Preparation method of special precipitated silicon dioxide for rice milling rubber roller

By adopting the silica synthesis method under specific conditions in the production of rice milling rubber rollers, the problems of insufficient hardness and wear resistance are solved, high oil absorption value and reinforcement performance are improved, ensuring the processing performance and performance of the rubber rollers. Security of the production environment.

CN118744992APending Publication Date: 2024-10-08ANHUI QUECHEN SILICON CHEM CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410742442.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-11
Publication Date
2024-10-08

AI Technical Summary

Technical Problem

The silica produced by the existing technology has low hardness and average wear resistance after being made into rubber. It is difficult to balance high specific surface area and high oil absorption value, resulting in high manufacturing costs and unstable quality of the product, which cannot fully reflect the reinforcing performance.

Method used

Silica is synthesized by using solid sodium silicate with a modulus of 3.0 to 3.5, 25 to 35 wt% sulfuric acid solution and solid potassium chloride under specific stirring and heating conditions, and then pressed through filtration, beating and colloid mill grinding. Type spray drying, control the BET/CTAB ratio between 1.0 and 1.02 to ensure high oil absorption and structure.

Benefits of technology

The prepared silica has high BET and CTAB values, high structure, better reinforcement effect, and smooth processing performance. The rubber roller product has appropriate hardness and excellent wear resistance, and the production process has no flying dust and a better environment. For comfort and the environment.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a preparation method of special precipitated silicon dioxide for a rice milling rubber roller, and relates to the technical field of rice milling rubber rollers, and the preparation method specifically comprises the following steps: (1) selecting solid sodium silicate with modulus of 3.0-3.5, preparing a sodium silicate solution with concentration of 20-25wt%, preparing a certain volume of sulfuric acid solution with concentration of 25-35wt%, and preparing potassium chloride for later use; (2) adding the prepared sodium silicate solution into the reaction kettle, and adding potassium chloride at the stirring speed of 70-110r / min until sodium silicate is completely dissolved; the silicon dioxide prepared by the preparation method has high BET and CTAB values, the ratio of BET to CTAB is 1.0-1.02, the silicon dioxide has high oil absorption value, high structural degree and better reinforcing effect, potassium chloride is selected as a reaction structure control agent, and high reinforcing performance and good dispersity of the silicon dioxide product are guaranteed.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of rice milling rubber rollers, in particular to a method for preparing precipitated silicon dioxide special for rice milling rubber rollers. Background Art

[0002] Silica is an acidic oxide, and its corresponding hydrate is silicic acid (H2S iO3). The most common form of silica in nature is quartz. The raw materials for precipitated silica in industry are generally sodium silicate and sulfuric acid. The products are widely used in tires, shoes, silicone rubber, feed, coatings, toothpaste and other industries, especially in rubber as an important reinforcing material.

[0003] Rice processing is the process of removing the rice husk (husk) and cortex (bran layer) with the purpose of separating the endosperm from other parts with the minimum degree of crushing to produce rice with better edible quality. Rice processing is divided into three steps: cleaning, husking and milling. The working principle of the rice mill is that two rubber rollers rotate at opposite speeds to squeeze, tear and peel the rice between the two rollers, so as to achieve the effect of husking and making rice. Therefore, higher requirements are placed on the physical and mechanical properties of the rubber rollers, such as elongation at break, hardness, elasticity, etc. Silica, as a filling and reinforcing agent, can well improve the strength and wear resistance of the rice milling rubber rollers.

[0004] The shortcomings of the prior art are that after the silica produced by the prior art is made into rubber, most of them have low hardness and average wear resistance, and the high reinforcement performance of silica is not fully reflected; and although some silica has the characteristics of high reinforcement and high wear resistance, it is slow to eat, difficult to disperse, and has poor processing performance during rubber processing, resulting in high product manufacturing costs, unstable quality, and unable to take into account the characteristics of high specific surface area and high oil absorption value. Therefore, those skilled in the art provide a method for preparing precipitated silica for rice milling rubber rollers to solve the problems raised in the above background technology. Summary of the invention

[0005] The purpose of the present invention is to provide a method for preparing precipitated silica specifically for rice milling rubber rollers, so as to solve the problems raised in the above-mentioned background technology.

[0006] To achieve the above object, the present invention provides the following technical solution: a method for preparing precipitated silica for rice milling rubber rollers, which specifically comprises the following steps:

[0007] (1): Select solid sodium silicate with a modulus of 3.0 to 3.5, prepare a sodium silicate solution with a concentration of 20 to 25 wt%, prepare a certain volume of sulfuric acid solution with a concentration of 25 to 35 wt%, and prepare potassium chloride for standby use;

[0008] (2): Add the prepared sodium silicate solution into the reaction kettle, and add potassium chloride at a stirring speed of 70 to 110 r / min until the sodium silicate is completely dissolved;

[0009] (3): Keep the stirring speed unchanged, raise the temperature of the reaction system to 70-100°C, add the prepared sulfuric acid solution until the pH value of the reaction system reaches 9.0-11.0, stop adding the sulfuric acid solution and stop stirring, and age the reaction solution for 80-120 minutes;

[0010] (4): After the aging is completed, stirring is continued at the same speed, and sulfuric acid solution is added. When the pH value of the reaction system is between 6.0 and 7.5, the addition of sulfuric acid solution is stopped, and the synthesis reaction is carried out under stirring. After the reaction is completed, a silicon dioxide slurry is obtained;

[0011] (5): After the above-mentioned silica slurry is filtered and beaten, it is ground by a colloid mill and then sent to a thick slurry tank, and then pumped to a pressure spray dryer for drying to obtain finished silica.

[0012] As a further solution of the present invention: the potassium chloride is solid potassium chloride, and the addition amount of solid potassium chloride is 0.5% of the mass of silicon dioxide.

[0013] As a further solution of the present invention: the reaction time of the synthesis reaction is 120 to 200 minutes.

[0014] As a further solution of the present invention: the BET / CTAB ratio of the silicon dioxide is 1.0 to 1.02.

[0015] As a further solution of the present invention: the silicon dioxide BET is 215-255m 2 / g.

[0016] As a further solution of the present invention: the silicon dioxide CTAB is 210-250m 2 / g.

[0017] As a further solution of the present invention: the bulk density of the silicon dioxide is 250 to 320 g / L.

[0018] As a further solution of the present invention: the oil absorption value of the silica is 200-300 mL / 100 g.

[0019] As a further solution of the present invention: the median diameter (D50) of the silica is 200 to 300 um.

[0020] As a further solution of the present invention: the 45um water-washed residue of the silicon dioxide is less than 0.1%.

[0021] Compared with the prior art, the present invention has the following beneficial effects:

[0022] 1. The silicon dioxide prepared by the preparation method of the present invention has high BET and CTAB values, and the BET / CTAB ratio is between 1.0 and 1.02.

[0023] 2. The silicon dioxide prepared by the preparation method of the present invention has a higher oil absorption value, a high structural degree and a better reinforcement effect.

[0024] 3. The preparation method of the present invention uses potassium chloride as a reaction structure controller, which ensures high reinforcement performance and good dispersibility of the silicon dioxide product, and has smooth processing performance during the rubber processing, which not only gives the rubber roller product suitable hardness and excellent wear resistance, but also ensures good processing performance of the rubber roller.

[0025] 4. The preparation method of the present invention adopts coarse granular silicon dioxide obtained by pressure spray drying, which has no dust flying and leakage loss during production and use, which not only ensures the accuracy of the rubber formula, but also makes the production environment more comfortable and environmentally friendly. DETAILED DESCRIPTION

[0026] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0027] In the embodiment of the present invention,

[0028] Example 1

[0029] A method for preparing precipitated silica for rice milling rubber rollers, comprising the following steps:

[0030] (1): solid sodium silicate with a modulus of 3.0 is selected to prepare a sodium silicate solution with a concentration of 20 wt%, a certain volume of sulfuric acid solution with a concentration of 25 wt%, and potassium chloride is prepared for standby use, wherein the potassium chloride is solid potassium chloride, and the amount of solid potassium chloride added is 0.5% of the mass of silicon dioxide;

[0031] (2): Add the prepared sodium silicate solution into the reactor, and add potassium chloride at a stirring speed of 70 r / min until the sodium silicate is completely dissolved;

[0032] (3): Keep stirring at the same speed, raise the temperature of the reaction system to 70°C, add the prepared sulfuric acid solution, and stop adding the sulfuric acid solution and stirring when the pH value of the reaction system reaches 9.0. The reaction solution is aged for 80 minutes.

[0033] (4): After the aging is completed, stirring is continued at the same speed, and sulfuric acid solution is added. When the pH value of the reaction system is 6.0, the addition of sulfuric acid solution is stopped, and the synthesis reaction is carried out under stirring. The reaction time of the synthesis reaction is 120 minutes. After the reaction is completed, a silica slurry is obtained;

[0034] (5): After the above-mentioned silica slurry is filtered and beaten, it is ground by a colloid mill and then sent to a thick slurry tank, and then pumped to a pressure spray dryer for drying to obtain finished silica.

[0035] Example 2

[0036] A method for preparing precipitated silica for rice milling rubber rollers, comprising the following steps:

[0037] (1): solid sodium silicate with a modulus of 3.5 is selected to prepare a sodium silicate solution with a concentration of 25wt%, a certain volume of sulfuric acid solution with a concentration of 35wt%, and potassium chloride is prepared for standby use, wherein the potassium chloride is solid potassium chloride, and the amount of solid potassium chloride added is 0.5% of the mass of silicon dioxide;

[0038] (2): Add the prepared sodium silicate solution into the reactor, and add potassium chloride at a stirring speed of 110 r / min until the sodium silicate is completely dissolved;

[0039] (3): Keep stirring at the same speed, raise the temperature of the reaction system to 100°C, add the prepared sulfuric acid solution, and when the pH value of the reaction system reaches 11.0, stop adding the sulfuric acid solution and stop stirring, and age the reaction solution for 120 minutes;

[0040] (4): After the aging is completed, stirring is continued at the same speed, and sulfuric acid solution is added. When the pH value of the reaction system reaches 7.5, the addition of sulfuric acid solution is stopped, and a synthesis reaction is carried out under stirring. The reaction time of the synthesis reaction is 200 minutes. After the reaction is completed, a silicon dioxide slurry is obtained;

[0041] (5): After the above-mentioned silica slurry is filtered and beaten, it is ground by a colloid mill and then sent to a thick slurry tank, and then pumped to a pressure spray dryer for drying to obtain finished silica.

[0042] Example 3

[0043] A method for preparing precipitated silica for rice milling rubber rollers, comprising the following steps:

[0044] (1): solid sodium silicate with a modulus of 3.2 is selected to prepare a sodium silicate solution with a concentration of 23 wt%, a certain volume of sulfuric acid solution with a concentration of 30 wt%, and potassium chloride is prepared for standby use, wherein the potassium chloride is solid potassium chloride, and the amount of solid potassium chloride added is 0.5% of the mass of silicon dioxide;

[0045] (2): Add the prepared sodium silicate solution into the reactor, and add potassium chloride at a stirring speed of 90 r / min until the sodium silicate is completely dissolved;

[0046] (3): Keep stirring at the same speed, raise the temperature of the reaction system to 85°C, add the prepared sulfuric acid solution, and stop adding the sulfuric acid solution and stirring when the pH value of the reaction system reaches 10.0. The reaction solution is aged for 100 minutes;

[0047] (4): After the aging is completed, stirring is continued at the same speed, and sulfuric acid solution is added. When the pH value of the reaction system reaches 7, the addition of sulfuric acid solution is stopped, and a synthesis reaction is carried out under stirring. The reaction time of the synthesis reaction is 160 minutes. After the reaction is completed, a silica slurry is obtained;

[0048] (5): After the above-mentioned silica slurry is filtered and beaten, it is ground by a colloid mill and then sent to a thick slurry tank, and then pumped to a pressure spray dryer for drying to obtain finished silica.

[0049] The products obtained in the above examples 1-3 were tested for performance. The test results showed that the BET / CTAB ratio of the finished silica of the present invention was 1.0 to 1.02, and the BET was 215 to 3.

[0050] 255m 2 / g, CTAB is 210~250m 2 / g, bulk density is 250-320g / L, oil absorption value is 200-300mL / 100g, median diameter (D50) is 200-300um, 45um water washing residue is <0.1%, pH (5% aqueous solution) is 6.0-7.5, and silicon dioxide content (burning product) is ≥95%.

[0051] In summary, the silica prepared by the preparation method of the present invention has high BET and CTAB values, and the BET / CTAB ratio is between 1.0 and 1.02, has a higher oil absorption value, a high structural degree, and a better reinforcement effect. In addition, the present invention uses potassium chloride as a reaction structure controller to ensure the high reinforcement performance and good dispersibility of the silica product, and has smooth processing performance during the rubber processing process, which not only gives the rubber roller product suitable hardness and excellent wear resistance, but also ensures good processing performance of the rubber roller.

[0052] It will be apparent to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above and that the present invention can be implemented in other specific forms without departing from the spirit or essential features of the present invention. Therefore, the embodiments should be considered exemplary and non-restrictive in all respects, and the scope of the present invention is defined by the appended claims rather than the above description, and it is intended that all changes falling within the meaning and scope of the equivalent elements of the claims be included in the present invention.

[0053] In addition, it should be understood that although the present specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.

Claims

1. A method for preparing precipitated silica for rice milling rubber rollers, characterized in that: The specific steps include: (1): Select solid sodium silicate with a modulus of 3.0 to 3.5, prepare a sodium silicate solution with a concentration of 20 to 25 wt%, prepare a certain volume of sulfuric acid solution with a concentration of 25 to 35 wt%, and prepare potassium chloride for standby use; (2): Add the prepared sodium silicate solution into the reaction kettle, and add potassium chloride at a stirring speed of 70 to 110 r / min until the sodium silicate is completely dissolved; (3): Keep the stirring speed unchanged, raise the temperature of the reaction system to 70-100°C, add the prepared sulfuric acid solution until the pH value of the reaction system reaches 9.0-11.0, stop adding the sulfuric acid solution and stop stirring, and age the reaction solution for 80-120 minutes; (4): After the aging is completed, stirring is continued at the same speed, and sulfuric acid solution is added. When the pH value of the reaction system is between 6.0 and 7.5, the addition of sulfuric acid solution is stopped, and the synthesis reaction is carried out under stirring. After the reaction is completed, a silicon dioxide slurry is obtained; (5): After the above-mentioned silica slurry is filtered and beaten, it is ground by a colloid mill and then sent to a thick slurry tank, and then pumped to a pressure spray dryer for drying to obtain finished silica.

2. The method for preparing precipitated silica for rice milling rubber roller according to claim 1, characterized in that: The potassium chloride is solid potassium chloride, and the addition amount of the solid potassium chloride is 0.5% of the mass of silicon dioxide.

3. The method for preparing precipitated silica for rice milling rubber roller according to claim 1, characterized in that: The reaction time of the synthesis reaction is 120 to 200 minutes.

4. The method for preparing precipitated silica for rice milling rubber roller according to claim 1, characterized in that: The BET / CTAB ratio of the silicon dioxide is 1.0 to 1.

02.

5. The method for preparing precipitated silica for rice milling rubber roller according to claim 1, characterized in that: The silicon dioxide BET is 215 to 255 m 2 / g.

6. The method for preparing precipitated silica for rice milling rubber roller according to claim 1, characterized in that: The silicon dioxide CTAB is 210 to 250 m 2 / g.

7. The method for preparing precipitated silica for rice milling rubber roller according to claim 1, characterized in that: The bulk density of the silicon dioxide is 250-320 g / L.

8. The method for preparing precipitated silica for rice milling rubber roller according to claim 1, characterized in that: The silica oil absorption value is 200-300 mL / 100 g.

9. The method for preparing precipitated silica for rice milling rubber roller according to claim 1, characterized in that: The median diameter (D50) of the silicon dioxide is 200 to 300 um.

10. The method for preparing precipitated silica for rice milling rubber roller according to claim 1, characterized in that: The 45 um water-washed sieve residue of the silicon dioxide is less than 0.1%.

Citation Information

Patent Citations

  • Method for controlling gel amount in white carbon black by using precipitation method

    CN102408115A

  • Silicon dioxide for reinforcing rice milling rubber roller and preparation process of silicon dioxide

    CN112850720A

  • Process for preparing nm silicon dioxide from alkali metal silicate

    CN1524785A

  • Highly dispersible silica for using in rubber

    WO2004065299A1