Production method for improving husking efficiency of low-carbon wire drawing material
By precisely controlling high-temperature rolling process parameters in the production of low-carbon wire drawing materials, the problem of strong adhesion of iron oxide scale is solved, the uniformity of iron oxide scale is separated from the matrix, and the surface quality and yield rate of the finished product are improved.
Patent Information
- Application Number
- CN202410835509.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-26
- Publication Date
- 2024-10-08
AI Technical Summary
During the production process of low-carbon wire drawing materials, the iron oxide scale has strong adhesion and is difficult to remove, resulting in surface quality defects of the finished product, affecting the yield rate and product grade.
By precisely controlling the fine rolling temperature, spinning temperature, fan opening and cooling rate in the high-temperature rolling process, it is ensured that the thickness of the iron oxide scale is uniform and separated from the matrix, and the whole piece is peeled off quickly.
The uniformity of the iron oxide scale of the low-carbon wire drawing material is separated from the matrix, reducing the iron oxide scale residue and improving the surface quality and yield rate of the finished product.
Smart Images

Figure CN118744154A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of steelmaking, and specifically relates to a production method for improving the shelling efficiency of low-carbon drawn wire materials. Background Art
[0002] In order to ensure good ductility and low mechanical properties during the production of low-carbon drawn wire, high-temperature rolling is generally used. However, the iron oxide scale is thick, which affects the yield rate of cold-processed products and has the problem of strong adhesion. If the iron oxide scale of low-carbon drawn wire has strong adhesion, it will be difficult to remove the iron oxide scale by peeling methods such as pickling, sandblasting, and grinding. After further drawing, it will be pressed into the matrix, which will cause surface quality defects of the finished material. Improper control of iron oxide scale on the surface of steel is the main factor causing the decline in surface quality. It not only increases steel loss and reduces the yield rate, but also causes defects such as incomplete descaling, iron oxide scale pressing in, red iron scale on the surface, and pickling residue, which seriously restricts the improvement of the grade of steel products.
[0003] There are generally three types of iron oxide scale. The iron oxide scale formed on the surface of the steel billet when it comes into contact with oxygen under high temperature conditions is called primary iron oxide scale; after the rolled material is spun at 820-980°C, it comes into direct contact with air, forming secondary iron oxide scale; when the secondary iron oxide scale oxide film thickens to a certain extent, the oxide film ruptures under the action of internal stress in the film, the iron oxide scale separates, and the internal matrix comes into contact with air again, forming tertiary iron oxide scale. The iron oxide scale on the surface of the wire rod generally consists of a three-layer structure, the surface layer is a very thin layer of iron oxide (Fe 2 O 3 ), the middle layer is ferroferric oxide (Fe 3 O 4 ), the inner layer is a thicker ferrous oxide (FeO), and the ratio of the three layers is close to 1:4:95 under high temperature conditions.
[0004] The common state of the hard-to-peel iron oxide scale is that the iron oxide scale is generally discontinuous, and the connection with the substrate is directly detached or tightly connected. The thickness of the iron oxide scale varies from 37 to 58 μm, and the thickness is uneven. Discontinuous iron oxide scale is easy to appear during peeling, and the iron oxide scale that is tightly connected to the substrate is attached, making it difficult to peel and the process parameters difficult to control. Summary of the invention
[0005] The purpose of the present invention is to provide a production method for improving the shelling efficiency of low-carbon drawn wire materials.
[0006] Specifically, a production method for improving the shelling efficiency of low-carbon drawn wire material controls the finishing temperature of the finishing rolling mill group to be 850±10°C in the finishing rolling process of the high-temperature rolling process.
[0007] Furthermore, in the spinning process of the high-temperature rolling process, the spinning temperature of the spinning machine is controlled to be 935±10°C.
[0008] Furthermore, in the cooling process of the high temperature rolling process, the opening degree of the No. 1 fan is 70%, and the opening degree of the No. 5 fan is 50% to blow the oxide scale to a uniform thickness.
[0009] Furthermore, the cooling rate was controlled at 2.1-2.4°C / s.
[0010] Advantages of the present invention:
[0011] The present invention does not require the addition of additional equipment, and the purpose can be achieved by simply accurately controlling the temperature of key points.
[0012] The present invention optimizes the fine-rolling temperature, spinning temperature, fan opening and cooling rate. The thickness of the iron oxide scale of the obtained low-carbon drawn wire material is uniform and basically separated from the substrate. It can isolate the substrate from direct contact with the air to achieve the purpose of short-term rust prevention, and can also quickly peel off the substrate in one piece under the action of external force, reducing the adhesion of the iron oxide scale residue to the surface, thereby not affecting the surface quality of the processed product. BRIEF DESCRIPTION OF THE DRAWINGS
[0013] Figure 1 This is an electron microscope image of the sample cross section (100 times). DETAILED DESCRIPTION
[0014] The present invention will be further described below in conjunction with specific embodiments.
[0015] The high-temperature rolling process of low-carbon wire drawing materials includes the initial rolling process, the finishing rolling process, the wire laying process and the cooling process. The steel billet from the initial rolling process enters the finishing rolling unit for the finishing rolling process, and the finishing rolling temperature is controlled at 850±10℃-880±10℃. The steel billet from the finishing rolling process enters the wire laying machine for the wire laying process, and the wire laying temperature is controlled at 935±10℃-965±10℃. In the cooling process, the opening of fan No. 1 is 50-70%, and the opening of fan No. 5 is 50% to blow the thickness of the oxide scale evenly, and the cooling rate is controlled at 2.1-2.4℃ / s.
[0016] In the embodiment, according to the set finishing temperature, the water tank closed-loop feedback regulation function in front of the finishing machine and the water cooling system between the frames of the finishing machine are used to adjust the water tank flow rate and control the finishing temperature. The water tank closed-loop feedback regulation function is used to control the spinning temperature.
[0017] Table 1 Iron oxide scale state under different conditions
[0018]
[0019] like Figure 1As shown, the oxidized iron scale that is easy to peel off has a uniform thickness and is basically separated from the substrate, presenting a continuous shape. The oxidized iron scale of Example 2-3 has a uniform thickness and is basically separated from the substrate, which can isolate the substrate from direct contact with the air to achieve the purpose of short-term rust prevention, and can also be quickly peeled off from the substrate in one piece under the action of external force, reducing the oxidized iron scale residue adhering to the surface and affecting the surface quality of the processed finished product.
Claims
1. A production method for improving the peeling efficiency of low-carbon drawn wire material, characterized in that: In the finishing process of the high temperature rolling process, the finishing temperature of the finishing rolling mill is controlled to be 850±10℃.
2. In the spinning process of the high temperature rolling process according to claim 1, it is characterized in that: In the spinning process of the high temperature rolling process, the spinning temperature of the spinning machine is controlled to be 935±10°C.
3. In the spinning process of the high temperature rolling process according to claim 1, it is characterized in that: In the cooling process of the high temperature rolling process, the opening degree of the No. 1 fan is 50%, and the opening degree of the No. 5 fan is 50%.
4. In the spinning process of the high temperature rolling process according to claim 1, 2 or 3, it is characterized in that: In the cooling process, the cooling rate is controlled at 2.1-2.4°C / s.