Method for preparing iron phosphate by recovering iron phosphate waste residues through mechanical alloying method
The graphite powder and impurities in the iron phosphate waste residue are separated by mechanical alloying method, which improves the leaching rate and purity of iron and phosphorus, solves the problems of high recycling cost and complicated process in the existing technology, and realizes efficient iron phosphate recycling.
Patent Information
- Application Number
- CN202410837751.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-26
- Publication Date
- 2024-10-08
AI Technical Summary
In the existing process of recycling ferric phosphate waste residue to prepare ferric phosphate, graphite powder impurities affect the leaching rate and purity of iron and phosphorus, increase the recycling cost, and require additional phosphorus sources. The process is complex and costly.
Mechanical alloying method is used through ball milling and water immersion steps to mix iron phosphate waste residue with control agent and sulfuric acid to generate iron-copper-aluminum ternary alloy, separate graphite powder and phosphate ions, reduce the amount of acid, and realize phosphoric acid under adjusted pH conditions The precipitation of iron avoids impurity doping and improves the leaching rate of iron and phosphorus.
It greatly increases the leaching rate of iron and phosphorus, reduces the amount of acid and recycling costs, avoids the need to supplement additional phosphorus sources, and achieves high-purity iron phosphate recovery. The leaching rate can reach 99%, reducing process complexity and costs.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of recycling waste lithium-ion batteries, and in particular to a method for preparing iron phosphate by recycling iron phosphate waste residues through a mechanical alloying method. Background Art
[0002] Lithium iron phosphate batteries are widely used due to their excellent safety performance, long cycle life and low cost. When the battery life ends, a large number of waste lithium-ion batteries will inevitably be generated. If they are not handled properly, they will have a negative impact on the environment. If they can be recycled, it will not only solve the problem of environmental pollution, but also generate economic benefits.
[0003] Since iron phosphate is an important precursor for preparing positive electrode materials for lithium iron phosphate batteries, the quality of iron phosphate products is related to the performance of lithium iron phosphate batteries, so the purity of iron phosphate is required to be high. However, the iron phosphate waste residue obtained during the recycling process of waste lithium iron phosphate batteries often contains impurities such as aluminum, copper and graphite powder. These impurities have a great impact on the extraction and preparation of iron phosphate. More graphite powder will affect the leaching rate of iron and phosphorus, and aluminum and copper impurities will affect the purity of iron phosphate.
[0004] Research has found that the existing process for recycling iron phosphate waste to prepare iron phosphate has the following shortcomings: a large amount of graphite powder remains in the iron phosphate waste, which will not only be mixed with the iron and phosphorus elements in the positive electrode powder, reducing the yield of Fe and P, but also consume more acid in the subsequent acid leaching process, increasing the recycling cost; more phosphorus will be lost during the magnetic separation process, requiring additional phosphorus source, and the process is complicated and the recycling cost is high. How to effectively solve the above problems will produce certain economic and social benefits for the recycling of iron phosphate waste. Summary of the invention
[0005] Based on the technical problems existing in the background technology, the present invention proposes a method for preparing iron phosphate by recycling iron phosphate waste residue by mechanical alloying method. The present invention adopts mechanical alloying to generate powder B, and effectively separates graphite powder from powder B and phosphate ions by the coordination of a control agent and sulfuric acid, and combines the water leaching step, thereby greatly reducing the amount of acid used and reducing the recovery cost; and avoiding the problem of graphite powder doped with iron and phosphorus and reducing the leaching rate, greatly improving the leaching rate of iron and phosphorus, and the leaching rate can reach 99%; in addition, no additional phosphorus source is required, further reducing the recovery cost. The present invention is simple to operate, and the equipment used is also conventional equipment, and no new equipment needs to be added, so industrial recovery can be achieved.
[0006] The invention provides a method for preparing ferric phosphate by recycling ferric phosphate waste residue by mechanical alloying method, comprising the following steps: taking ferric phosphate waste residue, a control agent and sulfuric acid, and performing ball milling to obtain material A; mixing material A and water, standing, and taking precipitation to obtain powder B; taking the remaining solution, separating the solid from the liquid, and taking the liquid to evaporate to obtain a phosphorus source; mixing the powder B and an acidic substance to obtain a pH value of 1.5-2, adding a phosphorus source, adjusting the iron-phosphorus ratio, reacting, separating the solid from the liquid, and taking the solid to dry to obtain ferric phosphate.
[0007] A large amount of graphite powder remains in the ferric phosphate waste residue, and the impurities include aluminum and copper, which will affect the purity of the recovered ferric sulfate. The present invention mixes the ferric phosphate waste residue with a control agent and sulfuric acid, and combines the process with low-temperature and high-energy ball milling. On the one hand, the iron, copper and aluminum in the ferric phosphate waste residue are diffused in a solid state to undergo mechanical alloying, and on the other hand, the graphite powder is made finer, which is beneficial to the separation by adding water later. At the same time, the control agent can prevent the iron, copper and aluminum elements from adhering to the surface of the graphite powder, accelerate the alloying rate of the three elements, and finally form an iron-copper-aluminum ternary alloy (i.e., powder B). The addition of sulfuric acid provides an acidic environment on the one hand, which can promote the formation of the iron-copper-aluminum ternary alloy, and on the other hand, it can make the graphite powder and the iron-copper-aluminum ternary alloy easier to separate. The control agent can also prevent the powder from agglomerating during the mechanical alloying process and prevent the problem of cold welding of the alloy.
[0008] Material A is stirred and mixed with water. After the stirring is completed, the powder B is easily and quickly precipitated to effectively separate it from the graphite, thereby avoiding the problem that the graphite powder is easily doped with iron and the iron leaching rate is reduced; the graphite powder is dispersed in the remaining solution, and the graphite powder can be effectively removed (the graphite powder can also be recycled) after solid-liquid separation treatment, thereby avoiding the problem that the graphite powder is easily doped with phosphorus and the phosphorus leaching rate is reduced. The liquid contains phosphate ions, and phosphate is obtained after evaporation and drying. The phosphate ions have less impurities and can be used as a phosphorus source to reduce the impurity content, and no additional phosphorus source needs to be supplemented, thereby reducing the recycling cost;
[0009] Through the cooperation of the above-mentioned processes, graphite powder can be effectively separated, the leaching rate of iron and phosphorus can be greatly improved, the amount of acid used can be greatly reduced, and the amount of acid used in subsequent steps can be reduced, thereby reducing the recovery cost;
[0010] Powder B is mixed with an acidic substance and a phosphorus source, and the pH is adjusted to 1.5-2; under this pH condition, iron phosphate is insoluble and precipitates, while copper phosphate and aluminum phosphate are still dissolved, so that the reaction proceeds to generate iron phosphate precipitation, thereby achieving effective separation of iron phosphate from copper and aluminum elements, recovering a large amount of high-purity dihydrate iron phosphate, and then drying to remove crystal water to obtain iron phosphate.
[0011] Preferably, the ball-to-material mass ratio is 1:10-20; more preferably 1:15-20.
[0012] Preferably, the diameter of the grinding balls is 5-7 mm and 9-11 mm.
[0013] Preferably, the weight ratio of the grinding balls with a diameter of 5-7 mm to the grinding balls with a diameter of 9-11 mm is 1:2-3.
[0014] Preferably, the grinding balls are made of agate.
[0015] The present invention selects appropriate ball-to-material ratio and grinding ball size to further promote the formation of mechanical alloying.
[0016] Preferably, the ball milling is performed simultaneously with ultrasonic treatment.
[0017] Preferably, the ultrasound frequency is 20-40 KHz.
[0018] Preferably, the ball milling temperature is -10 to -5°C, and the ball milling time is 40-60h.
[0019] During the ball milling, the temperature of the ball mill is controlled to be -10 to -5°C; during the ball milling process, the actual temperature of the ball milled material is about 10-20°C.
[0020] Performing ultrasonic treatment while ball milling and selecting appropriate ball milling parameters can further promote the formation of Fe-Cu-Al ternary alloy.
[0021] Preferably, the sulfuric acid is a 0.8-1.2 mol / l sulfuric acid aqueous solution.
[0022] Preferably, the sulfuric acid is 5-8 wt% of the weight of the ferric phosphate waste residue.
[0023] Preferably, the control agent is at least one of anhydrous ethanol, n-heptane and ethylene glycol.
[0024] Preferably, the controlling agent is 5-10 wt% of the weight of the ferric phosphate waste residue.
[0025] By selecting a control agent of appropriate weight and dosage and a suitable concentration of sulfuric acid, graphite powder can be separated from iron, copper and aluminum more easily, and can further promote the formation of the iron, copper and aluminum ternary alloy and improve the purity of the iron, copper and aluminum ternary alloy.
[0026] Preferably, the weight ratio of material A to water is 1:2.5-3.5.
[0027] Preferably, let stand for 25-35 seconds.
[0028] Preferably, the reaction temperature is 80-90°C and the reaction time is 2-4h.
[0029] Preferably, the iron to phosphorus ratio is 1:0.96-0.98.
[0030] The above iron-to-phosphorus ratio refers to the molar ratio of iron to phosphorus.
[0031] Preferably, the acidic substance is at least one of sulfuric acid and phosphoric acid.
[0032] The recovery of ferric sulfate can be further increased by selecting appropriate reaction temperature and dosage of each substance.
[0033] The above-mentioned waste iron phosphate residue may be waste iron phosphate residue after lithium is removed, etc.
[0034] Beneficial effects:
[0035] The present invention adopts mechanical alloying to generate an iron-copper-aluminum ternary alloy (i.e., powder B), and effectively separates graphite powder from powder B and phosphate ions by combining a control agent and sulfuric acid and a water immersion step, thereby greatly reducing the amount of acid used and reducing the recycling cost; and avoids the problem of graphite powder being doped with iron and phosphorus, which leads to a reduced leaching rate; greatly improves the leaching rate of iron and phosphorus, and the leaching rate can reach 99%; in addition, no additional phosphorus source needs to be added, further reducing the recycling cost. The present invention is simple to operate, and the equipment used is also conventional equipment, and no new equipment needs to be added, so that industrial recycling can be achieved. DETAILED DESCRIPTION
[0036] The technical solution of the present invention is described in detail below through specific embodiments.
[0037] Example 1
[0038] A method for preparing iron phosphate by recycling iron phosphate waste residue by mechanical alloying method comprises the following steps: adding 20g of dried iron phosphate waste residue to a planetary ball mill, and then adding agate grinding balls so that the ball-to-material mass ratio is 1:10, wherein the grinding balls have diameters of 6mm and 10mm; the weight ratio of the grinding balls with a diameter of 6mm to the grinding balls with a diameter of 10mm is 1:3;
[0039] Then add 1g of the control agent and 1g of a 1.2mol / l sulfuric acid aqueous solution, start the ball mill and ultrasonic assistance, adjust the ultrasonic frequency to 40KHz, control the ball mill temperature to -10 to -5°C, and the actual temperature of the ball milled material during the ball milling process is about 10-20°C. Ball milling treatment for 40h to obtain material A;
[0040] Mix 10g of material A with 30g of water, stir for 1h to mix, let stand for 30s, take the precipitate, wash with water, and dry to obtain powder B; take the remaining solution and filter, the filter cake contains graphite powder which can be recycled, take the filtrate and concentrate and evaporate to dryness to obtain the phosphorus source;
[0041] Add 5 g of powder B to a sulfuric acid aqueous solution, adjust the pH to 1.5, then heat to 90°C, add a phosphorus source, adjust the iron-phosphorus ratio to 1:0.96, stir and react for 2 h, filter, take the solid and wash with water to obtain ferric phosphate dihydrate, and then dry at 300°C to remove crystal water to obtain ferric phosphate.
[0042] Example 2
[0043] A method for preparing iron phosphate by recycling iron phosphate waste residue by mechanical alloying method comprises the following steps: adding 20g of dried iron phosphate waste residue to a planetary ball mill, and then adding agate grinding balls so that the ball-to-material mass ratio is 1:20, wherein the grinding balls have diameters of 6mm and 10mm; the weight ratio of the grinding balls with a diameter of 6mm to the grinding balls with a diameter of 10mm is 1:2;
[0044] Then, 2 g of the control agent and 1.6 g of a 0.8 mol / l sulfuric acid aqueous solution were added, the ball mill and ultrasonic assistance were turned on, the ultrasonic frequency was adjusted to 20 KHz, the temperature of the ball mill was controlled to be -10 to -5 °C, the actual temperature of the ball milled material during the ball milling process was about 10-20 °C, and the ball milling treatment was performed for 60 hours to obtain material A;
[0045] Mix 10g of material A with 35g of water, stir for 0.5h to mix, let stand for 35s, take the precipitate, wash with water, and dry to obtain powder B; take the remaining solution and filter, the filter cake contains graphite powder which can be recycled, take the filtrate and concentrate and evaporate to dryness to obtain the phosphorus source;
[0046] Add 5 g of powder B to a sulfuric acid aqueous solution, adjust the pH to 2, then heat to 80°C, add a phosphorus source, adjust the iron-phosphorus ratio to 1:0.98, stir and react for 4 hours, filter, take the solid and wash with water to obtain ferric phosphate dihydrate, and then dry at 300°C to remove crystal water to obtain ferric phosphate.
[0047] Example 3
[0048] A method for preparing iron phosphate by recycling iron phosphate waste residue by mechanical alloying method comprises the following steps: adding 20g of dried iron phosphate waste residue to a planetary ball mill, and then adding agate grinding balls so that the ball-to-material mass ratio is 1:15, wherein the grinding balls have diameters of 6mm and 10mm; the weight ratio of the grinding balls with a diameter of 6mm to the grinding balls with a diameter of 10mm is 1:2.5;
[0049] Then, 1.5 g of a control agent and 1.4 g of a 1.0 mol / l sulfuric acid aqueous solution were added, the ball mill and ultrasonic assistance were turned on, the ultrasonic frequency was adjusted to 30 KHz, the temperature of the ball mill was controlled to be -10 to -5 °C, the actual temperature of the ball milled material during the ball milling process was about 10-20 °C, and the ball milling process was performed for 50 hours to obtain material A;
[0050] Mix 10g of material A with 25g of water, stir for 1.5h to mix, let stand for 25s, take the precipitate, wash with water, and dry to obtain powder B; take the remaining solution and filter, the filter cake contains graphite powder which can be recycled, take the filtrate and concentrate and evaporate to dryness to obtain the phosphorus source;
[0051] Add 5 g of powder B to a sulfuric acid aqueous solution, adjust the pH to 1.7, then heat to 85°C, add a phosphorus source, adjust the iron-phosphorus ratio to 1:0.97, stir and react for 3 hours, filter, take the solid and wash with water to obtain ferric phosphate dihydrate, and then dry at 300°C to remove the crystal water to obtain ferric phosphate.
[0052] Comparative Example 1
[0053] During ball milling, no sulfuric acid aqueous solution was added, and the rest was the same as in Example 3.
[0054] Comparative Example 2
[0055] During ball milling, no controlling agent and sulfuric acid aqueous solution were added, and the rest was the same as in Example 3.
[0056] Comparative Example 3
[0057] pH=2.5, other conditions are the same as those in Example 3.
[0058] Comparative Example 4
[0059] pH=1.0, other conditions are the same as those in Example 3.
[0060] Comparative Example 5
[0061] The diameter of the grinding ball is 10 mm, and the rest is the same as in Example 3.
[0062] Comparative Example 6
[0063] The diameter of the grinding ball is 6 mm, and the rest is the same as in Example 3.
[0064] The iron phosphate waste residues used in the above examples 1-3 and comparative examples 1-6 are from the same batch, the iron and phosphorus contents in the iron phosphate waste residues are detected, the total amount of iron phosphate obtained in each group is counted, and the leaching rate and recovery rate of phosphorus and iron are calculated. The results are shown in Table 1.
[0065] Leaching rate = X / weight of elements in ferric phosphate waste residue*100%, wherein X is the weight of iron in powder B or the weight of phosphorus in the remaining solution.
[0066] Recovery rate = weight of the final ferric phosphate obtained / weight of the ferric phosphate in the ferric phosphate waste residue*100%.
[0067] Table 1 Test results
[0068]
[0069]
[0070] By comparing Example 3 with Comparative Examples 1-2, it can be seen that the control agent and the aqueous sulfuric acid solution are matched with each other in an appropriate ratio, so that the present invention can have good iron and phosphorus leaching rates and a high recovery rate of iron phosphate.
[0071] By comparing Examples 1-3 and Comparative Examples 3-4, it can be seen that adjusting the appropriate pH value can increase the leaching rate of iron and phosphorus, reduce the impurity content, and increase the recovery rate of iron phosphate.
[0072] Comparison of Example 3 and Comparative Examples 5-6 shows that setting a suitable ball milling method can improve the leaching rate of iron and phosphorus and improve the recovery rate of iron phosphate.
[0073] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
Claims
1. A method for preparing ferric phosphate by recycling ferric phosphate waste residue by mechanical alloying, characterized in that: The method comprises the following steps: taking ferric phosphate waste residue, a control agent and sulfuric acid, and ball-milling to obtain material A; mixing material A and water, standing, and taking a precipitate to obtain powder B; taking the remaining solution, separating the solid from the liquid, and evaporating the liquid to obtain a phosphorus source; mixing the powder B and an acidic substance to obtain a pH value of 1.5-2, adding a phosphorus source, adjusting the iron-phosphorus ratio, reacting, separating the solid from the liquid, and taking the solid to dry to obtain ferric phosphate.
2. The method for preparing ferric phosphate by recycling ferric phosphate waste slag by mechanical alloying method according to claim 1, characterized in that: The ball-to-material mass ratio is 1:10-20; preferably, the diameters of the grinding balls are 5-7mm and 9-11mm; preferably, the weight ratio of grinding balls with a diameter of 5-7mm and grinding balls with a diameter of 9-11mm is 1:2-3; preferably, the grinding balls are made of agate.
3. The method for preparing ferric phosphate by recycling ferric phosphate waste residue by mechanical alloying method according to claim 1 or 2, characterized in that: Ultrasonic treatment is performed while ball milling; preferably, the ultrasonic frequency is 20-40 KHz.
4. The method for preparing ferric phosphate by recycling ferric phosphate waste slag by mechanical alloying method according to any one of claims 1 to 3, characterized in that: The ball milling temperature is -10 to -5°C, and the ball milling time is 40-60h.
5. The method for preparing ferric phosphate by recycling ferric phosphate waste slag by mechanical alloying method according to any one of claims 1 to 4, characterized in that: The sulfuric acid is a 0.8-1.2 mol / l sulfuric acid aqueous solution; preferably, the sulfuric acid is 5-8 wt % of the weight of the ferric phosphate waste residue.
6. The method for preparing ferric phosphate by recycling ferric phosphate waste slag by mechanical alloying method according to any one of claims 1 to 5, characterized in that: The controlling agent is at least one of anhydrous ethanol, n-heptane and ethylene glycol; preferably, the controlling agent is 5-10wt% of the weight of the ferric phosphate waste residue.
7. The method for preparing ferric phosphate by recycling ferric phosphate waste slag by mechanical alloying method according to any one of claims 1 to 6, characterized in that: The weight ratio of material A to water is 1:2.5-3.5; preferably, the mixture is allowed to stand for 25-35 seconds.
8. The method for preparing ferric phosphate by recycling ferric phosphate waste residue by mechanical alloying method according to any one of claims 1 to 7, characterized in that: The reaction temperature is 80-90°C and the reaction time is 2-4h.
9. The method for preparing ferric phosphate by recycling ferric phosphate waste residue by mechanical alloying method according to any one of claims 1 to 8, characterized in that: The iron-phosphorus ratio is 1:0.96-0.
98.
10. The method for preparing ferric phosphate by recycling ferric phosphate waste residue by mechanical alloying method according to any one of claims 1 to 9, characterized in that: The acidic substance is at least one of sulfuric acid and phosphoric acid.