Manufacturing method of micro-foaming fluffy hot air non-woven fabric
By introducing micro-foaming technology into hot-air non-woven fabrics, using foaming masterbatch and cross-linking agent to form micro-foamed fiber filaments, combined with the sheath-core structure of polypropylene fiber filaments, the problem of hard texture and poor hygroscopicity of hot-air non-woven fabrics is solved. solve the problem, improve the structural stability and breathability, and achieve better application scenarios.
Patent Information
- Application Number
- CN202410914922.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-09
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2044-07-09
AI Technical Summary
Due to material characteristics and structural factors, hot air non-woven fabrics have a hard texture, poor hygroscopicity and air permeability, which limits its application scenarios, and the three-dimensional forming process affects the structural stability and tensile strength.
Using micro-foaming technology, by adding foaming masterbatch and cross-linking agent to polyethylene fiber filaments, hot air is used to melt the fiber filaments and generate foaming gas to form micro-foamed fiber filaments, which are combined with polypropylene fiber filaments to form a sheath core. Structure's composite fiber mesh improves structural stability and bulk.
It improves the structural stability, tensile strength, bulkiness and hygroscopicity of hot-air non-woven fabrics, improves touch, enhances breathability, and is close to the texture and performance of spunlaced non-woven fabrics.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of non-woven fabric production, and in particular to a method for producing a micro-foamed, fluffy hot-air non-woven fabric. Background Art
[0002] Hot air non-woven fabric is a non-woven fabric produced by combing the fibers and then using the hot air on the drying equipment to penetrate the fiber web and melt it under heat. Since the melt bonding generated when the hot air penetrates the fiber web is point-like rather than regional, the hot air non-woven fabric has the advantages of good fluffiness and breathability. In addition, the production process of hot air non-woven fabric is simple, the production efficiency is high, and the production cost is low. However, due to the characteristics of the materials used to make hot air non-woven fabrics and the structure of the internal fibers, hot air non-woven fabrics are usually made of one or more of polyethylene, polypropylene, and polyethylene terephthalate. The material has a relatively obvious plastic texture and feels hard to the touch. The texture of hot air non-woven fabrics is not as delicate and soft as spunlace non-woven fabrics, and their hygroscopicity is not as good as spunlace non-woven fabrics and meltblown non-woven fabrics, which limits the application scenarios of hot air non-woven fabrics.
[0003] Chinese patent publication number CN104988660A discloses a method for producing a three-dimensional hot air non-woven fabric, which includes the following steps: step 1, an opening process, in which the fibers are opened; step 2, a combing process, in which the opened fibers are combed into a fiber web; step 3, a hot air shaping process, in which the fiber web is sent into an oven for hot air penetration shaping, so that the fibers adhere to each other to form a flat hot air non-woven fabric; step 4, a three-dimensional forming process, in which the three-dimensional forming equipment consists of a pair of heatable, mutually meshing concave and convex rollers, the protrusions on the convex rollers are needles, the three-dimensional forming equipment is located at the outlet of the oven in step 3, and a hot air non-woven fabric preheating equipment is provided before the three-dimensional forming equipment; step 5, a winding process.
[0004] The above-mentioned hot air non-woven fabric has a three-dimensional effect through a three-dimensional forming process, so that the hot air non-woven fabric has a larger surface area and porosity, thereby having better fluffiness, hygroscopicity and air permeability, but the three-dimensional forming process will affect the stability of the hot air non-woven fabric structure, reduce the tensile strength of the hot air non-woven fabric, and it is difficult to maintain the three-dimensional effect under a certain temperature or pressure. At the same time, the hot air non-woven fabric has a three-dimensional effect by forming a three-dimensional structure through several protrusions on the surface. The three-dimensional structure will make the surface roughness of the hot air non-woven fabric higher and further highlight the harder texture of the material, thereby further reducing the surface touch of the hot air non-woven fabric, resulting in poor comfort of the hot air non-woven fabric, so there is still room for improvement. Summary of the invention
[0005] In view of the technical defects existing in the background technology, the present invention proposes a method for manufacturing a micro-foamed fluffy hot air non-woven fabric, which solves the above technical problems and meets the actual needs. The specific technical solution is as follows: A method for making a slightly foamed fluffy hot air nonwoven fabric comprises the following steps: S1. After heating 15-50 parts by mass of polyethylene until it is melted, 0.5-3 parts of a crosslinking agent, 0.1-1 parts of a foaming masterbatch, 0.02-0.2 parts of a dispersant, and 0.01-0.1 parts of an antioxidant are added, and the mixture is stirred to obtain a first component; S2, heating 50-100 parts by mass of polypropylene until it melts to obtain a second component; S3, spinning the first component and the second component through a composite spinning device to obtain composite fiber filaments, the composite fiber filaments are composed of polyethylene fiber filaments and polypropylene fiber filaments with a plurality of foaming masterbatches dispersed therein, and opening and combing the composite fibers to obtain a composite fiber web; S4, heating the polyethylene fiber filaments to a molten state by passing hot air through the composite fiber web so that the composite fiber filaments are bonded to each other, then increasing the temperature of the hot air to decompose the foaming masterbatch to generate foaming gas, the foaming gas foams the molten polyethylene fiber filaments and forms a plurality of pores on the surface, the polyethylene fiber filaments are foamed to obtain micro-foamed fiber filaments, and the micro-foamed fiber filaments and the polypropylene fiber filaments together form a micro-foamed fiber web; S5. The micro-foamed fiber web is aged, cooled and formed to obtain a hot air non-woven fabric composed of micro-foamed fiber filaments and polypropylene fiber filaments.
[0006] As a further technical solution of the present invention, in step S1, the polyethylene is heated to a melting temperature of 120-130°C.
[0007] As a further technical solution of the present invention, the cross-linking agent is dicumyl peroxide.
[0008] As a further technical solution of the present invention, the foaming masterbatch is modified sodium bicarbonate, and the foaming temperature of the foaming masterbatch is 140-155°C.
[0009] As a further technical solution of the present invention, the foaming masterbatch is prepared by the following method: dissolving 1 part of epoxy resin by mass in a sufficient amount of anhydrous ethanol under the action of ultrasound, then adding 4-5 parts of sodium bicarbonate powder, 0.1 parts of a surfactant, and 0.1 parts of a curing agent, and then stirring evenly to obtain a mixed solution, then heating the mixed solution to react and cure the epoxy resin, and after the reaction is completed, filtering the mixed solution to obtain a solid product, and washing and drying the solid product to obtain a sodium bicarbonate foaming masterbatch wrapped with epoxy resin.
[0010] As a further technical solution of the present invention, the surfactant is selected from one or more of sodium dodecylbenzene sulfonate, sodium tetrapropylenebenzene sulfonate, sodium diisooctyl sulfosuccinate, and sodium dibutylnaphthalene sulfonate; the curing agent is selected from one of diethylenetriamine, triethylenetetramine, and diethylaminopropylamine.
[0011] As a further technical solution of the present invention, the dispersant is selected from one or more of polyvinyl alcohol, sodium polyacrylate, polyvinyl pyrrolidone, and hydroxypropyl methylcellulose.
[0012] As a further technical solution of the present invention, the antioxidant is selected from one or more of butylated hydroxytoluene, AO-1010, AO-1076, AO-3114, and AO-330.
[0013] As a further technical solution of the present invention, in step S2, the polypropylene is heated to a melting temperature of 165-180°C.
[0014] As a further technical solution of the present invention, in step S4, the hot air temperature for heating the polyethylene fiber filaments to melt is 125-135°C, and the hot air temperature for decomposing the foaming masterbatch to generate foaming gas is 140-155°C.
[0015] The beneficial effects of the present invention are: The present invention forms composite fiber yarns of a skin-core structure by spinning polyethylene and polypropylene, wherein foaming masterbatch is added inside the polyethylene fiber yarn as the skin layer, and the polyethylene fiber yarn is melted by hot air to make the composite fiber yarns mutually bonded, and the foaming masterbatch is decomposed to generate gas at the same time, and the polyethylene fiber yarn is slightly foamed into micro-foamed fiber yarns by the gas, and the hot air non-woven fabric is composed of a fiber structure in which a plurality of micro-foamed fiber yarns wrap the polypropylene fiber yarns, and the contact area of the micro-foamed fiber yarns mutually bonded is large, so that the hot air non-woven fabric has good structural stability and tensile strength; in addition, since the surface of each fiber structure is the foamed micro-foamed fiber yarn, the hot air non-woven fabric has good fluffiness and comfort, and at the same time, the plurality of pores on the surface of the micro-foamed fiber yarn make the hot air non-woven fabric have good hygroscopicity and air permeability. DETAILED DESCRIPTION
[0016] The implementation mode of the present invention is described below in conjunction with relevant embodiments. The implementation mode of the present invention is not limited to the following embodiments, and the present invention relates to relevant necessary components in the technical field, which should be regarded as the known technology in the technical field and can be known and mastered by the technical personnel in the technical field.
[0017] A method for making a slightly foamed fluffy hot air nonwoven fabric comprises the following steps: S1. After heating 15-50 parts by mass of polyethylene until it is melted, 0.5-3 parts of a crosslinking agent, 0.1-1 parts of a foaming masterbatch, 0.02-0.2 parts of a dispersant, and 0.01-0.1 parts of an antioxidant are added, and the mixture is stirred to obtain a first component; S2, heating 50-100 parts by mass of polypropylene until it melts to obtain a second component; S3, spinning the first component and the second component through a composite spinning device to obtain composite fiber filaments, the composite fiber filaments are composed of polyethylene fiber filaments and polypropylene fiber filaments with a plurality of foaming masterbatches dispersed therein, and opening and combing the composite fibers to obtain a composite fiber web; S4, heating the polyethylene fiber filaments to a molten state by passing hot air through the composite fiber web so that the composite fiber filaments are bonded to each other, then increasing the temperature of the hot air to decompose the foaming masterbatch to generate foaming gas, the foaming gas foams the molten polyethylene fiber filaments and forms a plurality of pores on the surface, the polyethylene fiber filaments are foamed to obtain micro-foamed fiber filaments, and the micro-foamed fiber filaments and the polypropylene fiber filaments together form a micro-foamed fiber web; S5. The micro-foamed fiber web is aged, cooled and formed to obtain a hot air non-woven fabric composed of micro-foamed fiber filaments and polypropylene fiber filaments.
[0018] The invention discloses a method for preparing a two-component hot air nonwoven fabric, wherein the polyethylene in step S1 is a component with a low melting point in the hot air nonwoven fabric, and the polypropylene in step S2 is a component with a high melting point in the hot air nonwoven fabric. The polyethylene serves as an adhesive structure inside the hot air nonwoven fabric, and has good adhesive performance, low temperature resistance, and chemical stability, and can effectively bond polypropylene fibers together to form a stable and continuous nonwoven fabric structure, which is beneficial to improving the tensile strength and stability of the hot air nonwoven fabric. The polypropylene has good acid and alkali resistance, high temperature resistance, air permeability, antibacterial properties, etc. The two-component hot air nonwoven fabric formed by the polyethylene and the polypropylene has good chemical stability, air permeability, antibacterial properties, etc.
[0019] In step S1, a cross-linking agent, a foaming masterbatch, a dispersant, and an antioxidant are added to the polyethylene. The dispersant improves the dispersibility of the foaming masterbatch in the first component by adsorbing on the surface of the foaming masterbatch to form a protective film and reacting with the groups on the surface of the foamed particles, so that the foaming masterbatch is evenly distributed in the polyethylene melt. The foaming masterbatch is used to make the polyethylene foam and expand when the hot air non-woven fabric is formed by bonding with polyethylene. The uniform distribution of the foaming masterbatch is conducive to uniform foaming of the polyethylene to form a foam with a uniform pore structure. The cross-linking agent increases the viscosity, elasticity and melt strength of the polyethylene melt by cross-linking reaction with the polyethylene, so that the polyethylene melt has sufficient strength to The foaming process is carried out to improve the strength of the foamed body. The antioxidant can prevent the polyethylene from being oxidized and degraded in a high temperature environment, thereby improving the durability of the hot air non-woven fabric. It should be noted that the foaming temperature of the foaming masterbatch needs to be higher than the melting temperature of the polyethylene and lower than the melting temperature of the polypropylene, so that the foaming masterbatch will not foam in the first component, and the first component will maintain a stable melt structure. In addition, in the subsequent process of heating the polyethylene to melt and bonding the composite fiber filaments to each other into a non-woven fabric, the polypropylene fiber filaments will not be in a molten state when the foaming particles are foamed, so that the polypropylene fiber filaments remain in a solid state during the bonding process of the composite fiber filaments, thereby improving the stability of the hot air non-woven fabric structure after bonding.
[0020] In step S3, the first component is mainly composed of polyethylene melt, and the second component is polypropylene melt. The first component and the second component are spun through a composite spinning device to form composite fiber filaments, wherein the first component and the second component can be respectively sprayed out through parallel spinneret holes to form composite fiber filaments composed of polyethylene fiber filaments and polypropylene fiber filaments in parallel, or can be spun through coaxial spinneret holes to form composite fiber filaments with a skin-core structure in which the polyethylene fiber filaments are the skin layer and the polypropylene fiber filaments are the core layer. The composite fiber filaments of the present invention are preferably of a skin-core structure. After the composite fiber filaments are sprayed out through the spinneret holes, they are continuously formed under the traction of the airflow, and then collected by a receiving device. After the composite fiber filaments are cooled, they are opened and combed to form a composite fiber web composed of a plurality of composite fiber filaments, and the composite fiber web has a structure of a non-woven fabric.
[0021] In step S4, since the composite fiber filaments are of a skin-core structure, the hot air will heat the polyethylene on the surface to a molten state after penetrating the composite fiber web, and the composite fiber filaments will be bonded to each other through the molten polyethylene. If the composite fiber web is cooled at this time to solidify the polyethylene, a conventional two-component hot air non-woven fabric with a skin-core structure will be obtained. In the present invention, it is necessary to further increase the temperature of the hot air to increase the temperature of the foaming masterbatch inside the polyethylene fiber filaments to the foaming temperature. The foaming masterbatch will decompose to produce gas, and since the polyethylene fiber filaments are in a molten state, these gases will cause the polyethylene fiber filaments to expand inside or escape to the surface of the polyethylene fiber filaments, thereby causing the polyethylene fiber filaments to expand and A plurality of pore structures are formed, that is, the polyethylene fiber filaments are foamed into a foam body through the foaming masterbatch, and the foam body is a micro-foamed fiber filament wrapped on the outer surface of the polypropylene fiber. At this time, the fibers inside the composite fiber web are still a skin-core structure, the skin layer is the micro-foamed fiber filaments, and the core layer is the polypropylene fiber filaments. The fiber filaments of the skin-core structure are bonded to each other through the micro-foamed fiber filaments to form a micro-foamed fiber web. After the polyethylene fiber filaments are foamed into micro-foamed fiber filaments, the thickness increases, and the contact area of the micro-foamed fiber filaments in the micro-foamed fiber web is increased, which ensures the bonding strength of the micro-foamed fiber web, and can make the final hot air non-woven fabric have good structural stability and tensile strength.
[0022] In step S5, the micro-foam fiber web is placed in an environment of a certain temperature for aging. During the aging process, the polyethylene molecular structure inside the micro-foam fiber filaments will be rearranged and cross-linked to form a more compact and ordered structure, which is beneficial to improving the heat resistance, chemical resistance and mechanical properties of the micro-foam fiber filaments. After the micro-foam fiber filaments are aged and cooled and shaped, the polypropylene fiber filaments are firmly wrapped inside and together form a skin-core fiber filament with a skin-core structure. Several skin-core fiber filaments are adhered to each other through the micro-foam fibers on the surface to form a hot air non-woven fabric. It should be noted that the amount of foaming masterbatch added in the first component is small, and the amount of gas generated by the foaming masterbatch during the foaming process is small. The polyethylene fiber filaments will only produce slight foaming during the foaming process, so that the foamed micro-foam fiber filaments can still maintain a fibrous shape. The diameter of the foam fiber is about twice that of the polyethylene fiber, and the diameter of the core-skin fiber is about 1.2-1.5 times that of the composite fiber. The gaps between the fibers in the composite fiber web will not disappear due to the foaming of the polyethylene fiber. Therefore, the hot air non-woven fabric is still a fiber web structure, and there are still a large number of gaps between the core-skin fiber and maintain a certain air permeability. The surface of each core-skin fiber is a micro-foamed fiber formed by foaming and has good softness and fluffiness, which makes the hot air non-woven fabric have a good touch and improves its comfort. The micro-foamed fiber has many pore structures and increases the gaps between the fiber filaments during its foaming process to maintain good air permeability. At the same time, the hot air non-woven fabric exhibits a strong capillary action when in contact with liquid through these pores, thereby having good hygroscopicity.
[0023] In summary, the present invention forms a composite fiber filament with a skin-core structure by spinning polyethylene and polypropylene, and a foaming masterbatch is added to the polyethylene fiber filament as the skin layer. The polyethylene fiber filament is melted by hot air to make the composite fiber filaments bonded to each other, and the foaming masterbatch is decomposed to generate gas at the same time. The gas causes the polyethylene fiber filament to be slightly foamed into micro-foamed fiber filaments. The hot air non-woven fabric is composed of a fiber structure in which a plurality of micro-foamed fiber filaments wrap the polypropylene fiber filaments. The contact area of the micro-foamed fiber filaments bonded to each other is large, so that the hot air non-woven fabric has good structural stability and tensile strength. In addition, since the surface of each fiber structure is a foamed micro-foamed fiber filament, the hot air non-woven fabric has good fluffiness and comfort. At the same time, the plurality of pores on the surface of the micro-foamed fiber filaments make the hot air non-woven fabric have good hygroscopicity and air permeability.
[0024] As one of the preferred embodiments of the present invention, in step S1, the polyethylene is heated to a melting temperature of 120-130°C.
[0025] The melting point of polyethylene is 110-130°C. In step S1 of the present invention, the polyethylene is heated to 120-130°C in order to make the polyethylene completely molten and have good fluidity and plasticity. The good fluidity makes it easier to disperse the foaming masterbatch evenly in the first component, and the good plasticity enables the first component to be reshaped into fibrous polyethylene fibers through the spinning process.
[0026] As one of the preferred embodiments of the present invention, the cross-linking agent is dicumyl peroxide.
[0027] Since polyethylene has a high gas permeability, the foaming gas generated by the decomposition of the foaming agent can easily penetrate the polyethylene melt to escape and reduce the foaming effect. After the cross-linking agent is added to the polyethylene, the cross-linking agent will react with the polyethylene to increase the viscosity, elasticity and strength of the polyethylene melt, making it difficult for the foaming gas to penetrate the polyethylene melt to escape, thereby causing the polyethylene fiber to foam inside to form a number of pore structures and obtain micro-foamed fiber filaments; diisopropylbenzene oxide decomposes to generate active free radicals, which capture hydrogen on the polyethylene carbon chain and form large molecular free radicals, thereby generating carbon-carbon coupling cross-linking to form a network structure.
[0028] As one of the preferred embodiments of the present invention, the foaming masterbatch is modified sodium bicarbonate, and the foaming temperature of the foaming masterbatch is 140-155°C.
[0029] The foaming masterbatch of the present invention uses modified sodium bicarbonate which is modified and starts to decompose and generate carbon dioxide only after being heated to 140-155°C. Since the foaming masterbatch needs to be added to the polyethylene melt and mixed with other additives to form the first component, and the polyethylene needs to be heated to 120-130°C to be converted into a molten state, the foaming masterbatch can be prevented from being thermally decomposed in this process. Therefore, during the hot air bonding process of the composite fiber web, the polyethylene fiber filaments can be converted into a molten state by the foaming temperature of the foaming masterbatch, and the foaming masterbatch can be decomposed to generate carbon dioxide, thereby foaming the polyethylene fiber filaments into micro-foamed fiber filaments.
[0030] As one of the preferred embodiments of the present invention, the foaming masterbatch is prepared by the following method: dissolving 1 part of epoxy resin by mass in a sufficient amount of anhydrous ethanol under the action of ultrasound, then adding 4-5 parts of sodium bicarbonate powder, 0.1 parts of a surfactant, and 0.1 parts of a curing agent and continuing to stir evenly to obtain a mixed solution, then heating the mixed solution to react and cure the epoxy resin, and after the reaction is completed, filtering the mixed solution to obtain a solid product, washing and drying the solid product to obtain a sodium bicarbonate foaming masterbatch wrapped with epoxy resin.
[0031] The foaming masterbatch of the present invention is a microcapsule of sodium bicarbonate wrapped in epoxy resin. During the production process of the foaming masterbatch, the epoxy resin is dissolved in anhydrous ethanol by ultrasonic wave to obtain an epoxy resin solution, and then micron-grade sodium bicarbonate powder, surfactant and curing agent are added. The sodium bicarbonate powder is difficult to dissolve in the epoxy resin solution and is dispersed in the solution, while the surfactant and curing agent are dissolved in the epoxy resin solution. The surfactant can reduce the surface tension of the epoxy resin solution and increase the wettability and dispersibility of the sodium bicarbonate powder in the solution. Then, the epoxy resin solution is kept stirred and heated to 60-80°C so that the curing agent promotes the epoxy resin to dissolve in the epoxy resin solution. The epoxy resin is cured by the epoxy resin, and the cured epoxy resin cannot be further dissolved in the anhydrous ethanol and is precipitated on the surface of the sodium bicarbonate powder. After all the epoxy resins are cured, a plurality of particles of the sodium bicarbonate powder wrapped by the epoxy resin are dispersed in the solution. Then the solution is filtered to obtain a solid product. The solid product is washed and dried to obtain a foaming masterbatch. The foaming temperature of the foaming masterbatch obtained after the sodium bicarbonate is modified by wrapping with the epoxy resin is 140-155° C., which is suitable for foaming the polyethylene fiber filaments of the present invention. The foaming masterbatch is a micron-sized particle, which ensures that the polyethylene fiber filaments can be formed through a spinning process after being mixed in the polyethylene melt.
[0032] As one of the preferred embodiments of the present invention, the surfactant is selected from one or more of sodium dodecylbenzene sulfonate, sodium tetrapropylenebenzene sulfonate, sodium diisooctyl sulfosuccinate, and sodium dibutylnaphthalene sulfonate; the curing agent is selected from one of diethylenetriamine, triethylenetetramine, and diethylaminopropylamine.
[0033] The surfactant of the invention can form a thin film on the surface of the epoxy resin solution, thereby reducing the surface tension of the epoxy resin solution and making it easier to flow and disperse. The surfactant can also be adsorbed on the interface between the epoxy resin solution and the sodium bicarbonate powder, and serve as an intermediary between two immiscible substances to improve the compatibility of the two substances, thereby promoting the uniform dispersion of the sodium bicarbonate powder in the epoxy resin solution. After heating the epoxy resin solution, the curing agent and the epoxy resin are promoted to undergo a condensation reaction to generate a cross-linking structure, thereby forming a fixed three-dimensional network structure and hardened epoxy resin. The cured epoxy resin is precipitated on the surface of the sodium bicarbonate powder because it cannot be dissolved in anhydrous ethanol, thereby obtaining a foaming masterbatch consisting of the sodium bicarbonate powder wrapped by the epoxy resin.
[0034] As one of the preferred embodiments of the present invention, the dispersant is selected from one or more of polyvinyl alcohol, sodium polyacrylate, polyvinyl pyrrolidone, and hydroxypropyl methylcellulose.
[0035] Among the dispersants of the present invention, polyvinyl alcohol and sodium polyacrylate are non-ionic dispersants. Such dispersants can react with the carbonyl structure in the epoxy resin on the surface of the foaming masterbatch through their functional groups, which helps to evenly disperse the foaming masterbatch in the polyethylene melt; sodium polyacrylate, polyvinyl pyrrolidone and hydroxypropyl methylcellulose are polymer dispersants. Such dispersants can form a protective film on the surface of the foaming masterbatch by adsorption, so that the foaming masterbatch forms a stable dispersion system in the polyethylene melt.
[0036] As one of the preferred embodiments of the present invention, the antioxidant is selected from one or more of butylated hydroxytoluene, AO-1010, AO-1076, AO-3114, and AO-330.
[0037] The antioxidant of the present invention performs antioxidant effects by inhibiting thermal oxidative degradation and the reaction of free radicals with oxygen during the heating process of polyethylene, thereby improving the thermal stability, weather resistance and other properties of polyethylene, avoiding thermal degradation that leads to a decrease in the performance and shortened life of the polyethylene material, and enabling the polyethylene to maintain good physical and chemical properties in a high temperature environment, thereby increasing the service life of the polyethylene material.
[0038] As one of the preferred embodiments of the present invention, in step S2, the polypropylene is heated to a melting temperature of 165-180°C.
[0039] In the present invention, the polypropylene fiber filaments are the main components of the hot air non-woven fabric, and their melting temperature is higher than the foaming temperature of the foaming masterbatch. When the polyethylene fiber filaments bond the composite fiber filaments to each other and the foaming particles are foamed, the polypropylene fiber filaments will be in a solid state. The polypropylene fiber filaments can be used as a skeleton structure in this process to keep the original structure of the composite fiber web stable, thereby ensuring the stability of the hot air non-woven fabric structure after bonding and foaming.
[0040] As one of the preferred embodiments of the present invention, in step S4, the hot air temperature for heating the polyethylene fiber filaments to melt is 125-135°C, and the hot air temperature for decomposing the foaming masterbatch to generate foaming gas is 140-155°C.
[0041] The melting point of polyethylene is 110-130°C, and the hot air heating temperature of 125-135°C can make polyethylene completely molten and have good fluidity and plasticity, so that the composite fiber filaments are bonded to each other through the molten polyethylene fiber filaments. When the hot air temperature rises to 140-155°C, the sodium bicarbonate inside the foaming masterbatch will gradually decompose to produce carbon dioxide, and the carbon dioxide will foam the molten polyethylene fiber filaments into micro-foamed fiber filaments. The foaming temperature of the foaming masterbatch is higher than the melting temperature of polyethylene and lower than the melting temperature of polypropylene, so that the foaming masterbatch will not foam in the first component but foam when the composite fiber filaments are bonded to each other, thereby finally obtaining a hot air non-woven fabric with good fluffiness, comfort, hygroscopicity and air permeability.
[0042] The present invention is further described below by way of examples and comparative examples.
[0043] Example 1
[0044] S1. Heat 20 parts of polyethylene by mass until it is melted, add 1 part of a cross-linking agent, 0.3 parts of a foaming masterbatch, 0.08 parts of a dispersant, and 0.03 parts of an antioxidant, mix and stir evenly to obtain a first component; S2, heating 80 parts by mass of polypropylene until it melts to obtain a second component; S3, spinning the first component and the second component through a composite spinning device to obtain composite fiber filaments with a core-skin structure, and opening and combing the composite fibers to obtain a composite fiber web; S4, heating the polyethylene fiber filaments to a molten state by passing hot air through the composite fiber web so that the composite fiber filaments are bonded to each other, then increasing the temperature of the hot air to decompose the foaming masterbatch to generate foaming gas, the foaming gas foams the molten polyethylene fiber filaments and forms a plurality of pores on the surface, the polyethylene fiber filaments are foamed to obtain micro-foamed fiber filaments, and the micro-foamed fiber filaments and the polypropylene fiber filaments together form a micro-foamed fiber web; S5. The micro-foamed fiber web is aged, cooled and formed to obtain a hot air non-woven fabric composed of micro-foamed fiber filaments and polypropylene fiber filaments.
[0045] Example 2
[0046] S1. Heat 35 parts of polyethylene by mass until it is melted, add 1.8 parts of a crosslinking agent, 0.55 parts of a foaming masterbatch, 0.15 parts of a dispersant, and 0.06 parts of an antioxidant, mix and stir evenly to obtain a first component; S2, heating 65 parts by mass of polypropylene until it melts to obtain a second component; S3, spinning the first component and the second component through a composite spinning device to obtain composite fiber filaments with a core-skin structure, and opening and combing the composite fibers to obtain a composite fiber web; S4, heating the polyethylene fiber filaments to a molten state by passing hot air through the composite fiber web so that the composite fiber filaments are bonded to each other, then increasing the temperature of the hot air to decompose the foaming masterbatch to generate foaming gas, the foaming gas foams the molten polyethylene fiber filaments and forms a plurality of pores on the surface, the polyethylene fiber filaments are foamed to obtain micro-foamed fiber filaments, and the micro-foamed fiber filaments and the polypropylene fiber filaments together form a micro-foamed fiber web; S5. The micro-foamed fiber web is aged, cooled and formed to obtain a hot air non-woven fabric composed of micro-foamed fiber filaments and polypropylene fiber filaments.
[0047] Example 3
[0048] S1. Heat 50 parts of polyethylene by mass until it is melted, add 2.5 parts of a crosslinking agent, 0.8 parts of a foaming masterbatch, 0.2 parts of a dispersant, and 0.08 parts of an antioxidant, mix and stir evenly to obtain a first component; S2, heating 50 parts by mass of polypropylene until it melts to obtain a second component; S3, spinning the first component and the second component through a composite spinning device to obtain composite fiber filaments with a core-skin structure, and opening and combing the composite fibers to obtain a composite fiber web; S4, heating the polyethylene fiber filaments to a molten state by passing hot air through the composite fiber web so that the composite fiber filaments are bonded to each other, then increasing the temperature of the hot air to decompose the foaming masterbatch to generate foaming gas, the foaming gas foams the molten polyethylene fiber filaments and forms a plurality of pores on the surface, the polyethylene fiber filaments are foamed to obtain micro-foamed fiber filaments, and the micro-foamed fiber filaments and the polypropylene fiber filaments together form a micro-foamed fiber web; S5. The micro-foamed fiber web is aged, cooled and formed to obtain a hot air non-woven fabric composed of micro-foamed fiber filaments and polypropylene fiber filaments.
[0049] Comparative Example 1 20 parts of polyethylene and 80 parts of polypropylene by mass are heated to a molten state respectively and then spun through a composite spinning device to obtain a composite fiber filament with a core-sheath structure. The composite fibers are opened and combed to obtain a composite fiber web. Hot air penetrates the composite fiber web to heat the polyethylene fiber filaments to a molten state so that the composite fiber filaments are bonded to each other, and then cooled and formed to obtain a hot air non-woven fabric.
[0050] Comparative Example 2 35 parts of polyethylene and 65 parts of polypropylene by mass are heated to a molten state respectively and then spun through a composite spinning device to obtain a composite fiber filament with a core-sheath structure. The composite fibers are opened and combed to obtain a composite fiber web. Hot air is passed through the composite fiber web to heat the polyethylene fiber filaments to a molten state so that the composite fiber filaments are bonded to each other, and then cooled and formed to obtain a hot air non-woven fabric.
[0051] Comparative Example 3 50 parts of polyethylene and 50 parts of polypropylene by mass are respectively heated to a molten state and then spun through a composite spinning device to obtain composite fiber filaments with a core-sheath structure. The composite fibers are opened and combed to obtain a composite fiber web. Hot air penetrates the composite fiber web to heat the polyethylene fiber filaments to a molten state so that the composite fiber filaments are bonded to each other, and then cooled and formed to obtain a hot air non-woven fabric.
[0052] According to Part 3: Determination of breaking strength and breaking elongation, Part 6: Absorbency determination, and Part 15: Air permeability determination in GB / T24218 "Test methods for textile nonwovens", the breaking strength, liquid absorption, and air permeability of the hot air nonwoven fabrics obtained in the above embodiments and comparative examples were tested respectively. In order to more intuitively compare the absorbency of the hot air nonwoven fabric, the liquid absorption obtained by the absorbency determination needs to be calculated based on the dry weight of the hot air nonwoven fabric before the test. The above test results are shown in Table 1 below:
[0053] Table 1 According to the data in Table 1, the breaking strength of the hot air nonwoven fabrics in Examples 1-3 increases first and then decreases with the increase in the amount of polyethylene added. This is because the fiber filaments in the hot air nonwoven fabric are bonded and fixed to each other by polyethylene and the polyethylene exists in the state of foam. The increase in the amount of polyethylene added will increase the contact area between the fiber filaments, thereby increasing the bonding strength between the fiber filaments. However, the tensile strength of the polyethylene foam is low, and the higher its content, the lower the tensile strength of the hot air nonwoven fabric. Therefore, the amount of polyethylene added needs to be within a reasonable range, and the addition ratio of polyethylene in Example 2 is more reasonable; the water absorption rate of the hot air nonwoven fabrics in Examples 1-3 increases with the increase in the amount of polyethylene added. This is because the polyethylene exists in the form of foam. The hot air nonwoven fabric exists in a state of a body, which has many pore structures and absorbs and locks a large amount of liquid through capillary action. Therefore, increasing the amount of polyethylene added is beneficial to improving the hygroscopicity of the hot air nonwoven fabric; the air permeability of the hot air nonwoven fabric in Examples 1-3 decreases slightly with the increase in the amount of polyethylene added. This is because the fiber filaments in the hot air nonwoven fabric are bonded and fixed to each other by polyethylene. The higher the amount of polyethylene added, the tighter the degree of bonding and fixing between the internal fiber filaments, resulting in a decrease in the gaps between the fiber filaments, while polyethylene will increase the gaps between the fiber filaments during the foaming process, and the polyethylene foam has a number of pore structures. Therefore, the air permeability of the hot air nonwoven fabric will not decrease significantly with the increase in the amount of polyethylene added, thereby maintaining good air permeability.
[0054] Comparing the data of the embodiment and the comparative example in Table 1, although the hot air non-woven fabrics prepared with the same ratio are compared, the hot air non-woven fabric obtained in the embodiment has a lower tensile strength, but better hygroscopicity and air permeability, especially the hygroscopicity is significantly improved; in addition, when the hot air non-woven fabric is touch tested, the hot air non-woven fabric obtained in the embodiment has a more delicate texture and good softness, and its touch, softness and hygroscopicity are comparable to the common spunlace non-woven fabrics on the market, while the hot air non-woven fabric obtained in the comparative example continues the disadvantage of the traditional hot air non-woven fabric being harder to touch; it can be seen that the hot air non-woven fabric obtained based on the technical solution of the present invention improves the defects of the traditional hot air non-woven fabric such as poor texture and poor hygroscopicity, combined with the relatively simple production process and high production efficiency of the hot air non-woven fabric, the hot air non-woven fabric can be applied to more products and fields.
[0055] The above is only a preferred embodiment of the present invention. It should be pointed out that ordinary technicians in this technical field can make several improvements and modifications without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for making a slightly foamed fluffy hot air nonwoven fabric, It is characterized in that The following steps are involved: S1. After heating 15-50 parts by mass of polyethylene until it is melted, 0.5-3 parts of a crosslinking agent, 0.1-1 parts of a foaming masterbatch, 0.02-0.2 parts of a dispersant, and 0.01-0.1 parts of an antioxidant are added, and the mixture is stirred to obtain a first component; S2, heating 50-100 parts by mass of polypropylene until it melts to obtain a second component; S3, spinning the first component and the second component through a composite spinning device to obtain composite fiber filaments, the composite fiber filaments are composed of polyethylene fiber filaments and polypropylene fiber filaments with a plurality of foaming masterbatches dispersed therein, and opening and combing the composite fibers to obtain a composite fiber web; S4, heating the polyethylene fiber filaments to a molten state by passing hot air through the composite fiber web so that the composite fiber filaments are bonded to each other, then increasing the temperature of the hot air to decompose the foaming masterbatch to generate foaming gas, the foaming gas foams the molten polyethylene fiber filaments and forms a plurality of pores on the surface, the polyethylene fiber filaments are foamed to obtain micro-foamed fiber filaments, and the micro-foamed fiber filaments and the polypropylene fiber filaments together form a micro-foamed fiber web; S5. The micro-foamed fiber web is aged, cooled and formed to obtain a hot air non-woven fabric composed of micro-foamed fiber filaments and polypropylene fiber filaments.
2. The method for making the micro-foamed fluffy hot air nonwoven fabric according to claim 1, It is characterized in that In step S1, polyethylene is heated to a melting temperature of 120-130°C.
3. The method for making the micro-foamed fluffy hot air nonwoven fabric according to claim 1, It is characterized in that The cross-linking agent is dicumyl peroxide.
4. The method for making the micro-foamed fluffy hot air nonwoven fabric according to claim 1, It is characterized in that The foaming masterbatch is made of modified sodium bicarbonate, and the foaming temperature of the foaming masterbatch is 140-155°C.
5. The method for making the micro-foamed fluffy hot air non-woven fabric according to claim 4, It is characterized in that The foaming masterbatch is prepared by the following method: dissolving 1 part of epoxy resin by mass in sufficient anhydrous ethanol under the action of ultrasound, then adding 4-5 parts of sodium bicarbonate powder, 0.1 parts of surfactant, and 0.1 parts of curing agent, and then stirring evenly to obtain a mixed solution, then heating the mixed solution to react and cure the epoxy resin, filtering the mixed solution after the reaction is completed to obtain a solid product, and washing and drying the solid product to obtain the sodium bicarbonate foaming masterbatch wrapped by the epoxy resin.
6. The method for making the micro-foamed fluffy hot air nonwoven fabric according to claim 5, It is characterized in that The surfactant is selected from one or more of sodium dodecylbenzene sulfonate, sodium tetrapropylenebenzene sulfonate, sodium diisooctyl sulfosuccinate, and sodium dibutylnaphthalene sulfonate; the curing agent is selected from one of diethylenetriamine, triethylenetetramine, and diethylaminopropylamine.
7. The method for making the micro-foamed fluffy hot air nonwoven fabric according to claim 1, It is characterized in that The dispersant is selected from one or more of polyvinyl alcohol, sodium polyacrylate, polyvinyl pyrrolidone and hydroxypropyl methylcellulose.
8. The method for making the micro-foamed fluffy hot air nonwoven fabric according to claim 1, It is characterized in that The antioxidant is selected from one or more of butylated hydroxytoluene, AO-1010, AO-1076, AO-3114, and AO-330.
9. The method for making the micro-foamed fluffy hot air nonwoven fabric according to claim 1, It is characterized in that In step S2, the polypropylene is heated to a melting temperature of 165-180°C.
10. The method for making the micro-foamed fluffy hot air nonwoven fabric according to claim 1, It is characterized in that In step S4, the hot air temperature for heating the polyethylene fiber filaments to melt is 125-135°C, and the hot air temperature for decomposing the foaming masterbatch to generate foaming gas is 140-155°C.
Citation Information
Patent Citations
Hot-wind nonwoven cloth and producing method thereof
CN101487171A
Nontoxic, odorless and environment-friendly damping compound foam and preparation process thereof
CN108893866A
Microporous skin-core structured bi-component composite fiber preparation method
CN110359129A
Flow guide non-woven fabric and water-absorbing hygienic product with flow guide non-woven fabric
CN117403377A
Nonwoven fabric sheet, and hydrous sheet and cosmetic each including the same