100 may also be a particle composed of the solid electrolyte contained in the solid electrolyte material of the first embodiment.

[0067] The oxide particles 102 are particles containing the oxide material contained in the solid electrolyte material of the first embodiment. The oxide particles 102 may also be particles containing the oxide material contained in the solid electrolyte material of the first embodiment as a main component. The so-called particles containing the oxide material contained in the solid electrolyte material of the first embodiment as a main component refer to particles whose largest component is the oxide material contained in the solid electrolyte material of the first embodiment. The oxide particles 102 may also be particles composed of the oxide material contained in the solid electrolyte material of the first embodiment.

[0068] The positive electrode 201 contains a material that can absorb and release metal ions such as lithium ions. The positive electrode 201 contains, for example, a positive electrode active material (for example, positive electrode active material particles 204).

[0069] Examples of positive electrode active materials are lithium-containing transition metal oxides, transition metal fluorides, polyanionic materials, fluorinated polyanionic materials, transition metal sulfides, transition metal oxysulfides or transition metal oxynitrides. Examples of lithium-containing transition metal oxides are Li(Ni, Co, Al)O2, LiCoO2 or Li(Ni, Co, Mn)O2.

[0070] In the present disclosure, "(A, B, C)" means "at least one selected from A, B, and C." However, A, B, and C all represent elements.

[0071] From the perspective of battery cost and safety, lithium phosphate may be used as the positive electrode active material.

[0072] The positive electrode 201 contains the solid electrolyte material of the first embodiment, and when X contains I (i.e., iodine), lithium iron phosphate can also be used as the positive electrode active material. The solid electrolyte contained in the solid electrolyte material of the first embodiment containing I is easily oxidized. If lithium iron phosphate is used as the positive electrode active material, the oxidation reaction of the solid electrolyte can be suppressed. In other words, the formation of an oxide layer with low lithium ion conductivity can be suppressed. As a result, the battery has a high charge and discharge efficiency.

[0073] The positive electrode 201 contains not only the solid electrolyte material of the first embodiment, but also a transition metal fluoride oxide as a positive electrode active material. Even if the solid electrolyte contained in the solid electrolyte material of the first embodiment is fluorinated by the transition metal fluoride, it is difficult to form a resistance layer. As a result, the battery has a high charge and discharge efficiency.

[0074] Transition metal fluoride oxide contains oxygen and fluorine. As an example, the transition metal fluoride oxide can also be a composition formula Li p Me q O m Fn wherein Me is at least one element selected from the group consisting of Mn, Co, Ni, Fe, Al, Cu, V, Nb, Mo, Ti, Cr, Zr, Zn, Na, K, Ca, Mg, Pt, Au, Ag, Ru, W, B, Si and P, and satisfies the following mathematical formula: 0.5≤p≤1.5, 0.5≤q≤1.0, 1≤m<2 and 0<n≤1. Examples of such transition metal fluoride oxides are Li 1.05 (Ni 0.35 Co 0.35 Mn 0.3 ) 0.95 O 1.9 F 0.1 .

[0075] The positive electrode active material particles 204 may also have a median particle size of 0.1 μm or more and 100 μm or less. When the positive electrode active material particles 204 have a median particle size of 0.1 μm or more, in the positive electrode 201, the positive electrode active material particles 204 and the solid electrolyte particles 100 can form a good dispersion state. As a result, the charge and discharge characteristics of the battery are improved. When the positive electrode active material particles 204 have a median particle size of 100 μm or less, the lithium diffusion rate in the positive electrode active material particles 204 is increased. As a result, the battery can operate at a high output power.

[0076] The positive electrode active material particles 204 may have a larger median diameter than the solid electrolyte particles 100. This allows the positive electrode active material particles 204 and the solid electrolyte particles 100 to be in a well-dispersed state.

[0077] To improve the energy density and output of the battery, in the positive electrode 201 , the ratio of the volume of the positive electrode active material particles 204 to the total volume of the positive electrode active material particles 204 and the volume of the solid electrolyte particles 100 may be 0.30 or more and 0.95 or less.

[0078] Figure 2 A cross-sectional view of an electrode material 1100 according to a second embodiment is shown. The electrode material 1100 is contained in, for example, a positive electrode 201. In order to prevent the electrode active material particles 206 from reacting with the solid electrolyte particles 100, a coating layer 216 may be formed on the surface of the electrode active material particles 206. This can suppress the increase in the reaction overvoltage of the battery. Examples of the coating material contained in the coating layer 216 are sulfide solid electrolytes, oxide solid electrolytes, or halide solid electrolytes.

[0079] When the solid electrolyte particle 100 is a sulfide solid electrolyte, the coating material may be a solid electrolyte contained in the solid electrolyte material of the first embodiment, and X is at least one element selected from Cl and Br. The solid electrolyte material contained in the solid electrolyte material of the first embodiment is less susceptible to oxidation than the sulfide solid electrolyte. As a result, the increase in the reaction overvoltage of the battery can be suppressed.

[0080] When the solid electrolyte particle 100 is the solid electrolyte contained in the solid electrolyte material of the first embodiment, and X contains I, the coating material may also be the solid electrolyte contained in the solid electrolyte material of the first embodiment, and X is at least one element selected from Cl and Br. The solid electrolyte contained in the solid electrolyte material of the first embodiment not containing I is less likely to be oxidized than the solid electrolyte contained in the solid electrolyte material of the first embodiment containing I. As a result, the battery has high charge and discharge efficiency.

[0081] When the solid electrolyte particle 100 is the solid electrolyte contained in the solid electrolyte material of the first embodiment, and X includes I, the coating material may also contain an oxide solid electrolyte. The oxide solid electrolyte may also be lithium niobate which has excellent stability even at high potentials. Thus, the battery has high charge and discharge efficiency.

[0082] The positive electrode 201 may also be composed of a first positive electrode layer containing a first positive electrode active material and a second positive electrode layer containing a second positive electrode active material. Among them, the second positive electrode layer is arranged between the first positive electrode layer and the electrolyte layer 202, and the first positive electrode layer and the second positive electrode layer contain a solid electrolyte contained in the solid electrolyte material of the first embodiment containing I, and a coating layer 216 is formed on the surface of the second positive electrode active material. According to the above structure, the solid electrolyte contained in the solid electrolyte material of the first embodiment contained in the electrolyte layer 202 can be suppressed from being oxidized by the second positive electrode active material. As a result, the battery has a high charging capacity. Examples of the coating material contained in the coating layer 206 are sulfide solid electrolytes, oxide solid electrolytes, polymer solid electrolytes, or halide solid electrolytes. However, when the coating material is a halide solid electrolyte, I is not contained as a halogen element. The first positive electrode active material may also be the same material as the second positive electrode active material, or may be a material different from the second positive electrode active material.

[0083] In order to increase the energy density and output of the battery, the positive electrode 201 may have a thickness of 10 μm or more and 500 μm or less.

[0084] The electrolyte layer 202 contains an electrolyte material. The electrolyte material is, for example, a solid electrolyte. The electrolyte layer 202 may also be a solid electrolyte layer.

[0085] The electrolyte layer 202 may contain the solid electrolyte material of the first embodiment. The electrolyte layer 202 may be composed only of the solid electrolyte material of the first embodiment.

[0086] The solid electrolyte contained in the electrolyte layer 202 may also be composed of only a solid electrolyte different from the solid electrolyte contained in the solid electrolyte material of the first embodiment. Examples of solid electrolytes different from the solid electrolyte contained in the solid electrolyte material of the first embodiment are Li2MgX'4, Li2FeX'4, Li(Al, Ga, In)X'4, Li3(Al, Ga, In)X'6 or LiI. Here, X' is at least one element selected from F, Cl, Br and I.

[0087] Hereinafter, the solid electrolyte contained in the solid electrolyte material of the first embodiment is referred to as a first solid electrolyte. A solid electrolyte different from the solid electrolyte contained in the solid electrolyte material of the first embodiment is referred to as a second solid electrolyte.

[0088] The electrolyte layer 202 may contain not only the first solid electrolyte but also the second solid electrolyte. The first solid electrolyte and the second solid electrolyte may be uniformly dispersed.

[0089] The electrolyte layer 202 may have a thickness of 1 μm or more and 100 μm or less. When the electrolyte layer 202 has a thickness of 1 μm or more, the positive electrode 201 and the negative electrode 203 are less likely to short-circuit. When the electrolyte layer 202 has a thickness of 100 μm or less, the battery can operate at a high output power.

[0090] Another electrolyte layer may be further provided between the electrolyte layer 202 and the negative electrode 203. For example, when the electrolyte layer 202 contains a first solid electrolyte, in order to more stably maintain the high ion conductivity of the solid electrolyte, an electrolyte layer composed of another solid electrolyte that is electrochemically more stable than the solid electrolyte may be further provided.

[0091] The negative electrode 203 contains a material that can insert and remove metal ions (eg, lithium ions). The negative electrode 203 contains, for example, a negative electrode active material (eg, negative electrode active material particles 205).

[0092] Examples of negative electrode active materials are metal materials, carbon materials, oxides, nitrides, tin compounds or silicon compounds. The metal material may be a simple metal or an alloy. Examples of metal materials are lithium metal or lithium alloys. Examples of carbon materials are natural graphite, coke, graphitizable carbon, carbon fiber, spherical carbon, artificial graphite or amorphous carbon. From the viewpoint of capacity density, suitable examples of negative electrode active materials are silicon (i.e. Si), tin (i.e. Sn), silicon compounds or tin compounds.

[0093] The negative electrode active material can also be selected based on the reduction resistance of the solid electrolyte contained in the negative electrode 203. When the negative electrode 203 contains the first solid electrolyte, a material that can embed and deintercalate lithium ions at more than 0.27V relative to lithium can also be used as the negative electrode active material. As long as the negative electrode active material is such a material, it is possible to suppress the first solid electrolyte contained in the negative electrode 203 from being reduced. As a result, the battery has a high charge and discharge efficiency. Examples of the material are titanium oxide, indium metal or lithium alloy. An example of titanium oxide is Li4Ti5O 12 , LiTi2O4 or TiO2.

[0094] The negative electrode active material particles 205 may also have a median particle size of 0.1 μm or more and 100 μm or less. When the negative electrode active material particles 205 have a median particle size of 0.1 μm or more, the negative electrode active material particles 205 and the solid electrolyte particles 100 can form a good dispersion state in the negative electrode 203. As a result, the charge and discharge characteristics of the battery are improved. When the negative electrode active material particles 205 have a median particle size of 100 μm or less, the lithium diffusion rate in the negative electrode active material particles 205 is increased. As a result, the battery can operate at a high output power.

[0095] The negative electrode active material particles 205 may have a larger median diameter than the solid electrolyte particles 100. This allows the negative electrode active material particles 205 and the solid electrolyte particles 100 to be in a well-dispersed state.

[0096] To improve the energy density and output of the battery, in the negative electrode 203 , the ratio of the volume of the negative electrode active material particles 205 to the total volume of the negative electrode active material particles 205 and the volume of the solid electrolyte particles 100 may be 0.30 or more and 0.95 or less.

[0097] Figure 2The electrode material 1100 shown may also be contained in the negative electrode 203. In order to prevent the solid electrolyte particles 100 from reacting with the negative electrode active material (i.e., the electrode active material particles 206), a coating layer 216 may also be formed on the surface of the electrode active material particles 206. As a result, the battery has a high charge and discharge efficiency. Examples of the coating material contained in the coating layer 216 are sulfide solid electrolytes, oxide solid electrolytes, polymer solid electrolytes, or halide solid electrolytes.

[0098] When the solid electrolyte particle 100 is the first solid electrolyte, the coating material may also be a sulfide solid electrolyte, an oxide solid electrolyte, or a polymer solid electrolyte. An example of a sulfide solid electrolyte is Li2S-P2S5. An example of an oxide solid electrolyte is trilithium phosphate. An example of a polymer solid electrolyte is a composite compound of polyethylene oxide and a lithium salt. An example of such a polymer solid electrolyte is lithium bistrifluoromethanesulfonimide.

[0099] In order to increase the energy density and output of the battery, the negative electrode 203 may have a thickness of 10 μm or more and 500 μm or less.

[0100] At least one selected from the positive electrode 201, the electrolyte layer 202, and the negative electrode 203 may contain a second solid electrolyte for the purpose of improving ion conductivity. Examples of the second solid electrolyte are sulfide solid electrolytes, oxide solid electrolytes, halide solid electrolytes, or organic polymer solid electrolytes.

[0101] In the present disclosure, the so-called "sulfide solid electrolyte" refers to a solid electrolyte containing sulfur. The so-called "oxide solid electrolyte" refers to a solid electrolyte containing oxygen. The oxide solid electrolyte may also contain anions other than oxygen (but excluding sulfur anions and halogen anions). The so-called "halide solid electrolyte" refers to a solid electrolyte containing halogen elements and no sulfur. The halide solid electrolyte contains not only halogen elements but also oxygen.

[0102] Examples of sulfide solid electrolytes are Li2S-P2S5, Li2S-SiS2, Li2S-B2S3, Li2S-GeS2, Li 3.25 Ge 0.25 P 0.75 S4 or Li 10 GeP2S 12 .

[0103] Examples of oxide solid electrolytes are:

[0104] (i) NASICON type solid electrolytes such as LiTi2(PO4)3 or its element substitution products,

[0105] (ii) Perovskite-type solid electrolytes such as (LaLi)TiO3,

[0106] (iii)Li 14 ZnGe4O 16 , LISICON type solid electrolytes such as Li4SiO4, LiGeO4 or their element substitution products,

[0107] (iv)Li7La3Zr2O 12 Or a garnet-type solid electrolyte such as an element-substituted body thereof, or (v) Li3PO4 or its N-substituted body.

[0108] An example of a halide solid electrolyte is Li a Me' b Y c A compound represented by Z6. Wherein, the mathematical formulas are satisfied: a+mb+3c=6 and c>0. Me' is at least one selected from metal elements and semi-metal elements other than Li and Y. Z is at least one selected from F, Cl, Br and I. The value of m represents the valence of Me'.

[0109] The so-called "semi-metallic elements" are B, Si, Ge, As, Sb and Te. The so-called "metallic elements" are all elements contained in Groups 1 to 12 of the periodic table (but excluding hydrogen) and all elements contained in Groups 13 to 16 of the periodic table (but excluding B, Si, Ge, As, Sb, Te, C, N, P, O, S and Se). Me' may also be at least one element selected from Mg, Ca, Sr, Ba, Zn, Sc, Al, Ga, Bi, Zr, Hf, Ti, Sn, Ta and Nb.

[0110] Examples of halide solid electrolytes are Li3YCl6 or Li3YBr6.

[0111] When the electrolyte layer 202 contains the first solid electrolyte, the negative electrode 203 may also contain a sulfide solid electrolyte. Thus, the sulfide solid electrolyte, which is electrochemically stable with respect to the negative electrode active material, suppresses the mutual contact between the first solid electrolyte and the negative electrode active material. As a result, the battery has a low internal resistance.

[0112] An example of an organic polymer solid electrolyte is a compound of a polymer compound and a lithium salt. The polymer compound may also have an ethylene oxide structure. A polymer compound having an ethylene oxide structure can contain a large amount of lithium salt and thus has a higher ion conductivity.

[0113] Examples of lithium salts include LiPF6, LiBF4, LiSbF6, LiAsF6, LiSO3CF3, LiN(SO2CF3)2, LiN(SO2C2F5)2, LiN(SO2CF3)(SO2C4F9) or LiC(SO2CF3)3. One lithium salt selected from these may be used alone. Alternatively, a mixture of two or more lithium salts selected from these may be used.

[0114] At least one selected from the positive electrode 201 , the electrolyte layer 202 , and the negative electrode 203 may contain a non-aqueous electrolyte solution, a gel electrolyte, or an ionic liquid for the purpose of facilitating the transfer of lithium ions and improving the output characteristics of the battery.

[0115] The non-aqueous electrolyte contains a non-aqueous solvent and a lithium salt dissolved in the non-aqueous solvent. Examples of non-aqueous solvents are cyclic carbonate solvents, chain carbonate solvents, cyclic ether solvents, chain ether solvents, cyclic ester solvents, chain ester solvents or fluorine solvents. Examples of cyclic carbonate solvents are ethylene carbonate, propylene carbonate or butylene carbonate. Examples of chain carbonate solvents are dimethyl carbonate, ethyl methyl carbonate or diethyl carbonate. Examples of cyclic ether solvents are tetrahydrofuran, 1,4-dioxane or 1,3-dioxolane. Examples of chain ether solvents are 1,2-dimethoxyethane or 1,2-diethoxyethane. Examples of cyclic ester solvents are γ-butyrolactone. Examples of chain ester solvents are methyl acetate. Examples of fluorine solvents are fluoroethylene carbonate, methyl fluoropropionate, fluorobenzene, ethyl fluoromethyl carbonate or dimethylene fluorocarbonate. One non-aqueous solvent selected from them can be used alone. Alternatively, a mixture of two or more nonaqueous solvents selected from these may be used.

[0116] Examples of lithium salts include LiPF6, LiBF4, LiSbF6, LiAsF6, LiSO3CF3, LiN(SO2CF3)2, LiN(SO2C2F5)2, LiN(SO2CF3)(SO2C4F9) or LiC(SO2CF3)3. One lithium salt selected from these may be used alone. Alternatively, a mixture of two or more lithium salts selected from these may be used. The concentration of the lithium salt is, for example, in the range of 0.5 mol / liter or more and 2 mol / liter or less.

[0117] As the gel electrolyte, a polymer material impregnated with a non-aqueous electrolyte can be used. Examples of the polymer material are polyethylene oxide, polyacrylonitrile, polyvinylidene fluoride, polymethyl methacrylate, or a polymer having an ethylene oxide bond.

[0118] Examples of cations contained in ionic liquids are:

[0119] (i) aliphatic chain quaternary salts such as tetraalkylammonium or tetraalkylphosphonium,

[0120] (ii) an aliphatic cyclic ammonium such as pyrrolidinium, morpholinium, imidazolinium, tetrahydropyrimidinium, piperazinium or piperidinium, or

[0121] (iii) Nitrogen-containing heterocyclic aromatic cations such as pyridinium and imidazolium cations.

[0122] An example of an anion contained in an ionic liquid is PF6 - 、BF4 - 、SbF6 - 、AsF6 - 、SO3CF3 - 、N(SO2CF3)2 - 、N(SO2C2F5)2 - 、N(SO2CF3)(SO2C4F9) - or C(SO2CF3)3 - .

[0123] The ionic liquid may also contain a lithium salt.

[0124] At least one selected from the positive electrode 201 , the electrolyte layer 202 , and the negative electrode 203 may contain a binder for the purpose of improving the adhesion between particles.

[0125] The example of binding agent is polyvinylidene fluoride, polytetrafluoroethylene, polyethylene, polypropylene, aramid resin, polyamide, polyimide, polyamide-imide, polyacrylonitrile, polyacrylic acid, polymethyl acrylate, polyethyl acrylate, polyhexyl acrylate, polymethacrylic acid, polymethyl methacrylate, polyethyl methacrylate, polyhexyl methacrylate, polyvinyl acetate, polyvinyl pyrrolidone, polyether, polyether sulfone, polyhexafluoropropylene, styrene-butadiene rubber or carboxymethyl cellulose. As binding agent, copolymer can also be used. The example of this binding agent is a copolymer of two or more materials selected from tetrafluoroethylene, hexafluoroethylene, hexafluoropropylene, perfluoroalkyl vinyl ether, vinylidene fluoride, chlorotrifluoroethylene, ethylene, propylene, pentafluoropropylene, fluoromethyl vinyl ether, acrylic acid and hexadiene. A mixture of two or more selected from the above-mentioned materials can also be used.

[0126] At least one selected from the positive electrode 201 and the negative electrode 203 may contain a conductive auxiliary agent in order to improve electron conductivity.

[0127] Examples of conductive additives are:

[0128] (i) Graphites such as natural graphite or artificial graphite,

[0129] (ii) Carbon blacks such as acetylene black or Ketjen black,

[0130] (iii) Conductive fibers such as carbon fibers or metal fibers,

[0131] (iv) fluorinated carbon,

[0132] (v) Metal powders such as aluminum,

[0133] (vi) Conductive whiskers such as zinc oxide or potassium titanate,

[0134] (vii) conductive metal oxides such as titanium oxide, or

[0135] (viii) Conductive polymer compounds such as polyaniline, polypyrrole or polythiophene For cost reduction, the conductive auxiliary agent described in (i) or (ii) above may be used.

[0136] For the purpose of cost reduction, the conductive auxiliary agent (I) or (II) described above may be used.

[0137] Examples of the shape of the battery of the second embodiment include a coin shape, a cylindrical shape, a square shape, a sheet shape, a button shape, a flat shape, or a laminated shape.

[0138] Example

[0139] Hereinafter, the present disclosure will be described in more detail with reference to examples.

[0140] (Example 1)

[0141] [Preparation of solid electrolyte]

[0142] In a dry atmosphere with a dew point below -30°C (hereinafter referred to as "dry atmosphere"), Li2O, LiOH and TaCl5 are prepared as raw material powders in a molar ratio of Li2O:LiOH:TaCl5=0.4:0.4:1.0. These raw material powders are crushed and mixed in a mortar to obtain a mixed powder. Then, it is placed in a quartz glass filled with argon and fired at 350°C for 3 hours. The obtained fired product is crushed in an agate mortar. In this way, the solid electrolyte of Example 1 is obtained. The molar ratio Li / M is 2.0. In addition, the molar ratio Li / M is 0.9, and O / X is 0.19. Furthermore, regarding the molar ratios Li / M and O / X, Li and M were determined by ICP emission spectrometry, X was determined by ion chromatography, and O was determined by inert gas fusion-infrared absorption. The devices used in the composition measurement are ICP emission spectrometry, ion chromatography and oxygen analysis.

[0143] [Production of solid electrolyte materials]

[0144] In a dry atmosphere, the solid electrolyte of Example 1 and ZnO were prepared so that the mass ratio of ZnO to the solid electrolyte was 1.6%. These were pulverized and mixed in a mortar to obtain the solid electrolyte material of Example 1.

[0145] The average particle size of ZnO is about 20 nm.

[0146] [Evaluation of ion conductivity]

[0147] Figure 3 A schematic diagram showing a press mold 300 for evaluating the ion conductivity of a solid electrolyte material.

[0148] The press forming die 300 includes a punch upper portion 301, a frame die 302, and a punch lower portion 303. The frame die 302 is formed of insulating polycarbonate. The punch upper portion 301 and the punch lower portion 303 are both formed of electronically conductive stainless steel.

[0149] use Figure 3 The press molding die 300 shown was used to measure the ion conductivity of the solid electrolyte material of Example 1 by the following method.

[0150] In a dry atmosphere, the powder of the solid electrolyte material of Example 1 (i.e. Figure 3 The solid electrolyte material powder 101 is filled in the press mold 300. In the press mold 300, a pressure of 300 MPa is applied to the solid electrolyte material of Example 1 using the punch upper portion 301.

[0151] Keeping the state of the applied pressure unchanged, the punch upper part 301 and the punch lower part 303 are connected to a potentiostat (Versa STAT4 manufactured by Princeton Applied Research) equipped with a frequency response analyzer. The punch upper part 301 is connected to the working electrode and the potential measurement terminal. The punch lower part 303 is connected to the counter electrode and the reference electrode. At room temperature, the ionic conductivity of the solid electrolyte material of Example 1 was measured by electrochemical impedance spectroscopy. As a result, the ionic conductivity measured at 22°C was 5.1mS / cm.

[0152] [Determination of Hydrogen Chloride Gas]

[0153] The solid electrolyte material (30 mg) of Example 1 was kept in a 1 L glass container filled with a dry atmosphere for 5 minutes. Then, a hydrogen chloride gas detection tube (14M manufactured by GASTEC Co., Ltd.) was introduced from the inlet installed in the glass container to measure the hydrogen chloride gas concentration. As a result, the measured hydrogen chloride gas concentration was 79 ppm / L.

[0154] (Examples 2 to 9 and Comparative Example 1)

[0155] [Production of solid electrolyte materials]

[0156] In Examples 2 to 5, solid electrolyte materials of Examples 2 to 5 were obtained in the same manner as in Example 1 except for the mass ratio of ZnO to the solid electrolyte. The mass ratios are shown in Table 1.

[0157] In Example 6, La2O3 was used instead of ZnO. The mass ratio of La2O3 to the solid electrolyte was 20.1%. The solid electrolyte material of Example 6 was obtained in the same manner as in Example 1 except for the above matters.

[0158] The average particle size of La2O3 is about 100nm.

[0159] In Example 7, CaO was used instead of ZnO. The mass ratio of CaO to the solid electrolyte was 10.3%. The solid electrolyte material of Example 7 was obtained in the same manner as in Example 1 except for the above matters.

[0160] The average particle size of CaO is about 160 nm.

[0161] In Example 8, MgO was used instead of ZnO. The mass ratio of MgO to the solid electrolyte was 11.1%. The solid electrolyte material of Example 8 was obtained in the same manner as in Example 1 except for the above matters.

[0162] The average particle size of MgO is about 50 nm.

[0163] In Example 9, Fe2O3 was used instead of ZnO. The mass ratio of Fe2O3 to the solid electrolyte was 16.2%. The solid electrolyte material of Example 8 was obtained in the same manner as in Example 1 except for the above matters.

[0164] The average particle size of Fe2O3 is about 50nm.

[0165] In Comparative Example 1, no oxide material was used. That is, the solid electrolyte material of Comparative Example 1 was composed of the solid electrolyte of Example 1.

[0166] [Evaluation of ion conductivity]

[0167] The ion conductivity of the solid electrolyte materials of Examples 2 to 9 and Comparative Example 1 was measured in the same manner as in Example 1. Table 1 shows the measurement results.

[0168] [Determination of Hydrogen Chloride Gas]

[0169] The hydrogen chloride of the solid electrolyte materials of Examples 2 to 9 and Comparative Example 1 was measured in the same manner as in Example 1. The measurement results are shown in Table 1.

[0170] (Example 10 and Comparative Example 2)

[0171] [Preparation of solid electrolyte]

[0172] In Example 10 and Comparative Example 2, Li2O, Li2O2 and ZrCl4 were prepared as raw material powders in a dry atmosphere in a molar ratio of Li2O:Li2O2:ZrCl4=0.6:1.4:2. These raw material powders were crushed and mixed in a mortar to obtain a mixed powder. The obtained mixed powder was ground using a planetary ball mill at 600 rpm for 24 hours. In this way, the solid electrolyte of Example 10 was obtained. The composition of the obtained solid electrolyte was analyzed in the same manner as in Example 1, and the molar ratio Li / M was calculated from the analyzed composition. The molar ratio Li / M was 2.0.

[0173] [Production of solid electrolyte materials]

[0174] In Example 10, the solid electrolyte and ZnO of Example 10 were prepared so that the mass ratio of ZnO to the solid electrolyte was 12.3%. The solid electrolyte material of Example 10 was obtained in the same manner as in Example 1 except for the above matters.

[0175] No oxide material was used in Comparative Example 2. That is, the solid electrolyte material of Comparative Example 2 was composed of the solid electrolyte of Example 10.

[0176] Table 1

[0177]

[0178] (Inspection)

[0179] Table 1 shows that by comparing Examples 1 to 9 with Comparative Example 1, which have the same constituent elements of the solid electrolytes as "Li, Ta, O, and Cl", it is found that the solid electrolyte materials of Examples 1 to 9 containing oxide materials generate less hydrogen chloride gas than the solid electrolyte material of Comparative Example 1 that does not contain oxide materials. In addition, by comparing Example 10 with Comparative Example 2, which have the same constituent elements of the solid electrolytes as "Li, Zr, O, and Cl", it is found that the solid electrolyte material of Example 10 containing oxide materials generates less hydrogen chloride gas than the solid electrolyte material of Comparative Example 2 that does not contain oxide materials.

[0180] Comparison between Example 3 and Comparative Examples 1 and 2 revealed that the solid electrolyte material containing 17.3 mass % of ZnO had a small amount of gas generation and high ion conductivity.

[0181] As described above, the solid electrolyte material of the present disclosure can reduce the amount of hydrogen halide gas generated and can also have higher lithium ion conductivity. Therefore, the solid electrolyte material of the present disclosure is a material suitable for providing a battery with excellent charge and discharge characteristics at a low manufacturing cost.

[0182] Industrial Applicability

[0183] The battery disclosed herein can be used, for example, as an all-solid lithium ion secondary battery.

[0184] Explanation of symbols:

[0185] 100 solid electrolyte particles

[0186] 101 Solid Electrolyte Material Powder

[0187] 102 oxide particles

[0188] 201 positive electrode

[0189] 202 electrolyte layer

[0190] 203 negative electrode

[0191] 204 Positive electrode active material particles

[0192] 205 Negative electrode active material particles

[0193] 206 Electrode active material particles

[0194] 216 coating layer

[0195] 300 Pressurized Forming Die

[0196] 301 punch upper part

[0197] 302 frame mold

[0198] 303 punch lower part

[0199] 1000 battery

[0200] 1100 Electrode Materials

Claims

1. A solid electrolyte material, wherein: Contains solid electrolyte and oxide materials, The solid electrolyte contains Li, M, О and X, M is at least one selected from Nb, Ta and Zr, X is at least one selected from F, Cl, Br and I, The oxide material contains at least one selected from the group consisting of an oxide of a divalent metal element and an oxide of a trivalent metal element, The mass ratio of the oxide material to the solid electrolyte is 1% or more and 50% or less.

2. The solid electrolyte material according to claim 1, wherein The oxide material contains at least one selected from ZnO, MgO, CaO, La2O3 and Fe2O3.

3. The solid electrolyte material according to claim 2, wherein The oxide material contains ZnO.

4. The solid electrolyte material according to any one of claims 1 to 3, wherein A mass ratio of the oxide material to the solid electrolyte is 1.6% or more and 39.0% or less.

5. The solid electrolyte material according to any one of claims 1 to 4, wherein The mass ratio of the oxide material to the solid electrolyte is 25% or less.

6. The solid electrolyte material according to any one of claims 1 to 5, wherein The solid electrolyte has a composition represented by the following composition formula (1): Li a MO b X c (1) Among them, 0.1≤a≤7.0, 0.4≤b≤1.9 and 1.0≤c≤11 are satisfied.

7. The solid electrolyte material according to any one of claims 1 to 6, wherein In the solid electrolyte, X includes Cl.

8. The solid electrolyte material according to any one of claims 1 to 7, wherein In the solid electrolyte, a molar ratio of Li to M is 0.6 or more and 3.0 or less.

9. A battery comprising: positive electrode, Negative electrode, and An electrolyte layer is provided between the positive electrode and the negative electrode, in, At least one selected from the positive electrode, the negative electrode, and the electrolyte layer contains the solid electrolyte material according to any one of claims 1 to 8.