Lubricating grease composition and preparation method thereof, and commercial vehicle chassis system lubricating grease

By adding phosphorothioate amine salts and other specific components to the grease, a grease composition with excellent high temperature resistance, oxidation resistance, and extreme pressure and anti-wear properties is formed, which solves the problem of short grease replacement intervals for commercial vehicle chassis systems. and insufficient performance, extending the service life of the grease.

CN118745367APending Publication Date: 2024-10-08FAW JIEFANG AUTOMOTIVE CO
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411068880.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-06
Publication Date
2024-10-08

AI Technical Summary

Technical Problem

The grease replacement cycle of commercial vehicle chassis systems is short and requires frequent maintenance, and the existing grease has insufficient antioxidant and anti-wear properties under high temperature and heavy load conditions.

Method used

A grease composition is used, including hydrogenated base oil, thickener, structure improver, phosphorothioate amine salt and rust inhibitor. Through the addition of phosphorothioate amine salt, a specific ratio of thickener and anti-rust agent is combined. Rust agent, forming a protective film with excellent high temperature resistance, oxidation resistance and extreme pressure and wear resistance.

Benefits of technology

It extends the grease replacement cycle, improves the chemical stability and functional performance of the grease, and ensures long-term lubrication protection under high temperature and heavy load conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure QLYQS_1
    Figure QLYQS_1
  • Figure QLYQS_2
    Figure QLYQS_2
  • Figure QLYQS_3
    Figure QLYQS_3
Patent Text Reader

Abstract

The invention relates to the technical field of lubricating grease, in particular to a lubricating grease composition, a preparation method thereof and commercial vehicle chassis system lubricating grease. The lubricating grease composition provided by the invention is prepared from the following components in parts by weight: 80 to 90 parts of base oil, 7 to 12 parts of a thickening agent, 0.8 to 1.5 parts of a structure improving agent, 2 to 6 parts of ammonium thiophosphate and 0.03 to 0.07 part of an anti-rust agent, wherein the base oil is hydrogenated base oil, and the viscosity of the base oil at the temperature of 40 DEG C is 120 mm < 2 > / s to 160 mm < 2 > / s. The lubricating grease composition provided by the invention has excellent high temperature resistance, oxidation resistance and extreme pressure wear resistance. Therefore, the lubricating grease replacement mileage can be effectively prolonged, and the problem of short lubricating grease replacement mileage at present is solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of lubricating greases, and in particular to a lubricating grease composition and a preparation method thereof, and a lubricating grease for a commercial vehicle chassis system. Background Art

[0002] Grease is a liquid or semi-solid lubricant used in various types of automobiles and mechanical equipment to reduce friction and protect machinery and processed parts. It mainly plays the role of lubrication, auxiliary cooling, rust prevention, cleaning, sealing and buffering. At present, the grease replacement cycle of commercial vehicle chassis system is short, and users need to perform frequent maintenance, which is time-consuming and costly. In order to extend the grease replacement cycle, in addition to maintaining the stability of the grease structure and reducing the oxidation or loss of the base oil, the lubricating layer formed on the friction pair surface must also provide long-term lubrication protection. Therefore, the long-replacement grease should have excellent high temperature resistance, oxidation resistance and extreme pressure and wear resistance.

[0003] At present, zinc dialkyl dithiophosphate (ZDDP) additives added to grease can improve the oxidation resistance of grease, but ZDDP has poor thermal stability and will decompose at high temperatures, resulting in slightly poor wear resistance and fatigue loss resistance. Dialkyl dithiocarbamate / ester (MDTC) additives added to grease have high temperature resistance, but grease containing this additive has the disadvantage of poor anti-wear performance. Summary of the invention

[0004] Based on this, the present application provides a grease composition and a preparation method thereof, and a commercial vehicle chassis system grease. The grease composition provided in the present application can have excellent high temperature resistance, oxidation resistance, and extreme pressure and anti-wear properties by adding thiophosphate amine salt and in coordination with other components.

[0005] In a first aspect of the present application, a grease composition is provided, wherein the grease composition comprises the following components, in parts by weight: 80 to 90 parts of base oil, 7 to 12 parts of thickener, 0.8 to 1.5 parts of structure improver, 2 to 6 parts of thiophosphate amine salt, and 0.03 to 0.07 parts of rust inhibitor;

[0006] Wherein, the base oil is a hydrogenated base oil, and the viscosity of the base oil at 40°C is 120 mm 2 / s~160mm 2 / s.

[0007] In one embodiment, the structure of the thiophosphate amine salt is ;

[0008] Among them, R 11 Each time it appears, it is independently S 1 Substituted or unsubstituted C1 ~C 6 Alkyl, S 2 Substituted or unsubstituted C 6 ~C 10 Aromatic group; S 1 and S 2 Each is independently selected from one or more of hydroxyl, nitro and halogen;

[0009] R 12 C 1 ~C 6 Alkylene; R 13 , R 14 are independently H, hydroxy-substituted or unsubstituted C 1 ~C 6 Alkyl, hydroxy substituted or unsubstituted C 6 ~C 10 aromatic group, and R 13 , R 14 Not H at the same time.

[0010] In one embodiment, R 11 Each occurrence is independently hydroxy-substituted or unsubstituted C 1 ~C 3 Alkyl, hydroxy substituted or unsubstituted C 6 ~C 10 Aromatic group;

[0011] R 12 C 1 ~C 3 Alkylene; R 13 , R 14 are independently H, hydroxy-substituted or unsubstituted C 1 ~C 4 Alkyl, and R 13 , R 14 Not H at the same time.

[0012] In one embodiment, the preparation steps of the thiophosphate amine salt include:

[0013] Mixing a phosphoric acid diester with a nitrogen-containing compound to prepare the thiophosphate amine salt;

[0014] Wherein, the structure of the phosphodiester is ; The structure of the nitrogen-containing compound is NHR 13 R 14 .

[0015] In one embodiment, the preparation steps of the phosphodiester include:

[0016] Using phosphorus pentoxide as a raw material, carrying out an esterification reaction with a hydroxyl-containing compound, and preparing the phosphoric acid diester after purification;

[0017] Wherein, the structure of the hydroxyl-containing compound is ;

[0018] R 21 Each time it appears, it is independently S 3 Substituted or unsubstituted C 1 ~C 6 Alkylene, S 4 Substituted or unsubstituted C 6 ~C 10 Arylene; S 3 and S 4 Each is independently selected from one or more of hydroxyl, nitro and halogen; R 22 is H or benzyloxy.

[0019] In one embodiment, the preparation steps of the hydroxyl-containing compound include:

[0020] Carrying out a substitution reaction between a dithiophosphate and a diol compound to prepare the hydroxyl-containing compound;

[0021] Wherein, the structure of the dithiophosphate is , the structure of the diol compound is .

[0022] In one embodiment, the preparation steps of the dithiophosphate include:

[0023] P 2 S 5 Carrying out an esterification reaction with a monophenol compound or a monoalcohol compound to prepare the dithiophosphate;

[0024] Wherein, the structures of the phenolic compound and the alcohol compound are independently R 22 -R 21 -OH.

[0025] In one embodiment, the thickener is a complex lithium soap; and

[0026] The thickener is prepared by saponification reaction of hydroxystearic acid, aliphatic dicarboxylic acid and lithium hydroxide.

[0027] In one embodiment, the thickener has one or more of the following characteristics:

[0028] (1) The aliphatic dicarboxylic acid includes one or more of sebacic acid, azelaic acid, glutaric acid, adipic acid and pimelic acid;

[0029] (2) The mass ratio of the hydroxystearic acid, the aliphatic dicarboxylic acid and the lithium hydroxide is (3.5-4.5):1:(1.01-1.04);

[0030] (3) The temperature of the saponification reaction is 125°C to 140°C.

[0031] In one embodiment, the structure improving agent includes one or more of cyclopentane salts and aromatic carboxylates;

[0032] Optionally, the naphthenate includes one or more of vanadium naphthenate, copper naphthenate, nickel naphthenate and sodium naphthenate;

[0033] Optionally, the aromatic carboxylate includes one or more of disodium terephthalate, disodium phthalate and disodium isophthalate.

[0034] In one embodiment, the structure of the rust inhibitor is , where R 2 H, halogen, C 1 ~C 6 Alkyl or C 1 ~C 6 Alkoxy.

[0035] In a second aspect of the present application, there is provided a method for preparing the grease composition according to any one of the embodiments of the first aspect of the present application, comprising the following steps:

[0036] Preheating hydroxystearic acid, aliphatic dicarboxylic acid and base oil accounting for 28% to 35% of the total mass to 80° C. to prepare a first mixed material;

[0037] Adding lithium hydroxide solution to the first mixed material to perform saponification reaction, thereby preparing the thickener to obtain a second mixed material;

[0038] Adding a structure improving agent to the second mixed material, and mixing at 200° C. to 210° C. to prepare a third mixed material;

[0039] The third mixed material is cooled to 170° C. to 180° C., and thiophosphate amine salt is added and mixed to prepare a fourth mixed material;

[0040] The fourth mixed material is cooled to 70° C. to 80° C., and a rust inhibitor and a base oil accounting for 65% to 72% of the total mass are added and mixed to prepare the grease composition.

[0041] The third aspect of the present application provides a commercial vehicle chassis system grease, comprising the grease composition described in any embodiment of the first aspect of the present application.

[0042] The grease composition selected in the present application can effectively ensure the oxidation stability of the grease composition by selecting a low-viscosity hydrogenated base oil with a high saturated hydrocarbon content; in addition, the ammonium thiophosphate has excellent chemical stability, and the sulfur and phosphorus elements contained therein can form a protective film with extreme pressure and anti-wear properties on the friction surface under heavy load and high temperature conditions to reduce direct contact between metals. At the same time, the ammonium thiophosphate and the hydrogenated base oil have good compatibility with a specific content of thickener, structure improver and rust inhibitor, so that the grease composition provided in the present application has excellent high temperature resistance, oxidation resistance and extreme pressure and anti-wear properties. Therefore, the grease composition provided in the present application can effectively extend the grease replacement mileage and solve the current problem of short grease replacement mileage. DETAILED DESCRIPTION

[0043] The following is a further complete and clear description of the grease composition and preparation method thereof, and the commercial vehicle chassis system grease of the present application in conjunction with specific examples. The present application can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the disclosure of the present application more thoroughly understood.

[0044] In the present application, "substituted" means that a hydrogen atom in a substituted group is replaced by a substituent.

[0045] In the present application, "substituted or unsubstituted" means that the defined group may be substituted or unsubstituted.

[0046] The term "alkyl" refers to a saturated hydrocarbon group containing primary (normal) carbon atoms, or secondary carbon atoms, or tertiary carbon atoms, or quaternary carbon atoms, or a combination thereof. Phrases containing this term, such as "C 1 ~C 6 "Alkyl" refers to an alkyl group containing 1 to 6 carbon atoms, each occurrence of which can be independently C 1 Alkyl, C 2 Alkyl, C 3 Alkyl, C 4 Alkyl, C 5 Alkyl, C 6 Suitable examples include, but are not limited to, methyl (Me, -CH 3 ), ethyl (Et, -CH 2 CH 3 ), 1-propyl (n-propyl, n-Pr, n-propyl, -CH 2 CH 2 CH 3 ), 2-propyl (i-Pr, i-propyl, -CH (CH 3 ) 2 ), 1-butyl (n-butyl, n-Bu, n-butyl, -CH2 CH 2 CH 2 CH 3 ), 2-methyl-1-propyl (i-Bu, i-butyl, -CH 2 CH(CH 3 ) 2 ), 2-butyl (s-Bu, s-butyl, -CH (CH 3 )CH 2 CH 3 ), tert-butyl(1,1-dimethylethyl, t-Bu, t-butyl, -C(CH 3 ) 3 ), 1-pentyl (n-pentyl, n-pentyl, -CH 2 CH 2 CH 2 CH 2 CH 3 ).

[0047] "Aromatic group" refers to an aromatic hydrocarbon group derived from an aromatic ring compound by removing a hydrogen atom. It can be a monocyclic aromatic group, a condensed aromatic group, or a polycyclic aromatic group. For polycyclic rings, at least one is an aromatic ring system. Phrases containing this term, such as "C 6 ~C 10 "Aryl" refers to an aromatic group containing 6 to 10 carbon atoms, each occurrence of which can be independently C 6 Aryl, C 10 Suitable examples include, but are not limited to, benzene, biphenyl, naphthalene and their derivatives.

[0048] "Alkylene" refers to a hydrocarbon group having two monovalent radical centers derived from an alkyl group by removing a hydrogen atom, which may be a saturated branched alkyl group or a saturated straight chain alkyl group. For example, "C 1 ~C 6 "Alkylene" means that the alkyl portion contains 1 to 6 carbon atoms, each occurrence can be independently C 1 Alkylene, C 4 Alkylene, C 5 Alkylene, C 6 Suitable examples include, but are not limited to, methylene (-CH 2 -), 1,1-ethyl (-CH(CH 3 )-), 1,2-ethyl (-CH 2 CH 2 -), 1,1-propyl (-CH(CH 2 CH 3 )-), 1,2-propyl (-CH 2 CH(CH 3)-), 1,3-propyl (-CH 2 CH 2 CH 2 -) and 1,4-butyl (-CH 2 CH 2 CH 2 CH 2 -).

[0049] In the present application, the single bond to which the substituent is connected runs through the corresponding ring, indicating that the substituent can be connected to any position of the ring, for example R is connected to any substitutable position of the benzene ring.

[0050] In the present application, "alkoxy" refers to a group having an -O-alkyl group, i.e., an alkyl group as defined above connected to a core structure via an oxygen atom. Phrases containing this term, for example, "C1-C6 alkoxy" means that the alkyl part contains 1 to 6 carbon atoms, and each occurrence can be independently C1 alkoxy, C4 alkoxy, C5 alkoxy, C6 alkoxy. Suitable examples include, but are not limited to: methoxy (-O-CH 3 or -OMe), ethoxy (-O-CH 2 CH 3 or -OEt) and tert-butyloxy (-OC(CH 3 ) 3 or -OtBu).

[0051] In a first aspect of the present application, a grease composition is provided, wherein the grease composition comprises the following components, in parts by weight: 80 to 90 parts of base oil, 7 to 12 parts of thickener, 0.8 to 1.5 parts of structure improver, 2 to 6 parts of thiophosphate amine salt, and 0.03 to 0.07 parts of rust inhibitor;

[0052] Wherein, the base oil is a hydrogenated base oil, and the viscosity of the base oil at 40°C is 120 mm 2 / s~160mm 2 / s.

[0053] Generally, grease compositions are less sensitive to additives, that is, the compatibility and reactivity between additives and base oils are weak, which limits the solubility, stability and function of additives in grease compositions. In addition, in traditional methods, in order to ensure that the grease composition can still form a thicker oil film under heavy load conditions and provide additional protection, a base oil with a relatively high viscosity is selected.

[0054] Based on rich experience and a large number of experiments, the inventors of this application have found that the grease composition composed of the base oil, thickener, structure improver, thiophosphate amine salt and rust inhibitor with the above-mentioned specific component content has excellent compatibility, so the stability and functional performance of each additive can be guaranteed. At the same time, the grease composition selected in this application can effectively ensure the oxidation stability of the grease composition by selecting a low-viscosity hydrogenated base oil with a high saturated hydrocarbon content; in addition, the thiophosphate ammonium salt has excellent chemical stability, and the sulfur and phosphorus elements contained therein can cooperate with the slightly lower viscosity base oil under heavy load and high temperature conditions to form a protective film with extreme pressure and anti-wear properties on the friction surface to reduce direct contact between metals.

[0055] At the same time, the ammonium thiophosphate salt and the hydrogenated base oil have good compatibility with the specific content of thickener, structure improver and rust inhibitor, so that the grease composition provided by the present application has excellent high temperature resistance, oxidation resistance and extreme pressure and anti-wear properties. Therefore, the grease composition provided by the present application can effectively extend the grease replacement mileage and solve the current problem of short grease replacement mileage.

[0056] It is understood that in the present application, the viscosity of the base oil at 40°C can be selected from 120 mm 2 / s~160mm 2 Specifically, the viscosity of the base oil at 40°C includes but is not limited to 120 mm 2 / s, 121 mm 2 / s, 122 mm 2 / s, 125 mm 2 / s, 130 mm 2 / s, 135 mm 2 / s, 140 mm 2 / s, 150 mm 2 / s, 155 mm 2 / s, 159 mm 2 / s or 160 mm 2 / s.

[0057] It is understandable that in the present application, the weight percentage of the base oil can be selected from any value between 80 and 90. Specifically, the weight percentage of the base oil includes but is not limited to 80, 82, 82.5, 82.6, 82.8, 82.9, 82.94, 82.95, 82.96, 83, 84, 85, 86, 87, 87.5, 87.6, 87.7, 87.8, 87.9, 87.94, 87.95, 87.96, 88, 89 or 90. Specifically, the weight percentage of the thickener includes but is not limited to 7, 8, 9, 10, 11 or 12. The weight parts of the structure improver include but are not limited to 0.8 parts, 0.9 parts, 1 parts, 1.1 parts, 1.2 parts, 1.3 parts, 1.4 parts or 1.5 parts. The weight parts of the thiophosphate amine salt include but are not limited to 2 parts, 2.2 parts, 2.5 parts, 2.8 parts, 3 parts, 3.2 parts, 3.5 parts, 3.8 parts, 4 parts, 4.1 parts, 4.2 parts, 4.3 parts, 4.5 parts, 5 parts, 5.5 parts, 5.8 parts or 6 parts. Preferably, the weight parts of the thiophosphate amine salt are 3.5 parts to 4.5 parts. The weight parts of the rust inhibitor include but are not limited to 0.03 parts, 0.04 parts, 0.05 parts, 0.06 parts or 0.07 parts.

[0058] In one example, the structure of the thiophosphate amine salt is ;

[0059] Among them, R 11 Each time it appears, it is independently S 1 Substituted or unsubstituted C 1 ~C 6 Alkyl, S 2 Substituted or unsubstituted C 6 ~C 10 Aromatic group; S 1 and S 2 Each is independently selected from one or more of hydroxyl, nitro and halogen;

[0060] R 12 C 1 ~C 6 Alkylene; R 13 , R 14 are independently H, hydroxy-substituted or unsubstituted C 1 ~C 6 Alkyl, hydroxy substituted or unsubstituted C 6 ~C 10 aromatic group, and R 13 , R 14 Not H at the same time.

[0061] Specifically, R 11Each occurrence is independently hydroxy-substituted or unsubstituted C 1 ~C 3 Alkyl, hydroxy substituted or unsubstituted C 6 ~C 10 Aromatic group;

[0062] R 12 C 1 ~C 3 Alkylene; R 13 , R 14 are independently H, hydroxy-substituted or unsubstituted C 1 ~C 4 Alkyl, and R 13 , R 14 Not H at the same time.

[0063] More specifically, the thiophosphate amine salt is selected from one or more compounds represented by the following structures: , , , , ,

[0064] , , , or .

[0065] The present application provides a specific structure of the thiophosphate amine salt, wherein the amine salt structure is consistent with the thiophosphate group P=S, the phosphate group POR 11 The phosphorus-oxygen double bond P=O and the phosphorus-sulfur double bond P=S can react with the metal surface at high temperature to form a stable phosphide film to provide excellent extreme pressure performance; at the same time, the phosphorus-oxygen double bond P=O also helps to improve the anti-oxidation performance of the grease. Furthermore, PSR 12 and POR 11 The groups can give the thiophosphate amine salt good thermal stability and dispersion stability. The mutual synergy of the functional groups enables the addition of the thiophosphate amine salt to increase the extreme pressure anti-wear, oxidation resistance and thermal stability of the grease composition.

[0066] In one example, the steps for preparing the thiophosphate amine salt include:

[0067] Mixing a phosphoric acid diester with a nitrogen-containing compound to prepare the thiophosphate amine salt;

[0068] Wherein, the structure of the phosphodiester is ; The structure of the nitrogen-containing compound is NHR 13R 14 .

[0069] Understandably, R 11 , R 12 , R 13 , R 14 The functional groups represented are as described above. In this step, the phosphoric acid diester and the nitrogen-containing compound are mixed, and at this time, the hydrogen on the phosphorus hydroxyl group and the nitrogen-containing compound form an ammonium radical. In one specific example, the molar ratio of the phosphoric acid diester to the nitrogen-containing compound is (0.9~1.1):1. Furthermore, the mixing process parameters include: a stirring speed of 90r / min~110r / min and a temperature of 75℃~85℃.

[0070] The specific reaction process is as follows: .

[0071] In one example, the steps of preparing the phosphodiester include:

[0072] Using phosphorus pentoxide as a raw material, carrying out an esterification reaction with a hydroxyl-containing compound, and preparing the phosphoric acid diester after purification;

[0073] Wherein, the structure of the hydroxyl-containing compound is ;

[0074] R 21 Each time it appears, it is independently S 3 Substituted or unsubstituted C 1 ~C 6 Alkylene, S 4 Substituted or unsubstituted C 6 ~C 10 Arylene; S 3 and S 4 Each is independently selected from one or more of hydroxyl, nitro and halogen; R 22 is H or benzyloxy. In the above steps, when the esterification reaction is carried out, the molar ratio of phosphorus pentoxide to the hydroxyl-containing compound is (0.9-1.1):2. The temperature for the esterification reaction is 55°C-65°C.

[0075] The specific reaction steps that occur at this time are:

[0076] Understandably, R 22 When it is H, then -R 21 -R 22 For-R 11 At this time, the structure of the phosphodiester is .

[0077] R 22When the benzyloxy group is present, the purification step includes a hydrogenation purification step. Specifically, the benzyloxy-containing phosphate diester The phosphoric acid diester is prepared by hydrogenation under the condition of Pd / C catalyst and hydrogen gas, and purification. .

[0078] The specific steps include: .

[0079] In one example, the steps of preparing the hydroxyl-containing compound include:

[0080] Carrying out a substitution reaction between a dithiophosphate and a diol compound to prepare the hydroxyl-containing compound;

[0081] Wherein, the structure of the dithiophosphate is , the structure of the diol compound is In the above steps, the molar ratio of the dithiophosphate and the diol compound is (0.9-1.1): 1. The temperature for the substitution reaction is 65°C-75°C.

[0082] The specific steps include:

[0083] .

[0084] In one example, the steps of preparing the dithiophosphate include:

[0085] P 2 S 5 Carrying out an esterification reaction with a monophenol compound or a monoalcohol compound to prepare the dithiophosphate;

[0086] Wherein, the structures of the phenolic compound and the alcohol compound are independently R 22 -R 21 -OH. In the above steps, P 2 S 5 The molar ratio of monophenolic compounds or monoalcoholic compounds is (0.9-1.1): 2. The temperature of the esterification reaction is 140°C-170°C.

[0087] The specific steps include:

[0088] .

[0089] In one example, the thickener is a lithium complex soap.

[0090] In one example, the thickener is prepared by saponification of hydroxystearic acid, aliphatic dicarboxylic acid and lithium hydroxide.

[0091] The thickener is prepared by saponification reaction of hydroxystearic acid, aliphatic dicarboxylic acid and lithium hydroxide. It has high high temperature resistance. In addition, even under high stress, it can still maintain structural integrity and is not easy to soften or flow.

[0092] In one example, the aliphatic dicarboxylic acid includes one or more of sebacic acid, azelaic acid, glutaric acid, adipic acid, and pimelic acid.

[0093] In one example, the mass ratio of the hydroxystearic acid, the aliphatic dicarboxylic acid and the lithium hydroxide is (3.5-4.5):1:(1.01-1.04). Specifically, the mass ratio of the hydroxystearic acid, the aliphatic dicarboxylic acid and the lithium hydroxide includes but is not limited to 3.5:1:1.01, 3.5:1:1.02, 3.5:1:1.03, 3.5:1:1.04, 3.8:1:1.01, 3.8:1:1.02, 3.8:1:1.03, 3.8:1:1.04, 4:1:1.01, 4:1:1.02, 4:1:1.03, 4:1:1.04, 4.01:1:1. 01, 4.01:1:1.02, 4.01:1:1.03, 4.01:1:1.04, 4.1:1:1.01, 4.1:1:1.02, 4.1:1:1.03, 4.1:1:1.04, 4.3:1:1.01, 4.3:1:1.02, 4.3:1:1.03, 4.3:1:1.04, 4.5:1:1.01, 4.5:1:1.02, 4.5:1:1.03, or 4.5:1:1.04.

[0094] In one specific example, the hydroxystearic acid is 12-hydroxystearic acid.

[0095] In one specific example, the aliphatic dicarboxylic acid is azelaic acid.

[0096] In one example, the temperature of the saponification reaction is 125°C to 140°C.

[0097] In one specific example, the specific steps of the saponification reaction include: preliminary saponification, aging treatment and post-treatment. Specifically, the process parameters of the preliminary saponification include: temperature of 80°C to 100°C. The process parameters of the aging treatment include: pressure of 0.5MPa to 0.6MPa and temperature of 125°C to 130°C. The process parameters of the post-treatment include: temperature of 130°C to 140°C.

[0098] Specifically, the preparation steps of the thickener include: preheating hydroxystearic acid and aliphatic dicarboxylic acid to 80° C. to 100° C.; adding lithium hydroxide solution to prepare a mixed solution;

[0099] The mixed solution is sequentially subjected to a preliminary saponification reaction at 80° C. to 100° C., an aging treatment at 125° C. to 130° C., and a post-treatment at 130° C. to 140° C. to prepare the thickener.

[0100] The thickener preparation method provided by the present application includes three steps carried out in sequence, wherein the initial saponification stage can generate lithium-based soap; further aging treatment is beneficial to the integrity of the reaction to form a more uniform, dense and stable soap fiber network, thereby ensuring that the grease has good colloidal stability and mechanical stability. Finally, after the post-treatment stage, this step can ensure the thoroughness of the saponification reaction, and the residual moisture or volatile by-products can be removed to ensure the quality of the thickener.

[0101] It can be understood that, in the preparation method mentioned in the present application, except for the process steps that emphasize pressure, other process steps that do not mention pressure are all carried out under normal pressure or under pressure that can be known to those skilled in the art.

[0102] In one example, the structure improving agent includes one or more of cyclopentane salts and aromatic carboxylates.

[0103] Optionally, the cyclopentane salt is one or more of sodium cyclopentaneate and potassium cyclopentaneate.

[0104] Optionally, the aromatic carboxylate includes one or more of disodium terephthalate, disodium phthalate and disodium isophthalate.

[0105] In one example, the structure of the rust inhibitor is , where R 2 H, halogen, C 1 ~C 6 Alkyl or C 1 ~C 6 Alkoxy.

[0106] When benzotriazole and its derivatives are used as rust inhibitors, they can form stable covalent bonds and coordination bonds with metal atoms such as copper atoms to construct a multi-layer protective film; at the same time, in conjunction with the base oil, thickener, structure improver and thiophosphate ammonium salt components, they can have a corrosion inhibition effect on metals.

[0107] Specifically, the rust inhibitor is selected from one or more compounds shown in the following structures: , , , or .

[0108] In a second aspect of the present application, there is provided a method for preparing the grease composition as described in any example of the first aspect of the present application, comprising the following steps:

[0109] S10, preheating hydroxystearic acid, aliphatic dicarboxylic acid and 28% to 35% of base oil by weight to 80° C. to prepare a first mixed material;

[0110] S20, adding lithium hydroxide solution to the first mixed material, performing saponification reaction, preparing the thickener, and obtaining a second mixed material;

[0111] S30, adding a structure improving agent to the second mixed material, mixing at 200° C. to 210° C., to prepare a third mixed material;

[0112] S40, cooling the third mixed material to 170° C. to 180° C., adding thiophosphate amine salt and mixing, to prepare a fourth mixed material;

[0113] S50, cooling the fourth mixed material to 70° C. to 80° C., adding a rust inhibitor and 65% to 72% of the base oil by weight to prepare the grease composition.

[0114] It can be understood that the properties of the base oil in step S10 and step S20 of the present application are the same, and the above description is only to emphasize the step-by-step addition of the base oil. Among them, the addition of the base oil in step S10 can prepare the temperature and viscosity of the initial reaction, and its presence can be used as a heat carrier and solvent to disperse the reactants, while also avoiding the high energy-consuming temperature caused by the full addition of the base oil; adding the base oil in step S50 can further adjust the viscosity, promote the structuring of the grease, and keep the product stable during long-term storage and use, and prevent the occurrence of oil separation.

[0115] In addition, what is mentioned here is only the preferred preparation method of the grease composition of the present application. Those skilled in the art may also choose a preparation method of first preparing a thickener and then mixing the components.

[0116] In one example, in step S20, the temperature of the saponification reaction is 125°C to 140°C.

[0117] In one specific example, in step S20, the specific steps of the saponification reaction include: preliminary saponification, aging treatment and post-treatment. Specifically, the process parameters of the preliminary saponification include: temperature of 80°C to 100°C. The process parameters of the aging treatment include: pressure of 0.5 MPa to 0.6 MPa and temperature of 125°C to 130°C. The process parameters of the post-treatment include: temperature of 130°C to 140°C.

[0118] Specifically, the specific steps in step S20 include: adding lithium hydroxide solution to the first mixed material, performing a preliminary saponification reaction at 80°C~100°C, performing an aging treatment at 125°C~130°C, and then performing a post-treatment at 130°C~140°C to prepare the thickener and obtain a second mixed material.

[0119] The third aspect of the present application provides a commercial vehicle chassis system grease, including the grease composition described in any example of the first aspect of the present application.

[0120] The following further specific examples are provided to explain the present application in detail. It should also be understood that the following examples are only used to further explain the present application and cannot be understood as limiting the scope of protection of the present application. Some non-essential improvements and adjustments made by those skilled in the art based on the above content of the present application belong to the scope of protection of the present application. The specific process parameters of the following embodiments are also only examples within a suitable range, that is, those skilled in the art can make a selection within a suitable range through the description herein, and are not necessarily limited to the specific values ​​of the embodiments below.

[0121] Preparation Example 1

[0122] (1) Preparation steps of dithiophosphates:

[0123] Add a certain amount of phenolic compound 4-benzyloxyphenol into a 250 ml four-necked flask with a stirring and condensing device. and an appropriate amount of xylene, pass dry nitrogen for 10 minutes before heating, stir at a speed of 100 r / min, slowly heat to 140°C, during which the molar ratio of 4-benzyloxyphenol to phosphorus pentasulfide is 2:1, slowly add phosphorus pentasulfide, keep at 140°C for 0.5h, after phosphorus pentasulfide is completely dissolved, heat to 170°C, keep for 8h, absorb the gas generated by the reaction with sodium hydroxide aqueous solution, remove xylene by reduced pressure distillation, and obtain oily dithiophosphate .

[0124] The specific steps are: .

[0125] (2) Preparation of hydroxyl-containing compounds:

[0126] A certain amount of propylene glycol was added to a 250 ml four-necked flask with a stirring and condensing device. The stirring speed was 100 r / min. Dry nitrogen was introduced during the reaction. The temperature was slowly raised to 60°C. Propylene glycol and the above dithiophosphate were reacted according to the reaction conditions. The molar ratio is 1:1, and the above dithiophosphate is slowly added , raise the temperature to 70℃ and maintain for 4h to obtain a hydroxyl-containing compound .

[0127] The specific preparation steps include:

[0128]

[0129] (3) Preparation steps of phosphodiester:

[0130] The preparation steps of phosphoric acid diester include: Slowly add phosphorus pentoxide to make the molar ratio of hydroxyl-containing compound to phosphorus pentoxide 2:1, and carry out esterification reaction at 60°C for 2h to prepare benzyl-containing phosphoric acid diester .

[0131] The specific steps include:

[0132] In the presence of 10% palladium / carbon, at an initial hydrogen pressure of 3.4 MPa, the above benzyl-containing phosphate diester Hydrogenate in ethanol containing 1M hydrochloric acid for 8 h. Purify the product by silica gel chromatography with toluene-ethanol (3:1) to obtain a phosphate diester. Nuclear magnetic hydrogen spectrum test shows that the structure of the phosphate diester is .

[0133]

[0134] (4) Preparation steps of thiophosphate amine salt:

[0135] Phosphodiester n-Butylamine was added to the mixture, the molar ratio of phosphoric acid diester to n-butylamine was 1:1, the stirring speed was 100 r / min, dry nitrogen was introduced during the reaction, the mixture was heated to 80°C and kept warm for 1 hour to obtain thiophosphate amine salt. .

[0136] Example 1

[0137] The grease composition of Example 1 includes, by mass, 87.95 parts of base oil, 7 parts of thickener, 1 part of structure improver, 4 parts of thiophosphate amine salt obtained in Preparation Example 1, and 0.05 parts of rust inhibitor.

[0138] The steps of preparing the grease composition include:

[0139] (1) 232.2 g of 12-hydroxystearic acid, 58 g of azelaic acid and 1466 g of hydrogenated base oil (the kinematic viscosity of the hydrogenated base oil at 40°C is 120 mm 2 / s), preheating to 90°C; preparing a first mixed material;

[0140] (2) A lithium hydroxide solution (consisting of 59.8 g of lithium hydroxide and 299 g of water) was added to the first mixed material, and a preliminary saponification reaction was carried out at 90° C. for 60 min, the pressure was increased to 0.55 MPa, and an aging treatment was carried out at 130° C. for 165 min, the pressure was released to normal pressure, and a post-treatment was carried out at 135° C. for 60 min to prepare the thickener and obtain a second mixed material.

[0141] (3) adding 50 g of a structure improving agent (disodium terephthalate) to the second mixed material, and mixing at a constant temperature of 200° C. for 15 min to prepare a third mixed material;

[0142] (4) Cooling the third mixed material to 175° C., adding 200 g of the thiophosphate amine salt prepared in Preparation Example 1 and mixing, to prepare a fourth mixed material;

[0143] (5) The fourth mixed material was cooled to 75°C, and 2.5 g of benzotriazole and 2931.5 g of hydrogenated base oil (the kinematic viscosity of the hydrogenated base oil at 40°C was 120 mm 2 / s) to thicken, and after shearing, filtering and degassing, 5000g of grease composition was prepared.

[0144] Example 2

[0145] The grease composition of Example 2 includes, by mass, 89.95 parts of base oil, 7 parts of thickener, 1 part of structure improver, 2 parts of thiophosphate amine salt obtained in Preparation Example 1, and 0.05 parts of rust inhibitor.

[0146] The steps of preparing the grease composition include:

[0147] (1) 232.2 g of 12-hydroxystearic acid, 58 g of azelaic acid and 1499.5 g of hydrogenated base oil (the kinematic viscosity of the hydrogenated base oil at 40°C is 120 mm 2 / s), preheating to 90°C; preparing a first mixed material;

[0148] (2) A lithium hydroxide solution (consisting of 59.8 g of lithium hydroxide and 299 g of water) was added to the first mixed material, and a preliminary saponification reaction was carried out at 90° C. for 60 min, the pressure was increased to 0.55 MPa, and an aging treatment was carried out at 130° C. for 165 min, the pressure was released to normal pressure, and a post-treatment was carried out at 135° C. for 60 min to prepare the thickener and obtain a second mixed material.

[0149] (3) adding 50 g of a structure improving agent (disodium terephthalate) to the second mixed material, and mixing at a constant temperature of 200° C. for 15 min to prepare a third mixed material;

[0150] (4) Cooling the third mixed material to 175° C., adding 100 g of the thiophosphate amine salt prepared in Preparation Example 1 and mixing, to prepare a fourth mixed material;

[0151] (5) The fourth mixed material was cooled to 75°C, and 2.5 g of benzotriazole and 2998 g of hydrogenated base oil (the kinematic viscosity of the hydrogenated base oil at 40°C was 120 mm 2 / s) to thicken, and after shearing, filtering and degassing, 5000g of grease composition was prepared.

[0152] Example 3

[0153] The grease composition of Example 3 includes, by mass, 82.95 parts of base oil, 12 parts of thickener, 1 part of structure improver, 4 parts of thiophosphate amine salt obtained in Preparation Example 1, and 0.05 parts of rust inhibitor.

[0154] The steps of preparing the grease composition include:

[0155] (1) 398 g of 12-hydroxystearic acid, 99.5 g of azelaic acid and 1382.5 g of hydrogenated base oil (the kinematic viscosity of the hydrogenated base oil at 40°C is 120 mm 2 / s), preheating to 90°C; preparing a first mixed material;

[0156] (2) A lithium hydroxide solution (composed of 102.5 g of lithium hydroxide and 299 g of water) was added to the first mixed material, and a preliminary saponification reaction was carried out at 90° C. for 60 min, the pressure was increased to 0.55 MPa, and an aging treatment was carried out at 130° C. for 165 min, the pressure was released to normal pressure, and a post-treatment was carried out at 135° C. for 60 min to prepare the thickener and obtain a second mixed material.

[0157] (3) adding 50 g of a structure improving agent (disodium terephthalate) to the second mixed material, and mixing at a constant temperature of 200° C. for 15 min to prepare a third mixed material;

[0158] (4) Cooling the third mixed material to 175° C., adding 200 g of the thiophosphate amine salt prepared in Preparation Example 1 and mixing, to prepare a fourth mixed material;

[0159] (5) The fourth mixed material was cooled to 75°C, and 2.5 g of benzotriazole and 2765 g of hydrogenated base oil (the kinematic viscosity of the hydrogenated base oil at 40°C was 120 mm 2 / s) to thicken, and after shearing, filtering and degassing, 5000g of grease composition was prepared.

[0160] Example 4

[0161] The grease composition of Example 4 includes, by mass, 87.95 parts of base oil, 7 parts of thickener, 1 part of structure improver, 4 parts of thiophosphate amine salt obtained in Preparation Example 1, and 0.05 parts of rust inhibitor.

[0162] The steps of preparing the grease composition include:

[0163] (1) 232.2 g of 12-hydroxystearic acid, 58 g of azelaic acid and 1466 g of hydrogenated base oil (the kinematic viscosity of the hydrogenated base oil at 40°C is 120 mm 2 / s), preheating to 90°C; preparing a first mixed material;

[0164] (2) A lithium hydroxide solution (consisting of 59.8 g of lithium hydroxide and 299 g of water) was added to the first mixed material, and a preliminary saponification reaction was carried out at 90° C. for 60 min, the pressure was increased to 0.55 MPa, and an aging treatment was carried out at 130° C. for 165 min, the pressure was released to normal pressure, and a post-treatment was carried out at 135° C. for 60 min to prepare the thickener and obtain a second mixed material.

[0165] (3) adding 50 g of a structure improving agent (sodium cyclohexane acid salt) to the second mixed material, and mixing at a constant temperature of 200° C. for 15 min to prepare a third mixed material;

[0166] (4) Cooling the third mixed material to 175° C., adding 200 g of the thiophosphate amine salt prepared in Preparation Example 1 and mixing, to prepare a fourth mixed material;

[0167] (5) The fourth mixed material was cooled to 75°C, and 2.5 g of benzotriazole and 2931.5 g of hydrogenated base oil (the kinematic viscosity of the hydrogenated base oil at 40°C was 120 mm 2 / s) to thicken, and after shearing, filtering and degassing, 5000g of grease composition was prepared.

[0168] Example 5

[0169] The grease composition of Example 5 includes, by mass, 82.95 parts of base oil, 12 parts of thickener, 1 part of structure improver, 4 parts of thiophosphate amine salt obtained in Preparation Example 1, and 0.05 parts of rust inhibitor.

[0170] The steps of preparing the grease composition include:

[0171] (1) 398 g of 12-hydroxystearic acid, 99.5 g of azelaic acid and 1382.5 g of hydrogenated base oil (the kinematic viscosity of the hydrogenated base oil at 40°C is 160 mm 2 / s), preheating to 95°C; preparing a first mixed material;

[0172] (2) A lithium hydroxide solution (composed of 102.5 g of lithium hydroxide and 299 g of water) was added to the first mixed material, and a preliminary saponification reaction was carried out at 95° C. for 60 min, the pressure was increased to 0.55 MPa, and an aging treatment was carried out at 130° C. for 180 min, the pressure was released to normal pressure, and a post-treatment was carried out at 135° C. for 60 min to prepare the thickener and obtain a second mixed material.

[0173] (3) adding 50 g of a structure improving agent (disodium terephthalate) to the second mixed material, and mixing at a constant temperature of 200° C. for 15 min to prepare a third mixed material;

[0174] (4) Cooling the third mixed material to 175° C., adding 200 g of the thiophosphate amine salt prepared in Preparation Example 1 and mixing, to prepare a fourth mixed material;

[0175] (5) The fourth mixed material was cooled to 75°C, and 2.5 g of benzotriazole and 2765 g of hydrogenated base oil (the kinematic viscosity of the hydrogenated base oil at 40°C was 160 mm 2 / s) to thicken, and after shearing, filtering and degassing, 5000g of grease composition was prepared.

[0176] Example 6

[0177] The grease composition of Example 6 includes, by mass, 80.95 parts of base oil, 12 parts of thickener, 1 part of structure improver, 6 parts of thiophosphate amine salt obtained in Preparation Example 1, and 0.05 parts of rust inhibitor.

[0178] The steps of preparing the grease composition include:

[0179] (1) 398 g of 12-hydroxystearic acid, 99.5 g of azelaic acid and 1349.5 g of hydrogenated base oil (the kinematic viscosity of the hydrogenated base oil at 40°C is 160 mm 2 / s), preheating to 95°C; preparing a first mixed material;

[0180] (2) A lithium hydroxide solution (composed of 102.5 g of lithium hydroxide and 299 g of water) was added to the first mixed material, and a preliminary saponification reaction was carried out at 95° C. for 60 min, the pressure was increased to 0.55 MPa, and an aging treatment was carried out at 130° C. for 165 min, the pressure was released to normal pressure, and a post-treatment was carried out at 135° C. for 60 min to prepare the thickener and obtain a second mixed material.

[0181] (3) adding 50 g of a structure improving agent (disodium terephthalate) to the second mixed material, and mixing at a constant temperature of 200° C. for 15 min to prepare a third mixed material;

[0182] (4) Cooling the third mixed material to 175° C., adding 300 g of the thiophosphate amine salt prepared in Preparation Example 1 and mixing, to prepare a fourth mixed material;

[0183] (5) The fourth mixed material was cooled to 75°C, and 2.5 g of benzotriazole and 2698 g of hydrogenated base oil (the kinematic viscosity of the hydrogenated base oil at 40°C was 160 mm 2 / s) to thicken, and after shearing, filtering and degassing, 5000g of grease composition was prepared.

[0184] Comparative Example 1

[0185] The grease composition of Comparative Example 1 includes, by weight, 86.95 parts of base oil, 12 parts of thickener, 1 part of structure improver and 0.05 part of rust inhibitor.

[0186] The steps of preparing the grease composition include:

[0187] (1) 398 g of 12-hydroxystearic acid, 99.5 g of azelaic acid and 1449.5 g of hydrogenated base oil (the kinematic viscosity of the hydrogenated base oil at 40°C is 160 mm 2 / s), preheating to 95°C; preparing a first mixed material;

[0188] (2) A lithium hydroxide solution (composed of 102.5 g of lithium hydroxide and 299 g of water) was added to the first mixed material, and a preliminary saponification reaction was carried out at 95° C. for 60 min, the pressure was increased to 0.55 MPa, and an aging treatment was carried out at 130° C. for 165 min, the pressure was released to normal pressure, and a post-treatment was carried out at 135° C. for 60 min to prepare the thickener and obtain a second mixed material.

[0189] (3) adding 50 g of a structure improving agent (disodium terephthalate) to the second mixed material, and mixing at a constant temperature of 200° C. for 15 min to prepare a third mixed material;

[0190] (4) The third mixed material was cooled to 75°C, and 2.5 g of benzotriazole and 2898 g of hydrogenated base oil (the kinematic viscosity of the hydrogenated base oil at 40°C was 160 mm 2 / s) to thicken, and after shearing, filtering and degassing, 5000g of grease composition was prepared.

[0191] Comparative Example 2

[0192] The grease composition of Comparative Example 2 includes, by weight, 82.95 parts of base oil, 12 parts of thickener, 1 part of structure improver, 4 parts of zinc dialkyl dithiophosphate (ZDDP) and 0.05 parts of rust inhibitor.

[0193] The steps of preparing the grease composition include:

[0194] (1) 398 g of 12-hydroxystearic acid, 99.5 g of azelaic acid and 1382.5 g of ester base oil (the kinematic viscosity of the ester base oil at 40°C is 220 mm 2 / s), preheating to 100°C; preparing a first mixed material;

[0195] (2) A lithium hydroxide solution (composed of 102.5 g of lithium hydroxide and 299 g of water) was added to the first mixed material, and a preliminary saponification reaction was carried out at 100° C. for 60 min, the pressure was increased to 0.55 MPa, and an aging treatment was carried out at 130° C. for 165 min, the pressure was released to normal pressure, and a post-treatment was carried out at 135° C. for 60 min to prepare the thickener and obtain a second mixed material.

[0196] (3) adding 50 g of a structure improving agent (disodium terephthalate) to the second mixed material, and mixing at a constant temperature of 200° C. for 15 min to prepare a third mixed material;

[0197] (4) cooling the third mixed material to 175° C., adding 200 g of zinc dialkyl dithiophosphate ZDDP and mixing to prepare a fourth mixed material;

[0198] (5) The fourth mixed material was cooled to 80°C, and 2.5 g of benzotriazole and 2765 g of ester base oil (the kinematic viscosity of the ester base oil at 40°C was 220 mm 2 / s) to thicken, and after shearing, filtering and degassing, 5000g of grease composition was prepared.

[0199] The contents of the components of the embodiments and comparative examples are shown in Table 1:

[0200] Table 1

[0201]

[0202] Test Case

[0203] The grease compositions obtained in the examples and preparation examples were subjected to dropping point, four-ball extreme pressure, four-ball test, oxidation induction period and FE9 test tests, wherein the corresponding test methods and test results are shown in Table 2.

[0204] Table 2

[0205]

[0206] As can be seen from Table 2, the grease composition provided in the present application has improved high temperature resistance, extreme pressure resistance, wear resistance, oxidation resistance, etc., and the increased content of additives such as thickeners, structure improvers, thiophosphate amine salts and rust inhibitors can compensate for the lubrication risk caused by the reduced viscosity of the base oil.

[0207] Compared with Example 2, the amount of thiophosphate amine salt added in Example 1 is increased from 2% to 4%, which can improve the wear resistance and oxidation resistance of the grease composition; compared with Example 3, the amount of thickener added in Example 1 is increased from 7% to 12%, which can improve high temperature resistance and wear resistance, and the oxidation resistance of the two is not significantly affected by the action of thiophosphate amine salt; compared with Example 4, the structure improver has no significant effect on the performance; compared with Example 5, the base oil viscosity in Example 3 is increased from 120 mm 2 / s increased to 160 mm 2 / s, thus improving the anti-wear properties of the grease composition.

[0208] Compared with Comparative Example 1, the addition amount of thiophosphate amine salt in Example 5 was increased from 0% to 4%, which significantly improved the wear resistance and oxidation resistance. Compared with Comparative Example 2, the addition amount of thiophosphate amine salt and hydrogenated mineral base oil (kinematic viscosity 160mm at 40°C) in Example 5 was increased from 0% to 4%, which significantly improved the wear resistance and oxidation resistance. 2 / s) can achieve the same anti-wear and anti-oxidation properties as ZDDP and ester synthetic base oil (kinematic viscosity 220mm at 40°C). 2 / s) combination level, because the cost of hydrogenated mineral base oil is lower than that of ester synthetic base oil, the economic efficiency of Example 5 is better than that of Comparative Example 2; compared with Example 6, the amount of thiophosphate amine salt added in Example 5 is increased from 4% to 6%, and the addition of thiophosphate amine salt is slightly more, resulting in slightly poor anti-wear and anti-oxidation properties of the grease. Comprehensive performance and cost, Example 5 is the best product.

[0209] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0210] The above-described embodiments only express several implementation methods of the present application, which is convenient for understanding the technical solution of the present application in detail, but it cannot be understood as limiting the scope of protection of the invention patent. It should be pointed out that for ordinary technicians in this field, without departing from the concept of the present application, several modifications and improvements can be made, which all belong to the scope of protection of the present application. It should be understood that the technical solutions obtained by those skilled in the art through logical analysis, reasoning or limited experiments on the basis of the technical solutions provided in the present application are all within the scope of protection of the claims attached to the present application. Therefore, the scope of protection of the patent of this application shall be based on the content of the attached claims, and the description can be used to interpret the content of the claims.

Claims

1. A grease composition, characterized in that: The grease composition comprises the following components in parts by weight: 80 to 90 parts of base oil, 7 to 12 parts of thickener, 0.8 to 1.5 parts of structure improver, 2 to 6 parts of thiophosphate amine salt and 0.03 to 0.07 parts of rust inhibitor; Wherein, the base oil is a hydrogenated base oil, and the viscosity of the base oil at 40°C is 120 mm 2 / s~160mm 2 / s.

2. The grease composition according to claim 1, characterized in that The structure of the thiophosphate amine salt is ; Among them, R 11 Each occurrence is independently S1 substituted or unsubstituted C1~C6 alkyl, S2 substituted or unsubstituted C6~C 10 Aromatic group; S1 and S2 are each independently selected from one or more of hydroxyl, nitro and halogen; R 12 is C1~C6 alkylene; R 13 , R 14 are independently H, hydroxy-substituted or unsubstituted C1~C6 alkyl, hydroxy-substituted or unsubstituted C6~C 10 aromatic group, and R 13 , R 14 Not H at the same time.

3. The grease composition according to claim 2, characterized in that R 11 Each occurrence is independently hydroxy-substituted or unsubstituted C1~C3 alkyl, hydroxy-substituted or unsubstituted C6~C 10 Aromatic group; R 12 is C1~C3 alkylene; R 13 , R 14 are each independently H, hydroxy-substituted or unsubstituted C1~C4 alkyl, and R 13 , R 14 Not H at the same time.

4. The grease composition according to claim 2 or 3, characterized in that The preparation steps of the thiophosphate amine salt include: Mixing a phosphoric acid diester with a nitrogen-containing compound to prepare the thiophosphate amine salt; Wherein, the structure of the phosphodiester is ; The structure of the nitrogen-containing compound is NHR 13 R 14 .

5. The grease composition according to claim 4, characterized in that The preparation steps of the phosphoric acid diester include: Using phosphorus pentoxide as a raw material, carrying out an esterification reaction with a hydroxyl-containing compound, and preparing the phosphoric acid diester after purification; Wherein, the structure of the hydroxyl-containing compound is ; R 21 Each occurrence is independently S3 substituted or unsubstituted C1~C6 alkylene, S4 substituted or unsubstituted C6~C 10 S3 and S4 are each independently selected from one or more of hydroxyl, nitro and halogen; R 22 is H or benzyloxy.

6. The grease composition according to claim 5, characterized in that The preparation steps of the hydroxyl-containing compound include: Carrying out a substitution reaction between a dithiophosphate and a diol compound to prepare the hydroxyl-containing compound; Wherein, the structure of the dithiophosphate is , the structure of the diol compound is .

7. The grease composition according to claim 6, characterized in that The preparation steps of the dithiophosphate include: The dithiophosphate is prepared by subjecting P2S5 to an esterification reaction with a monophenol compound or a monoalcohol compound; Wherein, the structures of the phenolic compound and the alcohol compound are independently R 22 -R 21 -OH.

8. The grease composition according to any one of claims 1 to 3 and 5 to 7, characterized in that: The thickener is a complex lithium soap; and The thickener is prepared by saponification reaction of hydroxystearic acid, aliphatic dicarboxylic acid and lithium hydroxide.

9. The grease composition according to claim 8, characterized in that The thickener has one or more of the following characteristics: (1) The aliphatic dicarboxylic acid includes one or more of sebacic acid, azelaic acid, glutaric acid, adipic acid and pimelic acid; (2) The mass ratio of the hydroxystearic acid, the aliphatic dicarboxylic acid and the lithium hydroxide is (3.5-4.5):1:(1.01-1.04); (3) The temperature of the saponification reaction is 125°C to 140°C.

10. The grease composition according to any one of claims 1 to 3 and 5 to 7, characterized in that: The structure improving agent includes one or more of cyclopentane salts and aromatic carboxylates; Optionally, the naphthenate includes one or more of vanadium naphthenate, copper naphthenate, nickel naphthenate and sodium naphthenate; Optionally, the aromatic carboxylate includes one or more of disodium terephthalate, disodium phthalate and disodium isophthalate.

11. The grease composition according to any one of claims 1 to 3 and 5 to 7, characterized in that: The structure of the rust inhibitor is , wherein R2 is H, halogen, C1~C6 alkyl or C1~C6 alkoxy.

12. A method for preparing the grease composition according to any one of claims 1 to 11, characterized in that: The following steps are involved: Preheating hydroxystearic acid, aliphatic dicarboxylic acid and base oil accounting for 28% to 35% of the total mass to 80° C. to prepare a first mixed material; Adding lithium hydroxide solution to the first mixed material to perform saponification reaction, thereby preparing the thickener to obtain a second mixed material; Adding a structure improving agent to the second mixed material, and mixing at 200° C. to 210° C. to prepare a third mixed material; The third mixed material is cooled to 170° C. to 180° C., and thiophosphate amine salt is added and mixed to prepare a fourth mixed material; The fourth mixed material is cooled to 70° C. to 80° C., and a rust inhibitor and a base oil accounting for 65% to 72% of the total mass are added and mixed to prepare the grease composition.

13. A commercial vehicle chassis system grease, characterized in that: A grease composition comprising the grease composition according to any one of claims 1 to 11.