Synthetic method for dispersing MoO2 nanoparticles on MoO2 nanosheets

MoO2 nanoparticles are precipitated in situ on MoO2 nanosheets through a one-step reduction reaction method, which solves the problems of complex high-temperature processes and agglomeration of nanomaterials in the existing technology, and achieves uniform dispersion and high activity of MoO2 nanomaterials, which is suitable for catalysis and battery fields. application.

CN118745002APending Publication Date: 2024-10-08CHINA THREE GORGES UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410747188.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-11
Publication Date
2024-10-08

AI Technical Summary

Technical Problem

The existing preparation process of MoO2 nanomaterials requires high-temperature synthesis, which is complex and costly. Moreover, the prepared nanomaterials are easy to agglomerate, which reduces the surface area and activity, limiting its application in the fields of catalysis and batteries.

Method used

A one-step reduction reaction method is used to precipitate MoO2 nanoparticles in situ on MoO2 nanosheets. By controlling the relative content of sodium hypophosphite and MoO3-x and the heat treatment process, the uniform dispersion of MoO2 nanoparticles is achieved, avoiding high-temperature processes and the use of toxic and harmful substances.

Benefits of technology

It achieves uniform dispersion of MoO2 nanoparticles and exposure of highly active sites, improves material dispersion and charge transfer channels, reduces process costs and equipment requirements, is suitable for industrial production, and significantly improves the performance of catalytic and battery materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118745002A_ABST
    Figure CN118745002A_ABST
Patent Text Reader

Abstract

The invention discloses a synthesis method for dispersing MoO2 nanoparticles on a MoO2 nanosheet, and belongs to the field of nano material preparation. According to the preparation method, a one-step low-temperature thermal reduction technology is adopted, and MoO < 3-x > nanosheets containing oxygen defects and sodium hypophosphite are subjected to thermal treatment in inert gas (argon and nitrogen), so that the material with MoO < 2 > nanoparticles dispersed on the nanosheets is obtained. The MoO2 nano material is prepared by adopting a one-step method, sodium hypophosphite is used as a reducing agent, and compared with an existing high-temperature heat treatment method, the method is simple, economical, environmentally friendly and suitable for batch production. Meanwhile, according to the obtained MoO2 nanoparticles, MoO2 nanoparticles are dispersed and distributed on the surface of the MoO2 nanosheet, and the nanoparticles have good dispersity and large specific surface area and have good application prospects in the fields of batteries, photocatalysis and electro-catalysis.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a synthesis method of MoO2 nanoparticles dispersed on MoO2 nanosheets, belonging to the field of nano material preparation. Background Art

[0002] Molybdenum dioxide (MoO2) is a typical transition metal oxide with a rutile structure, unique plasmon LSPR characteristics and metallic properties. 6 m -1 300 K), high melting point, corrosion resistance and other characteristics make it show good performance in the fields of light, electrocatalysis, batteries, etc. Studies have found that the edges of Mo atoms and O atoms are both catalytic active sites. However, the current preparation process of MoO2 nanomaterials usually requires high-temperature synthesis, which is complex, harsh, low in economic benefits, high in cost, and the MoO2 nanomaterials prepared under high temperature conditions are easy to agglomerate, which reduces the surface area and activity, limiting its application. In order to solve the agglomeration problem of MoO2 nanomaterials and obtain high activity, it is key to construct MoO2 nanoparticles with good dispersion. At the same time, two-dimensional nanosheet structure materials are widely used in energy storage and conversion because of their advantages such as fast electron transmission channels, more active sites and reduced agglomeration. Evenly dispersing MoO2 nanoparticles on the surface of the two-dimensional nanosheet structure can, on the one hand, improve the dispersibility of MoO2 nanoparticles and expose more active sites of the nanomaterials; on the other hand, the two-dimensional nanosheet structure can stabilize the MoO2 nanoparticles and improve the fast channel of charge transfer. Therefore, synthesizing a two-dimensional nanosheet structure with dispersed distribution of MoO2 nanoparticles is of great significance for the development of efficient and stable catalysts and battery materials. Summary of the invention

[0003] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a method for preparing MoO2 nanoparticles dispersed in MoO2 nanosheets. The method can achieve the preparation of MoO2 nanoparticles dispersed in MoO2 nanosheet materials through a simple one-step reduction reaction method without the need for high-temperature processes and the use of toxic and hazardous substances.

[0004] The MoO2 nanoparticles prepared by the present invention are in-situ precipitated from the MoO2 nanosheets, and there is a strong interface contact between the two. The MoO2 nanoparticles are evenly dispersed in the MoO2 nanosheets, and the relative content of the two can be adjusted by changing the sodium hypophosphite and MoO 3-x The relative content and heat treatment process are controlled.

[0005] A method for preparing a material in which MoO2 nanoparticles are dispersed on MoO2 nanosheets adopts a one-step reduction method, comprising the following steps: A certain amount of MoO rich in oxygen defects 3-x The nanosheets and sodium hypophosphite are placed in a tubular furnace filled with inert gas according to proportion and position, with the sodium hypophosphite located above the gas, and then heated and reduced to obtain MoO2 nanomaterials.

[0006] Preferably, the MoO 3-x The nanosheets are rich in oxygen vacancies, and the content of oxygen vacancies is 10%~30%.

[0007] Preferably, the MoO 3-x The mass ratio with sodium hypophosphite is 1:2~1:10.

[0008] Preferably, the sodium hypophosphite is located 2-5 cm from the inlet of the inert gas.

[0009] Preferably, the oxygen-deficient MoO 3-x The nanosheets were located at the outlet of the inert gas, 1 to 5 cm away from the sodium hypophosphite.

[0010] Preferably, the heating rate is 1-5° / min, the heat treatment temperature is 200°C-500°C, and the reaction time is 1-4h.

[0011] The MoO2 nanoparticles prepared by the present invention are dispersed on the MoO2 nanosheets, and compared with the prior art, the beneficial effects are: The activity of MoO2 nanosheets can be determined by the size of the MoO 3-x The oxygen defect content in the nanosheet is regulated, and the obtained material has both nanoparticle and nanosheet morphology. The nanoparticles are dispersed on the surface of the nanosheet, and there is a close contact interface structure between the two. The nanoparticles are small in size and evenly distributed. The adopted process is simple, low in cost, low in equipment requirements, and easy to realize industrialization. The nanoparticles obtained by the present invention have many active sites and strong interface contact, and have great advantages in the fields of catalysis and batteries. BRIEF DESCRIPTION OF THE DRAWINGS

[0012] Figure 1 : XRD spectrum of the material of MoO2 nanoparticles dispersed on MoO2 nanosheets prepared in Example 1.

[0013] Figure 2 : Transmission electron microscope image of the material of MoO2 nanoparticles dispersed on MoO2 nanosheets prepared in Example 1.

[0014] Figure 3 : The photocatalytic hydrogen production effect when the MoO2 nanoparticles prepared in Example 1 are dispersed on MoO2 nanosheets and used as a co-catalyst. DETAILED DESCRIPTION

[0015] The present invention is further explained below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not used to limit the scope of the present invention. After reading the present invention, various equivalent forms of modifications to the present invention by those skilled in the art all fall within the scope defined by the claims attached to this application.

[0016] Example 1 Weigh 2 mmol Mo powder in a beaker, add 24 mL of anhydrous ethanol and stir, then add 11 mL of 30% H2O2 dropwise and stir for 30 min to obtain a yellow transparent solution, finally transfer to a 50 mL polytetrafluoroethylene high temperature and high pressure reactor, react in a 160 ° C oven for 12 h, cool to room temperature, centrifuge and wash with anhydrous ethanol and deionized water, and finally place in a 60 ° C vacuum drying oven overnight to obtain MoO 3-x .

[0017] Take 0.1 g MoO with an oxygen vacancy content of 27% 3-x Place it in an ark and place it in the middle of the Ar tube furnace; then place 0.5 g of sodium hypophosphite in another ark and place it upstream of MoO 3-x The ark is 1 cm. Then the temperature is raised to 350℃ at a heating rate of 3℃ / min and kept for 2 hours, and then naturally cooled to room temperature to obtain a material in which MoO2 nanoparticles are dispersed on MoO2 nanosheets. The XRD diffraction pattern of the obtained nanomaterial is shown in Figure 1 As shown, the product is pure MoO2 material. The transmission electron microscope image of MoO2 nanomaterial is shown in Figure 2 As shown, the nanoparticles are evenly distributed on the surface of the nanosheets. The size of MoO2 nanoparticles is about 100 nm, and the width and thickness of MoO2 nanosheets are about 500 nm and 100 nm, respectively. Figure 3 This is a HRTEM photo obtained by high-resolution observation of the nanosheet, where obvious lattice fringes can be seen.

[0018] The MoO2 nanoparticles of this embodiment were used as a co-catalyst to improve the photocatalytic activity of ZnIn2S4 nanoflowers: 3 mmol ZnCl2, 3 mmol InCl3 and 1.2 mmol thioacetamide were weighed and dissolved in 50 mL deionized water. After fully dissolved, a certain amount of MoO2 was added and stirred for 30 min, and then transferred to an 80°C water bath for reaction for 4 h. After the reaction was completed, the mixture was washed with anhydrous ethanol and deionized water 3 times each, and the obtained product was placed in a 60°C vacuum drying oven, dried for 12 h and collected to obtain a MoO2 / ZnIn2S4 photocatalytic composite material.

[0019] 20 mg of the photocatalytic composite was dispersed in 80 ml of a solution containing lactic acid (8 ml) and water (72 ml). A xenon lamp (MC-XF300) was used as a visible light source (λ ≥ 420 nm) to illuminate the reactor horizontally. Before illumination, the reactor was evacuated and a circulating cooling system was used to keep the temperature stable (7 °C) during illumination. The generated hydrogen was detected by gas chromatography every 1 h using Ar as a carrier gas.

[0020] Figure 3 This is a diagram of the photocatalytic hydrogen production effect obtained in the experiment of the MoO2 / ZnIn2S4 photocatalytic composite materials with different mass ratios obtained in this embodiment. It can be seen from the figure that when the MoO2 mass is 5, 10, 15 and 20 mg, the H2 production of the MoO2 / ZnIn2S4 composite material is 2.57 mmol / h / g, 3.58 mmol / h / g, 2.72 mmol / h / g and 2.48 mmol / h / g respectively.

[0021] Example 2 MoO2 sample preparation is the same as in Example 1, and the MoO2 nanomaterial of this embodiment is used as a co-catalyst to improve the photocatalytic activity of CdS nanorods. The preparation process of CdS is as follows: 16.2 mmol of cadmium nitrate tetrahydrate and 48.6 mmol of thiourea are dissolved in 80 ml of ethylenediamine and stirred vigorously to obtain a transparent light green solution, and then 40 mL of the solution is placed in a reactor and reacted at 140 ° C for 24 h to finally obtain a light yellow CdS photocatalytic material. 100 mg of CdS photocatalytic material is ground with 1 mg, 5 mg, 10 mg, 15 mg and 20 mg of MoO2 to obtain a composite material. 20 mg of the composite material is placed in a reaction vessel, 8 ml of lactic acid and 80 ml of aqueous solution are added to the reaction vessel, and a photocatalytic hydrogen production test is performed under a xenon light source equipped with a 420 nm filter. When the mass of MoO2 is 10 mg, the photocatalytic hydrogen production activity of the composite material is 12.3 mmol / h*g, which is 6 times that of pure CdS. The photocatalytic hydrogen production activity cycle test of the composite material showed that MoO2 can significantly improve the stability of CdS. The hydrogen production activity of pure CdS was only 38% of the initial state after 6 cycles, while the MoO2-modified CdS still maintained 100% activity after 15 cycles.

[0022] Example 3 MoO2 sample preparation is the same as in Example 1. The MoO2 nanomaterial of this embodiment is used to make a sodium ion battery electrode: MoO2 nanomaterial, acetylene black conductive agent, and polyvinylidene fluoride binder with a mass ratio of 8:1:1 are weighed respectively, and polyvinylidene fluoride is dissolved in 1-methyl-2-pyrrolidone to form solution A, and then the MoO2 nanomaterial and acetylene black are added to the above solution A, and then the slurry is evenly coated on a disc copper foil, vacuum dried, and finally pressed on a tablet press to obtain an electrode. The obtained electrode sheet is assembled into a button battery with a sodium sheet and a diaphragm in a glove box. It is circulated 1000 times at a current density of 100 mA / g, and the capacity is as high as 850 mAh / g.

Claims

1. MoO 2 Nanoparticles dispersed in MoO 2 Synthesis methods of composite materials on nanosheets, It is characterized in that The following steps are involved: A certain amount of MoO rich in oxygen defects 3-x Nanosheets and sodium hypophosphite are placed in a tubular furnace with inert gas according to the ratio and position, with the sodium hypophosphite located above the gas, and then heated and reduced to obtain MoO 2 Nanomaterials; The MoO 2 The nanoparticles are dispersed on the surface of the nanosheets; The MoO 2 The diameter of nanoparticles is 20-300 nm; The MoO 2 The nanosheets have a thickness of 20-100 nm and a width of 400-500 nm.

2. MoO according to claim 1 2 Nanoparticles dispersed in MoO 2 Synthesis methods of composite materials on nanosheets, It is characterized in that The MoO 3-x The nanosheets are rich in oxygen vacancies, and the content of oxygen vacancies is 10%~30%.

3. MoO according to claim 1 2 Nanoparticles dispersed in MoO 2 Synthesis methods of composite materials on nanosheets, It is characterized in that The MoO 3-x The mass ratio with sodium hypophosphite is 1:2~1:

10.

4. MoO according to claim 1 2 Nanoparticles dispersed in MoO 2 Synthesis methods of composite materials on nanosheets, It is characterized in that Sodium hypophosphite is located 2-5 cm from the inlet of the inert gas.

5. MoO according to claim 1 2 Nanoparticles dispersed in MoO 2 Synthesis methods of composite materials on nanosheets, It is characterized in that Oxygen-deficient MoO 3-x The nanosheets were located at the outlet of the inert gas, 1 to 5 cm away from the sodium hypophosphite.

6. MoO according to claim 1 2 Nanoparticles dispersed in MoO 2 Synthesis methods of composite materials on nanosheets, It is characterized in that The heating rate is 1~5° / min, the heat treatment temperature is 200℃~500℃, and the reaction time is 1~4h.

7. MoO prepared according to claim 1-6 2 Nanoparticles dispersed in MoO 2 Composite materials on nanosheets for battery applications.

8. MoO prepared according to claim 1-6 2 Nanoparticles dispersed in MoO 2 Composite materials on nanosheets for application in electrocatalytic hydrogen evolution.

9. MoO prepared according to claim 1-6 2 Nanoparticles dispersed in MoO 2 Composite materials on nanosheets for electrocatalytic oxygen evolution.