Polyester solid phase tackifying method

By performing polyester solid-phase tackification under nitrogen positive pressure, combined with infrared heating and air convection, the problems of uneven reaction and low production efficiency in the existing technology are solved, and high molecular weight and high-performance polyester products are achieved, simplifying the production process.

CN118745242APending Publication Date: 2024-10-08CHINA SHENHUA COAL TO LIQUID & CHEM CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410731269.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-06
Publication Date
2024-10-08

AI Technical Summary

Technical Problem

The existing polyester solid-phase tackification method performs polycondensation reaction in a negative pressure environment, resulting in uneven reaction, unable to meet the needs of high molecular weight and high performance, and requires crushing treatment to reduce production efficiency.

Method used

The solid phase viscosity is increased under a nitrogen positive pressure atmosphere (1kpa ~ 500kpa), combined with infrared heating and air convection, and the circulating air flow in the polycondensation tower is used to take away unreacted monomers and oligomers to ensure that the material is heated evenly and passes through The infrared auxiliary heating system adjusts the heating amount to avoid excessive local temperature.

Benefits of technology

It achieves efficient solid-phase tackification of polyester, improves the weight average molecular weight and performance of the final product, simplifies the production process, reduces the need for crushing processing, and improves production efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118745242A_ABST
    Figure CN118745242A_ABST
Patent Text Reader

Abstract

The invention provides a polyester solid-phase tackifying method which comprises the following steps: crystallizing a polyester polymer in a crystallizer, feeding the polyester polymer into a polycondensation tower for solid-phase tackifying, and cooling and screening to obtain polyester particles; wherein the crystallized polyester polymer is subjected to solid-phase tackifying in the polycondensation tower in a heating manner of nitrogen convection and infrared radiation, the pressure in the polycondensation tower is 1-500kpa, the temperature is 190-220 DEG C, and the retention time is 2-20 hours. The solid-phase tackifying reaction is carried out under the nitrogen positive-pressure atmosphere (1kpa-500kpa), so that the materials are uniformly heated in the polycondensation tower, unreacted monomers and oligomers can be taken away by a gas phase in the polycondensation tower, and the quality and the performance of a final product are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of polyester preparation, and in particular to a solid phase viscosity increasing method for polyester. Background Art

[0002] Polyester has good mechanical properties and molding processing properties, and has been widely used in fibers, packaging, films, engineering plastics, etc., and has become one of the most important chemical synthetic materials in the world. Among them, aliphatic polyesters such as polyglycolic acid and polylactic acid can be decomposed by water, microorganisms or enzymes existing in the soil, ocean and other natural places. Such biodegradable polymer materials have received more and more attention.

[0003] At present, high molecular weight polyglycolic acid mainly includes ring-opening polymerization and direct polycondensation. The ring-opening polymerization method first needs to obtain high-purity glycolide, and then prepare polyglycolic acid through ring-opening polymerization of glycolide, which is costly. The direct polycondensation method is synthesized by dehydration or demethylation polycondensation of glycolic acid / or methyl glycolate, but the molecular weight of the polyglycolic acid prepared by this method is low and cannot meet the application requirements of most scenarios. Therefore, solid-state polycondensation is usually required later to increase viscosity in order to achieve the ideal molecular weight.

[0004] The existing solid phase thickening or solid phase polycondensation system usually allows polyester polymers to undergo polycondensation reaction under negative pressure. For example, patent CN106432698B discloses a method for preparing polyglycolic acid by polymerizing glycolic acid, wherein glycolic acid is purified and dehydrated for pre-polycondensation, and then a polymerization aid is added, and thermal polymerization is carried out in a vacuum sealed container, and then microwave polymerization is carried out. After cooling to room temperature, the polymer is filtered, washed, and dried to obtain a polymer, and the dried polyglycolic acid polymer is crushed to obtain a 100-mesh polyglycolic acid solid powder; the obtained polyglycolic acid solid powder is further solid-phase polymerized to obtain polyglycolic acid with a higher intrinsic viscosity; the solid-phase polycondensation adopts a gradually increasing heating method, and the solid-phase polymerization pressure is 20-30 Pa, the temperature is 195-215° C., and the time is 4-8 hours.

[0005] Patent CN102718947B discloses a polyhydroxycarboxylate and a preparation method thereof. Using Lewis acid as a catalyst, a hydroxycarboxylate monomer is subjected to a solid phase polymerization reaction to obtain a polyhydroxy acid oligomer, and then the polyhydroxycarboxylate oligomer is crushed under the protection of an inert gas; finally, the polyhydroxycarboxylate is obtained after reacting for 10 to 300 hours under the conditions of 10Pa to 100KPa and 100 to 250°C.

[0006] Patent CN106633017B discloses a method for preparing modified polylactic acid, including modified lactic acid water prepolymer, dehydration, polycondensation, and solid phase polycondensation steps. The solid phase polycondensation includes the following process: in the molten state of the copolyester, phthalic anhydride is added under N2 protection, the addition amount is 0.01% to 0.5% of the mass of the copolyester, cooled and crushed to obtain a powder of 60 to 100 mesh; the powder is heated by a gradually increasing temperature method, the heating temperature range is 145 to 185°C, the reaction time is 4 to 7h, and the vacuum degree in the solid phase polycondensation reactor is ≤0.1MPa. Summary of the invention

[0007] The object of the present invention is to overcome the shortcomings of the prior art and provide a method for solid-phase viscosity enhancement of polyester. By carrying out a solid-phase viscosity enhancement reaction under a nitrogen positive pressure atmosphere (1 kPa to 500 kPa) and ensuring that the nitrogen in the polycondensation tower is in a circulating flow state, continuous production can be carried out, and the material is heated evenly in the polycondensation tower. The gas phase in the polycondensation tower can take away unreacted monomers and oligomers, thereby improving the quality / performance of the final product.

[0008] In order to achieve the above object, the present invention adopts the following technical solutions:

[0009] The present invention provides a method for solid phase viscosity enhancement of polyester, wherein the polyester polymer is crystallized in a crystallizer and then enters a polycondensation tower for solid phase viscosity enhancement, and then is cooled and sieved to obtain polyester particles;

[0010] The crystallized polyester polymer is subjected to solid phase viscosity enhancement in the polycondensation tower by nitrogen convection and infrared radiation heating. The pressure in the polycondensation tower is 1 kpa to 500 kpa, the temperature is 190 to 220° C., and the residence time is 2 to 20 hours.

[0011] In the method of the present invention, a feed port connected to a crystallizer is provided at the top of the polycondensation tower, and a discharge port is provided at the bottom of the polycondensation tower to control the polyester polymer to enter and exit the polycondensation tower; a main air inlet for charging nitrogen gas into the polycondensation tower is provided at the lower end of the polycondensation tower, and a main air outlet for discharging gas in the polycondensation tower is provided at the upper end. The main air inlet and the main air outlet form a second circulation loop from bottom to top, which is used to transport high-temperature nitrogen into the inner cavity of the polycondensation tower to form convection with the polyester polymer entering from the top feed port, so as to perform solid phase viscosity enhancement.

[0012] In some specific embodiments, a gas purification component is also provided on the second circulation loop, and the gas purification component includes a cooler and a cyclone separator arranged in sequence from the main gas outlet to the main gas inlet, so as to cool the gas coming out of the main gas outlet, perform gas-solid separation and other purification treatments, and the purified gas is then transported to the main gas inlet at the bottom of the polycondensation tower. Specifically, the temperature of the cooler is lower than 85°C, so as to cool the monomers and oligomers in the gas flow to below their melting point.

[0013] In some specific embodiments, a spiral coil is provided at the bottom of the polycondensation tower, and a through hole is provided on the coil, so that nitrogen flows out from the top of the polycondensation tower, is purified by the gas purification component, and then enters the coil of the polycondensation tower to perform heat exchange with the polyester polymer at the bottom before flowing out.

[0014] In some specific embodiments, an infrared auxiliary heating system for auxiliary heating of materials is provided on the side wall of the polycondensation tower. Specifically, the infrared auxiliary heating system is arranged between the outer shell and the inner shell of the side wall of the polycondensation tower. The radiation range includes at least the entire reaction area of ​​the polycondensation tower. The heating radiation emitted by it is controllable, and the radiation amount for each part in the polycondensation tower can be regulated, so that the heating amount inside the polycondensation tower is adjusted to gradually decrease or the heating temperature gradually decreases along the direction from the feed inlet to the discharge port of the polycondensation tower. It can be reduced or decreased linearly from top to bottom, or it can be reduced or decreased in equal proportion from top to bottom, and reduced or decreased in steps or sections with intervals as units. Specifically, the infrared auxiliary heating system includes an infrared heating tube that radiates infrared rays into the interior of the polycondensation tower, and the heating amount of the infrared rays radiated by the infrared heating tube gradually decreases along the direction from the feed inlet to the discharge port of the polycondensation tower. More specifically, the heating amount inside the polycondensation tower is adjusted by setting the infrared wavelength radiated by the infrared auxiliary heating system. In some specific embodiments, the infrared wavelength radiated by the infrared auxiliary heating system can be 2.5 to 10 μm, for example, 2.5 to 3.5 μm, 8 to 10 μm.

[0015] During the reaction, the polycondensation of polyester polymer is a process of absorbing heat first and then releasing heat, especially in the later stage, which is easy to cause local over-temperature, which has an adverse effect on the performance of the final product, such as aging resistance and color. In some more specific embodiments, the infrared auxiliary heating system includes at least two groups of infrared heating tubes, A and B. The infrared heating tubes of group A are arranged close to the feed inlet of the polycondensation tower, and the infrared heating tubes of group B are arranged close to the discharge port of the polycondensation tower, wherein the infrared heating tubes of group A and group B respectively include 3 to 5 infrared heating tubes, and the power of the infrared heating tubes is 300 to 1200W; the infrared wavelength radiated by the infrared heating tubes of group A is 2.5 to 3.5 μm, and the infrared wavelength radiated by the infrared heating tubes of group B is 6 to 10 μm, for example, 6 to 8 μm.

[0016] In some specific embodiments, the particle size of the polyester polymer entering the polycondensation tower is below 6 mm, preferably 2 to 4 mm, for example, 3 mm.

[0017] In some specific embodiments, the gas-to-material ratio entering the polycondensation tower is controlled to be 1:(50-130) L / g, for example, 1:60 L / g, 1:70 L / g, 1:80 L / g, 1:90 L / g, 1:100 L / g, 1:110 L / g, 1:120 L / g.

[0018] In some specific embodiments, the upper end of the crystallizer is provided with a crystallization feed port connected to the silo, the lower end of the crystallizer is provided with a crystallization discharge port and a crystallization air inlet connected to the polycondensation tower, and the upper end of the crystallizer is provided with a crystallization air outlet, and the crystallization air inlet and the crystallization air outlet form a first circulation loop from bottom to top. In some specific embodiments, nitrogen is continuously introduced into the crystallizer in a bottom-in-top-out manner. In the present invention, the blanking direction of the crystallizer is from top to bottom, and the flow direction of the gas in the crystallizer is from bottom to top in the opposite direction of the blanking direction, so that the crystallizer can efficiently and stably perform the crystallization reaction, and the impurities are taken away by the airflow, which plays an important role in the pre-process of solid phase viscosity enhancement.

[0019] In some more specific embodiments, a gas purification component is also provided on the first circulation loop connected to the crystallizer, and the gas purification component includes a pressure relief port, a cyclone separator, a fan and a heater to purify the gas coming out of the crystallization outlet.

[0020] In some specific embodiments, the gas-to-material ratio entering the crystallizer is controlled to be 1:(50-130) L / g, for example, 1:60 L / g, 1:70 L / g, 1:80 L / g, 1:90 L / g, 1:100 L / g, 1:110 L / g, 1:120 L / g.

[0021] In some specific embodiments, the crystallization reaction temperature in the crystallization tower is controlled to be 170-205°C, for example, 180°C, 190°C, 200°C; the crystallization reaction time is less than 2h, for example, 30min, 40min, 50min, 60min, 1.5h.

[0022] In some specific embodiments, in the method provided by the present invention, the polyester polymer is selected from polyglycolic acid.

[0023] In some specific embodiments, the weight average molecular weight of the polyester polymer is 100,000 to 150,000, the residual monomer content is 1 to 5%, and the melt index is 20 to 50 g / 10 min; the migration amount is not less than 53 mg / L in terms of glycolic acid. After solid phase viscosity enhancement in the polycondensation tower, the weight average molecular weight of the polyester particles is 130,000 to 200,000, for example, 140,000, 150,000, 160,000, 170,000, 180,000, 190,000, the residual monomer content is 0.5 to 1%, for example, 0.6%, 0.7%, 0.8%, 0.9%, and the melt index is 10 to 30 g / 10 min, for example, 15 g / 10 min, 16 g / 10 min, 18 g / 10 min, 20 g / 10 min , 22g / 10min, 24g / 10min, 26g / 10min; calculated in terms of glycolic acid, the migration amount is not higher than 28mg / L (calculated in terms of glycolic acid, the conditions are 70℃, 2h, 10% ethanol), for example, 2mg / L, 4mg / L, 6mg / L, 8mg / L, 10mg / L, 12mg / L, 14mg / L, 16mg / L, 18mg / L, 20mg / L, 22mg / L, 24mg / L.

[0024] The above technical solution has the following technical effects:

[0025] Compared with solid-phase viscosity enhancement or solid-phase polycondensation systems that perform polycondensation reactions in an intermittent, negative pressure environment, the solid-phase polycondensation method provided by the present invention performs solid-phase viscosity enhancement under a nitrogen positive pressure atmosphere (1 kpa to 500 kpa), which can ensure that the nitrogen in the polycondensation tower is in a circulating flow state, can carry out continuous production and ensure that the materials are heated evenly in the polycondensation tower; at the same time, during the polycondensation process, the gas phase in the polycondensation tower can carry away unreacted monomers and oligomers, further improving the quality / performance of the final product.

[0026] The method of the present invention adopts a combination of infrared heating and positive pressure to ensure the uniformity of heating of the material and the uniformity of the heat of the system, so that the particle size of the raw material entering the polycondensation tower does not need to be crushed, and can directly enter the polycondensation tower from the crystallizer in the polymerization production line for solid-phase viscosity enhancement, and the output particles can be directly packaged, thereby improving production efficiency; while the existing solid-phase viscosity enhancement technology requires advance crushing treatment to the material particle size within the range of 0.005mm to 2mm before solid-phase viscosity enhancement can be performed; and small-sized particles need to be subsequently granulated after being discharged, thereby reducing production efficiency.

[0027] The method of the present invention adopts convection between the material in the polycondensation tower and the nitrogen gas flow, and the radiation wavelength of the infrared auxiliary heating system increases along the direction from the inlet to the outlet of the polycondensation tower (that is, the radiation heat decreases along the direction from the inlet to the outlet of the polycondensation tower). For the polycondensation reaction that first absorbs heat and then releases heat, it can avoid the local temperature from being too high, and at the same time ensure that the material in the tower is heated evenly. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 A schematic diagram of the specific structure of a viscosity-enhancing system used in the solid-phase viscosity-enhancing method provided by the present invention;

[0029] Among them, 1. crystallizer;

[0030] 2. a first circulation loop, 21. a first gas purification component, 211. a heater, 212. a first cyclone separator, 213. a first fan;

[0031] 3. polycondensation tower, 31. main air inlet, 32. main air outlet;

[0032] 4. Infrared auxiliary heating system;

[0033] 5. Second circulation loop, 51. Second gas purification component, 511. Cooler, 512. Second cyclone separator, 513. Second fan. DETAILED DESCRIPTION

[0034] The specific embodiments of the present invention are described in detail below. It should be understood that the specific embodiments described herein are only used to illustrate and explain the present invention, and are not used to limit the present invention.

[0035] Unless otherwise specified, the raw materials and reagents used in the following examples are commercially available or can be prepared by known methods.

[0036] Source of raw materials:

[0037] Polyglycolic acid: a series of products with a weight average molecular weight of 100,000 to 150,000 purchased from Inner Mongolia Pujing Polymer Material Technology Co., Ltd., and a particle size of less than 6 mm.

[0038] The following detection methods are used in the following examples:

[0039] 1. Melt index test

[0040] 1) drying the polymer in a vacuum drying oven at 105°C;

[0041] 2) Set the test temperature of the test instrument to 230°C and preheat the instrument;

[0042] 3) 6-8 g of dry polymer is loaded into a barrel through a funnel and compacted with a piston;

[0043] 4) After heating for 4 minutes, cut a section every 10 seconds under a weight of 2.16 kg, and obtain ten sections in total;

[0044] 5) Weigh the mass of each sample and calculate its MFR.

[0045] MFR = 600 W / t (g / 10 min), where W is the average mass of each sample segment and t is the cutting time interval of each segment.

[0046] 2. Determination of weight average molecular weight

[0047] The sample was dissolved in a 5 mmol / L sodium trifluoroacetate hexafluoroisopropanol solution to prepare a 0.05-0.3 wt% (mass fraction) solution; then, the solution was filtered through a polytetrafluoroethylene filter with a pore size of 0.4 μm; 20 μL of the filtered solution was added to a gel permeation chromatography (GPC) injector to determine the molecular weight of the sample. Five standard molecular weights of methyl methacrylate with different molecular weights were used for molecular weight calibration.

[0048] 3. Residual monomer test

[0049] Take about 0.5g of the sample and place it in a sealed container. Accurately add 15ml of hexafluoroisopropanol to dissolve it. After the dissolution is complete, transfer the test solution to a 100ml round-bottom (flat-bottom) flask, add 15ml of hexafluoroisopropanol, brush it clean in a sealed container, transfer it to the flask, accurately add 10ml of acetone, shake to precipitate the polymer, shake to dissolve, filter, and take the filtrate; take 1μl of the above-mentioned reference solution and test solution respectively, inject them into the gas chromatograph, record the chromatogram, and calculate the content of residual small molecules.

[0050] 4. Migration test

[0051] 1) Mix the sample to be tested with the simulated liquid (10% ethanol aqueous solution), seal it, and keep it at a constant temperature of 70°C for 2 hours, then take out the sample to be tested;

[0052] 2) then cooling the simulated liquid to room temperature to obtain a solution to be tested;

[0053] 3) the solution to be tested is mixed with the alkaline aqueous solution and subjected to a thermal reaction to obtain a pretreatment solution;

[0054] 4) The content of glycolate in the pretreatment solution is detected by ion chromatography. Based on the content of glycolate, the upper limit of the total migration amount of glycolic acid and glycolate oligomers with a molecular weight less than 1000 can be determined.

[0055] 5. Particle size test

[0056] Place the particles in a 4-10 mesh sieve and use mechanical vibration or manual method to make the particles pass through the sieve until the desired particles are obtained.

[0057] The polyester solid phase viscosity increasing system used in the following embodiments of the present invention is as follows:

[0058] like Figure 1As shown, the system includes a first circulation loop 2, a crystallizer 1 connected to the first circulation loop 2, a condensation tower 3 connected to the crystallizer 1, and a second circulation loop 5; the crystallizer 1 and the first circulation loop 2 form a gas channel from bottom to top, so that a positive pressure gas environment from bottom to top is formed inside the crystallizer 1 to carry away impurities of the crystallization reaction in the crystallizer 1, such as monomers and oligomers.

[0059] The upper end of the crystallizer 1 is provided with a crystallization feed port connected to the silo, the lower end of the crystallizer 1 is provided with a crystallization discharge port and a crystallization air inlet connected to the condensation tower 3, and the upper end of the crystallizer 1 is provided with a crystallization air outlet, forming a first circulation loop 2 from bottom to top at the crystallization air inlet and the crystallization air outlet.

[0060] The polycondensation tower 3 is connected to the second circulation loop 5. The lower end of the polycondensation tower 3 has a main air inlet 31 for charging gas into the polycondensation tower 3, and the upper end of the polycondensation tower 3 has a main air outlet 32 ​​for discharging the gas in the polycondensation tower 3. The second circulation loop 5 is respectively connected to the main air inlet 31 and the main air outlet 32, and the polycondensation tower 3 and the second circulation loop 5 form a gas channel from bottom to top.

[0061] In the first circulation loop 2 and the second circulation loop 5, the gas must first be cooled and then passed through a cyclone separator to remove impurities, specifically by cooling the temperature of the monomers and oligomers to below their melting point to achieve removal, before it can return to the crystallizer 1 or the condensation tower 3 again. Therefore, a first gas purification component 21 is provided on the first circulation loop 2 to purify the monomers and oligomers taken away from the crystallizer 1 under a positive pressure gas environment, and a second gas purification component 51 is provided on the second circulation loop 5 to purify the monomers and oligomers taken away from the condensation tower 3 under a positive pressure gas environment.

[0062] In some specific embodiments, the second gas purification component 51 includes a cooler 511 , a second cyclone separator 512 , a second pressure relief port, and a second fan 513 which are arranged in sequence from the main gas outlet 32 ​​to the main gas inlet 31 .

[0063] In some specific embodiments, the first gas purification component 21 includes a pressure relief port, a first cyclone separator 212, a first fan 213 and a heater 211 arranged in sequence from the crystallization outlet to the crystallization inlet to purify and heat the gas coming out of the crystallization outlet.

[0064] An infrared auxiliary heating system 4 for auxiliary heating of materials is provided on the side wall of the polycondensation tower 3. In the direction from the main air outlet 32 ​​to the main air inlet 31, specifically, the infrared auxiliary heating system 4 includes two groups of infrared heating tubes, A and B, each of which has three infrared heating tubes. The infrared heating tubes of group A are close to the feed port at the top of the polycondensation tower 3, and the infrared heating tubes of group B are close to the discharge port at the bottom of the polycondensation tower 3. By adjusting the radiation amount of the infrared heating tubes of groups A and B, the heating amount inside the polycondensation tower 3 is adjusted to gradually decrease in the direction from the feed port to the discharge port of the polycondensation tower 3.

[0065] Example 1

[0066] Polyglycolic acid enters the crystallizer from the feed port at the top of the crystallizer, and nitrogen is introduced into the crystallizer from the air inlet at the bottom. The nitrogen in the crystallizer crystallizes the polyester in the opposite direction of the polyglycolic acid falling. The gas-to-material ratio in the crystallizer is 1:100L / g, and the temperature of the crystallizer is 170°C.

[0067] After 20 minutes of crystallization, the product is discharged from the crystallization outlet at the bottom of the crystallizer, and then enters the polycondensation tower through the feed port set at the top of the polycondensation tower. High-temperature nitrogen is transported from the main air inlet at the lower end of the polycondensation tower to the inner cavity of the polycondensation tower to form convection with the polyester polymer for solid phase viscosity enhancement.

[0068] An infrared auxiliary heating system for auxiliary heating of materials is provided on the side wall of the polycondensation tower. The infrared auxiliary heating system includes two groups of infrared heating tubes, A and B. The infrared heating tubes of group A are close to the feed port at the top of the polycondensation tower, and the infrared heating tubes of group B are close to the discharge port at the bottom of the polycondensation tower. The infrared wavelength of the infrared heating tubes of group A is 2.5-3.5 μm, and the infrared wavelength of the infrared heating tubes of group B is 6-10 μm; the infrared heating tubes of groups A and B respectively include 3 infrared heating tubes, the power of the infrared heating tubes is 500 W, the condensation temperature in the polycondensation tower is 190°C, the pressure of the nitrogen gas in the polycondensation tower is 1 kpa, and the gas-to-material ratio is 1:80 L / g.

[0069] After solid phase thickening for 10 hours, the polyglycolic acid was discharged from the discharge port at the bottom of the polycondensation tower, and polyglycolic acid particles were obtained after cooling and sieving.

[0070] After testing, the performance comparison of polyglycolic acid before and after solid phase polycondensation is shown in the following table:

[0071] Melt index (g / 10min) Weight average molecular weight Residual monomer (%) Migration amount (mg / L) Before polycondensation 46 111000 4.20 84 After polycondensation 28 168000 0.85 26

[0072] Example 2

[0073] Polyglycolic acid enters the crystallizer from the feed port at the top of the crystallizer, and nitrogen is introduced into the crystallizer from the air inlet at the bottom. The nitrogen in the crystallizer crystallizes the polyester in the opposite direction of the polyglycolic acid falling. The gas-to-material ratio in the crystallizer is 1:100L / g, and the temperature of the crystallizer is 180°C.

[0074] After 20 minutes of crystallization, the polyester is discharged from the discharge port at the bottom of the crystallizer, and then enters the polycondensation tower through the feed port set at the top of the polycondensation tower. High-temperature nitrogen is transported from the main air inlet at the lower end of the polycondensation tower to the inner cavity of the polycondensation tower to form convection with the polyester polymer for solid phase viscosity enhancement.

[0075] An infrared auxiliary heating system for auxiliary heating of materials is provided on the side wall of the polycondensation tower. The infrared auxiliary heating system includes two groups of infrared heating tubes, A and B. The infrared heating tubes of group A are close to the feed port at the top of the polycondensation tower, and the infrared heating tubes of group B are close to the discharge port at the bottom of the polycondensation tower. The infrared wavelength of the infrared heating tubes of group A is 2.5-3.5 μm, and the infrared wavelength of the infrared heating tubes of group B is 6-8 μm; the infrared heating tubes of groups A and B respectively include 3 infrared heating tubes, the power of the infrared heating tubes is 700 W, the condensation temperature in the polycondensation tower is 195°C, the nitrogen gas pressure in the polycondensation tower is 20 kpa, and the gas-to-material ratio is 1:80 L / g.

[0076] After solid phase thickening for 5 hours, the polyglycolic acid was discharged from the discharge port at the bottom of the polycondensation tower, and polyglycolic acid particles were obtained after cooling and sieving.

[0077] After testing, the performance comparison of polyglycolic acid before and after solid phase polycondensation is shown in the following table:

[0078] Melt index (g / 10min) Weight average molecular weight Residual monomer (%) Migration amount (mg / L) Before polycondensation 41 130000 4.00 78 After polycondensation 20 176000 0.70 25

[0079] Example 3

[0080] Polyglycolic acid enters the crystallizer from the feed port at the top of the crystallizer, and nitrogen is introduced into the crystallizer from the air inlet at the bottom. The nitrogen in the crystallizer crystallizes the polyester in the opposite direction of the polyglycolic acid falling. The gas-to-material ratio in the crystallizer is 1:100L / g, and the temperature of the crystallizer is 185°C.

[0081] After 30 minutes of crystallization, the product is discharged from the crystallization outlet at the bottom of the crystallizer, and then enters the polycondensation tower through the feed port set at the top of the polycondensation tower. High-temperature nitrogen is transported from the main air inlet at the lower end of the polycondensation tower to the inner cavity of the polycondensation tower to form convection with the polyester polymer for solid phase viscosity enhancement.

[0082] An infrared auxiliary heating system for auxiliary heating of materials is provided on the side wall of the polycondensation tower. The infrared auxiliary heating system includes two groups of infrared heating tubes, A and B. The infrared heating tubes of group A are close to the feed port at the top of the polycondensation tower, and the infrared heating tubes of group B are close to the discharge port at the bottom of the polycondensation tower. The infrared wavelength of the infrared heating tubes of group A is 2.5-3.5 μm, and the infrared wavelength of the infrared heating tubes of group B is 6-8 μm. The infrared heating tubes of groups A and B respectively include 3 infrared heating tubes, the power of the infrared heating tubes is 500 W, the condensation temperature in the polycondensation tower is 200 ° C, the nitrogen gas pressure in the polycondensation tower is 50 kpa, and the gas-to-material ratio is 1:100 L / g.

[0083] After solid phase thickening for 3 hours, the polyglycolic acid was discharged from the discharge port at the bottom of the polycondensation tower, and polyglycolic acid particles were obtained after cooling and sieving.

[0084] After testing, the performance comparison of polyglycolic acid before and after solid phase polycondensation is shown in the following table:

[0085]

[0086] Example 4

[0087] Polyglycolic acid enters the crystallizer from the feed port at the top of the crystallizer, and nitrogen is introduced into the crystallizer from the air inlet at the bottom. The nitrogen in the crystallizer crystallizes the polyester in the opposite direction of the polyglycolic acid falling. The gas-to-material ratio in the crystallizer is 1:100L / g, and the temperature of the crystallizer is 190°C.

[0088] After 60 minutes of crystallization, the product is discharged from the crystallization outlet at the bottom of the crystallizer, and then enters the polycondensation tower through the feed port set at the top of the polycondensation tower. High-temperature nitrogen is transported from the main air inlet at the lower end of the polycondensation tower to the inner cavity of the polycondensation tower to form convection with the polyester polymer for solid phase viscosity enhancement.

[0089] An infrared auxiliary heating system for auxiliary heating of materials is provided on the side wall of the polycondensation tower. The infrared auxiliary heating system includes two groups of infrared heating tubes, A and B. The infrared heating tubes of group A are close to the feed port at the top of the polycondensation tower, and the infrared heating tubes of group B are close to the discharge port at the bottom of the polycondensation tower. The infrared wavelength of the infrared heating tubes of group A is 2.5-3.5 μm, and the infrared wavelength of the infrared heating tubes of group B is 8-10 μm. The infrared heating tubes of groups A and B respectively include 3 infrared heating tubes, the power of the infrared heating tubes is 1000 W, the condensation temperature in the polycondensation tower is 210°C, the nitrogen gas pressure in the polycondensation tower is 100 kpa, and the gas-to-material ratio is 1:130 L / g.

[0090] After solid phase thickening for 3 hours, the polyglycolic acid was discharged from the discharge port at the bottom of the polycondensation tower, and polyglycolic acid particles were obtained after cooling and sieving.

[0091] After testing, the performance comparison of polyglycolic acid before and after solid phase polycondensation is shown in the following table:

[0092] Melt index (g / 10min) Weight average molecular weight Residual monomer (%) Migration amount (mg / L) Before polycondensation 30 142000 2.00 66 After polycondensation 15 189000 0.61 15

[0093] Example 5

[0094] Polyglycolic acid enters the crystallizer from the feed port at the top of the crystallizer, and nitrogen is introduced into the crystallizer from the air inlet at the bottom. The nitrogen in the crystallizer crystallizes the polyester in the opposite direction of the polyglycolic acid falling. The gas-to-material ratio in the crystallizer is 1:100L / g, and the temperature of the crystallizer is 190°C.

[0095] After 90 minutes of crystallization, the product is discharged from the crystallization outlet at the bottom of the crystallizer, and then enters the polycondensation tower through the feed port set at the top of the polycondensation tower. High-temperature nitrogen is transported from the main air inlet at the lower end of the polycondensation tower to the inner cavity of the polycondensation tower to form convection with the polyester polymer for solid phase viscosity enhancement.

[0096] An infrared auxiliary heating system for auxiliary heating of materials is provided on the side wall of the polycondensation tower. The infrared auxiliary heating system includes two groups of infrared heating tubes, A and B. The infrared heating tubes of group A are close to the feed port at the top of the polycondensation tower, and the infrared heating tubes of group B are close to the discharge port at the bottom of the polycondensation tower. The infrared wavelength of the infrared heating tubes of group A is 2.5-3.5 μm, and the infrared wavelength of the infrared heating tubes of group B is 8-10 μm. The infrared heating tubes of groups A and B respectively include 3 infrared heating tubes, the power of the infrared heating tubes is 1000 W, the condensation temperature in the polycondensation tower is 205°C, the nitrogen gas pressure in the polycondensation tower is 200 kpa, and the gas-to-material ratio is 1:130 L / g.

[0097] After 2 hours of solid phase thickening, the polyglycolic acid was discharged from the discharge port at the bottom of the polycondensation tower, and polyglycolic acid particles were obtained after cooling and sieving.

[0098] After testing, the performance comparison of polyglycolic acid before and after solid phase polycondensation is shown in the following table:

[0099] Melt index (g / 10min) Weight average molecular weight Residual monomer (%) Migration amount (mg / L) Before polycondensation 25 145000 1.70 60 After polycondensation 12 192000 0.58 13

[0100] Example 6

[0101] Polyglycolic acid enters the crystallizer from the feed port at the top of the crystallizer, and nitrogen is introduced into the crystallizer from the air inlet at the bottom. The nitrogen in the crystallizer crystallizes the polyester in the opposite direction of the polyglycolic acid falling. The gas-to-material ratio in the crystallizer is 1:100L / g, and the temperature of the crystallizer is 200℃.

[0102] After 30 minutes of crystallization, the product is discharged from the crystallization outlet at the bottom of the crystallizer, and then enters the polycondensation tower through the feed port set at the top of the polycondensation tower. High-temperature nitrogen is transported from the main air inlet at the lower end of the polycondensation tower to the inner cavity of the polycondensation tower to form convection with the polyester polymer for solid phase viscosity enhancement.

[0103] An infrared auxiliary heating system for auxiliary heating of materials is provided on the side wall of the polycondensation tower. The infrared auxiliary heating system includes two groups of infrared heating tubes, A and B. The infrared heating tubes of group A are close to the feed port at the top of the polycondensation tower, and the infrared heating tubes of group B are close to the discharge port at the bottom of the polycondensation tower. The infrared wavelength of the infrared heating tubes of group A is 2.5-3.5 μm, and the infrared wavelength of the infrared heating tubes of group B is 8-10 μm. The infrared heating tubes of groups A and B respectively include 3 infrared heating tubes, the power of the infrared heating tubes is 1200 W, the condensation temperature in the polycondensation tower is 220°C, the nitrogen gas pressure in the polycondensation tower is 100 kpa, and the gas-to-material ratio is 1:130 L / g.

[0104] After 2 hours of solid phase thickening, the polyglycolic acid was discharged from the discharge port at the bottom of the polycondensation tower, and polyglycolic acid particles were obtained after cooling and sieving.

[0105] After testing, the performance comparison of polyglycolic acid before and after solid phase polycondensation is shown in the following table:

[0106] Melt index (g / 10min) Weight average molecular weight Residual monomer (%) Migration amount (mg / L) Before polycondensation 22 147000 1.30 55 After polycondensation 12 193000 0.55 12

[0107] The method of the present invention firstly crystallizes the material through a crystallizer, and then performs solid-state polycondensation and viscosity enhancement in a polycondensation tower in the later stage to achieve an ideal molecular weight; from the test data in the above tables, the method of the present invention performs polyester solid-phase viscosity enhancement under a slightly positive pressure atmosphere (1kpa-500kpa), reduces the melt index of the polymer, and further increases the weight-average molecular weight of the polymer to 130,000-200,000; at the same time, the method of the present invention adopts a material and gas opposite material dropping method in the polycondensation and crystallization process, and impurities are taken away by air flow, so that the content of residual monomers in polyglycolic acid after polycondensation is reduced by 0.8-3 percentage points, and the migration amount after solid-phase viscosity enhancement is also greatly reduced.

Claims

1. A method for solid phase viscosity enhancement of polyester, It is characterized in that After the polyester polymer is crystallized in the crystallizer, it enters the polycondensation tower for solid phase viscosity enhancement, and then is cooled and sieved to obtain polyester particles; The crystallized polyester polymer is subjected to solid phase viscosity enhancement in the polycondensation tower by nitrogen convection and infrared radiation heating. The pressure in the polycondensation tower is 1 kpa to 500 kpa, the temperature is 190 to 220° C., and the residence time is 2 to 20 hours.

2. The method according to claim 1, It is characterized in that An infrared auxiliary heating system for auxiliary heating of materials is provided on the side wall of the polycondensation tower. The infrared auxiliary heating system includes an infrared heating tube for radiating infrared rays into the interior of the polycondensation tower. The heating amount of the infrared rays radiated by the infrared heating tube gradually decreases along the direction from the feed port to the discharge port of the polycondensation tower.

3. The method according to claim 2, It is characterized in that The infrared wavelength radiated by the infrared heating tube is 2.5-10 μm.

4. The method according to any one of claims 1 to 3, It is characterized in that The particle size of the polyester polymer entering the polycondensation tower is below 6 mm, preferably 2 to 4 mm.

5. The method according to any one of claims 1 to 4, It is characterized in that The gas-to-material ratio entering the polycondensation tower is controlled to be 1:(50-130) L / g.

6. The method according to any one of claims 1 to 5, It is characterized in that The crystallization reaction temperature in the crystallization tower is controlled to be 170-205° C., and the crystallization reaction time is less than 2 hours.

7. The method according to claim 6, It is characterized in that The crystallization tower uses nitrogen and material convection to perform crystallization treatment on the polyester polymer.

8. The method according to claim 7, It is characterized in that The gas-to-material ratio entering the crystallizer is controlled to be 1:(50-130) L / g.

9. The method according to any one of claims 1 to 8, It is characterized in that The polyester polymer is selected from polyglycolic acid.

10. The method according to any one of claims 1 to 9, It is characterized in that The polyester polymer has a weight average molecular weight of 100,000 to 150,000, a residual monomer content of 1 to 5%, a melt index of 20 to 50 g / 10 min, and a migration amount of not less than 53 mg / L based on glycolic acid; After solid phase viscosity enhancement in the polycondensation tower, the weight average molecular weight of the polyester particles is 130,000 to 200,000, the residual monomer content is 0.5 to 1%, and the melt index is 10 to 30 g / 10 min; the migration amount is no more than 28 mg / L based on glycolic acid.