Wafer thinning equipment and wafer thinning method
Through specially designed wafer thinning equipment, high-speed rotational friction technology is used to achieve efficient removal of SiC wafers, solving the problems of complex processes and high costs in the existing technology, obtaining high-quality damage-free surfaces, and reducing environmental pollution. .
Patent Information
- Application Number
- CN202410820900.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-24
- Publication Date
- 2024-10-08
AI Technical Summary
The existing SiC wafer thinning process is complex and costly, making it difficult to achieve a high-quality, damage-free surface, and the waste liquid produced pollutes the environment.
Specifically designed wafer thinning equipment, including removable grinding discs and clamping equipment, equipped with heating, cooling and wetting equipment, grooves on the surface of the grinding disc, made of a combination of Ti, Ni, Fe, Mo or Cr , one-step processing is achieved through high-speed rotation and friction, which avoids the use of polishing fluid and grinding fluid and reduces environmental pollution.
Efficient removal of SiC wafers is achieved, with surface roughness lower than 0.25nm, TTV ≤ 0.2μm, and C-surface smooth without obvious damage, reducing production costs and avoiding waste liquid disposal issues.
Smart Images

Figure CN118744400A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of wafer surface processing, and in particular to a wafer thinning device and a wafer thinning method. Background Art
[0002] At present, silicon carbide is a wide bandgap semiconductor material, which has attracted much attention due to its good thermal conductivity, high temperature resistance, high breakdown field, high saturated electron drift velocity and strong radiation resistance. It will become a composite key semiconductor material widely used in light-emitting diode substrates and high-power devices in the future. In the manufacturing and epitaxial growth of the next generation of power devices, there are strict requirements for the final surface quality control of SiC single crystal materials. Atomically flat, damage-free and defect-free SiC substrates are crucial. Any micro defects on the substrate surface may affect the growth results of the epitaxial layer.
[0003] At present, domestically produced SiC wafers generally undergo rough grinding (double-sided grinding) and fine grinding (single-sided grinding) to remove a large amount of material, and then CMP polishing is used to repair the damaged layer caused by fine grinding to obtain a damage-free surface that meets the quality requirements of subsequent processes. However, the ultra-high mechanical hardness and ultra-strong chemical inertness make it difficult for SiC wafers to achieve high removal rates and atomic-level flat surfaces.
[0004] For example, CN105470122A discloses a SiC thinning method, which includes the following contents: uniformly coating the front side of a SiC wafer with photoresist; adhering sapphire to the photoresist with a high-temperature adhesive; mounting the sapphire on a thinning device, and thinning the back side of the SiC wafer with a coarse diamond wheel; thinning the back side of the SiC wafer with a fine diamond wheel; placing the SiC wafer on a rotating polishing pad, with the back side of the SiC wafer against the polishing pad, and pressing a polishing head against the front side of the SiC wafer; and injecting a polishing liquid onto the polishing pad on one side of the SiC wafer to perform CMP thinning.
[0005] CN117506708A discloses a polishing method for SiC wafers, which includes: using a grinding wheel to grind the Si surface and C surface of the SiC wafer to be processed respectively, and when the temperature of the SiC wafer to be processed is greater than 85°C, adding grinding liquid to polish the Si surface and C surface of the SiC wafer to be processed.
[0006] At present, there are two main thinning and grinding and polishing processes in the manufacturing process of SiC wafer substrates, namely double-sided grinding (rough grinding) + single-sided grinding (fine polishing) + CMP polishing process and thinning + CMP polishing process. Double-sided grinding and single-sided grinding processes mostly use diamond grinding liquid to thin the wafer to achieve a large amount of material removal, and then use CMP polishing to repair the mechanical scratches and sub-surface damage caused by the grinding process. SiC wafers have higher hardness, greater brittleness, and higher manufacturing costs. When using traditional double-polishing processes, brittle fractures, edge collapse, sub-surface cracks, etc. are prone to occur, which affect device performance. In severe cases, batch fragmentation will occur. Therefore, grinding and thinning methods are mostly used. The wafer grinding and thinning process uses an ultra-precision wafer thinning machine combined with a diamond thinning wheel to thin the wafer. Since the contact area between the grinding wheel and the wafer is constant, it has the characteristics of stable grinding force, low breakage rate, and full process automation. It is suitable for thinning and grinding of large-size wafers and ingots. Subsequently, the mechanical scratches and sub-surface damage generated during the thinning process are repaired by CMP polishing to obtain a nearly damageless SiC wafer surface.
[0007] Although the above method can obtain the ideal surface of SiC wafers, it takes a very long time to remove the scratches and dents left by mechanical polishing. The process is complicated and the cost is high, which is not conducive to the mass production of SiC wafers. In addition, the waste liquid generated will also cause certain pollution to the environment, and the waste liquid treatment is relatively complicated. Summary of the invention
[0008] In view of the problems existing in the prior art, the purpose of the present invention is to provide a wafer thinning device and a wafer thinning method to solve the problem that the current process for producing high-quality, damage-free SiC wafers is relatively complex and the production cost is too high.
[0009] To achieve this object, the present invention adopts the following technical solutions:
[0010] In a first aspect, the present invention provides a wafer thinning device, the wafer thinning device comprising: a grinding disc and a wafer clamping device arranged opposite to each other;
[0011] The wafer holding device and / or grinding disc are movable;
[0012] A driving device for driving the grinding disc and the wafer clamping device to rotate;
[0013] The grinding disc is equipped with a heating device, a cooling device and a wetting device;
[0014] The surface of the grinding disc is provided with grooves;
[0015] The material of the grinding disc working surface includes one or a combination of at least two of Ti, Ni, Fe, Mo or Cr;
[0016] The working surface of the grinding disc is a concave structure.
[0017] The wafer thinning equipment provided by the present invention can process the wafer quickly and efficiently by using a specially designed grinding wheel to process the wafer, thereby replacing the thinning, grinding and polishing steps to achieve one-step processing. Moreover, this process method does not require consumables such as polishing liquid and grinding liquid, does not involve waste liquid treatment and environmental pollution, and is energy-saving and environmentally friendly.
[0018] As a preferred technical solution of the present invention, the grinding disc comprises a grinding disc in which a support body and a working metal layer are combined or a metal integral grinding disc.
[0019] Preferably, the material of the grinding disc working surface is a corresponding pure metal material or alloy material.
[0020] As a preferred technical solution of the present invention, the depth of the groove is 220-270 μm.
[0021] Preferably, the width of the groove is 1-5 mm.
[0022] Preferably, the spacing between adjacent grooves is 8-15 mm.
[0023] As a preferred technical solution of the present invention, the working surface of the grinding disc is a concave structure, and the angle between the plane where the edge of the grinding disc working surface to the center of the grinding disc working surface is located and the horizontal plane is 0.1-0.5°.
[0024] In a second aspect, the present invention provides a wafer thinning method, which is performed using the wafer thinning equipment as described in the first aspect, and includes pre-processing, main processing and post-processing performed in sequence.
[0025] As a preferred technical solution of the present invention, the grinding disc and the wafer rotate in the same direction during the pre-processing.
[0026] Preferably, the rotation speed of the grinding disc in the pre-processing is 130-330 r / min.
[0027] Preferably, the rotation speed of the wafer during the pre-processing is 100-300 r / min.
[0028] Preferably, in the pre-processing, the rotation speed of the grinding disc is greater than the rotation speed of the wafer, and the rotation speed difference is ≤30 r / min.
[0029] As a preferred technical solution of the present invention, a pressure of 3-20 psi is applied to the wafer along the axial direction during the pre-processing.
[0030] Preferably, the flow rate of the wetting liquid in the pre-processing is 200-600 mL / min.
[0031] Preferably, the pre-processing time is 10-60s.
[0032] As a preferred technical solution of the present invention, the grinding disc and the wafer rotate in the same direction during the main processing.
[0033] Preferably, the rotation speed of the grinding disc in the main processing is 180-5500r / min.
[0034] Preferably, the rotation speed of the wafer in the main processing is 100-5000r / min.
[0035] Preferably, in the main processing, the rotation speed of the grinding disc is greater than the rotation speed of the wafer, and the rotation speed difference is 10-50 r / min.
[0036] As a preferred technical solution of the present invention, a pressure of 8-30 psi is applied to the wafer along the axial direction during the main processing.
[0037] Preferably, the operating temperature in the main processing is 350-1450°C.
[0038] Preferably, when the material of the grinding disc processing surface in the main processing is Ni, the operating temperature is 350-650°C.
[0039] Preferably, when the material of the grinding disc processing surface in the main processing is Mo, the operating temperature is 1200-1450°C.
[0040] Preferably, when the material of the grinding disc processing surface in the main processing is Fe, the operating temperature is 800-1100°C.
[0041] Preferably, when the material of the grinding disc processing surface in the main processing is Ti material, the operating temperature is 900-1200°C.
[0042] Preferably, when the material of the grinding disc processing surface in the main processing is Cr material, the operating temperature is 1100-1400°C.
[0043] Preferably, the main processing operation time is 1-10 minutes.
[0044] As a preferred technical solution of the present invention, the grinding disc and the wafer rotate in the same direction during the post-processing.
[0045] Preferably, during the post-processing, a pressure of 3-10 psi, preferably 5-7 psi, is applied to the wafer along the axial direction.
[0046] Preferably, the rotation speed of the grinding disc in the post-processing treatment is 100-300 r / min, preferably 120-150 r / min.
[0047] Preferably, the rotation speed of the wafer in the post-processing is 60-260 r / min, preferably 120-150 r / min.
[0048] Preferably, in the post-processing, the rotation speed of the grinding disc is greater than the rotation speed of the wafer, and the rotation speed difference is 10-30 r / min.
[0049] Preferably, the flow rate of the wetting liquid in the post-processing treatment is 200-800 mL / min, preferably 400-500 mL / min.
[0050] Compared with the prior art solutions, the present invention has the following beneficial effects:
[0051] The wafer processing equipment and processing method provided by the present invention adopt a specific processing process to apply a certain pressure to the SiC wafer so that it acts on a pure metal disk to perform high-speed rotation friction. After processing, the Si surface removal rate in the SiC wafer is not less than 4.5μm / min, the surface roughness Ra≤0.25nm, there is no scratch, and the surface TTV≤0.2μm; the C surface removal rate is not less than 7μm / min, and the surface of the C surface is flat after metal grinding and polishing, without obvious pits, cracks and other damage, and is close to a smooth and undamaged surface. BRIEF DESCRIPTION OF THE DRAWINGS
[0052] Figure 1 is a schematic diagram of a wafer thinning device provided by an embodiment of the present invention;
[0053] Figure 2 is a schematic diagram of a grinding disc provided by an embodiment of the present invention in which the grooves are distributed in a concentric circle manner;
[0054] Figure 3 is a schematic diagram of a grinding disc provided by an embodiment of the present invention in which the grooves are distributed in concentric circles and in a radial manner;
[0055] Figure 4 It is a schematic diagram of the concave structure of the grinding disc provided in an embodiment of the present invention.
[0056] In the figure: 1-wafer clamping equipment, 2-grinding disc, 3-pressure detection equipment, 4-cooling equipment, 5-wetting equipment, 6-heating equipment, 7-wafer to be processed.
[0057] The present invention is further described in detail below. However, the following examples are only simplified examples of the present invention and do not represent or limit the scope of protection of the present invention. The scope of protection of the present invention shall be subject to the claims. DETAILED DESCRIPTION
[0058] To better illustrate the present invention and facilitate understanding of the technical solution of the present invention, typical but non-limiting embodiments of the present invention are as follows:
[0059] This embodiment provides a wafer thinning device, such as Figure 1 As shown, the wafer thinning device comprises: a grinding disc 2 and a wafer clamping device 1 which are arranged opposite to each other;
[0060] The wafer holding device 1 and / or the grinding disc 2 are movable;
[0061] A driving device for driving the grinding disc 2 and the wafer clamping device 1 to rotate;
[0062] The grinding disc 2 is equipped with a heating device 6, a cooling device 4 and a wetting device 5;
[0063] The surface of the grinding disc 2 is provided with grooves;
[0064] The material of the working surface of the grinding disc 2 includes one or a combination of at least two of Ti, Ni, Fe, Mo or Cr;
[0065] The working surface of the grinding disc 2 is a concave structure.
[0066] In the present invention, the wafer clamping device 1 and / or the grinding wheel 2 are movably configured to achieve contact between the working surface of the grinding wheel 2 and the processing surface of the wafer 7 to be processed, and further advance after contact, thereby applying a certain pressure during the processing. The pressure can be optionally detected by a pressure detection device 3 to meet the processing requirements.
[0067] In the present invention, the heating device 6 and the cooling device 4 configured for the grinding disc 2 are used to control the operating temperature during the processing to ensure that the processing requirements are met.
[0068] In the present invention, the wetting device 5 configured for the grinding disc 2 is used to provide a wetting liquid such as water or other wetting agents to wet the metal disc during processing to prevent dry grinding during processing to damage the SiC wafer, and can also play a role in rinsing and temperature control.
[0069] In the present invention, the Mohs hardness of SiC in the wafer is much higher than that of metal, so it is difficult to remove SiC only under mechanical force. When the present invention uses the grinding disc 2 to process the wafer, chemical and mechanical reactions occur almost simultaneously. While the chemical reaction generates the metal silicide, the mechanical action between the grinding disc 2 and the wafer will also remove these reaction products at the same time; specifically, when the SiC wafer surface is in contact with the metal and is in a high-speed friction process, the Si-C bond breaks, and the silicon atoms react with the oxygen in the air at high temperature to form metal oxides and silicon dioxide. High temperature further promotes metal diffusion and reacts with SiC to form metal silicide. The products of these chemical reactions are relatively soft, and the modified layer can be removed by the mechanical friction between the grinding disc 2 and the modified layer on the surface of the SiC wafer. The appearance of the modified layer usually accelerates the chemical reaction, and a high-quality, damage-free SiC surface is finally obtained through repeated alternation of chemical reactions and mechanical removal.
[0070] Since the SiC-C surface is more easily oxidized, its chemical reaction is stronger than that of the Si surface. A sufficient reaction can make the surface modification layer bear more pressure and reduce the damage to the SiC substrate. Therefore, the surface quality of the SiC-C surface after the present invention is processed is higher than that of the SiC-Si surface, and a high-quality C surface without damage can be achieved.
[0071] The grinding wheel 2 comprises a grinding wheel in which a support body and a working metal layer are combined or a metal integral grinding wheel.
[0072] Specifically, the material of the support body can be selected according to the conventional techniques in the art, such as other metal disk supports or polymer material supports of equal strength, and can be designed specifically according to the processing requirements during the processing to ensure that the processing can be achieved.
[0073] The material configuration of the working surface of the grinding disc 2 can be directly processed with a corresponding pure metal substrate and then set on the support, or it can be set on the support by sputtering, electrochemical deposition and other processes. If it is a metal integral grinding disc 2, it can be directly processed and formed with the corresponding metal material.
[0074] In the present invention, the support body and the working metal layer in the grinding disc combined with the support body and the working metal layer can be connected by bonding, or by fastener connection such as bolt connection, or by welding and other commonly used connection methods in the art.
[0075] In the present invention, the working surface of the grinding disc 2 refers to the surface of the grinding disc 2 that contacts the surface of the wafer to be processed during the processing.
[0076] The material of the working surface of the grinding disc 2 is a limited corresponding pure metal material or alloy material. When the alloy material is used, the sufficiency of the reaction with SiC can be further increased due to the synergistic effect between the elements.
[0077] In the present invention, the thickness and shape of the grinding disc 2 can be designed and selected according to actual needs and industrial requirements. A circular grinding disc is usually used in the art.
[0078] Specifically, the depth of the groove is 220-270μm, for example, it can be 220μm, 222μm, 224μm, 226μm, 228μm, 230μm, 232μm, 234μm, 236μm, 238μm, 240μm, 242μm, 244μm, 246μm, 248μm, 250μm, 252μm, 254μm, 256μm, 258μm, 260μm, 262μm, 264μm, 266μm, 268μm or 270μm, but is not limited to the listed values, and other unlisted values within the range also meet the requirements.
[0079] In the present invention, if the groove depth is too large, the uniformity of the film thickness of the processed SiC wafer will be affected; if the groove depth is too shallow, the removal rate will be slow and multiple grooves will be required, which will affect the operation efficiency.
[0080] Specifically, the width of the groove is 1-5mm, for example, it can be 1mm, 1.2mm, 1.4mm, 1.6mm, 1.8mm, 2mm, 2.2mm, 2.4mm, 2.6mm, 2.8mm, 3mm, 3.2mm, 3.4mm, 3.6mm, 3.8mm, 4mm, 4.2mm, 4.4mm, 4.6mm, 4.8mm or 5mm, but is not limited to the listed values, and other values not listed in this range also meet the requirements.
[0081] Specifically, the cross-sectional shape of the groove includes a V-shape.
[0082] Specifically, the extension modes of the groove include linear extension and arc-shaped extension, etc. The linear extension corresponds to a linear groove, and the arc-shaped extension corresponds to an arc-shaped groove such as an annular groove.
[0083] Specifically, the spacing between adjacent grooves is 8-15 mm, for example, it can be 8 mm, 9 mm, 10 mm, 11 mm, 12 mm, 13 mm, 14 mm or 15 mm, but is not limited to the listed values, and other unlisted values within the range also meet the requirements.
[0084] In the present invention, the spacing between adjacent grooves is the distance between the closest edges of the adjacent grooves.
[0085] Specifically, the grooves are arranged in a manner including one or a combination of at least two of an annular arrangement, a radial arrangement or a parallel arrangement.
[0086] The annular arrangement is to arrange the grooves in a concentric or non-concentric manner according to the limitation, wherein: Figure 2 Annular grooves arranged in concentric circles are shown.
[0087] In the present invention, due to processing limitations, a plane such as a circular surface will exist in the center of the grinding disc during the processing of the grinding disc. The equivalent circular diameter of the circular surface is 1 / 12-1 / 10 of the equivalent circular diameter of the grinding disc. If processing conditions permit, processing can be continued until no groove can be formed.
[0088] The radial setting is to distribute the grooves toward the edge with a point on the surface of the grinding disc 2 as the center.
[0089] The parallel arrangement means that the grooves are arranged in parallel lines on the surface of the grinding disc 2 according to the definition.
[0090] Among them, the grooves of various styles can be arranged in a partitioned or cross-shaped manner. For example, parallel grooves are arranged in an annular groove, or an annular groove and a radial groove are arranged at the same time, such as Figure 3 shown.
[0091] The working surface of the grinding disc 2 is a concave structure, and the angle between the plane where the edge of the working surface of the grinding disc 2 and the center of the working surface of the grinding disc 2 is located and the horizontal plane is 0.1-0.5°. Figure 4 As shown, the working surface for contact processing of the wafer gradually becomes higher from the center of the grinding wheel 2 to the edge of the grinding wheel 2. The specific angle can be 0.1°, 0.15°, 0.2°, 0.25°, 0.3°, 0.35°, 0.4°, 0.45° or 0.5°, etc., but is not limited to the listed values. Other values not listed in this range also meet the requirements.
[0092] In the present invention, the concave grinding disc 2 is tilted at a certain angle to avoid slight deformation of the central area of the grinding disc 2 during the processing, thereby solving the problem of uneven removal rate to the greatest extent.
[0093] Furthermore, the present invention provides a wafer thinning method based on the aforementioned processing equipment, wherein the wafer thinning method includes pre-processing, main processing and post-processing performed in sequence.
[0094] Wherein, during the pre-processing, the grinding disc 2 and the wafer rotate in the same direction.
[0095] In the present invention, if the grinding disc 2 and the wafer rotate in different directions during pre-processing, the removal rate difference between the edge and the center of the wafer will be large, the TTV will be deteriorated, and the processing efficiency will be slowed down.
[0096] Among them, the rotation speed of the grinding wheel 2 in the pre-processing is 130-330r / min, for example, it can be 130r / min, 140r / min, 160r / min, 180r / min, 200r / min, 220r / min, 240r / min, 260r / min, 280r / min, 300r / min, 320r / min or 330r / min, but is not limited to the listed values, and other unlisted values within the range also meet the requirements.
[0097] Among them, the rotation speed of the wafer in the pre-processing is 100-300r / min, for example, it can be 100r / min, 120r / min, 140r / min, 160r / min, 180r / min, 200r / min, 220r / min, 240r / min, 260r / min, 280r / min or 300r / min, but is not limited to the listed values, and other unlisted values within the range also meet the requirements.
[0098] Among them, the rotation speed of the grinding disc 2 in the pre-processing is greater than the rotation speed of the wafer, and the speed difference is ≤30r / min, for example, it can be 30r / min, 28r / min, 24r / min, 22r / min, 20r / min, 18r / min, 16r / min, 14r / min, 12r / min, 10r / min, 8r / min, 6r / min, 4r / min, 2r / min or 1r / min, but is not limited to the listed values, and other values not listed in the range also meet the requirements.
[0099] Among them, during the pre-processing, a pressure of 3-20psi is applied to the wafer along the axial direction, for example, it can be 3psi, 4psi, 5psi, 6psi, 7psi, 8psi, 9psi, 10psi, 11psi, 12psi, 13psi, 14psi, 15psi, 16psi, 17psi, 18psi, 19psi or 20psi, etc., but is not limited to the listed values, and other values not listed in this range also meet the requirements.
[0100] Wherein, the flow rate of the wetting liquid in the pre-processing is 200-600mL / min, for example, it can be 200mL / min, 220mL / min, 240mL / min, 260mL / min, 280mL / min, 300mL / min, 320mL / min, 340mL / min, 360mL / min, 380mL / min, 400mL / min, 420mL / min, 440mL / min, 460mL / min, 480mL / min, 500mL / min, 520mL / min, 540mL / min, 560mL / min, 580mL / min or 600mL / min, but is not limited to the listed values, and other values not listed within the range also meet the requirements.
[0101] Among them, the pre-processing time is 10-60s, for example, it can be 10s, 15s, 20s, 25s, 30s, 35s, 40s, 45s, 50s, 55s or 60s, but is not limited to the listed values, and other unlisted values within the range also meet the requirements.
[0102] Wherein, in the main processing, the grinding disc 2 and the wafer rotate in the same direction.
[0103] Among them, in the main processing, a pressure of 8-30psi is applied to the wafer along the axial direction, for example, it can be 8psi, 12psi, 14psi, 16psi, 18psi, 20psi, 22psi, 24psi, 26psi, 28psi or 30psi, but is not limited to the listed values, and other unlisted values within the range also meet the requirements.
[0104] The rotation speed of the grinding disc 2 in the main processing is 180-5500r / min, for example, it can be 180r / min, 200r / min, 400r / min, 600r / min, 800r / min, 1000r / min, 1200r / min, 1400r / min, 1600r / min, 1800r / min, 2000r / min, 2200r / min, 2400r / min, 2600r / min, 2800r / min. / min, 3000r / min, 3200r / min, 3400r / min, 3600r / min, 3800r / min, 4000r / min, 4200r / min, 4400r / min, 4600r / min, 4800r / min, 5000r / min, 5200r / min, 5400r / min or 5500r / min, etc., but not limited to the listed values. Other values not listed in the range also meet the requirements.
[0105] The rotation speed of the wafer in the main processing is 100-5000r / min, for example, it can be 100r / min, 200r / min, 400r / min, 600r / min, 800r / min, 1000r / min, 1200r / min, 1400r / min, 1600r / min, 1800r / min, 2000r / min, 2200r / min, 2400r / min, 2600r / min, 2800r / min, 3000r / min, 3200r / min, 3400r / min, 3600r / min, 3800r / min, 4000r / min, 4200r / min, 4400r / min, 4600r / min, 4800r / min or 5000r / min, etc., but not limited to the listed values. Other values not listed within the range also meet the requirements.
[0106] In the main processing, the rotation speed of the grinding disc 2 is greater than the rotation speed of the wafer, and the speed difference is 10-50r / min, for example, it can be 10r / min, 12r / min, 14r / min, 16r / min, 18r / min, 20r / min, 22r / min, 24r / min, 26r / min, 28r / min, 30r / min, 32r / min, 34r / min, 36r / min, 38r / min, 40r / min, 42r / min, 44r / min, 46r / min, 48r / min or 50r / min, but is not limited to the listed values, and other values not listed in this range also meet the requirements.
[0107] The operating temperature in the main processing is 350-1450°C, for example, it can be 350°C, 400°C, 450°C, 450°C, 500°C, 550°C, 600°C, 650°C, 700°C, 750°C, 800°C, 850°C, 900°C, 950°C, 1000°C, 1050°C, 1100°C, 1150°C, 1200°C, 1250°C, 1300°C, 1350°C, 1400°C or 1450°C, but is not limited to the listed values, and other values not listed in this range also meet the requirements.
[0108] Specifically, the reaction products of the metal and SiC involved in the main processing at high temperature are mainly composed of metal silicide, silicon oxide and metal oxide. The activation energy to be overcome is different, and the required temperature is different. Specifically, the heat generated by friction, the heating device 6 and the cooling device 4 configured by the grinding wheel 2 work together to maintain the reaction temperature in the corresponding range. The specific chemical reaction formula is as follows:
[0109] 2Ni+2SiC+3O2→SiO2+Ni2Si+NiO+2CO2Reaction temperature: 350-650℃
[0110] 5Mo+3SiC+4O2→Mo3Si2C2+SiO2+2MoO3+CO2Reaction temperature: 1200-1450℃
[0111] 3Fe+2SiC+4O2→SiO2+FeSi+Fe3O4+2CO2 Reaction temperature: 800-1100℃
[0112] 2Ti+4SiC+6O2→TiSi2+2SiO2+TiO2+4CO2 Reaction temperature: 900-1200℃
[0113] 7Cr+3SiC+7O2→Cr3Si2+3CO2+2Cr2O3+SiO2 Reaction temperature: 1100-1400℃.
[0114] For example, when the heating device 6 configured for the grinding disc 2 is a resistance heater, the working voltage is controlled to be 100-600V and the current is 5-20A. The voltage of the resistance heater is gradually increased from the initial value of 100V, and the change in the temperature of the metal disc is observed. The most suitable voltage value is determined by monitoring the temperature change so that the metal disc reaches the target temperature. After determining the appropriate voltage, the heating power of the heater is controlled by fine-tuning the current value, thereby adjusting the temperature of the metal disc to stabilize it near the target temperature. The specific temperature required is the following chemical reaction equation.
[0115] Preferably, when the material of the machining surface of the grinding wheel 2 in the main processing is Ni, the operating temperature is 350-650°C, for example, it can be 350°C, 360°C, 380°C, 400°C, 420°C, 440°C, 460°C, 480°C, 500°C, 520°C, 540°C, 560°C, 580°C, 600°C, 620°C, 640°C or 650°C, etc., but is not limited to the listed values, and other unlisted values within the range also meet the requirements.
[0116] Preferably, when the material of the machining surface of the grinding wheel 2 in the main processing is Mo, the operating temperature is 1200-1450°C, for example, it can be 1200°C, 1220°C, 1240°C, 1260°C, 1280°C, 1300°C, 1320°C, 1340°C, 1360°C, 1380°C, 1400°C, 1420°C, 1440°C or 1450°C, but is not limited to the listed values, and other unlisted values within the range also meet the requirements.
[0117] Preferably, when the material of the machining surface of the grinding disc 2 in the main machining is Fe, the operating temperature is 800-1100°C, for example, it can be 800°C, 820°C, 840°C, 860°C, 880°C, 900°C, 920°C, 940°C, 960°C, 980°C, 1000°C, 1020°C, 1040°C, 1060°C, 1080°C, 1100°C, 1120°C, 1140°C, 1160°C, 1180°C or 1200°C, etc., but is not limited to the listed values, and other unlisted values within the range also meet the requirements.
[0118] Preferably, when the material of the machining surface of the grinding disc 2 in the main processing is Ti material, the operating temperature is 900-1200°C, for example, it can be 900°C, 920°C, 940°C, 960°C, 980°C, 1000°C, 1020°C, 1040°C, 1060°C, 1080°C, 1100°C, 1120°C, 1140°C, 1160°C, 1180°C or 1200°C, but is not limited to the listed values, and other unlisted values within the range also meet the requirements.
[0119] Preferably, when the machining surface material of the grinding wheel 2 in the main machining is Cr material, the operating temperature is 1100-1400°C, for example, it can be 1100°C, 1120°C, 1140°C, 1160°C, 1180°C, 1200°C, 1220°C, 1240°C, 1260°C, 1280°C, 1300°C, 1320°C, 1340°C, 1360°C, 1380°C or 1400°C, but is not limited to the listed values, and other unlisted values within the range also meet the requirements.
[0120] In the present invention, when the material of the machining surface of the grinding disc 2 in the main machining is an alloy material of at least two elements among Ti, Ni, Fe, Mo, and Cr, the operating temperature of the main machining can be 100-200°C higher than the highest temperature in the single element operation. For example, the operating temperature range of Fe-Ti alloy is 1000-1400°C, among which, when Fe is used, the operating temperature is 800-1100°C, and when Ti is used, the operating temperature is 900-1200°C, that is, the operating temperature of Ti can be increased by 100-200°C.
[0121] Among them, the operation time of the main processing is 1-10 minutes, for example, it can be 1 minute, 2 minutes, 3 minutes, 4 minutes, 5 minutes, 6 minutes, 7 minutes, 8 minutes, 9 minutes or 10 minutes, but it is not limited to the listed values. Other values not listed within the range also meet the requirements.
[0122] In the present invention, no grinding fluid or polishing fluid is required during the main processing operation, and the thinning effect can be achieved only by the grinding disc 2.
[0123] Wherein, in the post-processing treatment, the grinding disc 2 and the wafer rotate in the same direction.
[0124] Among them, in the post-processing treatment, a pressure of 3-10psi is applied to the wafer along the axial direction, for example, it can be 3psi, 3psi, 3.5psi, 4psi, 4.5psi, 5psi, 5.5psi, 6psi, 6.5psi, 7psi, 7.5psi, 8psi, 8.5psi, 9psi, 9.5psi or 10psi, but is not limited to the listed values. Other unlisted values within the range also meet the requirements, preferably 5-7psi.
[0125] Among them, the rotation speed of the grinding wheel 2 in the post-processing treatment is 100-300r / min, for example, it can be 100r / min, 120r / min, 140r / min, 160r / min, 180r / min, 200r / min, 220r / min, 240r / min, 260r / min, 280r / min or 300r / min, but is not limited to the listed values. Other unlisted values within this range also meet the requirements, preferably 120-150r / min.
[0126] Among them, the rotation speed of the wafer in the post-processing is 60-260r / min, for example, it can be 60r / min, 80r / min, 100r / min, 120r / min, 140r / min, 160r / min, 180r / min, 200r / min, 220r / min, 240r / min or 260r / min, but is not limited to the listed values. Other unlisted values within the range also meet the requirements, preferably 120-150r / min.
[0127] Among them, in the post-processing, the rotation speed of the grinding wheel 2 is greater than the rotation speed of the wafer, and the speed difference is 10-30r / min, for example, it can be 10r / min, 12r / min, 14r / min, 16r / min, 18r / min, 20r / min, 22r / min, 24r / min, 26r / min, 28r / min or 30r / min, but not limited to the listed values, and other values not listed within the range also meet the requirements.
[0128] Among them, the flow rate of the wetting liquid in the post-processing treatment is 200-800mL / min, for example, it can be 200mL / min, 250mL / min, 300mL / min, 350mL / min, 400mL / min, 450mL / min, 500mL / min, 550mL / min, 600mL / min, 650mL / min, 700mL / min, 750mL / min or 800mL / min, but is not limited to the listed values. Other unlisted values within this range also meet the requirements, preferably 400-500mL / min.
[0129] In the present invention, spraying the wetting liquid in the post-processing treatment can remove particles, residues and by-products such as metal oxides and metal silicides generated during the main processing process on the surface of the sheet source and the surface of the metal disk, and can also achieve the purpose of cooling the surface of the metal disk.
[0130] Furthermore, in order to illustrate the processing effect achieved by the wafer processing equipment and processing method provided by the present invention, actual examples are used for illustration, as follows:
[0131] Example 1
[0132] This embodiment provides a wafer thinning device, which includes: a grinding disc 2 and a wafer clamping device 1 which are arranged opposite to each other;
[0133] The wafer clamping device 1 is a movable configuration;
[0134] A driving device for driving the grinding disc 2 and the wafer clamping device 1 to rotate;
[0135] The grinding disc 2 is equipped with a heating device 6, a cooling device 4 and a wetting device 5;
[0136] The grinding disc 2 is provided with grooves on its surface; the depth of the grooves is 240 μm; the width of the grooves is 3 mm; the spacing between adjacent grooves is 10 mm, and the grooves are concentric circular grooves, such as Figure 2 As shown;
[0137] The material of the working surface of the grinding disc 2 is Fe;
[0138] The working surface of the grinding disc 2 is a concave structure, and the angle between the plane where the edge of the working surface of the grinding disc 2 and the center of the working surface of the grinding disc 2 is located and the horizontal plane is 0.2°;
[0139] The grinding disc 2 is a metal integral grinding disc, that is, the grinding disc is an iron grinding disc.
[0140] The processing process is as follows:
[0141] Includes pre-processing, main processing and post-processing in sequence;
[0142] The grinding disc 2 and the wafer rotate in the same direction during the pre-processing; the rotation speed of the grinding disc 2 during the pre-processing is 250 r / min; the rotation speed of the wafer during the pre-processing is 235 r / min; the rotation speed of the grinding disc 2 during the pre-processing is greater than the rotation speed of the wafer, and the speed difference is 15 r / min; the pressure applied to the wafer along the axial direction during the pre-processing is 12 psi; the flow rate of the wetting liquid during the pre-processing is 300 mL / min; the pre-processing time is 30 s;
[0143] The grinding disc 2 and the wafer rotate in the same direction during the main processing; the rotation speed of the wafer during the main processing is 2000r / min; the rotation speed of the grinding disc 2 during the main processing is 2050r / min; the rotation speed of the grinding disc 2 during the main processing is greater than the rotation speed of the wafer, and the rotation speed difference is 50r / min; the pressure applied to the wafer along the axial direction during the main processing is 20psi; the processing surface of the grinding disc 2 during the main processing is made of Fe, and the operating temperature is 1000℃; the operating time of the main processing is 5min;
[0144] During the post-processing, the grinding disc 2 and the wafer rotate in the same direction; during the post-processing, a pressure of 5 psi is applied to the wafer along the axial direction; during the post-processing, the rotation speed of the grinding disc 2 is 150 r / min; during the post-processing, the rotation speed of the wafer is 140 r / min; during the post-processing, the rotation speed of the grinding disc 2 is greater than the rotation speed of the wafer, and the speed difference is 10 r / min; during the post-processing, the flow rate of the wetting liquid is 200-800 mL / min.
[0145] Example 2
[0146] This embodiment provides a wafer thinning device, which includes: a grinding disc 2 and a wafer clamping device 1 which are arranged opposite to each other;
[0147] The wafer clamping device 1 is a movable configuration;
[0148] A driving device for driving the grinding disc 2 and the wafer clamping device 1 to rotate;
[0149] The grinding disc 2 is equipped with a heating device 6, a cooling device 4 and a wetting device 5;
[0150] The grinding disc 2 is provided with grooves on its surface; the depth of the grooves is 260 μm; the width of the grooves is 5 mm; the spacing between adjacent grooves is 14 mm, and the grooves are grooves composed of concentric circular grooves and radial grooves, such as Figure 3 As shown;
[0151] The material of the working surface of the grinding disc 2 is Ti;
[0152] The working surface of the grinding disc 2 is a concave structure, and the angle between the plane where the edge of the working surface of the grinding disc 2 and the center of the working surface of the grinding disc 2 is located and the horizontal plane is 0.5°;
[0153] The grinding disc 2 comprises a grinding disc combined with a support body and a working metal layer, the support body is an aluminum support body, and the working metal layer is a titanium layer.
[0154] The processing process is as follows:
[0155] Includes pre-processing, main processing and post-processing in sequence;
[0156] The grinding disc 2 and the wafer rotate in the same direction during the pre-processing; the rotation speed of the grinding disc 2 during the pre-processing is 280r / min; the rotation speed of the wafer during the pre-processing is 255r / min; the rotation speed of the grinding disc 2 during the pre-processing is greater than the rotation speed of the wafer, and the speed difference is 25r / min; the pressure applied to the wafer along the axial direction during the pre-processing is 12psi; the flow rate of the wetting liquid during the pre-processing is 300mL / min; the pre-processing time is 30s;
[0157] The grinding disc 2 and the wafer rotate in the same direction during the main processing; the rotation speed of the grinding disc 2 during the main processing is 4030r / min; the rotation speed of the wafer during the main processing is 4000r / min; the rotation speed of the grinding disc 2 during the main processing is greater than the rotation speed of the wafer, and the speed difference is 30r / min; the pressure applied to the wafer along the axial direction during the main processing is 30psi; when the processing surface material of the grinding disc 2 during the main processing is Ti material, the operating temperature is 1000℃; the operating time of the main processing is 1min;
[0158] During the post-processing, the grinding disc 2 and the wafer rotate in the same direction; during the post-processing, a pressure of 5 psi is applied to the wafer along the axial direction; during the post-processing, the rotation speed of the grinding disc 2 is 150 r / min; during the post-processing, the rotation speed of the wafer is 140 r / min; during the post-processing, the rotation speed of the grinding disc 2 is greater than the rotation speed of the wafer, and the speed difference is 10 r / min; during the post-processing, the flow rate of the wetting liquid is 200-800 mL / min.
[0159] Example 3
[0160] This embodiment provides a wafer thinning device, which includes: a grinding disc 2 and a wafer clamping device 1 which are arranged opposite to each other;
[0161] The wafer clamping device 1 is a movable configuration;
[0162] A driving device for driving the grinding disc 2 and the wafer clamping device 1 to rotate;
[0163] The grinding disc 2 is equipped with a heating device 6, a cooling device 4 and a wetting device 5;
[0164] The surface of the grinding disc 2 is provided with grooves; the depth of the grooves is 230 μm; the width of the grooves is 1 mm; the spacing between adjacent grooves is 9 mm, and the grooves are concentric circular grooves, such as Figure 2 As shown;
[0165] The material of the working surface of the grinding disc 2 is Ni;
[0166] The working surface of the grinding disc 2 is a concave structure, and the angle between the plane where the edge of the working surface of the grinding disc 2 and the center of the working surface of the grinding disc 2 is located and the horizontal plane is 0.1°;
[0167] The grinding disc 2 is a metal integral grinding disc, that is, a nickel grinding disc.
[0168] The processing process is as follows:
[0169] Includes pre-processing, main processing and post-processing in sequence;
[0170] During the pre-processing, the grinding disc 2 and the wafer rotate in the same direction; the rotation speed of the grinding disc 2 during the pre-processing is 130 r / min; the rotation speed of the wafer during the pre-processing is 100 r / min; the rotation speed of the grinding disc 2 during the pre-processing is greater than the rotation speed of the wafer, and the speed difference is 30 r / min; the pressure applied to the wafer along the axial direction during the pre-processing is 6 psi; the flow rate of the wetting liquid during the pre-processing is 500 mL / min; the pre-processing time is 30 s;
[0171] The grinding disc 2 and the wafer rotate in the same direction during the main processing; the rotation speed of the grinding disc 2 during the main processing is 1530r / min; the rotation speed of the wafer during the main processing is 1500r / min; the rotation speed of the grinding disc 2 during the main processing is greater than the rotation speed of the wafer, and the speed difference is 30r / min; the pressure applied to the wafer along the axial direction during the main processing is 12psi; when the processing surface material of the grinding disc 2 during the main processing is Ni, the operating temperature is 500°C; the operating time of the main processing is 10min;
[0172] During the post-processing, the grinding disc 2 and the wafer rotate in the same direction; during the post-processing, a pressure of 5 psi is applied to the wafer along the axial direction; during the post-processing, the rotation speed of the grinding disc 2 is 100 r / min; during the post-processing, the rotation speed of the wafer is 90 r / min; during the post-processing, the rotation speed of the grinding disc 2 is greater than the rotation speed of the wafer, and the rotation speed difference is 10 r / min; during the post-processing, the flow rate of the wetting liquid is 300 mL / min.
[0173] Example 4
[0174] This embodiment provides a wafer thinning device, which includes: a grinding disc 2 and a wafer clamping device 1 which are arranged opposite to each other;
[0175] The wafer clamping device 1 is a movable configuration;
[0176] A driving device for driving the grinding disc 2 and the wafer clamping device 1 to rotate;
[0177] The grinding disc 2 is equipped with a heating device 6, a cooling device 4 and a wetting device 5;
[0178] The grinding disc 2 is provided with grooves on its surface; the depth of the grooves is 270 μm; the width of the grooves is 5 mm; the spacing between adjacent grooves is 12 mm, and the grooves are grooves composed of concentric circular grooves and radial grooves, such as Figure 3 As shown;
[0179] The material of the working surface of the grinding disc 2 is Cr;
[0180] The working surface of the grinding disc 2 is a concave structure, and the angle between the plane where the edge of the working surface of the grinding disc 2 and the center of the working surface of the grinding disc 2 is located and the horizontal plane is 0.3°;
[0181] The grinding disc 2 comprises a grinding disc combined with a support body and a working metal layer, the support body is a PVC material support body, and the working metal layer is a Cr layer.
[0182] The processing process is as follows:
[0183] Includes pre-processing, main processing and post-processing in sequence;
[0184] During the pre-processing, the grinding disc 2 and the wafer rotate in the same direction; the rotation speed of the grinding disc 2 during the pre-processing is 130 r / min; the rotation speed of the wafer during the pre-processing is 100 r / min; the rotation speed of the grinding disc 2 during the pre-processing is greater than the rotation speed of the wafer, and the speed difference is 30 r / min; the pressure applied to the wafer along the axial direction during the pre-processing is 3 psi; the flow rate of the wetting liquid during the pre-processing is 300 mL / min; the pre-processing time is 50 s;
[0185] The grinding disc 2 and the wafer rotate in the same direction during the main processing; the rotation speed of the grinding disc 2 during the main processing is 530r / min; the rotation speed of the wafer during the main processing is 500r / min; the rotation speed of the grinding disc 2 during the main processing is greater than the rotation speed of the wafer, and the speed difference is 30r / min; the pressure applied to the wafer along the axial direction during the main processing is 8psi; when the processing surface material of the grinding disc 2 during the main processing is Cr material, the operating temperature is 1200°C; the operating time of the main processing is 5min; in this embodiment, a resistance heater is used for auxiliary heating in the main processing, and the voltage value of the resistance heater is 400V and the current value is 10A;
[0186] During the post-processing, the grinding disc 2 and the wafer rotate in the same direction; during the post-processing, a pressure of 3 psi is applied to the wafer along the axial direction; during the post-processing, the rotation speed of the grinding disc 2 is 100 r / min; during the post-processing, the rotation speed of the wafer is 80 r / min; during the post-processing, the rotation speed of the grinding disc 2 is greater than the rotation speed of the wafer, and the rotation speed difference is 20 r / min; during the post-processing, the flow rate of the wetting liquid is 250 mL / min.
[0187] Example 5
[0188] The only difference from Example 1 is that the rotation speed of the wafer in the main processing is 2000 r / min; the rotation speed of the grinding disc in the main processing is 3050 r / min, that is, the rotation speed difference is not controlled.
[0189] Example 6
[0190] The difference from Example 1 is that the rotation speed of the wafer in the main processing is 100 r / min; the rotation speed of the grinding disc in the main processing is 180 r / min, that is, the rotation speed difference is not controlled. At this time, due to the low rotation speed, auxiliary heating is performed, and the voltage of the resistance heater is 500 V and the current is 12 A.
[0191] Comparative Example 1
[0192] The only difference from Example 1 is that the material of the grinding disc working surface is replaced by zinc.
[0193] Comparative Example 2
[0194] The only difference from Example 1 is that the material of the grinding disc working surface is replaced by tin.
[0195] Comparative Example 3
[0196] The only difference from Example 1 is that the material of the grinding disc working surface is replaced by copper.
[0197] Comparative Example 4
[0198] The only difference from Example 1 is that the working surface of the grinding disc is a planar structure.
[0199] Example 5
[0200] The only difference from Example 1 is that the depth of the groove is 300 μm.
[0201] Example 6
[0202] The only difference from Example 1 is that the angle between the plane from the edge of the grinding disc working surface to the center of the grinding disc working surface and the horizontal plane is 2°.
[0203] Example 7
[0204] The only difference from Example 1 is that the pressure applied to the wafer in the axial direction during the main process is 3 psi.
[0205] Example 8
[0206] The only difference from Example 1 is that the pressure applied to the wafer in the axial direction during the main process is 3 psi.
[0207] Example 9
[0208] The only difference from Example 1 is that in the main processing, the rotation speed of the wafer is greater than the rotation speed of the grinding disc, and the rotation speed difference remains unchanged, that is, the rotation speed of the wafer is 2050 r / min, and the rotation speed of the grinding disc is 2000 r / min.
[0209] Example 10
[0210] The only difference from Example 1 is that the rotation speed of the grinding disc is adjusted to 50 r / min.
[0211] The surface parameters of the wafers processed by the embodiment and the comparative example are shown in Table 1.
[0212] Table 1
[0213]
[0214]
[0215] In combination with Table 1, it can be seen from the comparison between Example 1 and Comparative Examples 1, 2, and 3 that when the material of the working surface of the grinding disc is replaced with zinc, tin, and copper, these metals have lower solid solubility and higher activity, and are easy to directly react with SiC to form zinc silicon compounds, tin silicon compounds, and copper oxide under high temperature and high-speed friction conditions. Metals such as Ti, Ni, Fe, Mo, or Cr are more inclined to form oxide layers or oxide films at high temperatures, and these oxide layers can provide more active sites to promote the reaction between metals and SiC. Therefore, the rate is slow under the action of zinc, tin, and copper metal grinding discs, and metals such as zinc, tin, and copper are relatively soft, and are prone to deformation or wear during high-speed friction, resulting in reduced processing efficiency, roughness, and TTV deterioration.
[0216] Combined with Table 1, it can be seen from the comparison between Example 1 and Comparative Example 4 that when the working surface of the grinding disc is a planar structure rather than a groove structure, the SiC processing rate has a significant downward trend, while the surface roughness and TTV become larger. The groove structure can provide a more uniform distribution of grinding force, making the grinding force more concentrated on the edge of the groove, thereby increasing the processing rate. At the same time, the groove structure helps to effectively discharge the grinding chips and by-products generated during grinding, disperse the heat generated during the grinding process, prevent it from contacting the wafer again during the grinding process, and reduce surface damage and roughness.
[0217] Combined with Table 1, by comparing Example 1 with Comparative Example 5, it can be seen that when the depth of the groove on the working surface of the grinding wheel is deeper, the processing rate of SiC will be improved, but too deep a groove will increase the unevenness of the grinding result, leaving uneven grinding marks on the surface of the wafer, thereby affecting the surface roughness and TTV uniformity of the SiC wafer.
[0218] Combined with Table 1, by comparing Example 1 with Comparative Example 6, it can be seen that when the angle between the edge of the grinding disc working surface to the plane where the center of the grinding disc working surface is located and the horizontal plane is large, that is, when the edge of the metal disc is too high compared to the middle area, the edge of the metal disc contacts the SiC wafer being processed more during the processing, resulting in a fast grinding rate at the edge and a slow grinding rate in the middle area, thereby causing the TTV uniformity and surface roughness of the SiC wafer to deteriorate.
[0219] Combined with Table 1, it can be seen from the comparison between Example 1 and Comparative Examples 7 and 8 that when the pressure applied to the wafer along the axial direction in the main processing is too low, the heat generated during the high-speed friction process is low, and it is difficult to form the high-temperature environment required for the chemical reaction between the metal and SiC. At this time, the mechanical friction effect is the dominant mechanism, the SiC wafer processing rate is significantly reduced, and the TTV uniformity and SiC surface roughness are increased. When the pressure applied to the wafer along the axial direction in the main processing is too high, the heat generated during the high-speed friction process is high, and it is easier to obtain the high-temperature environment required for the chemical reaction, and the SiC processing rate is significantly accelerated, but the excessive pressure will have a strong mechanical effect in the process of removing the softer byproducts generated by the chemical reaction, resulting in a decrease in the surface quality of the processed wafer and a significant increase in roughness.
[0220] Combined with Table 1, by comparing Example 1 with Comparative Example 9, it can be seen that when the rotation speed of the wafer in the main processing is greater than the rotation speed of the grinding wheel, a larger friction force and shear force can be generated to improve the processing rate of the SiC wafer, but too fast a wafer rotation speed may cause local over-grinding or scratches, thereby reducing the surface uniformity and surface quality of the wafer.
[0221] Combined with Table 1, by comparing Example 1 with Comparative Example 10, it can be seen that when the rotation speed of the grinding wheel during processing is as low as 100-100rpm, it is necessary to quickly reach the high-speed friction condition and the high temperature condition required for the chemical reaction with the assistance of the resistance heater. When the rotation speed is lower than 100rpm, the rotation speed condition required for high-speed friction is not reached, and it is difficult to achieve friction-induced chemical reaction at the interface. At this time, mechanical friction is the dominant mechanism, the SiC wafer processing rate is significantly reduced, and the TTV uniformity and SiC surface roughness are increased.
[0222] It is stated that the present invention illustrates the detailed structural features of the present invention through the above embodiments, but the present invention is not limited to the above detailed structural features, that is, it does not mean that the present invention must rely on the above detailed structural features to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of the components selected by the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.
[0223] The preferred embodiments of the present invention are described in detail above. However, the present invention is not limited to the specific details in the above embodiments. Within the technical concept of the present invention, a variety of simple modifications can be made to the technical solution of the present invention, and these simple modifications all belong to the protection scope of the present invention.
[0224] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not further describe various possible combinations.
[0225] In addition, various embodiments of the present invention may be arbitrarily combined, and as long as they do not violate the concept of the present invention, they should also be regarded as the contents disclosed by the present invention.
Claims
1. A wafer thinning device, characterized in that: The wafer thinning device comprises: a grinding disc and a wafer clamping device arranged opposite to each other; The wafer holding device and / or grinding disc are movable; A driving device for driving the grinding disc and the wafer clamping device to rotate; The grinding disc is equipped with a heating device, a cooling device and a wetting device; The surface of the grinding disc is provided with grooves; The material of the grinding disc working surface includes one or a combination of at least two of Ti, Ni, Fe, Mo or Cr; The working surface of the grinding disc is a concave structure.
2. The wafer thinning device according to claim 1, characterized in that: The grinding disc comprises a grinding disc in which a support body and a working metal layer are combined or a metal integral grinding disc; Preferably, the material of the grinding disc working surface is a corresponding pure metal material or alloy material.
3. The wafer thinning device according to claim 1 or 2, characterized in that: The depth of the groove is 220-270 μm; Preferably, the width of the groove is 1-5 mm; Preferably, the spacing between adjacent grooves is 8-15 mm.
4. The wafer thinning device according to any one of claims 1 to 3, characterized in that: The working surface of the grinding disc is a concave structure, and the angle between the plane where the edge of the working surface of the grinding disc is located to the center of the working surface of the grinding disc and the horizontal plane is 0.1-0.5°.
5. A wafer thinning method, characterized in that: The wafer thinning method is performed using the wafer thinning equipment as described in any one of claims 1 to 4, including pre-processing, main processing and post-processing performed in sequence.
6. The wafer thinning method according to claim 5, characterized in that: During the pre-processing, the grinding disc and the wafer rotate in the same direction; Preferably, the rotation speed of the grinding disc in the pre-processing is 130-330 r / min; Preferably, the rotation speed of the wafer during the pre-processing is 100-300 r / min; Preferably, in the pre-processing, the rotation speed of the grinding disc is greater than the rotation speed of the wafer, and the rotation speed difference is ≤30 r / min.
7. The wafer thinning method according to claim 5 or 6, characterized in that: During the pre-processing, a pressure of 3-20 psi is applied to the wafer along the axial direction; Preferably, the flow rate of the wetting liquid in the pre-processing is 200-600 mL / min; Preferably, the pre-processing time is 10-60s.
8. The wafer thinning method according to any one of claims 5 to 7, characterized in that: In the main processing, the grinding disc and the wafer rotate in the same direction; Preferably, the rotation speed of the grinding disc in the main processing is 180-5500r / min; Preferably, the rotation speed of the wafer in the main processing is 100-5000r / min; Preferably, in the main processing, the rotation speed of the grinding disc is greater than the rotation speed of the wafer, and the rotation speed difference is 10-50 r / min.
9. The wafer thinning method according to any one of claims 5 to 8, characterized in that: During the main processing, a pressure of 8-30 psi is applied to the wafer in the axial direction; Preferably, the operating temperature in the main processing is 350-1450°C; Preferably, when the material of the grinding disc processing surface in the main processing is Ni, the operating temperature is 350-650°C; Preferably, when the material of the grinding disc processing surface in the main processing is Mo, the operating temperature is 1200-1450°C; Preferably, when the material of the grinding disc processing surface in the main processing is Fe, the operating temperature is 800-1100°C; Preferably, when the material of the grinding disc processing surface in the main processing is Ti material, the operating temperature is 900-1200°C; Preferably, when the material of the grinding disc processing surface in the main processing is Cr material, the operating temperature is 1100-1400°C; Preferably, the main processing operation time is 1-10 minutes.
10. The wafer thinning method according to any one of claims 5 to 9, characterized in that: In the post-processing, the grinding disc and the wafer rotate in the same direction; Preferably, during the post-processing, a pressure of 3-10 psi, preferably 5-7 psi, is applied to the wafer in the axial direction; Preferably, the rotation speed of the grinding disc in the post-processing treatment is 100-300 r / min, preferably 120-150 r / min; Preferably, the rotation speed of the wafer in the post-processing treatment is 60-260 r / min, preferably 120-150 r / min; Preferably, in the post-processing, the rotation speed of the grinding disc is greater than the rotation speed of the wafer, and the rotation speed difference is 10-30 r / min; Preferably, the flow rate of the wetting liquid in the post-processing treatment is 200-800 mL / min, preferably 400-500 mL / min.
Citation Information
Patent Citations
Wafer thinning machine table and wafer thinning method
CN110416126A
Chemical-mechanical combined machining method for silicon carbide surface
CN114406825A
Metal millstone for stone grinding and polishing
CN210732136U
Chemical-mechanical polishing equipment having a multi-head
KR101678992B1
Cited By
Wafer cooling device and cooling method
CN119369264A