Molten aluminum adhesion resistant coating and preparation method thereof
Through HiPI MS technology and plasma feedback control, an Al CrN coating with high hardness and uniform and dense structure is prepared, which solves the problem that traditional coatings are prone to failure in extreme environments and significantly improves the oxidation resistance and mechanical wear resistance of the mold. performance.
Patent Information
- Application Number
- CN202410758611.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-13
- Publication Date
- 2024-10-08
AI Technical Summary
Traditional nitride coatings are prone to failure and have large performance differences in extreme service environments, making it difficult to meet the high hardness and oxidation resistance requirements of integrated die-casting molds.
High-power pulsed magnetron sputtering technology (HiPI MS) combined with plasma emission spectrum feedback control is used to prepare Al CrN functional coating. Through DC magnetron sputtering cleaning and feedback control deposition, a uniform and dense multi-element nitride coating is formed. .
It achieves high hardness and improved resistance to liquid aluminum adhesion. The coating structure is uniform and dense. It is suitable for the extreme environment of integrated die-casting molds and extends the service life of the mold.
Smart Images

Figure CN118745563A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of coating preparation, and in particular to an anti-aluminum liquid adhesion coating and a preparation method thereof. Background Art
[0002] The die-casting molds required for integrated die-casting technology are large-scale and complex. During the die-casting process, the high-speed aluminum liquid directly contacts the mold and cools and solidifies, and is subjected to extrusion, impact, corrosion, and alternating hot and cold. In order to meet the extreme service environment of integrated die-casting, multi-component nitrides are developed on the basis of binary nitride coatings. Multi-component nitride coatings have higher hardness, lower friction coefficient, better high-temperature friction performance and oxidation resistance than corresponding binary coatings. However, the current nitride coatings have two problems:
[0003] (1) Since the coatings prepared by traditional PVD technology have many defects, it is easy to form diffusion channels and cause pitting corrosion of the substrate, which is prone to failure in extreme service environments;
[0004] (2) There are significant differences in the performance of coatings with different phase structures. Selecting appropriate preparation parameters to prepare a coating with a specific structure has important application value.
[0005] At present, the coatings prepared by high-energy pulse magnetron sputtering technology (High Power Impulse Magnetron Sputtering, HiPIMS) at home and abroad are dense and smooth, and have good mechanical properties, which has great potential for improving the life of workpieces. The main feature of high-power pulse magnetron sputtering is to increase the ionization rate of sputtered particles. The size of the ionization rate directly affects the structure and properties of the deposited coating. Optical Emission Spectroscopy (OES) is usually used to analyze the evolution of plasma parameters during the discharge process, explore the relationship between preparation parameters and the bombardment energy of film-forming particles, and explore the influence of energy on the structure and preferred orientation of the coating. Further optimization of the structure and properties of the film provides a basis for engineering applications for the stable and rapid preparation of functional nitride coatings.
[0006] For example, in Chinese patent CN109735799A, Al CrN coating is prepared by HiPI MS technology, which has the advantages of high hardness, good adhesion to the substrate, smooth and dense coating surface, small friction coefficient and cutting force, and its mechanical wear resistance and high temperature oxidation resistance are greatly improved, which can meet the demand for better performance of tool materials in high-speed machining.
[0007] In addition, in another Chinese patent CN114649963A, the output characteristics of the HiPI MS power supply are adjusted in real time according to the glow conditions during the vacuum magnetron sputtering process, thereby effectively improving the control accuracy and stability of the high-power and high-density magnetron sputtering power supply and ensuring the stability and consistency of the coating process. However, due to the limited accuracy of glow regulation, a stable plasma state cannot be obtained. For extreme service environments such as integrated die casting, the use of HiPI MS technology to prepare high-performance nitride coatings is an effective solution. Using OES feedback control can generate stable plasma from the target surface during the entire coating deposition process, further optimizing the structure and performance of the coating.
[0008] Therefore, it is necessary to propose a new preparation process to solve the above problems. Summary of the invention
[0009] In view of the technical problems existing in the above-mentioned background technology, the present invention proposes a reasonable concept to realize the rapid and stable preparation of high-performance AlCrN functional coatings by HiPIMS, the coating has good surface quality, high hardness and anti-aluminum adhesion performance, and is suitable for the anti-aluminum liquid adhesion coating and its preparation method for the extreme service environment of integrated die-casting molds.
[0010] In order to solve the above technical problems, the present invention provides a method for preparing an anti-aluminum liquid adhesion coating, which mainly comprises the following steps:
[0011] (1) Pretreatment
[0012] Pre-treat the die-casting mold steel substrate and clean the vacuum chamber and gas path of the coating equipment;
[0013] (2) Plasma parameter calibration
[0014] The AlCr target and the Cr target are cleaned by direct current magnetron sputtering, the emission spectrum of the target surface plasma of the AlCr target is obtained by a plasma emission spectrum feedback system, the Al atomic spectrum line at 390-400 nm is selected as the monitoring spectrum line, and the relative intensity of the Al atomic spectrum line at 390-400 nm is set;
[0015] (3) Composite coating preparation
[0016] First, the die-casting mold steel substrate is glow cleaned, and then the Cr target is sputtered by DC magnetron sputtering to prepare a Cr bonding layer and a CrN transition layer; then based on the plasma emission spectrum, the Al Cr target is sputtered by Hi PI MS technology, and nitrogen is dynamically introduced into the vacuum chamber through feedback control to deposit the Al CrN functional layer.
[0017] The method for preparing the anti-aluminum liquid adhesion coating, wherein the process of pre-treating the die-casting mold steel substrate in step (1) is: removing various pollutants on the surface of the die-casting mold steel substrate, polishing it with sandpaper of different purposes to ensure that the surface of the sample is flat and smooth; the sample needs to be ultrasonically cleaned in deionized water containing metal cleaner, acetone, deionized water and anhydrous ethanol for 20 to 30 minutes, and then dried for 10 to 30 minutes, and placed in a vacuum chamber of a coating device.
[0018] The method for preparing the anti-aluminum liquid adhesion coating, wherein the process of cleaning the vacuum chamber and the gas path in step (1) is: the vacuum chamber pressure is pumped to 1.0×10 -3 Pa, argon and nitrogen are introduced into the vacuum chamber to clean the gas path.
[0019] The method for preparing the anti-aluminum liquid adhesion coating, wherein the process of cleaning the Al Cr target and the Cr target in the step (2) is: introducing argon gas with a purity of 99.999% into the vacuum chamber, setting the Ar gas flow rate to 60 to 250 sccm, raising the air pressure in the vacuum chamber to 0.5 to 3 Pa, turning on the Cr target and the Al Cr target, and sputtering and cleaning the cathode target for 5 to 20 minutes; and setting the target current of the Cr target and the Al Cr target to 1 to 8A, and the substrate bias to -600 to -900V.
[0020] The method for preparing the anti-aluminum liquid adhesion coating, wherein the process of setting the relative intensity of the Al atomic spectrum line at 390-400nm in the step (2) is as follows: setting the Ar gas flow rate to 60-200sccm, gradually increasing the reaction gas N2 flow rate, so that the air pressure in the vacuum chamber is 0.5-2Pa, setting the target voltage to 500-900V, the duty cycle to 10-80%, and the substrate bias to -40--150V; calibrating the Al atomic spectrum line intensity at 390-400nm sputtered in a pure Ar environment to be maximum; when the nitrogen flow rate is increased to 20-150sccm, the intensity of the Al atomic spectrum line at 390-400nm decreases to a minimum and remains stable, and at this time, the intensity of the Al atomic spectrum line at 390-400nm is calibrated to be extremely small.
[0021] The method for preparing the anti-adhesion coating of aluminum liquid, wherein the condition for glow cleaning of the die casting mold steel substrate in step (3) is: when the background vacuum degree of the vacuum chamber is 1×10 -4 ~1×10 -2 Pa, Ar gas was introduced and the pressure was controlled at 1×10 -2 ~8×10 -1 Pa, negative bias voltage -500~-900V, bombardment time 5~30min.
[0022] The method for preparing the anti-aluminum liquid adhesion coating, wherein the process of depositing the Cr bonding layer in step (3) is: adjusting the Ar gas flow rate to 40 to 300 sccm, and maintaining the gas pressure at about 0.3 to 0.8 Pa, setting the target current to 0.5 to 3A, and depositing the Cr bonding layer for 1 to 8 minutes at a bias voltage of -100 to -200V, and the coating thickness is 0.1 to 2μm.
[0023] The method for preparing the anti-aluminum liquid adhesion coating, wherein the process of depositing the CrN transition layer in step (3) is: adjusting the Ar gas flow rate to 60-200sccm, the N2 flow rate to 10-60sccm, and maintaining the gas pressure at about 0.3-2Pa, setting the target current to 0.5-3A, and depositing the CrN transition layer for 1-15min at a bias voltage of -50--150V, and the coating thickness is 0.1-2μm.
[0024] The method for preparing the anti-aluminum liquid adhesion coating, wherein: the deposition process of the AlCrN functional layer in the step (3) is as follows: fixing the Al spectral line intensity, setting the Ar gas flow rate to 60-200 sccm, making the vacuum chamber pressure 0.5-2 Pa, setting the target voltage to 400-900 V, the duty cycle to 10-80%, the substrate bias to -40--150 V, setting the relative intensity of the Al atomic spectral line at 390-400 nm to any value of 0-100% and keeping the intensity value unchanged according to research and preparation needs, continuing sputtering for 50-120 min, and the coating thickness of 1-5 μm; opening the nitrogen passage, and dynamically and real-timely regulating the nitrogen flow rate according to the real-time plasma parameters by the gas flow meter until the spectral line intensity is stabilized at the parameter setting value, and then the film preparation can be carried out, the whole adjustment process takes about 1-10 min, and the nitrogen flow rate is 0-100 sccm.
[0025] An anti-aluminum liquid adhesion coating is an AlCrN functional layer prepared by the above-mentioned anti-aluminum liquid adhesion coating preparation method, and the AlCrN functional layer comprises the following components in terms of atomic number percentage: Al: 30-40%, Cr: 15-25%, and N: 35-50%.
[0026] The AlCrN functional layer, wherein: the AlCrN functional layer also includes one selected from Si, B, C, O, W, Y and one or more other alloying elements, and the content of the other alloying elements in terms of atomic percentage is 1-4%.
[0027] By adopting the above technical solution, the present invention has the following beneficial effects:
[0028] The preparation method of the anti-aluminum liquid adhesion coating of the present invention is reasonably conceived. A surface multi-component nitride coating is prepared on the surface of a substrate by using high-power pulsed magnetron sputtering technology. The target material in the HiPI MS technology receives high-energy pulses, which increases the peak power density, exceeding the traditional magnetron sputtering by 2 to 3 orders of magnitude, and improves the ionization rate. It provides a new experimental means for controlling the deposition process, preparing special element compound coatings and optimizing their performance, thereby preparing a coating with a uniform and dense structure to meet the extreme service environment of integrated die casting.
[0029] The preparation method of the anti-aluminum liquid adhesion coating of the present invention controls the reaction deposition process of the multinary nitride through a plasma emission spectrum monitoring feedback system in a closed loop, accurately adjusts the amount of gas introduced in real time, and generates stable plasma from the target surface during the entire coating deposition process. The structure and performance of the coating are further optimized, and a multinary nitride coating with a specific crystal structure is stably and rapidly prepared.
[0030] The anti-molten aluminum adhesion coating of the present invention has a uniform and dense structure, the crystal structure is mainly fcc-Al CrN, and the highest hardness of 35GPa is obtained. It is a coating with great potential suitable for integrated die-casting molds.
[0031] At the same time, an Al CrN / CrN / Cr composite coating system for the mold surface was designed (i.e., a three-layer coating consisting of the Al CrN functional layer, the CrN transition layer, and the Cr bonding layer on the surface, as shown in the figure). Figure 2 ) to improve the bearing capacity of the coating; through the actual anti-aluminum adhesion test, the mold H13 steel sample coated with the present embodiment showed the characteristic of not sticking to aluminum, with good surface integrity, unchanged composition, and stable phase structure in the aluminum liquid, which provides a possibility for improving the anti-aluminum adhesion performance of the surface of the integrated die-casting mold. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings in the following description are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0033] Figure 1 The flowchart of the preparation method of the HiPI MS anti-aluminum adhesion Al CrN coating based on OES feedback control of the present invention;
[0034] Figure 2 This is a cross-sectional morphology of the anti-aluminum adhesion Al CrN coating based on OES feedback control HiPI MS in the present invention. DETAILED DESCRIPTION
[0035] The technical solution of the present invention will be described clearly and completely below in conjunction with the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0036] The present invention is further explained below in conjunction with specific implementation modes.
[0037] The present embodiment provides an anti-aluminum liquid adhesion coating, which is an AlCrN functional layer and includes the following components in terms of atomic percentage: Al: 30-40%, Cr: 15-25%, and N: 35-50%.
[0038] The AlCrN functional layer also includes one or more other alloying elements selected from Si, B, C, O, W, and Y, and the content of the other alloying elements in terms of atomic percentage is 1 to 4%, which can further optimize the performance and properties of the coating.
[0039] like Figure 1 As shown, the present embodiment provides a method for preparing an anti-molten aluminum adhesion coating, using an H13 steel substrate as a die-casting mold substrate, and using an Al 70Cr30 target and a Cr target as target materials; wherein common die-casting mold substrates include but are not limited to H13 steel, 4Cr5Mo2V mold steel, etc.; the composition of the target material is not necessarily Al 70Cr30, and Al Cr targets of different compositions are also applicable, and may also contain other metal elements such as Si, W, B, V, etc.; specifically comprising the following steps:
[0040] S100, Pretreatment
[0041] Pre-treat the H13 steel substrate and clean the vacuum chamber and gas path of the coating equipment; the specific process is as follows:
[0042] S101, workpiece pretreatment
[0043] Remove all kinds of pollutants on the surface of the H13 steel substrate, and polish it with sandpaper of different purposes to ensure that the surface of the sample is flat and smooth; the H13 steel sample needs to be ultrasonically cleaned in deionized water containing metal cleaner, acetone, deionized water and anhydrous ethanol for 20 to 30 minutes (the best implementation value of this embodiment is 20 minutes), and then dried for 10 to 30 minutes (the best implementation value of this embodiment is 10 minutes), and then placed in the vacuum chamber of the coating equipment;
[0044] S102, vacuum chamber and gas path cleaning
[0045] The vacuum chamber and gas line pressure were pumped down to 1.0×10 -3 Pa, argon and nitrogen are introduced into the vacuum chamber to clean the gas path.
[0046] S200, plasma parameter calibration
[0047] The Al 70Cr30 target and the Cr target are cleaned by using a DC magnetron sputtering technology; the emission spectrum of the target surface plasma is obtained by a plasma emission spectrum feedback system, the Al atomic spectrum line at 390 to 400 nm (the best implementation value of this embodiment is 394.4 nm) is selected as the monitoring spectrum line, and the relative intensity of the Al atomic spectrum line at 390 to 400 nm (the best implementation value of this embodiment is 394.4 nm) is set; the specific process is as follows:
[0048] S201, Cr target and Al 70Cr30 target cleaning
[0049] Introduce argon gas with a purity of 99.999%, set the Ar gas flow rate to 60-250 sccm, raise the pressure in the vacuum chamber to 0.5-3 Pa, turn on the Cr target and the Al 70Cr30 target, and sputter and clean the cathode target for 5-20 minutes; wherein, set the target current of the Cr target and the Al Cr target to 3-8A, and the duty cycle to 10-80%; the substrate bias voltage is -600--900V;
[0050] S202, spectral line intensity calibration
[0051] The plasma emission spectrum feedback control system is turned on to obtain the target surface plasma emission spectrum of the Al 70Cr30 target, and the Al atomic spectrum line at 390-400nm (the best implementation value of this embodiment is 394.4nm) is selected; wherein, the Ar gas flow rate is set to 60-200sccm, the reaction gas N2 flow rate is gradually increased, the gas pressure in the vacuum chamber is 0.5-2Pa, the target voltage is set to 500-900V, and the duty cycle is 10-80%; the substrate bias voltage is -40--150V; the intensity of the Al atomic spectrum line at 390-400nm (the best implementation value of this embodiment is 394.4nm) sputtered in a pure Ar environment is calibrated to be maximum; when the nitrogen flow rate is increased to 20-150sccm, the intensity of the Al atomic spectrum line at 390-400nm (the best implementation value of this embodiment is 394.4nm) decreases and remains stable, and the A The intensity of the atomic spectrum line at 390-400nm (the best implementation value in this embodiment is 394.4nm) is extremely small.
[0052] It should be noted that: This embodiment introduces a plasma emission spectrum feedback control system, and adopts high-energy pulsed magnetron sputtering (HiPI MS) to design and prepare a high-temperature resistant composite coating of Al CrN / CrN / Cr structure. The sputtering targets are Al70Cr30 alloy target (99.99%) and single Cr target (99.99%), both of which are Φ76.2mm in size. Argon and nitrogen are used as working gases, and the purity is 99.999%. H13 steel is used as the workpiece substrate of the die-casting mold. The turret system includes six rotating shaft frames, to which a rotating rack can be added, which can perform rotation, revolution and compound rotation, and apply bias voltage.
[0053] The plasma emission spectrum feedback control system is mainly composed of a plasma full spectrum analyzer (OES), a feedback controller and a gas flow meter. The detection optical fiber is inserted into the surface of the sputtering target to obtain the emission spectrum of the target surface plasma in real time, with a wavelength range of 200 to 1100 nm. The typical characteristic spectrum of the particles to be monitored is selected as needed, and the maximum (100%) and minimum (0%) values of the intensity are calibrated under experimental conditions. Then, the relative intensity of the spectrum line is set (0% to 100%) for thin film deposition. The controller will use this characteristic peak intensity as the calibration object to feedback and adjust the gas intake of the flow meter to ensure the stability of the particle content during the coating deposition process.
[0054] After a large number of experiments, it was found that in the high-power pulse magnetron sputtering of Al 70Cr30 target, the intensity of the aluminum atomic spectrum line has obvious hysteresis phenomenon, which can better reflect the poisoning state of the target material. According to different target element types, different metal particles can be selected as detection objects. In the preparation of the Al CrN coating of the present invention, the sputtered aluminum atoms of the cathode target are used as the monitoring object, and the spectrum line at 394.4nm is selected. The target material is completely poisoned, and the spectrum line intensity when the aluminum spectrum line intensity is the smallest is calibrated to be extremely small (0%). The power is turned on but nitrogen is not introduced, and the spectrum line intensity of pure argon sputtering is calibrated to be extremely large (100%). By using PEM set point feedback control, the relative intensity of the spectrum line is set (0-100%) for deposition. The entire preparation process is a dynamic balance of continuous feedback adjustment of the nitrogen intake, which can generate stable plasma from the target surface.
[0055] S300, composite coating preparation
[0056] Before preparation, the H13 steel substrate was glow cleaned, and then the Cr target was sputtered by DC magnetron sputtering to prepare the Cr bonding layer and the CrN transition layer. The deposition of the bonding layer and the transition layer is to improve the bearing capacity and bonding force of the coating structure; finally, based on plasma emission spectroscopy, the Al 70Cr30 target was sputtered by HiPI MS technology (i.e., high-power pulsed magnetron sputtering technology), and nitrogen was introduced into the vacuum chamber at the same time to deposit the Al CrN functional layer; the specific process is as follows:
[0057] S301, H13 steel substrate glow cleaning
[0058] The cleaning conditions of H13 steel substrate are: when the background vacuum degree of the vacuum chamber is 1×10 -4 ~1×10 -2 Pa, Ar gas was introduced and the pressure was controlled at 1×10 -2 ~8×10 -1 Pa, negative bias voltage -500~-900V, bombardment time 5~30min;
[0059] S302, Cr bonding layer deposition
[0060] The Ar gas flow rate is adjusted to 40-300 sccm, and the gas pressure is maintained at about 0.3-0.8 Pa. The target current is set to 0.5-3 A. The Cr bonding layer is deposited for 1-8 min at a bias voltage of -100--200 V, and the coating thickness is 0.1-2 μm.
[0061] S303, CrN transition layer deposition
[0062] The Ar gas flow rate is adjusted to 60-200 sccm, the N2 flow rate is 10-60 sccm, and the gas pressure is maintained at about 0.3-2 Pa. The target current is set to 0.5-3 A. The CrN transition layer is deposited for 1-15 min at a bias voltage of -50--150 V, and the coating thickness is 0.1-2 μm.
[0063] S304, surface functional Al CrN layer deposition
[0064] The intensity value of the Al atomic spectrum line at 390-400 nm is fixed, and sputtering is continued for 50-120 min. The coating thickness is 1-5 μm.
[0065] The Al spectral line intensity is fixed, the Ar gas flow rate is set to 60-200sccm, the air pressure in the vacuum chamber is 0.5-2Pa, the target voltage is set to 400-900V, and the duty cycle is 10-80%; the substrate bias is -40--150V, and the relative intensity of the Al atomic spectral line at 390-400nm (the best implementation value of this embodiment is 394.4nm) is set to an arbitrary value of 0-100% according to research and preparation needs; the nitrogen passage is opened, and the gas flowmeter dynamically and real-timely regulates the nitrogen flow rate according to the real-time plasma parameters until the spectral line intensity is stabilized at the parameter setting value, and then the film can be prepared. The entire adjustment process takes about 1-10 minutes, and the nitrogen introduction amount is 0-100sccm.
[0066] When the Al content is set to 30%, the cross-sectional morphology of the AlCrN coating with anti-aluminum adhesion based on OES feedback control HiPIMS is shown in Figure 2. Figure 2 shown.
[0067] The AlCrN / CrN / Cr composite coating system is designed to improve the load-bearing capacity of the coating and the bonding strength between the coating and the substrate.
[0068] The AlCrN coating prepared by the preparation method of the anti-aluminum liquid adhesion coating has a uniform and dense structure and a maximum hardness of 35GPa.
[0069] The present invention is based on the detection and feedback of the content of film-forming particles under a vacuum environment, eliminates the hysteresis effect caused by target poisoning during the preparation process, and successfully prepares an AlCrN film coating with an fcc structure, laying a good foundation for its engineering application and having very important industrial value; the coating has a high hardness of 35GPa and good stability and anti-adhesion in high-temperature aluminum liquid.
[0070] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for preparing a coating that resists aluminum liquid adhesion, characterized in that: The main steps include: (1) Pretreatment Pre-treat the die-casting mold steel substrate and clean the vacuum chamber and gas path of the coating equipment; (2) Plasma parameter calibration The AlCr target and the Cr target are cleaned by direct current magnetron sputtering, the emission spectrum of the target surface plasma of the AlCr target is obtained by a plasma emission spectrum feedback system, the Al atomic spectrum line at 390 to 400 nm is selected as the monitoring spectrum line, and the relative intensity of the Al atomic spectrum line at 390 to 400 nm is set; (3) Composite coating preparation First, the die-casting mold steel substrate is glow cleaned, and then the Cr target is sputtered by DC magnetron sputtering to prepare a Cr bonding layer and a CrN transition layer; then based on the plasma emission spectrum, the AlCr target is sputtered by HiPIMS technology, and nitrogen is dynamically introduced into the vacuum chamber through feedback control to deposit an AlCrN functional layer.
2. The method for preparing the anti-aluminum liquid adhesion coating according to claim 1, characterized in that: The process of pretreatment of the die-casting mold steel substrate in step (1) is as follows: removing various pollutants on the surface of the die-casting mold steel substrate, polishing with sandpaper of different purposes to ensure that the surface of the sample is flat and smooth; the sample needs to be ultrasonically cleaned in deionized water containing metal cleaner, acetone, deionized water and anhydrous ethanol for 20 to 30 minutes, then dried for 10 to 30 minutes, and placed in a vacuum chamber of a coating device.
3. The method for preparing the anti-aluminum liquid adhesion coating according to claim 1, characterized in that: The process of cleaning the vacuum chamber and the gas path in step (1) is as follows: the vacuum chamber pressure is pumped down to 1.0×10 -3 Pa, argon and nitrogen are introduced into the vacuum chamber to clean the gas path.
4. The method for preparing the anti-aluminum liquid adhesion coating according to claim 1, characterized in that: The cleaning process of the AlCr target and the Cr target in the step (2) is as follows: introducing argon gas with a purity of 99.999% into the vacuum chamber, setting the Ar gas flow rate to 60 to 250 sccm, raising the pressure in the vacuum chamber to 0.5 to 3 Pa, turning on the Cr target and the AlCr target, and sputtering and cleaning the cathode target for 5 to 20 minutes; and setting the target current of the Cr target and the AlCr target to 1 to 8 A, and the substrate bias to -600 to -900 V.
5. The method for preparing the anti-aluminum liquid adhesion coating according to claim 1, characterized in that: The process of setting the relative intensity of the Al atomic spectrum line at 390-400nm in the step (2) is as follows: setting the Ar gas flow rate to 60-200sccm, gradually increasing the reaction gas N2 flow rate, so that the pressure in the vacuum chamber is 0.5-2Pa, setting the target voltage to 500-900V, the duty cycle to 10-80%, and the substrate bias to -40--150V; calibrating the intensity of the Al atomic spectrum line at 390-400nm sputtered in a pure Ar environment to be maximum; when the nitrogen flow rate is increased to 20-150sccm, the intensity of the Al atomic spectrum line at 390-400nm decreases to a minimum and remains stable, and at this time, the intensity of the Al atomic spectrum line at 390-400nm is calibrated to be extremely small.
6. The method for preparing the anti-aluminum liquid adhesion coating according to claim 1, characterized in that: The conditions for glow cleaning of the die casting mold steel substrate in step (3) are: when the background vacuum degree of the vacuum chamber is 1×10 -4 ~1×10 -2 Pa, Ar gas was introduced and the pressure was controlled at 1×10 -2 ~8×10 -1 Pa, negative bias voltage -500~-900V, bombardment time 5~30min.
7. The method for preparing the anti-aluminum liquid adhesion coating according to claim 1, characterized in that: The process of depositing the Cr bonding layer in step (3) is as follows: adjusting the Ar gas flow rate to 40-300 sccm and maintaining the gas pressure at about 0.3-0.8 Pa, setting the target current to 0.5-3 A, and depositing the Cr bonding layer for 1-8 min at a bias voltage of -100--200 V, and the coating thickness is 0.1-2 μm.
8. The method for preparing the coating layer resistant to aluminum liquid adhesion according to claim 1, characterized in that: The process of CrN transition layer deposition in step (3) is as follows: adjusting the Ar gas flow rate to 60-200 sccm, the N2 flow rate to 10-60 sccm, and maintaining the gas pressure at about 0.3-2 Pa, setting the target current to 0.5-3 A, and depositing the CrN transition layer for 1-15 minutes at a bias voltage of -50--150 V, and the coating thickness is 0.1-2 μm.
9. The method for preparing the coating layer resistant to aluminum liquid adhesion according to claim 1, characterized in that: The deposition process of the AlCrN functional layer in the step (3) is as follows: fixing the Al spectral line intensity, setting the Ar gas flow rate to 60-200 sccm, making the pressure in the vacuum chamber 0.5-2 Pa, setting the target voltage to 400-900 V, the duty cycle to 10-80%, the substrate bias to -40--150 V, setting the relative intensity of the Al atomic spectral line at 390-400 nm to any value of 0-100% and keeping the intensity value unchanged according to research and preparation needs, continuing sputtering for 50-120 min, and the coating thickness is 1-5 μm; opening the nitrogen passage, and dynamically and real-timely regulating the nitrogen flow rate according to the real-time plasma parameters by the gas flow meter until the spectral line intensity is stabilized at the parameter setting value, and then the film preparation can be carried out. The whole adjustment process takes about 1-10 min, and the nitrogen flow rate is 0-100 sccm.
10. An anti-aluminum liquid adhesion coating, which is an AlCrN functional layer prepared by the method for preparing an anti-aluminum liquid adhesion coating according to any one of claims 1 to 10, characterized in that: The AlCrN functional layer has the following components in terms of atomic percentage: Al: 30-40%, Cr: 15-25%, and N: 35-50%.
11. The AlCrN functional layer according to claim 10, characterized in that: The AlCrN functional layer also includes one selected from Si, B, C, O, W, Y and one or more other alloying elements, and the content of the other alloying elements in terms of atomic percentage is 1-4%.
Citation Information
Patent Citations
Multi-layer gradient high-temperature wear-resistant coating on surface of cutting tool and preparation method thereof
CN109735799A
HiPIMS power supply system based on spectrum feedback control
CN114649963A
Cited By
A CrAlN coating and preparation method thereof
CN119776780A