Method for preparing composite calcium ferrite from industrial copperas
By mixing industrial green vitriol with calcium source and SiO2, then ball milling and calcining, composite calcium ferrite is generated, which solves the problem of large green vitriol by-products and pollution, and achieves high value-added utilization and environmental protection.
Patent Information
- Application Number
- CN202410736217.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-07
- Publication Date
- 2024-10-08
AI Technical Summary
Industrial green vitriol has large by-products, low added value and serious environmental pollution, which limits the sustainable development of titanium dioxide production. It is necessary to find high value-added utilization methods.
Industrial green vitriol is mixed with calcium source and SiO2, ball-milled, prepared into blocks, and then calcined and cooled to generate composite calcium ferrite. Through this process, the sulfur removal rate and the effective content of calcium ferrite are improved, and the strength, hardness and strength of the material are improved. Resistance to chemical attack.
It realizes the high value-added utilization of industrial green vitriol, reduces environmental pollution, improves the metallurgical properties of composite calcium ferrite, and promotes efficient and harmless utilization of resources.
Smart Images

Figure BDA0004881839760000061 
Figure BDA0004881839760000062 
Figure BDA0004881839760000071
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of metallurgy, and in particular to a method for preparing composite calcium ferrite from industrial green vitriol. Background Art
[0002] Green vitriol is a solid byproduct produced when concentrated sulfuric acid is used to leach ilmenite to prepare titanium dioxide. For every ton of titanium dioxide produced, 3 to 4 tons of green vitriol (FeSO4·7H2O) are produced as a byproduct. Due to its resource characteristics, the production of titanium dioxide in the Panxi region mainly adopts the sulfuric acid method titanium dioxide process, which has the advantages of low cost, mature technology, and low raw material requirements. However, the byproduct green vitriol has a large output, low added value, and environmental pollution. These problems are also its shortcomings that cannot be ignored, greatly limiting the green development of enterprises. At present, titanium dioxide enterprises produce about 3 tons of industrial green vitriol for every ton of titanium dioxide produced. Taking Panzhihua Iron and Steel as an example, the annual output of industrial green vitriol exceeds 660,000 tons. According to incomplete statistics, the total output of titanium dioxide in my country will reach 4.16 million tons in 2023 alone, and it is expected to produce 12.48 to 16.64 million tons of green vitriol. And with the increase in demand for titanium dioxide pigments, it will still increase at a rate of 10% per year.
[0003] Most Chinese manufacturers use concentrated sulfuric acid to extract ilmenite to produce titanium dioxide, which will inevitably produce a large amount of green vitriol. Since the by-product green vitriol contains a certain amount of impurities such as manganese, calcium, aluminum, magnesium, titanium, and zinc, it affects its practical application value in industry. Currently, only a small part of it is used for the production of flocculants, potassium ferrate, potassium sulfate, or nano-iron oxide, and the rest is still disposed of in the form of solid waste by stockpiling. This not only increases the construction cost of storage sites and occupies a large amount of effective arable land, but also restricts the sustainable development of sulfuric acid titanium dioxide production. In addition, the stockpiled green vitriol will cause air pollution under the action of wind erosion; under the shower of rainwater, the soluble heavy metal ions in the green vitriol will enter the surface water or penetrate into the groundwater, causing serious pollution of surface water and groundwater.
[0004] Therefore, it is urgent to utilize the by-product green vitriol to produce high value-added chemicals. Summary of the invention
[0005] The technical problem solved by the present invention is to provide a method for preparing composite calcium ferrite from industrial green vitriol, which can increase the sulfur removal rate in the industrial green vitriol and increase the effective content of calcium ferrite in the composite calcium ferrite.
[0006] In view of this, the present application provides a method for preparing composite calcium ferrite from industrial green vitriol, comprising the following steps:
[0007] S1) drying industrial green vitriol, mixing it with a calcium source, Al2O3 and SiO2, and ball milling to obtain a mixed material;
[0008] S2) preparing the mixed material into blocks and drying them, calcining the obtained blocks and then cooling them to obtain composite calcium ferrite;
[0009] or S2') calcining the mixture and then cooling it to obtain composite calcium ferrite.
[0010] Preferably, in step S1), the drying temperature is 100-150° C., and the calcium source is selected from one or both of calcium oxide and calcium carbonate.
[0011] Preferably, in step S1), the particle size of the mixed material is below 200 mesh.
[0012] Preferably, the mass ratio of the dried industrial green vitriol to the calcium source is (2-4):1, the Al2O3 is 0-5wt% of the mixed material, the SiO2 is 0-10wt% of the mixed material, and the content of the Al2O3 and the SiO2 is not zero.
[0013] Preferably, in step S2), water is added during the step of preparing the mixed material into blocks, and the amount of water added is 5-10 wt % of the mixed material.
[0014] Preferably, in step S2), the preparation method is pressing, and the drying temperature is 80-120° C. and the drying time is 1-2 hours.
[0015] Preferably, in step S2), the calcination temperature is 900-1300° C., the time is 0.5-3 h, and the calcination is carried out under negative pressure.
[0016] Preferably, in step S2'), the calcination temperature is 900-1300°C, the time is 0.5-3h, and the calcination is performed under negative pressure.
[0017] Preferably, in step S2), the sulfur-rich flue gas produced by the calcination is used to prepare sulfuric acid, and in step S2'), the sulfur-rich flue gas produced by the calcination is used to prepare sulfuric acid.
[0018] Preferably, the components of the industrial green vitriol include, by mass percentage: TFe: 20% to 35%, TS: 8% to 15%, MgO: 1% to 3%, Al2O3: 0% to 1%, TiO2: 0% to 1%, and SiO2: 0% to 1%.
[0019] The present application provides a method for preparing composite calcium ferrite from industrial green vitriol, which comprises drying the industrial green vitriol and mixing it with a calcium source, Al2O3 and SiO2, and ball milling to obtain a mixture; then preparing the mixture into blocks and drying them, and finally calcining the blocks and cooling them to obtain composite calcium ferrite, or calcining the mixture and cooling them to obtain composite calcium ferrite; in the method provided by the present application, the industrial green vitriol and the calcium source can be decomposed into calcium oxide, ferric oxide, sulfur dioxide and oxygen at high temperature, and the ferric oxide and calcium oxide react to form composite calcium ferrite, and at the same time, Al2O3 and SiO2 can improve the strength, hardness, fire resistance and chemical corrosion resistance of the composite calcium ferrite, and generate a new mineral phase Ca5(Fe,Al) at high temperature. 18 SiO 36 , changing the microstructure and macroscopic properties of the material, and lowering the melting point of calcium ferrite to below 1200°C. DETAILED DESCRIPTION
[0020] In order to further understand the present invention, preferred embodiments of the present invention are described below in conjunction with examples. However, it should be understood that these descriptions are only for further illustrating the features and advantages of the present invention, rather than limiting the claims of the present invention.
[0021] In view of the necessity of processing and reusing industrial green vitriol in the prior art, the present invention provides a method for preparing composite calcium ferrite from industrial green vitriol, which uses industrial green vitriol as the main raw material and adds a calcium source to prepare it into composite calcium ferrite for use in sintering pellets to improve the metallurgical properties of sintered pellets; after being processed by the above method, it can not only effectively alleviate the environmental hazards caused by the storage of industrial green vitriol, but also achieve its high added value utilization, achieving the purpose of efficient, harmless, resource-based and high added value utilization of solid waste. Specifically, an embodiment of the present invention discloses a method for preparing composite calcium ferrite from industrial green vitriol, comprising the following steps:
[0022] S1) drying industrial green vitriol, mixing it with a calcium source, Al2O3 and SiO2, and ball milling to obtain a mixed material;
[0023] S2) preparing the mixed material into blocks and drying them, calcining the obtained blocks and then cooling them to obtain composite calcium ferrite;
[0024] or S2') calcining the mixture and then cooling it to obtain composite calcium ferrite.
[0025] In the method for preparing composite calcium ferrite from industrial green vitriol provided in the present application, the present application first dries the industrial green vitriol to obtain ferrous sulfate monohydrate, which can reduce the energy consumption of subsequent reactions and avoid the generation of a large amount of water during the sintering process. The drying temperature is 100-150°C, specifically, the drying temperature is 100°C, 110°C, 120°C, 130°C, 140°C or 150°C.
[0026] The present application then mixes the dried calcium source, Al2O3, and SiO2, and obtains a mixed material after ball milling; in this process, the calcium source can provide calcium oxide during the subsequent calcination process, which can be selected from one or two of calcium oxide and calcium carbonate, and the mass ratio of the dried industrial green vitriol to the calcium source is (2-4):1, specifically, the mass ratio of the dried industrial green vitriol to the calcium source is (2.2-3.8):1, more specifically, the mass ratio of the dried industrial green vitriol to the calcium source is 2.5:1, 2.8:1, 3.0:1, 3.2:1, 3.5:1, 3.8:1 or 4:1. The Al2O3 accounts for 0-5wt% of the mixed material, the SiO2 accounts for 0-10wt% of the mixed material, and the contents of the Al2O3 and the SiO2 are not 0; specifically, the content of the SiO2 is 0.5-9.5wt%, more specifically, the content of the SiO2 is 1wt%, 1.8wt%, 2wt%, 2.2wt%, 2.5wt%, 3wt%, 3.5wt%, 4.0wt%, 4.3wt%, 4.8wt%, 5wt%, 5.6wt%, 6wt%, 6.5wt%, 7wt%, 7.6wt%, 7.7wt%, 8wt%, 8.6wt%, 8.8wt%, 9wt%, 9.5wt% or 10w%. Specifically, the content of Al2O3 is 0.4-4.8wt%, specifically, the content of Al2O3 is 1wt%, 1.6wt%, 1.8wt%, 2wt%, 2.3wt%, 2.8wt%, 3wt%, 3.3wt%, 3.5wt%, 4wt%, 4.2wt%, 4.6wt% or 5wt%. In the present application, the Al2O3 and SiO2 are added to reduce the melting point of the composite calcium ferrite, so that the obtained composite calcium ferrite is more suitable for use as a pre-solvent to improve the strength of the sintered pellets.
[0027] The above-mentioned Al2O3 and SiO2 have the following functions in the present application: 1) forming a solid solution: Al2O3 and SiO2 can form a solid solution in calcium ferrite, changing the crystal structure and physical and chemical properties of calcium ferrite; for example, Al2O3 can replace some aluminum or iron positions in the calcium ferrite lattice, while SiO2 can exist in the form of calcium silicate (CaSiO3); 2) improving physical properties: the addition of Al2O3 can improve the strength, hardness and fire resistance of calcium ferrite, while SiO2 can improve its ability to resist chemical corrosion, especially its stability in an acidic environment; 3) changing the melting point of calcium ferrite; 4) improving the melting point of calcium ferrite; 5) improving the melting point of calcium ferrite; 6) improving the melting point of calcium ferrite; 7) improving the melting point of calcium ferrite; 8) improving the melting point of calcium ferrite; 9) improving the melting point of calcium ferrite; 10) improving the melting point of calcium ferrite; 11) improving the melting point of calcium ferrite; 12) improving the melting point of calcium ferrite; 13) improving the melting point of calcium ferrite; 14) improving the melting point of calcium ferrite; 15) improving the melting point of calcium ferrite; 16) improving the melting point of calcium ferrite; 17) improving the melting point of calcium ferrite; 18) improving the melting point of calcium ferrite; 19) improving the melting point of calcium ferrite; 20) improving the melting point of calcium ferrite; 21) improving the melting point of calcium ferrite; 22) improving the melting point of calcium ferrite; 23) improving the melting point of calcium ferrite; 24) improving the melting point of calcium ferrite; 25) improving the melting point of calcium ferrite; 26) improving the melting point of calcium ferrite; 27) improving the melting point of calcium ferrite; 28) improving the melting point of 4) Mutual reaction to form new phases: At high temperatures, Al2O3 and SiO2 may react with other components in calcium ferrite to form new mineral phases; for example, Al2O3 and SiO2 can react with CaO (calcium oxide) to form calcium aluminum feldspar (CaAl2Si2O8) or calcium aluminum garnet (Ca3Al2Si3O 12 ) and other mineral phases; the formation of these new phases can significantly affect the microstructure and macroscopic properties of the material. Therefore, the role of Al2O3 and SiO2 in calcium ferrite is mainly reflected in the following aspects: improving material properties: improving strength, hardness, fire resistance and chemical corrosion resistance; changing melting point and sintering characteristics: affecting the melting point and sintering process conditions of the material; forming new mineral phases: generating new mineral phases at high temperatures, changing the microstructure and macroscopic properties of the material. The above-mentioned ball milling method is carried out in a manner well known to those skilled in the art, and this application does not impose any special restrictions on this. The ball milling is to make the particle size of the mixed material reach less than 200 meshes to facilitate the reaction.
[0028] The present application then prepares the mixed material into blocks and then dries them, and then cools the obtained blocks after calcination to obtain composite calcium ferrite. In this process, the agglomeration has the following functions in subsequent sintering: improving efficiency: promoting uniform reaction through uniformity and density control; improving material handling performance: reducing dust, facilitating transportation and storage; enhancing mechanical strength: improving the strength of the final product and reducing defects; promoting chemical reactions: enhancing reaction rate and improving material mixing; saving energy: reducing energy consumption and reducing reaction time. The agglomeration is to add water to the mixed material and then press it; the amount of water added is 5 to 10 wt% of the mixture, specifically, the amount of water added is 5.2 to 9.8 wt% of the mixture, and more specifically, the amount of water added is 5 wt%, 6 wt%, 7 wt%, 8 wt%, 9 wt% or 10 wt% of the mixture. The pressing is a method well known to those skilled in the art, and there is no particular limitation in this application. The drying temperature is 80-120°C, and the time is 1-2 hours; more specifically, the drying temperature is 82-118°C, and the time is 1.2-1.8 hours; more specifically, the drying temperature is 80°C, 82°C, 85°C, 87°C, 89°C, 90°C, 93°C, 95°C, 98°C, 100°C, 103°C, 108°C or 110°C. The calcination temperature is 900-1300°C, the time is 0.5-3h, and the calcination is carried out under negative pressure; specifically, the calcination temperature is 905-1280°C, the time is 0.8-2.6h; more specifically, the calcination temperature is 950°C, 1000°C, 1050°C, 1100°C, 1150°C, 1200°C, 1250°C or 1300°C, and the time is 1h, 1.2h, 1.5h, 1.8h, 2h, 2.4h, 2.6h, 2.8h or 3h. The calcination is carried out under negative pressure so that the sulfur dioxide generated by the decomposition can be diffused and discharged in time, and the decomposition reaction can be promoted to proceed in the forward direction.
[0029] Or, the mixed material is calcined and then cooled to obtain composite calcium ferrite. In this process, the calcination temperature is 900-1300°C, the time is 0.5-3h, and the calcination is carried out under negative pressure; specifically, the calcination temperature is 905-1280°C, the time is 0.8-2.6h; more specifically, the calcination temperature is 950°C, 1000°C, 1050°C, 1100°C, 1150°C, 1200°C, 1250°C or 1300°C, and the time is 1h, 1.2h, 1.5h, 1.8h, 2h, 2.4h, 2.6h, 2.8h or 3h. The calcination is carried out under negative pressure to diffuse and discharge the sulfur dioxide produced by decomposition in time, and promote the decomposition reaction to proceed in the forward direction. The sulfur-rich tail gas from the calcination is collected, which is mainly sulfur dioxide, and sulfuric acid is prepared by a contact method.
[0030] The present invention removes sulfur in industrial green vitriol in the form of sulfur dioxide at high temperature, and the sulfur removal rate reaches more than 95%, and calcium ferrite with an effective content of more than 60% in the composite calcium ferrite and sulfur dioxide flue gas are obtained, so that the iron and sulfur resources in the industrial green vitriol can be fully utilized; and the composite calcium ferrite prepared by the present application can be used for sintering pellets, and the sintered pellets have good metallurgical properties. The present invention fully mixes and contacts various materials by ball milling and briquetting, which is conducive to the full contact of solid-phase reactants, thereby reducing the calcination temperature and improving the conversion rate.
[0031] In order to further understand the present invention, the method for preparing composite calcium ferrite from industrial green vitriol provided by the present invention is described in detail below in conjunction with the examples. The protection scope of the present invention is not limited by the following examples.
[0032] Example
[0033] The industrial green vitriol in the following examples was obtained from a chemical enterprise, and after drying at 150°C, ferrous sulfate monohydrate was obtained. The main chemical components of the ferrous sulfate monohydrate were shown in Table 1.
[0034] Table 1 Main component data of ferrous sulfate monohydrate after industrial green vitriol drying
[0035]
[0036] The dried industrial green vitriol and calcium source in the above table are mixed, ball-milled in a ball mill to a particle size of less than 200 mesh, pressed into blocks with water, and calcined in a reactor after drying. The corresponding conditions and results of raw material selection are shown in Tables 2 and 3;
[0037] Table 2 Experimental conditions and results of industrial green vitriol and calcium oxide after drying
[0038]
[0039]
[0040] Table 3 Experimental conditions and results of industrial green vitriol and calcium carbonate after drying
[0041]
[0042] XRD analysis of the samples in Table 2 and Table 3 shows that the main phases are CaFe2O4, Ca2Fe2O5 and Ca5(Fe,Al) 18 SiO 36 ; It can be seen from the above table that Al2O3 and SiO2 can reduce the melting point of composite calcium ferrite, but excessive addition of SiO2 has little effect on reducing the melting point.
[0043] The above embodiments are only used to help understand the method and core idea of the present invention. It should be noted that, for those skilled in the art, several improvements and modifications can be made to the present invention without departing from the principles of the present invention, and these improvements and modifications also fall within the scope of protection of the claims of the present invention.
[0044] The above description of the disclosed embodiments enables one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. A method for preparing composite calcium ferrite from industrial green vitriol, comprising the following steps: S1) drying industrial green vitriol, mixing it with a calcium source, Al2O3 and SiO2, and ball milling to obtain a mixed material; S2) preparing the mixed material into blocks and drying them, calcining the obtained blocks and then cooling them to obtain composite calcium ferrite; or S2') calcining the mixture and then cooling it to obtain composite calcium ferrite.
2. The method according to claim 1, characterized in that In step S1), the drying temperature is 100-150° C., and the calcium source is selected from one or both of calcium oxide and calcium carbonate.
3. The method according to claim 1, characterized in that In step S1), the particle size of the mixed material is below 200 meshes.
4. The method according to claim 1, characterized in that: The mass ratio of the dried industrial green vitriol to the calcium source is (2-4):1, the Al2O3 accounts for 0-5wt% of the mixed material, the SiO2 accounts for 0-10wt% of the mixed material, and the content of the Al2O3 and the SiO2 is not zero.
5. The method according to claim 1, characterized in that In step S2), water is added during the step of preparing the mixed material into blocks, and the amount of water added is 5-10wt% of the mixed material.
6. The method according to claim 1, characterized in that In step S2), the preparation method is pressing, the drying temperature is 80-120° C., and the drying time is 1-2 hours.
7. The method according to claim 1, characterized in that In step S2), the calcination temperature is 900-1300° C., the time is 0.5-3 h, and the calcination is performed under negative pressure.
8. The method according to claim 1, characterized in that In step S2'), the calcination temperature is 900-1300°C, the time is 0.5-3h, and the calcination is performed under negative pressure.
9. The method according to claim 1, characterized in that: In step S2), the sulfur-rich flue gas generated by the calcination is used to prepare sulfuric acid, and in step S2'), the sulfur-rich flue gas generated by the calcination is used to prepare sulfuric acid.
10. The method according to any one of claims 1 to 9, characterized in that: The components of the industrial green vitriol include, by mass percentage, TFe: 20% to 35%, TS: 8% to 15%, MgO: 1% to 3%, Al2O3: 0% to 1%, TiO2: 0% to 1%, and SiO2: 0% to 1%.
Citation Information
Cited By
Method for synergistically harmlessly treating waste incineration fly ash and steelmaking furnace dust and preparing sintering-grade calcium ferrite
CN120648921A