High-nickel positive electrode material, preparation method thereof and battery
Through the preparation of hollow structure high-nickel cathode materials, the problem of low rate performance of lithium-ion battery cathode materials is solved, high capacity and high rate performance are improved, and energy and costs are saved.
Patent Information
- Application Number
- CN202411159455.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-22
- Publication Date
- 2024-10-08
AI Technical Summary
The polycrystalline polymer spherical or single crystal particle morphology of existing lithium-ion battery cathode materials limits the wettability of the electrolyte and the material, resulting in a decrease in rate performance, and cannot meet the needs of small-power mobile devices for high capacity and high rate performance. .
The hollow structure high-nickel cathode material is prepared through sand spray drying and sintering processes to form a hollow structure material with an average particle size of 1~40μm and a specific surface area of 0.15~1.5m2/g, which increases the reaction interface area between the electrolyte and the material. .
The diffusion rate of lithium ions and the capacity and rate performance of the battery are improved, and the process efficiency is high, the cost is low, and the structure is stable.
Smart Images

Figure CN118748249A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of lithium ion battery materials, and in particular relates to a high-nickel positive electrode material and a preparation method and application thereof. Background Art
[0002] With the expansion and development of small-power mobile devices in the application fields of power tools, AGV logistics vehicles, drones, etc., small-power mobile devices have higher and higher performance requirements for lithium-ion batteries. In order to meet the application scenario requirements of small-power mobile devices, lithium-ion batteries need higher capacity and greater rate. The most important aspect of increasing battery capacity is to use higher-capacity positive electrode materials. Increasing the Ni content in the positive electrode material is the most effective way to increase the capacity of the positive electrode material. In terms of improving the rate performance of the battery, improving the wettability of the positive electrode material in the electrolyte and increasing the specific surface area of the reaction with the electrolyte can improve the rate performance of the positive electrode material, thereby improving the rate performance of the battery.
[0003] The morphology of conventional positive electrode materials is polycrystalline aggregate sphere or single crystal particle. These two morphologies often limit the wettability of the electrolyte and the interior of the positive electrode material particles, resulting in the internal electrons and Li + The diffusion migration path increases and the rate performance decreases. Summary of the invention
[0004] In view of the problems existing in the prior art, the first object of the present invention is to provide a high nickel positive electrode material with a hollow structure. The second object of the present invention is to provide a method for preparing the high nickel positive electrode material with a hollow structure. The third object of the present invention is to provide a battery.
[0005] To achieve the above objectives, the present invention provides the following specific technical solutions.
[0006] First, the present invention provides a high-nickel positive electrode material, wherein the high-nickel positive electrode material is a hollow structure; the average particle size of the primary particles is 0.1-3 μm, preferably 0.5-1.0 μm, and more preferably 0.65-0.8 μm; the average particle size of the high-nickel positive electrode material is 1-40 μm, preferably 4-10 μm, and more preferably 5-8 μm; the SSA of the high-nickel positive electrode material satisfies 0.15 μm 2 / g≤SSA≤1.5 m 2 / g, preferably 0.25m 2 / g≤SSA≤0.5m 2 / g, more preferably 0.25m 2 / g≤SSA≤0.41m 2 / g.
[0007] Furthermore, as a preferred embodiment, the shell of the hollow structure includes 1 to 5 layers of primary particle stacking layers, preferably includes 1 to 4 layers of primary particle stacking layers, and more preferably includes 1 to 3 layers of primary particle stacking layers.
[0008] Furthermore, as a preferred embodiment, the chemical formula of the high nickel cathode material is Li a Ni x Co y M z M' β O2, wherein 0.95≤a≤1.2, 0.8≤x≤1, 0≤y≤0.2, 0≤z≤0.05, 0≤β≤0.05, x+y+z+β=1; M is one or more of Mn, Al, Zr, Mg, W, Ti, Y, La, B and Sr, preferably Al; M' is one or more of Mn, Al, Zr, Mg, W, Ti, Y, La, B, Sr, P, C, preferably at least one of Mg and Mn.
[0009] Based on the same inventive concept, the present invention provides a method for preparing the above-mentioned high-nickel positive electrode material, comprising the following steps: Step S1, adding lithium salt, a precursor of a high-nickel positive electrode material, and water into a sand mill for sand grinding to obtain a sand grinding slurry; Step S2, spray drying the sand-milled slurry to obtain a powder material; Step S3, sintering the powder material to obtain a high-nickel positive electrode material.
[0010] Furthermore, in some preferred embodiments of the present invention, in step S1, a compound of M' is added to a sand mill, and M' is one or more of Mn, Al, Zr, Mg, W, Ti, Y, La, B, Sr, P, and C, preferably at least one of Mn and Mg.
[0011] Further, in some preferred embodiments of the present invention, the chemical expression of the precursor of the high nickel cathode material is Ni x Co y M z (OH)2, 0.8≤x≤1, 0≤y≤0.2, 0≤z≤0.05, x+y+z=1; M is one or more of Mn, Al, Zr, Mg, W, Ti, Y, La, B and Sr, preferably Al.
[0012] Furthermore, in some preferred embodiments of the present invention, lithium salt and precursor materials are added into a sand mill in a ratio of the molar amount of Li to the sum of the molar amounts of Ni, Co, M and M' of 1.005-1.02:1.
[0013] Further, in some preferred embodiments of the present invention, the particle size of the sand-grinding slurry is 100-500 nm.
[0014] Furthermore, in some preferred embodiments of the present invention, the solid content of the sand-grinding slurry is controlled to be 5%-40%.
[0015] Furthermore, in some preferred embodiments of the present invention, the spray drying is carried out in a spray drying device using a two-fluid spray method.
[0016] Furthermore, in some preferred embodiments of the present invention, the air pressure of the spray drying dust collecting tower is less than -5Pa, the air inlet heating temperature is ≥350°C, the slurry feed rate is 1L / h-10L / h, and the compressed air inlet flow rate of the spray drying nozzle is 0.2-2m 3 / min, the compressed air pressure of the spray drying nozzle is 0.1-0.8Mpa.
[0017] Furthermore, in some preferred embodiments of the present invention, the sintering temperature is 250-900° C., more preferably 500-800° C.; and the sintering time is 4-12 hours.
[0018] In addition, the present invention provides a battery comprising the high-nickel positive electrode material.
[0019] Compared with the prior art, the above one or more technical solutions of the present invention can achieve at least one of the following beneficial effects: (1) After the precursor material is spray-dried, a hollow cathode material powder is obtained, which has high efficiency, high production capacity and stable structure; (2) The temperature required during the sintering process of the hollow powder is not high, and a high-nickel positive electrode material with a hollow structure can be obtained, saving energy and cost; (3) The obtained high nickel positive electrode material improves the capacity and rate performance of the battery. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 This is the SEM image of the positive electrode material obtained in Example 1.
[0021] Figure 2 This is a cross-sectional SEM image of the positive electrode material obtained in Example 1.
[0022] Figure 3 This is the XRD diagram of the positive electrode material obtained in Example 1.
[0023] Figure 4 This is a SEM image of the cross section of the positive electrode material obtained in Comparative Example 1.
[0024] Figure 5 This is a SEM image of the cross section of the positive electrode material obtained in Example 2.
[0025] Figure 6 This is a SEM image of the cross section of the positive electrode material obtained in Example 2. DETAILED DESCRIPTION
[0026] In order to facilitate the understanding of the present invention, the present invention will be described more comprehensively and meticulously below in conjunction with the accompanying drawings and preferred embodiments of the present invention, but the protection scope of the present invention is not limited to the following specific embodiments.
[0027] Unless otherwise defined, all the professional terms used below have the same meanings as those generally understood by those skilled in the art. The professional terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention.
[0028] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in the present invention can be purchased from the market or prepared by existing methods.
[0029] To achieve the first object of the present invention, some embodiments of the present invention provide a high-nickel positive electrode material, wherein the high-nickel positive electrode material is a hollow structure; the average particle size of the primary particles is 0.1-3 μm, preferably 0.5-1.0 μm, and more preferably 0.65-0.8 μm; the average particle size of the high-nickel positive electrode material is 1-40 μm, preferably 4-10 μm, and more preferably 5-8 μm; the SSA of the high-nickel positive electrode material satisfies 0.15 μm 2 / g≤SSA≤1.5 m 2 / g, preferably 0.25m 2 / g≤SSA≤0.5m 2 / g, more preferably 0.25m 2 / g≤SSA≤0.41m 2 / g.
[0030] By performing cross-section electron microscopy analysis on high-nickel positive electrode material powder, the number of stacking layers of primary particles can be observed.
[0031] In some embodiments of the present invention, the outer shell of the hollow structure includes 1 to 5 layers of primary particle stacking layers, preferably includes 1 to 4 layers of primary particle stacking layers, and more preferably includes 1 to 3 layers of primary particle stacking layers.
[0032] In some embodiments of the present invention, the general chemical formula of the high nickel cathode material is Li a Ni x Co y M z M' βO2, wherein 0.95≤a≤1.2, 0.8≤x≤1, 0≤y≤0.2, 0≤z≤0.05, 0≤β≤0.05, x+y+z+β=1,; M is one or more of Mn, Al, Zr, Mg, W, Ti, Y, La, B and Sr, and M is preferably Al. M' is one or more of Mn, Al, Zr, Mg, W, Ti, Y, La, B, Sr, P, and C, and is preferably at least one of Mg and Mn. M and M' are conventional doping elements currently contained in the positive electrode material and the precursor of the positive electrode material. P and C can be doped by phosphate or organic sintering.
[0033] The rate performance of lithium-ion battery positive electrode materials is related to the diffusion rate of lithium ions in the material. The diffusion rate of lithium ions in the material is positively correlated with the reaction interface area between the positive electrode material and the electrolyte, and negatively correlated with the size of the primary particles. The hollow structure of high-nickel positive electrode materials can ensure that the inside and outside of the agglomerated particles of the positive electrode material are in contact with the electrolyte, which can greatly increase the reaction interface area, thereby increasing the diffusion rate of lithium ions. The number of layers of primary particles stacked in the hollow structure shell is more than 5, which will increase the lithium ion diffusion path and reduce the lithium ion diffusion rate. In addition, if the primary particle size is less than 0.1μm, it will not be able to maintain a stable structure, and if the primary particle size is greater than 3μm, it will increase the lithium ion diffusion path and reduce the lithium ion diffusion rate. If the average particle size of the positive electrode material is less than 1μm, it will not be able to maintain a stable structure, and if it is greater than 40μm, it will increase the difficulty of coating. The specific surface area is less than 0.15m 2 / g will reduce the diffusion rate of lithium ions, and the specific surface area is higher than 1.5m 2 / g will not be able to maintain a stable structure. The higher the Ni content, the higher the capacity of the material. The molar ratio of Ni in the transition metal is lower than 0.8, the capacity of the material is low, and the Ni content can only be up to 1, preferably below 0.98, and more preferably 0.95. Some specific embodiments of the present invention further provide a method for preparing the above-mentioned high-nickel positive electrode material.
[0034] In the process of preparing high nickel positive electrode materials, there are mainly two thermal processes: Add lithium salt, precursor material, additives and water to the sand milling equipment, sand mill and obtain sand milling slurry. The precursor material can also be replaced by precursor slurry. Sand milling can be performed by passing a zirconium ball with a diameter of 0.3 mm, and the ball is subjected to the centrifugal force of the grinding disc to crush and mix the raw material particles. The particle size of the raw material is reduced and the mixture is evenly mixed. The sand milling slurry is spray dried, which is the first thermal process to obtain a hollow powder. During the spray drying process, the surface moisture of the precursor is rapidly dried by the high-temperature airflow, and the residual solid on the surface solidifies to form a shell layer. Due to the negative pressure and high temperature, the moisture inside the material quickly diffuses to the surface and dries and volatilizes to form a hollow spherical morphology powder.
[0035] After the first stage of heat treatment to obtain a powder with a hollow spherical morphology, it is further sintered to obtain a positive electrode material.
[0036] In a specific embodiment, the particle size of the sand-milled slurry is 100-500 nm.
[0037] In a specific embodiment, the spray drying is carried out in a spray drying device using a two-fluid spray method.
[0038] In a specific embodiment, the powder with hollow spherical morphology is obtained by controlling the air pressure, heating temperature, feed rate, air intake flow rate and compressed air pressure of the spray drying nozzle of the spray drying dust collecting tower. Preferably, the pressure of the spray drying dust collecting tower is less than -5Pa; the air intake heating temperature is ≥350℃, such as 350℃, 400℃, 500℃, etc.; the slurry feed rate is 1L / h-10L / h, and the compressed air intake flow rate of the spray drying nozzle is 0.2-2m 3 / min, the compressed air pressure of the spray drying nozzle is 0.1Mpa-0.8Mpa.
[0039] The powder obtained after spray drying is further sintered in an oxygen atmosphere, preferably at a sintering temperature of 250-900°C, more preferably 500-800°C, such as 500°C, 600°C, 700°C, 800°C; and a sintering time of 4-12h, preferably 8-11h.
[0040] After sintering, the temperature is naturally lowered to obtain the aforementioned high-nickel positive electrode material.
[0041] Assemble the high-nickel positive electrode material into a battery and test the battery performance.
[0042] The following is further described by means of specific examples.
[0043] Example 1 (1) Preparation of precursor: Ni was prepared by co-precipitation in a reactor. 0.88 Co 0.09 Al 0.03 (OH)2 precursor slurry.
[0044] (2) Lithium hydroxide and precursor slurry are added into a sand mill at a molar ratio of Li / (Ni+Co+Al)=1.02, and water is added at a solid content of 20%. Sand milling is performed until the particle size of the sand milled slurry is 400 nm. The sand milling is then completed.
[0045] (3) The sand-grinding slurry is spray-dried in a spray drying tower. The air pressure of the spray drying dust collecting tower is controlled to be -10Pa, the air inlet heating temperature is 350°C, the slurry feed rate is 10L / h, and the compressed air inlet flow rate is 1m 3 / min, the compressed air pressure of the spray drying nozzle is 0.6Mpa, and spray drying is performed. Powder material is obtained from the receiving port.
[0046] (4) The powder material is sintered at 720°C for 10 h in an oxygen atmosphere and then cooled naturally to obtain a positive electrode material.
[0047] Figure 1 This is a SEM image of the positive electrode material obtained in Example 1. As can be seen from the image, the material after sintering is a secondary sphere formed by agglomeration of primary particles, and the particle size of the secondary sphere particles is about 6.9 μm.
[0048] Figure 2 This is a cross-sectional SEM image of the positive electrode material obtained in Example 1. It can be seen from the image that the secondary spherical particles are hollow structures, and the outer shell is formed by 1-2 layers of primary particles. The hollow structure is regular.
[0049] Figure 3 This is the XRD diagram of the positive electrode material obtained in Example 1. It can be seen from the figure that a regular ternary crystal structure is formed after sintering.
[0050] Comparative Example 1 (1) Preparation of precursor: Ni was prepared by co-precipitation in a reactor. 0.88 Co 0.09 Al 0.03 (OH)2 precursor slurry. After washing, the slurry is filtered, dried and sieved to obtain precursor powder; (2) Lithium hydroxide and a precursor are mixed in a high-speed mixer at a molar ratio of Li / (Ni+Co+Al)=1.02, and the mixed material is sintered at 720°C for 10 hours in an oxygen atmosphere, and then cooled naturally to obtain a positive electrode material.
[0051] Figure 4 This is a SEM image of the cross section of the positive electrode material obtained in Example 1. It can be seen from the figure that Example 1 did not undergo the sanding spray process, and the solid spherical structure of the precursor was retained. The primary particles of the positive electrode material obtained in Example 1 are smaller, and the secondary particles are solid spheres. During the sintering process, material transfer is difficult and the particle growth space is limited.
[0052] Example 2 (1) Preparation of precursor: Ni was prepared by co-precipitation in a reactor. 0.88 Co 0.09 Al 0.03 (OH)2 precursor slurry.
[0053] (2) Add MgO powder at a molar ratio of Mg / (Ni+Co+Al)=0.01, add lithium hydroxide and precursor slurry into a sand mill at a molar ratio of Li / (Ni+Co+Al+Mg)=1.02, and add water at a solid content of 40%. Sand grind until the particle size of the sand-milled slurry is 500 nm. Sand grinding is completed.
[0054] (3) The sand-grinded slurry is spray-dried in a spray drying tower. The air pressure of the spray drying dust collecting tower is controlled to be -20 Pa, the drying temperature is 400 °C, the slurry feed rate is 5 L / h, and the compressed air intake flow rate is 0.2 m 3 / min, the compressed air pressure of the spray drying nozzle is 0.1Mpa, and spray drying is performed. Powder material is obtained from the receiving port.
[0055] (4) The powder material is sintered at 800°C for 8 hours in an oxygen atmosphere and then cooled naturally to obtain a positive electrode material.
[0056] Figure 5 This is a cross-sectional SEM image of the positive electrode material obtained in Example 2. It can be seen from the image that the secondary particles of the positive electrode material obtained in Example 2 present a hollow structure and have a shell formed by two layers of primary particles.
[0057] Example 3 (1) Preparation of precursor: Ni was prepared by co-precipitation in a reactor. 0.95 Co 0.03 Mn 0.02 (OH)2 precursor slurry.
[0058] (2) In a sand mill, add MnO powder at a molar ratio of Mn / (Ni+Co+Al)=0.02, and add lithium hydroxide and precursor slurry at a molar ratio of Li / Me=1.005. At the same time, add water at a solid content of 10%, and sand grind until the particle size of the sand-ground slurry is 100nm. Sand grinding is completed.
[0059] (3) The sand-grinding slurry is spray-dried in a spray drying tower. The air pressure of the spray drying dust collecting tower is controlled to be -30 Pa, the drying temperature is 500 °C, the slurry feed rate is 10 L / h, and the compressed air intake flow rate is 0.2 m 3 / min, the compressed air pressure of the spray drying nozzle is 0.8Mpa, and spray drying is performed. Powder material is obtained from the receiving port.
[0060] (4) The powder material is sintered at 500°C for 11 hours in an oxygen atmosphere and then cooled naturally to obtain a positive electrode material.
[0061] Figure 6This is a cross-sectional SEM image of the material obtained in Example 3. It can be seen from the image that the secondary particles of the positive electrode material obtained in Example 3 present a hollow structure and have a shell formed by three layers of primary particles.
[0062] The average particle size, average primary particle size, and SSA of the positive electrode materials obtained in Examples 1-3 and Comparative Example 1 were detected by the following means.
[0063] Average particle size of positive electrode material: measured by Malvern laser particle size analyzer. The particle sizes in the present invention are all volume cumulative particle sizes, such as D50, i.e. DV50.
[0064] Average particle size of primary particles: The surface micromorphology of the sample was analyzed using a scanning electron microscope with an electron acceleration voltage of 20 kV. After obtaining the electron microscope image, the average size of the primary particles was measured based on the image size scale and the primary particle grain boundaries.
[0065] Specific surface area (SSA): The specific surface area of the powder material was measured using a Micromeritics Tristar 3030 (temperature: 200 °C, degassing time: 2 hrs).
[0066] The results are shown in Table 1.
[0067] Table 1 The effects of the positive electrode materials prepared in Examples 1-3 and Comparative Example 1 on the performance of the battery were tested. The specific testing methods are as follows: (1) Preparation of positive electrode The prepared positive electrode material, conductive agent SuperP, binder polyvinylidene fluoride (PVDF) and N-methylpyrrolidone (NMP) were mixed and stirred evenly in a mass ratio of 90:5:5 to prepare a positive electrode slurry (solid content of about 43%), which was coated on the current collector aluminum foil, dried at 105°C, and then rolled at room temperature to a surface density of 2.5-5 mg / cm 2 , then punch and cut into φ14mm discs to make positive electrode sheets.
[0068] (2) Assembly of lithium-ion batteries The button cell was assembled in a glove box in the order of "negative electrode shell - nickel foam - lithium sheet - 8 drops of electrolyte - separator - 8 drops of electrolyte - positive electrode sheet - positive electrode shell", wherein the electrolyte consisted of ethylene carbonate (EC), ethyl methyl carbonate (EMC) and dimethyl carbonate (DMC) (EC: EMC: DMC volume ratio = 1:1:1), and contained 1.0M LiPF6.
[0069] The diameter of the positive electrode sheet is 14mm, the diameter of the lithium sheet is 18mm, the diameter of the diaphragm is 22mm, and the size of the battery shell (positive and negative shells) is 24mm. The diaphragm is a 20μm thick isolation film. Put the assembled button battery in the mold groove of the hydraulic sealing machine, lock it, and apply pressure >550kg / cm 2 , then unlock it and take out the sealed button battery.
[0070] (3) Performance test of button battery First coulombic efficiency and capacity retention test: At 25°C, the charge and discharge cycle characteristics of the button battery were tested using a blue electric test cabinet. The battery was charged and discharged at a charge and discharge rate of 0.1C in the voltage range of 3.0V-4.3V. Specifically, the battery was charged to 4.3V at a constant current of 0.1C, and then charged to a cutoff current of 0.02C at a constant voltage of 4.3V, left for 5 minutes, and discharged to 3.0V at 0.1C, left for 5 minutes, and the charge and discharge capacity after the first cycle was recorded. The battery was charged to 4.3V at a constant current of 1C, and then charged to a cutoff current of 0.02C at a constant voltage of 4.3V, left for 5 minutes, and discharged to 3.0V at 1C, left for 5 minutes, and the charge and discharge capacity of 1C was recorded. The battery was charged to 4.3V at a constant current of 1C, and then charged to a cutoff current of 0.02C at a constant voltage of 4.3V, left for 5 minutes, and discharged to 3.0V at 20C, left for 5 minutes, and the charge and discharge capacity of 20C was recorded.
[0071] After the positive electrode materials of Examples 1-3 and Comparative Example 1 were assembled into batteries, the performance parameters of the batteries were shown in Table 2.
[0072] Table 2 By comparing and analyzing the performance of the batteries assembled with the positive electrode materials obtained in Example 1 and Comparative Example 1, it is not difficult to find that the initial efficiency of the batteries is not much different, but the capacity performance and rate performance of the battery using the positive electrode material obtained in Example 1 are obviously superior.
[0073] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A high nickel positive electrode material, characterized in that: The high-nickel positive electrode material has a hollow structure; the average particle size of the primary particles of the high-nickel positive electrode material is 0.1-3 μm, preferably 0.65-0.8 μm; the average particle size of the high-nickel positive electrode material is 1-40 μm, preferably 5.0-8.0 μm; 0.15m 2 / g≤SSA≤1.5 m 2 / g, preferably 0.25m 2 / g≤SSA≤0.5 m 2 / g.
2. The high nickel positive electrode material according to claim 1, characterized in that The outer shell of the hollow structure includes 1 to 5 layers of primary particle stacking.
3. The high nickel positive electrode material according to claim 1 or 2, characterized in that: The general chemical formula of the high nickel cathode material is Li a Ni x Co y M z M' β O2, wherein 0.95≤a≤1.2, 0.8≤x≤1, 0≤y≤0.2, 0≤z≤0.05, 0≤β≤0.05, x+y+z+β=1; M is one or more of Mn, Al, Zr, Mg, W, Ti, Y, La, B and Sr, preferably Al; M' is one or more of Mn, Al, Zr, Mg, W, Ti, Y, La, B, Sr, P, C, preferably at least one of Mn and Mg.
4. A method for preparing a high-nickel positive electrode material according to any one of claims 1 to 3, characterized in that: The following steps are involved: Step S1, adding lithium salt, a precursor of a high-nickel positive electrode material, and water into a sand mill for sand grinding to obtain a sand grinding slurry; Step S2, spray drying the sand-milled slurry to obtain a powder material; Step S3, sintering the powder material to obtain a high-nickel positive electrode material.
5. The method for preparing a high-nickel positive electrode material according to claim 4, characterized in that: In step S1, a compound of M' is added to a sand mill; M' is one or more of Mn, Al, Zr, Mg, W, Ti, Y, La, B, Sr, P, and C; Preferably, the chemical expression of the precursor of the high nickel cathode material is Ni x Co y M z (OH)2, 0.8≤x≤1, 0≤y≤0.2, 0≤z≤0.05, x+y+z=1, 0≤β≤0.05; M is one or more of Mn, Al, Zr, Mg, W, Ti, Y, La, B and Sr, preferably Al.
6. The method for preparing a high-nickel positive electrode material according to claim 5, characterized in that: Adding lithium salt and precursor material into a sand mill according to the ratio of the molar amount of Li to the sum of the molar amounts of Ni, Co, M and M' being 1.005-1.02:1; Preferably, the particle size of the sand-grinding slurry is 100-500 nm; Preferably, the solid content of the sand-grinding slurry is controlled to be 5%-40%.
7. The method for preparing a high-nickel positive electrode material according to any one of claims 4 to 6, characterized in that: The spray drying adopts a two-fluid spraying method.
8. The method for preparing a high-nickel positive electrode material according to any one of claims 4 to 7, characterized in that: The air pressure of the spray drying dust collecting tower is less than -5Pa, the air inlet heating temperature is ≥350℃, the slurry feed rate is 1L / h-10L / h, and the compressed air inlet flow rate of the spray drying nozzle is 0.2-2m 3 / min, the compressed air pressure of the spray drying nozzle is 0.1-0.8Mpa.
9. The method for preparing a high-nickel positive electrode material according to any one of claims 4 to 8, characterized in that: The sintering temperature is 250-900°C, preferably 500-800°C; Preferably, the sintering time is 4 to 12 hours.
10. A battery, characterized in that: The invention comprises the high-nickel positive electrode material according to any one of claims 1 to 3 or the high-nickel positive electrode material prepared by the preparation method according to any one of claims 4 to 9.