Microencapsulated release agent, preparation method thereof and application of microencapsulated release agent in molding clay
By encapsulating the liquid release agent in the calcium carbonate shell to form a microencapsulated release agent, and using external force to break and release the release agent, the problem of adhesion and poor compatibility between the plastic clay and the mold is solved, and efficient three-dimensional molding is achieved. Decorative painting production.
Patent Information
- Application Number
- CN202410761274.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-13
- Publication Date
- 2024-10-08
AI Technical Summary
Due to its high viscosity, existing plastic clay materials are prone to adhesion to molds and cannot be used for mass production of three-dimensional decorative paintings by industrial methods such as imprinting. At the same time, traditional release agents have poor compatibility with plastic clay, which affects subsequent coloring. Grooming.
Using microencapsulated release agent, the liquid release agent is encapsulated in the calcium carbonate shell as the core material to form an olive-shaped microencapsulated release agent, and the calcium carbonate shell is broken by external force to release the release agent, achieving efficient release. mold.
The compatibility between the release agent and the modeling clay matrix is improved, and the release agent is quickly released by breaking the calcium carbonate shell through external force, achieving efficient demoulding and reducing the need for inorganic fillers in the modeling clay.
Smart Images

Figure CN118745286A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of clay materials, and in particular to a microencapsulated release agent, a preparation method thereof and application thereof in shaping clay. Background Art
[0002] In recent years, three-dimensional decorative paintings have been loved by a large number of consumers due to their unique modeling language. The combination of this two-dimensional painting and three-dimensional sculpture art makes the decorative paintings more visually impactful and artistically appealing, giving the works a higher artistic value. For example, Chinese patent CN201210140507.8 has developed a modeling clay material for making three-dimensional paintings, and the modeling clay has good plasticity and adhesion. When drawing three-dimensional decorative paintings, the creator can use tools such as scrapers to shape the modeling clay into a three-dimensional shape on the canvas, and then further color it after the clay is completely dried. However, the above-mentioned manual painting method has low production efficiency and cannot guarantee the consistency of the product. With the increasing market demand for three-dimensional decorative paintings, it is urgently needed to develop a modeling clay that can be used for industrialized methods such as embossing to mass-produce three-dimensional decorative paintings.
[0003] However, the existing modeling clay materials are easy to adhere to the mold due to their high viscosity, and cannot be used for industrial methods such as embossing to produce three-dimensional decorative paintings in large quantities. Traditional internal release agents such as silicone oil have poor compatibility with modeling clay and excessive enrichment on the surface of the profile, which affects the subsequent coloring and modification. They cannot be directly added to the modeling clay. Therefore, if the internal release agent can be microencapsulated with inorganic materials such as calcium carbonate, it can not only effectively improve the compatibility of the release agent with the modeling clay matrix, but also cleverly utilize the brittleness of inorganic materials. When producing three-dimensional decorative paintings, the inorganic shell material of the release agent microcapsule can be broken by production methods such as embossing to release the release agent to achieve efficient demolding. Summary of the invention
[0004] In order to solve the above technical problems, the present invention provides a microencapsulated mold release agent and a preparation method thereof and application in molding clay. The microencapsulated mold release agent of the present invention encapsulates a liquid mold release agent as a core material in a calcium carbonate shell layer, and uses it as a raw material for molding clay, which not only has good compatibility with the molding clay matrix, but also can cleverly utilize the brittleness of the calcium carbonate shell layer, and after molding, the calcium carbonate shell layer is broken by external force to release the mold release agent, thereby achieving efficient demoulding.
[0005] The specific technical scheme of the present invention is: In a first aspect, the present invention provides a microencapsulated release agent, comprising an olive-shaped calcium carbonate shell layer, and a liquid release agent core material encapsulated in the calcium carbonate shell layer.
[0006] The present invention ingeniously encapsulates a liquid release agent as a core material in a calcium carbonate shell layer to obtain a microencapsulated release agent. When used as a raw material for shaping clay, the microencapsulated release agent not only has good compatibility with the shaping clay matrix, but also can ingeniously utilize the brittleness of the calcium carbonate shell layer to break the calcium carbonate shell layer by embossing and other methods when producing three-dimensional decorative paintings, thereby releasing the release agent to achieve efficient demoulding. In addition, the calcium carbonate can be used as an inorganic filler for shaping clay, so that less or even no additional inorganic filler can be added to the shaping clay.
[0007] The present invention finds that the breakability of the microencapsulated release agent is affected by different morphologies. We further find that the olive-shaped calcium carbonate shell is more easily broken by external forces than the traditional spherical shell due to uneven force.
[0008] Preferably, the thickness of the calcium carbonate shell layer is 100-200 nm.
[0009] In order to further ensure that the microencapsulated release agent is broken after being subjected to external forces such as stamping, the thickness of the calcium carbonate shell layer is limited to the above range. If the calcium carbonate shell layer is too thin, it may lead to a low encapsulation rate of the liquid release agent core material and a large amount of core material leakage; if the calcium carbonate shell layer is too thick, it may require a greater external force to break the microencapsulated release agent in large quantities.
[0010] Preferably, the particle size of the microencapsulated release agent is in the range of 2-4 μm.
[0011] Preferably, the liquid release agent core material is a silicone oil-based release agent; more preferably, the silicone oil-based release agent is selected from one or more of siloxane compounds, silicone resin methyl branched silicone oil, methyl silicone oil, hydrogen-containing methyl silicone oil and silicone grease. Dimethyl silicone oil is most preferred.
[0012] In a second aspect, the present invention provides a method for preparing the above-mentioned microencapsulated release agent, comprising the following steps: 1) Mix and evenly stir a liquid release agent core material, an anionic surfactant and an organic solvent to obtain a microemulsion A.
[0013] 2) dissolving a soluble calcium salt in an organic solvent and adding the solution to the microemulsion for uniform mixing to obtain a microemulsion B; calcium ions are electrostatically adsorbed on the surface of emulsion droplets in the microemulsion B.
[0014] 3) The soluble carbonate aqueous solution is added dropwise to the microemulsion B and mixed evenly to obtain a mixed solution containing a microencapsulated release agent after reaction.
[0015] 4) separating the precipitated microencapsulated release agent in the mixed solution, washing and drying to obtain the microencapsulated release agent.
[0016] The preparation principle of the microencapsulated release agent of the present invention is as follows: a liquid release agent is dispersed in an organic solvent by an anionic surfactant to obtain a microemulsion, then calcium cations and anionic surfactants are adsorbed on the surface of emulsion droplets by electrostatic action, and finally an aqueous solution containing carbonate ions is added to react with calcium ions to in-situ precipitate on the surface of the emulsion droplets to form a calcium carbonate shell layer, thereby preparing the microencapsulated release agent.
[0017] Preferably, in step 1), the liquid release agent core material, anionic surfactant and organic solvent are used in a ratio of 1.8-2.2 g: 1.4-1.8 g: 20-30 mL. In step 2), the soluble calcium salt and organic solvent are used in a ratio of 0.8-1.2 g: 14-18 mL. In step 3), the content of soluble carbonate in the soluble carbonate aqueous solution is 0.8-1.2 g / 10-20 mL.
[0018] The present invention finds that the amount of liquid release agent core material, soluble calcium salt, soluble carbonate and organic solvent plays a decisive role in whether an ideal olive-shaped microcapsule can be formed and the thickness of the calcium carbonate shell layer. Specifically: high concentrations of calcium ions and carbonate ions can cause calcium carbonate to rapidly nucleate and grow, and then form an anisotropic olive-shaped microencapsulated release agent. The particle size of the emulsion droplets can be controlled by adjusting the amount of liquid release agent core material. When the amount of soluble calcium salt, soluble carbonate and organic solvent is fixed, the shell material thickness of the microencapsulated release agent will decrease as the particle size of the emulsion droplets increases. The present invention finds that by controlling the amount of the above substances within the above amount ratio range, an ideal olive-shaped microcapsule and a suitable thickness of the calcium carbonate shell layer can be obtained.
[0019] Preferably, in step 3), the dropping speed is 1-2 mL / min.
[0020] Preferably, in step 1) to step 3), the stirring speed is 600-800 rpm and the time is 1-3 h.
[0021] Preferably, in step 4), the separation is performed by centrifugation at a speed of 3000-4000 rpm for 3-5 min; the washing is performed by sequentially washing with deionized water and anhydrous ethanol for 3-5 times; the drying temperature is 30-40°C for 24-48 h.
[0022] Preferably, the anionic surfactant is sodium dodecyl sulfate; the soluble calcium salt is calcium chloride; the soluble carbonate is sodium carbonate; and the organic solvent is formamide.
[0023] In a third aspect, the present invention provides an easily demouldable plastic clay, comprising the following raw materials: 25-35 parts by weight of the microencapsulated demoulding agent according to any one of claims 1 to 3, and 8-12 parts by weight of a polymer emulsion.
[0024] Preferably, the polymer emulsion includes one or more of pure acrylic emulsion, silicone acrylic emulsion, and styrene acrylic emulsion, and pure acrylic emulsion is further preferred.
[0025] In a fourth aspect, the present invention provides a method for preparing plastic clay that is easy to demold, comprising: mixing a polymer emulsion, a dispersant, a wetting agent, a defoaming agent and water and stirring evenly; adding a microencapsulated demolding agent and stirring evenly; adding a thickener and stirring evenly to obtain plastic clay that is easy to demold.
[0026] Preferably, the usage ratio of the polymer emulsion, dispersant, wetting agent, defoamer, water and thickener is 8-12g: 0.3-0.7g: 0.05-0.15g: 0.5-1.5g: 2-4g: 0.1-0.3g.
[0027] Preferably, the dispersant includes one or more of sodium tripolyphosphate, sodium hexametaphosphate, sodium pyrophosphate, triethylhexyl phosphate, sodium dodecyl sulfate, methyl amyl alcohol, cellulose derivatives, sodium polyacrylate, guar gum, fatty acid polyethylene glycol esters and polyethers, and sodium polyacrylate is more preferred.
[0028] Preferably, the wetting agent includes one or more of alkyl polyoxyethylene ether, polyether silicone and non-ionic fluorocarbon polymers, and alkyl polyoxyethylene ether is further preferred.
[0029] Preferably, the defoaming agent includes one or more of silicones, mineral oils, polyethers and higher alcohols, and FB-50 silicone defoaming agent is further preferred.
[0030] Preferably, the thickener includes one or more of sodium carboxymethyl cellulose, polyacrylate and associative polyurethane, and sodium carboxymethyl cellulose is further preferred.
[0031] Preferably, the stirring speed is 300-500 rpm, and the stirring time is 20-40 min.
[0032] Compared with the prior art, the beneficial effects of the present invention are: (1) The microencapsulated release agent of the present invention encapsulates the liquid release agent as the core material in the calcium carbonate shell layer, and uses it as the raw material of the molding clay. It not only has good compatibility with the molding clay matrix, but also can cleverly utilize the brittleness of the calcium carbonate shell layer. After molding, the calcium carbonate shell layer is broken by external force to release the release agent, thereby achieving efficient demolding. In addition, the calcium carbonate can be used as an inorganic filler for molding clay, so less or even no additional inorganic filler can be added to the molding clay.
[0033] (2) The present invention adjusts the morphology of the microencapsulated release agent to be olive-shaped, and further adjusts the calcium carbonate shell to 100-200 nm, which can effectively encapsulate the liquid release agent core material and facilitate the calcium carbonate shell to break under the action of external force, thereby achieving rapid demolding. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] Figure 1 Schematic diagram of the preparation principle of the microencapsulated release agent of the present invention.
[0035] Figure 2 This is the XRD spectrum of the microencapsulated release agent in Example 1.
[0036] Figure 3 This is the FTIR spectrum of the microencapsulated release agent in Example 1.
[0037] Figure 4 This is the SEM image of the microencapsulated release agent in Example 1.
[0038] Figure 5 This is the TEM image of the microencapsulated release agent in Example 1.
[0039] Figure 6 This is the TEM image of the microencapsulated release agent in Comparative Example 1.
[0040] Figure 7 This is a digital photograph of the modeling clay containing microencapsulated release agent in Example 1 produced by mold stamping. DETAILED DESCRIPTION
[0041] The present invention will be further described below in conjunction with the embodiments.
[0042] Overall embodiment A microencapsulated demoulding agent comprises an olive-shaped calcium carbonate shell layer and a liquid demoulding agent core material encapsulated in the calcium carbonate shell layer.
[0043] In some specific implementation cases, the thickness of the calcium carbonate shell layer ranges from 100 to 200 nm.
[0044] In some specific implementation cases, the particle size of the microencapsulated release agent is in the range of 2-4 μm.
[0045] In some specific implementation cases, the liquid release agent core material is a silicone oil-based release agent; further preferably, it is one or more selected from siloxane compounds, silicone resin methyl branched silicone oil, methyl silicone oil, hydrogen-containing methyl silicone oil and silicone grease; and most preferably, it is dimethyl silicone oil.
[0046] First, a method for preparing the above-mentioned microencapsulated release agent, such as Figure 1 The schematic diagram of the preparation of the microencapsulated release agent of the present invention is shown, which specifically includes the following steps: 1) Mix and evenly stir a liquid release agent core material, an anionic surfactant and an organic solvent to obtain a microemulsion A.
[0047] In some specific implementation cases, the usage ratio of the liquid release agent core material, the anionic surfactant and the organic solvent is in the range of 1.8-2.2 g: 1.4-1.8 g: 20-30 mL.
[0048] In some specific implementation cases, the anionic surfactant is sodium dodecyl sulfate, and the organic solvent is formamide. In some specific implementation cases, the stirring speed ranges from 600 to 800 rpm, and the stirring time ranges from 1 to 3 hours.
[0049] 2) dissolving a soluble calcium salt in an organic solvent and adding the solution to the microemulsion for uniform mixing to obtain a microemulsion B; calcium ions are electrostatically adsorbed on the surface of emulsion droplets in the microemulsion B.
[0050] In some specific implementation cases, the ratio of the soluble calcium salt to the organic solvent is in the range of 0.8-1.2 g: 14-18 mL. In some specific implementation cases, the soluble calcium salt is calcium chloride; the organic solvent is formamide. In some specific implementation cases, the stirring speed is in the range of 600-800 rpm, and the stirring time is in the range of 1-3 h.
[0051] 3) The soluble carbonate aqueous solution is added dropwise to the microemulsion B and mixed evenly to obtain a mixed solution containing a microencapsulated release agent after reaction.
[0052] In some specific implementation cases, the content of soluble carbonate in the soluble carbonate aqueous solution is in the range of 0.8-1.2 g / 10-20 mL. In some specific implementation cases, the soluble carbonate is sodium carbonate. In some specific implementation cases, the speed of the dripping is in the range of 1-2 mL / min. In some specific implementation cases, the stirring speed is in the range of 600-800 rpm, and the stirring time is in the range of 1-3 h.
[0053] 4) separating the precipitated microencapsulated release agent in the mixed solution, washing and drying to obtain the microencapsulated release agent.
[0054] In some specific implementation cases, the separation is performed by centrifugation, the centrifugal speed ranges from 3000-4000rpm, and the centrifugal time ranges from 3-5min; the washing is performed sequentially with deionized water and anhydrous ethanol, the number of times ranges from 3-5 times, the drying temperature ranges from 30-40°C, and the drying time ranges from 24-48h.
[0055] Secondly, a plastic clay that is easy to demould comprises: 25-35 parts by weight of the microencapsulated demoulding agent prepared by the above method and 8-12 parts by weight of the polymer emulsion.
[0056] In some specific implementation cases, the polymer emulsion includes one or more of pure acrylic emulsion, silicone acrylic emulsion, and styrene acrylic emulsion, and pure acrylic emulsion with a solid content in the range of 50-60wt% is further preferred.
[0057] Furthermore, a method for preparing the above-mentioned easily demouldable plastic clay specifically comprises the following steps: mixing a polymer emulsion, a dispersant, a wetting agent, a defoaming agent and water and stirring evenly; adding a microencapsulated demoulding agent and stirring evenly; adding a thickener and stirring evenly to obtain an easily demouldable plastic clay.
[0058] In some specific implementation cases, the usage ratio of the polymer emulsion, dispersant, wetting agent, defoamer, water and thickener is in the range of 8-12g: 0.3-0.7g: 0.05-0.15g: 0.5-1.5g: 2-4g: 0.1-0.3g.
[0059] In some specific implementation cases, the dispersant includes one or more of sodium tripolyphosphate, sodium hexametaphosphate, sodium pyrophosphate, triethylhexyl phosphoric acid, sodium dodecyl sulfate, methyl amyl alcohol, cellulose derivatives, sodium polyacrylate, guar gum, fatty acid polyethylene glycol esters and polyethers, and sodium polyacrylate is further preferred. In some specific implementation cases, the wetting agent includes one or more of alkyl polyoxyethylene ether, polyether silicone and non-ionic fluorocarbon polymers, and alkyl polyoxyethylene ether is further preferred. In some specific implementation cases, the defoamer includes one or more of silicones, mineral oils, polyethers and high-carbon alcohols, and FB-50 type silicone defoamer is further preferred. In some specific implementation cases, the thickener includes one or more of sodium carboxymethyl cellulose, polyacrylate and associative polyurethane, and sodium carboxymethyl cellulose is further preferred.
[0060] In some specific implementation cases, the stirring speed ranges from 300-500 rpm, and the stirring time ranges from 20-40 min.
[0061] Specific Examples and Comparative Examples Example 1 The first step is to prepare a microencapsulated release agent, which specifically comprises the following steps: (1) Add 2.0 g of dimethyl silicone oil into a three-necked flask, then add 0.8 g of sodium dodecyl sulfate and 25 ml of formamide, and then mechanically stir and mix at a speed of 700 rpm for 2 h; (2) Dissolve 1.0 g of calcium chloride in 16 ml of formamide and slowly add the mixture into a three-necked flask and continue to mechanically stir and mix at 700 rpm for 2 h; (3) 1.0 g of sodium carbonate was dissolved in 15 ml of deionized water and slowly added to the three-necked flask at a rate of 1 ml / min using a peristaltic pump and mechanically stirred at 700 rpm for 2 h; (4) After the reaction is completed, the precipitate is separated by centrifugation at 3000 rpm for 3 min, washed with deionized water and anhydrous ethanol for 3 times respectively, and then dried in a forced air drying oven at 40° C. for 24 h to obtain a microencapsulated release agent.
[0062] The second step is to prepare a plasticine clay containing a microencapsulated release agent, which specifically comprises the following steps: (1) Add 10 g of pure acrylic emulsion with a solid content of 55 wt%, 0.5 g of sodium polyacrylate, 0.1 g of alkyl polyoxyethylene ether, 1.0 g of FB-50 type silicone defoamer and 3 g of water into a beaker and stir and mix at a speed of 400 rpm for 30 min; (2) adding 20 g of microencapsulated release agent and stirring at 400 rpm for 30 min; (3) Add 0.2 g of sodium carboxymethyl cellulose and stir at 400 rpm for 30 min to obtain a molding clay containing a microencapsulated release agent.
[0063] Example 2 The first step is to prepare a microencapsulated release agent, which specifically comprises the following steps: (1) Add 1.8 g of dimethyl silicone oil into a three-necked flask, then add 0.4 g of sodium dodecyl sulfate and 20 ml of formamide, and then mechanically stir and mix at 700 rpm for 1 h; (2) Dissolve 0.8 g of calcium chloride in 14 ml of formamide and slowly add the mixture into a three-necked flask and continue to mechanically stir and mix at 600 rpm for 1 h; (3) 0.8 g of sodium carbonate was dissolved in 10 ml of deionized water and slowly added to the three-necked flask at a rate of 1 ml / min using a peristaltic pump and mechanically stirred at a speed of 600 rpm for 1 h; (4) After the reaction is completed, the precipitate is separated by centrifugation at 3000 rpm for 3 min, washed with deionized water and anhydrous ethanol for 3 times respectively, and then dried in a forced air drying oven at 40° C. for 24 h to obtain a microencapsulated release agent.
[0064] The second step is to prepare a plasticine clay containing a microencapsulated release agent, which specifically comprises the following steps: (1) Add 8 g of pure acrylic emulsion with a solid content of 55 wt%, 0.3 g of sodium polyacrylate, 0.05 g of alkyl polyoxyethylene ether, 0.5 g of FB-50 type silicone defoamer and 2 g of water into a beaker and stir and mix at a speed of 300 rpm for 20 min; (2) adding 25 g of microencapsulated release agent and stirring at 300 rpm for 20 min; (3) Add 0.1 g of sodium carboxymethyl cellulose and stir at 300 rpm for 20 min to obtain a molding clay containing a microencapsulated release agent.
[0065] Example 3 The first step is to prepare a microencapsulated release agent, which specifically comprises the following steps: (1) Add 2.2 g of dimethyl silicone oil into a three-necked flask, then add 1.2 g of sodium dodecyl sulfate and 30 ml of formamide, and then mechanically stir and mix at a speed of 800 rpm for 3 h; (2) Dissolve 1.2 g of calcium chloride in 18 ml of formamide and slowly add the mixture into a three-necked flask and continue to mechanically stir and mix at 800 rpm for 3 h; (3) 1.2 g of sodium carbonate was dissolved in 20 ml of deionized water and slowly added to the three-necked flask at a rate of 1 ml / min using a peristaltic pump and mechanically stirred at a speed of 800 rpm for 3 h; (4) After the reaction is completed, the precipitate is separated by centrifugation at 3000 rpm for 3 min, washed with deionized water and anhydrous ethanol for 3 times respectively, and then dried in a forced air drying oven at 40° C. for 24 h to obtain a microencapsulated release agent.
[0066] The second step is to prepare a plasticine clay containing a microencapsulated release agent, which specifically comprises the following steps: (1) Add 12 g of pure acrylic emulsion with a solid content of 55 wt%, 0.7 g of sodium polyacrylate, 0.15 g of alkyl polyoxyethylene ether, 1.5 g of FB-50 type silicone defoamer and 4 g of water into a beaker and stir and mix at a speed of 500 rpm for 40 min; (2) adding 35 g of microencapsulated release agent and stirring at 500 rpm for 40 min; (3) 0.3 g of sodium carboxymethyl cellulose was added and stirred at 500 rpm for 40 min to obtain a molding clay containing a microencapsulated release agent.
[0067] Comparative Example 1 The first step is to prepare a microencapsulated release agent, which specifically comprises the following steps: (1) Add 1.0 g of dimethyl silicone oil into a three-necked flask, then add 0.8 g of sodium dodecyl sulfate and 25 ml of formamide, and then mechanically stir and mix at a speed of 700 rpm for 2 h; (2) Dissolve 1.0 g of calcium chloride in 16 ml of formamide and slowly add the mixture into a three-necked flask and continue to mechanically stir and mix at 700 rpm for 2 h; (3) 1.0 g of sodium carbonate was dissolved in 15 ml of deionized water and slowly added to the three-necked flask at a rate of 1 ml / min using a peristaltic pump and mechanically stirred at 700 rpm for 2 h; (4) After the reaction is completed, the precipitate is separated by centrifugation at 3000 rpm for 3 min, washed with deionized water and anhydrous ethanol for 3 times respectively, and then dried in a forced air drying oven at 40° C. for 24 h to obtain a microencapsulated release agent.
[0068] The second step is to prepare a plasticine clay containing a microencapsulated release agent, which specifically comprises the following steps: (1) Add 10 g of pure acrylic emulsion with a solid content of 55 wt%, 0.5 g of sodium polyacrylate, 0.1 g of alkyl polyoxyethylene ether, 1.0 g of FB-50 type silicone defoamer and 3 g of water into a beaker and stir and mix at a speed of 400 rpm for 30 min; (2) adding 20 g of microencapsulated release agent and stirring at 400 rpm for 30 min; (3) Add 0.2 g of sodium carboxymethyl cellulose and stir at 400 rpm for 30 min to obtain a molding clay containing a microencapsulated release agent.
[0069] Performance Test and Characterization The following are the test data of the microencapsulated release agent obtained in the above different embodiments and Comparative Example 1 and the plastic clay containing the microencapsulated release agent, wherein: (1) XRD test: Figure 2 The XRD spectrum of the microencapsulated release agent prepared in Example 1 is shown in FIG. Figure 2 It can be found that the diffraction peaks at 2θ angle positions of 23.1°, 29.4°, 35.9°, 39.4°, 43.1°, 47.5°, and 48.5° correspond to the (0 1 2), (1 0 4), (1 1 0), (1 1 3), (2 0 2), (0 1 8), and (116) crystal planes of calcite-type calcium carbonate, respectively (JCPDF 83-0578). The above data confirm the successful synthesis of the calcium carbonate shell layer in the microencapsulated release agent.
[0070] (2) Infrared test: Figure 3 FT-IR spectra of the liquid release agent core material dimethyl silicone oil and the final microencapsulated release agent in Example 1. Figure 3It can be found that dimethyl silicone oil is at 2962.12cm -1 The absorption peak at 1261.21 cm -1 The Si-CH3 bond bending vibration absorption peak is 1016.43 cm -1 The absorption peak at 863.95 cm is the Si-O-Si stretching vibration absorption peak. -1 The absorption peak at 796.45 cm belongs to the in-plane swing vibration of the CH bond. -1 The absorption peak at 1419.13cm belongs to the stretching vibration absorption peak of C-Si bond. -1 The broad absorption peak at is the CO3 in calcium carbonate 2- The antisymmetric stretching vibration of the group is at 875.52 cm -1 The absorption peak at is the CO3 in calcium carbonate 2- The out-of-plane bending vibration absorption peak of the group is at 711.60 cm -1 CO3 2- The above results further prove that the synthesized microencapsulated release agent has an ideal chemical composition, which is completely composed of calcium carbonate and dimethyl silicone oil.
[0071] (3) SEM observation: Figure 4 is the SEM of the microencapsulated release agent prepared in Example 1, from Figure 4 It can be seen that the shape of the microencapsulated release agent is olive-shaped. From the SEM image, it was measured that the average length of the long axis of the microencapsulated release agent was about 2.84 μm, and the average length of the short axis was about 1.74 μm. The formation of this shape is due to the influence of the specific ratio of calcium ions, carbonate ions and formamide. The high concentration of calcium ions and carbonate ions causes calcium carbonate to nucleate and grow rapidly, and then forms an anisotropic olive-shaped microencapsulated release agent. Compared with traditional spherical microcapsules, the olive-shaped microencapsulated release agent prepared by the present invention is easier to break to release the release agent.
[0072] (4) TEM observation: Figure 5 and Figure 6 The following are transmission electron microscope (TEM) images of the microencapsulated release agents prepared in Example 1 and Comparative Example 1, respectively. Figure 5 and Figure 6 It can be seen that the microencapsulated release agents prepared in Example 1 and Comparative Example 1 are both olive-shaped and have obvious core-shell structures. However, the difference is: Figure 5 The average shell thickness of the microencapsulated release agent in (Example 1) is about 160 nm, while Figure 6The average shell thickness of the microencapsulated release agent in (Comparative Example 1) is about 392nm. That is to say, the thickness of the calcium carbonate shell of the microencapsulated release agent prepared according to the method of Comparative Example 1 is significantly thicker than that of Example 1. This result first further proves that the microencapsulated release agent synthesized by the present invention is composed of a calcium carbonate shell and a liquid release agent core material (dimethyl silicone oil), and has an ideal microstructure; secondly, the above picture also proves that the calcium carbonate shell thickness of the microencapsulated release agent can be effectively controlled by adjusting the amount of the liquid release agent core material (dimethyl silicone oil) in the preparation method of the present invention. Compared with Comparative Example 1, the thinner calcium carbonate shell in Example 1 can be more easily broken to release the liquid release agent core material.
[0073] (5) Encapsulation efficiency test: Table 1 shows the dimethyl silicone oil encapsulation efficiency of the microencapsulated release agents prepared in the above different embodiments and comparative example 1. The microencapsulated release agents prepared in the different embodiments and comparative example 1 were completely dried and weighed, then repeatedly ground and washed with n-hexane and anhydrous ethanol for many times, and the ground and washed microencapsulated release agents were completely dried again and weighed, and the dimethyl silicone oil encapsulation efficiency of the microencapsulated release agents was calculated by the following formula: Where W1 is the weight before grinding and washing, and W2 is the weight after grinding and washing.
[0074] As can be seen from Table 1, the prepared microencapsulated release agent has a high encapsulation rate and contains a large amount of dimethyl silicone oil. After being added to the modeling clay as a filler, it can provide sufficient dimethyl silicone oil to promote demoulding.
[0075] Table 1 Sample name Encapsulation rate (%) Example 1 51.3% Example 2 34.6% Example 3 40.9% Comparative Example 1 15.9% (6) Demolding effect test: Figure 7 The following is a digital photo of the modeling clay containing microencapsulated release agent prepared in Example 1 produced by mold embossing. The prepared modeling clay containing microencapsulated release agent is filled into the mold and slightly higher than the mold surface, and then the mold is turned upside down on the canvas, and pressure is continuously applied for 25 minutes to complete the release of the release agent. Finally, the modeling clay is left to stand for 10 hours until the modeling clay is solidified and demoulding can be completed. It can be seen from the photo that the modeling clay containing microencapsulated release agent prepared in Example 1 of the present invention can be effectively demoulded when producing three-dimensional decorative paintings by embossing, and the resulting modeling shape is complete, and a vivid modeling can be formed on the canvas.
[0076] In summary, the microencapsulated release agent and the preparation method thereof provided by the present invention have the following beneficial effects compared with the prior art: (1) The present invention disperses a liquid release agent in an organic solvent by an anionic surfactant to obtain a microemulsion, then calcium cations and anionic surfactants are adsorbed on the surface of emulsion droplets by electrostatic action, and finally an aqueous solution containing carbonate ions is added to react with calcium ions to in-situ precipitate on the surface of the emulsion droplets to form a calcium carbonate shell layer, thereby preparing a microencapsulated release agent.
[0077] (2) The microencapsulated release agent of the present invention encapsulates the liquid release agent as the core material in the calcium carbonate shell layer, and uses it as the raw material of the molding clay. It not only has good compatibility with the molding clay matrix, but also can cleverly utilize the brittleness of the calcium carbonate shell layer. After molding, the calcium carbonate shell layer is broken by external force to release the release agent, thereby achieving efficient demolding. In addition, the calcium carbonate can be used as an inorganic filler for molding clay, so less or even no additional inorganic filler can be added to the molding clay.
[0078] (3) The present invention controls the morphology of the microencapsulated release agent to be olive-shaped. Compared with the traditional spherical shell, the olive-shaped calcium carbonate shell is more easily broken by external force due to uneven force and quickly releases the liquid release agent core material.
[0079] (4) The present invention further adjusts the calcium carbonate shell layer to 100-200 nm, which can facilitate the breaking of the calcium carbonate shell layer under the action of external force under the premise of effectively encapsulating the liquid release agent core material, thereby achieving rapid demolding.
[0080] The raw materials and equipment used in the present invention, unless otherwise specified, are all commonly used raw materials and equipment in the art; the methods used in the present invention, unless otherwise specified, are all conventional methods in the art.
[0081] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any way. Any simple modification, change and equivalent transformation made to the above embodiment based on the technical essence of the present invention still falls within the protection scope of the technical solution of the present invention.
Claims
1. A microencapsulated release agent, characterized in that: The invention comprises an olive-shaped calcium carbonate shell layer and a liquid release agent core material encapsulated in the calcium carbonate shell layer.
2. The microencapsulated release agent according to claim 1, characterized in that: The thickness of the calcium carbonate shell layer is 100-200 nm.
3. The microencapsulated release agent according to claim 1, characterized in that: The liquid release agent core material is a silicone oil-based release agent.
4. A method for preparing the microencapsulated release agent according to any one of claims 1 to 3, characterized in that The following steps are involved: 1) Mixing and uniformly stirring a liquid release agent core material, an anionic surfactant and an organic solvent to obtain a microemulsion A; 2) dissolving a soluble calcium salt in an organic solvent and adding the solution to the microemulsion, mixing the solution and dissolving the solution uniformly to obtain a microemulsion B; calcium ions are electrostatically adsorbed on the surface of the emulsion droplets in the microemulsion B; 3) adding the soluble carbonate aqueous solution dropwise to the microemulsion B and mixing evenly to obtain a mixed solution containing a microencapsulated release agent after reaction; 4) Separating the precipitated microencapsulated release agent from the mixed solution, and obtaining the microencapsulated release agent after washing and drying.
5. The preparation method according to claim 4, characterized in that: In step 1), The liquid release agent core material, anionic surfactant and organic solvent are used in a ratio of 1.8-2.2 g: 1.4-1.8 g: 20-30 mL; and / or The stirring speed is 600-800 rpm and the time is 1-3 h.
6. The preparation method according to claim 4, characterized in that: In step 2), The ratio of the soluble calcium salt to the organic solvent is 0.8-1.2 g:14-18 mL; and / or The stirring speed is 600-800 rpm and the time is 1-3 h.
7. The preparation method according to claim 4, characterized in that: In step 3), The content of soluble carbonate in the soluble carbonate aqueous solution is 0.8-1.2 g / 10-20 mL; and / or The dropping speed is 1-2 mL / min; and / or The stirring speed is 600-800 rpm and the time is 1-3 h.
8. The preparation method according to any one of claims 4 to 7, characterized in that: The anionic surfactant is sodium lauryl sulfate; and / or The soluble calcium salt is calcium chloride; and / or The soluble carbonate is sodium carbonate; and / or The organic solvent is formamide.
9. An easy-to-release plastic clay, characterized in that The method comprises the following raw materials: 25-35 parts by weight of the microencapsulated release agent according to any one of claims 1 to 3, and 8-12 parts by weight of a polymer emulsion.
10. A method for preparing plastic clay that is easy to demould, characterized in that include: The polymer emulsion, dispersant, wetting agent, defoamer and water are mixed and stirred evenly; the microencapsulated demoulding agent according to any one of claims 1 to 3 is added and stirred evenly; the thickener is added and stirred evenly to obtain plastic clay that is easy to demould.
Citation Information
Cited By
Water-based separant as well as preparation method and application thereof
CN121574640A