Method and apparatus for producing waste plastic pyrolysis oil with reduced chlorine content

By using coke slag and metal oxides as dechlorination agents in the waste plastic pyrolysis process, the problem of high chlorine content in waste plastic pyrolysis oil is solved, the production of pyrolysis oil with low chlorine content is achieved, and the process efficiency and Cost effective.

CN118749020AInactive Publication Date: 2024-10-08SK INNOVATION CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380025872.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-17
Filing Date
2023-03-09
Publication Date
2024-10-08
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

In the existing technology, the chlorine content in waste plastic pyrolysis oil is relatively high, which leads to equipment corrosion and product performance degradation during the hydrotreating process, and it is difficult to obtain high-quality pyrolysis oil due to residual dechlorination agents.

Method used

By using coke slag as a promoter in the waste plastic pyrolysis process, combined with metal oxides or metal hydroxides as dechlorination agents, the pyrolysis and adsorption processes are performed to reduce the chlorine content, and the adsorption is improved through the alcohol cleaning and recycling process. agent activity.

Benefits of technology

It effectively reduces the chlorine content in pyrolysis oil, improves process efficiency and cost-effectiveness, avoids additional post-treatment processes, and saves energy consumption.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The present invention provides a method for producing a waste plastic pyrolysis oil having a reduced chlorine content, the method comprising: a first step of charging a waste plastic raw material and a coke-containing accelerator into a reactor; a second step of pyrolyzing the waste plastic raw material in the reactor and recovering pyrolysis oil; and a third step of recovering the accelerator from the reactor.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method and an apparatus for producing pyrolysis oil with reduced chlorine content from waste plastics. Background Art

[0002] Solid fuel is a material produced by sorting, crushing, drying, chemical treatment and molding combustible waste, such as waste plastics, waste fibers, waste tires, waste paper, waste wood, oil and livestock byproducts in industrial waste and general waste. Recently, there has been a growing interest in utilizing waste resources such as solid fuels for energy conversion. Energy conversion of solid fuels can be achieved by combustion, gasification or pyrolysis processes, which produce a byproduct - char.

[0003] Meanwhile, among solid fuels, waste plastics produced from petroleum as raw materials cannot be recycled and are mostly treated as garbage. These wastes take a long time to degrade in nature, causing soil pollution and serious environmental pollution. As a method of recycling waste plastics, a method of converting waste plastics into oil by pyrolyzing waste plastics was conducted.

[0004] However, the pyrolysis oil obtained by pyrolyzing waste plastics cannot be directly used as a high-value-added fuel such as gasoline or diesel because it contains more impurities such as chlorine, nitrogen, metals and solid by-products than the fractions produced from crude oil by a general method. Therefore, the pyrolysis oil can be used as a fuel after adsorbing impurities through a refining process.

[0005] According to the relevant technology, in the refining process of pyrolysis oil, chlorine has been converted into hydrogen chloride by hydrogenation in the presence of a hydrotreatment catalyst, and is adsorbed and removed. However, due to the high chlorine content in waste plastic pyrolysis oil, excessive hydrogen chloride will be produced during the hydrotreatment process, resulting in equipment corrosion, abnormal reaction and deterioration of product performance.

[0006] In addition, in the method of reducing chlorine, nitrogen, etc. using a dechlorinating agent such as a metal hydroxide, a metal oxide or a waste fluid catalytic cracking (FCC) catalyst (E-cat), the dechlorinating agent should be used in excess (at a level of 2-50 times the oil to be refined). Therefore, the dechlorinating agent will remain in the produced pyrolysis oil, making it difficult to obtain high-quality pyrolysis oil. In addition, the adsorbent will deteriorate during the process of adsorbing chlorine, nitrogen, etc., resulting in a decrease in the adsorption capacity of the adsorbent. Therefore, the deactivated adsorbent should be continuously replaced.

[0007] Therefore, there is a need for a technology capable of producing waste plastic pyrolysis oil in which the chlorine content is minimized from waste plastic. Summary of the invention

[0008] Technical issues

[0009] The object of the present invention is to provide a method and apparatus for producing waste plastic pyrolysis oil, which can effectively reduce chlorine by using coke residue (which is a by-product generated in the waste plastic pyrolysis process) and can improve cost-effectiveness by recycling the coke residue.

[0010] Another object of the present invention is to provide a method and apparatus for producing waste plastic pyrolysis oil, which can effectively reduce chlorine by utilizing the physical and chemical properties of coke residue and dechlorinating agent.

[0011] Another object of the present invention is to provide a method and apparatus for producing waste plastic pyrolysis oil having a low chlorine content level, which allows the pyrolysis oil to be directly introduced into a refining process without the need for a post-treatment process for the pyrolysis oil.

[0012] Solutions to technical problems

[0013] In a general aspect, a method for producing waste plastic pyrolysis oil with low chlorine content includes: a first step of loading waste plastic raw materials and a promoter containing coke residue into a reactor; a second step of pyrolyzing the waste plastic raw materials in the reactor and recovering the pyrolysis oil; and a third step of recovering the promoter from the reactor.

[0014] In one embodiment, the accelerator in the first step may be charged into the reactor in an amount of 5-30 parts by weight relative to 100 parts by weight of the waste plastic raw material.

[0015] In one embodiment, the promoter may further contain one or more dechlorinating agents selected from metal oxides, metal hydroxides and metal carbonates.

[0016] In one embodiment, the dechlorinating agent may be a metal oxide.

[0017] In one embodiment, the promoter may be an aggregate in which a plurality of primary particles containing slag are bound and aggregated together by a dechlorination agent.

[0018] In one embodiment, the dechlorination agent may be a binder powder further containing moisture, and may bind a plurality of primary particles.

[0019] In one embodiment, the char residue may be included in the promoter in an amount greater than the weight of the dechlorination agent.

[0020] In one embodiment, the method may further include a fourth step of resupplying the promoter recovered in the third step to the first step.

[0021] In one embodiment, the fourth step may include: a step of washing the promoter recovered in the third step with alcohol; a step of replenishing the promoter washed with alcohol and a dechlorinating agent to prepare the promoter; and a step of resupplying the prepared promoter to the first step.

[0022] In one embodiment, the second step may be performed at a temperature of 300-600°C.

[0023] In one embodiment, the second step may be performed in a non-oxidizing atmosphere.

[0024] In one embodiment, the method may further include: before the step of resupplying the prepared accelerator to the first step, the step of additionally heating the prepared accelerator at a temperature of 500-1,000° C. to increase the activity of the accelerator.

[0025] In another general aspect, an apparatus for producing waste plastic pyrolysis oil with reduced chlorine content includes: a reactor, into which waste plastic feedstock and a accelerator containing char residue are charged and a pyrolysis process is carried out; and a storage tank, in which the pyrolysis oil is recovered from the reactor.

[0026] In one embodiment, the apparatus may further include a recovery tank for recovering the promoter from the reactor; and a recirculation line for resupplying the promoter from the recovery tank to the reactor.

[0027] Advantageous Effects of the Invention

[0028] According to the present invention, since slag, a byproduct generated in the waste plastic pyrolysis process, is reused and utilized as a useful resource, cost effectiveness is improved, and chlorine is effectively reduced by the excellent chemical resistance and adsorption of slag, thereby improving process efficiency.

[0029] According to the present invention, pyrolysis oil having a low impurity content suitable for a refining process can be produced without additional post-treatment process after pyrolysis of waste plastic raw materials.

[0030] According to the present invention, compared with the existing waste plastic pyrolysis process, energy consumption can be effectively saved. DETAILED DESCRIPTION

[0031] Unless the context clearly indicates otherwise, the singular forms of the terms used in this specification may be construed as including the plural forms.

[0032] The numerical range used in this specification includes upper and lower limits and all values ​​within these limits, all double limits, and all possible combinations of upper and lower limits within the numerical range defined in different forms. Unless otherwise clearly defined in this specification, values ​​that may exceed the numerical range due to experimental errors or rounding also belong to the defined numerical range.

[0033] The word "comprising" described in this specification is intended to be an open transition phrase, which means the same as "including", "containing", "having" or "characterized by", and does not exclude all those elements, materials or steps not further described in this document.

[0034] Unless otherwise defined, the unit "%" used in the present specification means "% by weight".

[0035] Unless otherwise defined, the unit "ppm" used in this specification means "mass ppm".

[0036] Waste plastics include polyethylene (PE), polypropylene (PP), polyethylene terephthalate (PET), polyvinyl chloride (PVC), polystyrene (PS), etc., and waste plastics contain impurities such as organic chlorine and inorganic chlorine. The pyrolysis oil produced by the waste plastic pyrolysis process cannot be directly used as a high-value-added fuel such as gasoline or diesel due to its high impurity content. Therefore, the pyrolysis oil can be used as a fuel after adsorbing impurities through a refining process. However, since the waste plastic pyrolysis oil contains a large amount of chlorine, excessive hydrogen chloride will be produced during the hydrogenation process, resulting in equipment corrosion, abnormal reactions and decreased product performance. Therefore, a technology for producing waste plastic pyrolysis oil with a low level of impurity content is needed, which allows the pyrolysis oil to directly enter the refining process without the need for additional post-treatment processes.

[0037] Therefore, one embodiment of the present invention provides a method for producing waste plastic pyrolysis oil with reduced chlorine content, which method includes: a first step of loading waste plastic raw materials and a slag-containing promoter into a reactor; a second step of pyrolyzing the waste plastic raw materials in the reactor and recovering the pyrolysis oil; and a third step of recovering the promoter from the reactor.

[0038] The waste plastic raw material may be household waste plastic, industrial waste plastic or mixed waste plastic thereof. Household waste plastic refers to plastics mixed with PVC, PS, PET, PBT, etc. in addition to PE and PP. In the present invention, as an example, household waste plastic may be waste plastics including more than 3% by weight of PVC, as well as PE and PP. The chlorine content may be more than 5,000 ppm relative to 100 parts by weight of household plastic waste, specifically, the chlorine content may be 5,000-15,000 ppm relative to 100 parts by weight of household plastic waste, but this is only an example, and the chlorine content is not limited thereto.

[0039] Industrial waste plastics are industrial wastes generated during industrial production, and may be waste plastics including PE and PP as main components. Since industrial waste plastics maintain a relatively clean state, the chlorine content is lower than that in domestic waste plastics. However, the organic chlorine content from adhesives or dye components is high, and the proportion of chlorine contained in the aromatic ring is particularly high. Relative to 100 parts by weight of waste plastics, the chlorine content may be 100-1000ppm, specifically, 500-1000ppm, and more specifically, 700-1000ppm, but this is only an example, and the chlorine content is not limited thereto.

[0040] Due to the low thermal conductivity of waste plastics, a large amount of fuel will be consumed in the pyrolysis process, and the waste plastics are heated unevenly, which will cause local temperature deviations and lead to low reaction efficiency. Therefore, in the first step, the waste plastic raw material and the promoter containing slag are loaded into the reactor, and then the pyrolysis process is carried out in the second step, which can promote pyrolysis, thereby improving the process efficiency, and effectively reduce the chlorine content in the produced pyrolysis oil. Since the promoter containing slag acts as a heat carrier in the pyrolysis process of waste plastics, it can compensate for the low thermal conductivity of waste plastics, thereby accelerating the heat transfer between waste plastic particles, saving fuel consumption, and speeding up the pyrolysis process, thereby improving the process efficiency. Incidentally, slag is mainly a by-product produced in the solid fuel energy conversion process, and the distribution cost is low, so the cost of the pyrolysis process of waste plastics can be reduced and the cost-effectiveness can be improved.

[0041] In addition, due to the well-developed pores of the coke residue, during the pyrolysis process, the coke residue can effectively adsorb organic chlorine and inorganic chlorine in the waste plastics, thereby effectively reducing the chlorine content in the generated pyrolysis oil. Specifically, the coke residue contains calcium carbonate, and the chlorine dissociated from the waste plastics during the pyrolysis process is retained while being adsorbed on the coke residue, thereby inhibiting the recombination of the dissociated chlorine with the olefins in the pyrolysis product, thereby inhibiting the regeneration of organic chlorine. Specifically, the chlorine content in the pyrolysis oil generated by the pyrolysis process can be reduced by more than 80% compared to the chlorine content in the waste plastic raw material. More specifically, the chlorine content in the pyrolysis oil generated by the pyrolysis process can be reduced by more than 90%, and can be reduced by more than 90% and less than 97%, but is not limited.

[0042] That is to say, since a accelerator containing coke residue is used in the waste plastic pyrolysis process, the chlorine content in the generated waste plastic pyrolysis oil can be effectively reduced, and at the same time, the pyrolysis process can be accelerated and the process efficiency can be improved.

[0043] In one embodiment, the promoter in the first step can be loaded into the reactor in an amount of 5-30 parts by weight relative to 100 parts by weight of the waste plastic raw material. Within the above range, chlorine can be effectively adsorbed to improve the reaction efficiency. When the amount of the promoter containing coke residue is less than 5 parts by weight, the adsorption effect of chlorine may be insufficient, and when the amount of the promoter containing coke residue is more than 30 parts by weight, the promoter may be saturated due to excessive addition, and the purity of the produced pyrolysis oil may be reduced. Specifically, the amount of the promoter containing coke residue can be 5-25 parts by weight, and more specifically, it can be 5-20 parts by weight.

[0044] In one embodiment, the promoter may further contain one or more dechlorinating agents selected from metal oxides, metal hydroxides and metal carbonates. Since the promoter further contains a dechlorinating agent, the chlorine adsorption effect of the promoter can be further improved. The metal can be an alkali metal or an alkaline earth metal, specifically, sodium, magnesium, potassium, calcium, etc. Specifically, the dechlorinating agent can be calcium hydroxide, sodium hydroxide, magnesium hydroxide, potassium hydroxide, calcium oxide, magnesium oxide, calcium carbonate, sodium carbonate, potassium carbonate, etc.

[0045] In one embodiment, the dechlorinating agent may be a metal oxide. In particular, when a metal oxide is used as a dechlorinating agent, chlorine generated in the waste plastic pyrolysis process can be further effectively adsorbed, and from the perspective of agglomeration with a plurality of particles containing slag as described below, it is preferred to use a metal oxide. Specifically, the dechlorinating agent may be calcium oxide, magnesium oxide, sodium oxide or potassium oxide, preferably calcium oxide.

[0046] In one embodiment, the promoter can be an aggregate, wherein a plurality of primary particles containing slag are combined and aggregated together by a dechlorinating agent. Slag is a carbide particle, and in this specification, a single slag particle is a primary particle, referred to as a primary particle. The dechlorinating agent is used as a binder, and the dechlorinating agent is arranged between a plurality of primary particles as a binder, so that the slag primary particles can form aggregates, i.e., secondary particles. Since the promoter has an aggregate structure, the heat conduction of the waste plastic can be accelerated, and the chlorine generated by the heat conduction can be effectively trapped by the promoter adjacent to the chlorine. Specifically, the physical adsorption of the pores of the slag contained in the promoter and the chemical adsorption of the dechlorinating agent are effectively implemented, so that the chlorine removal effect can be maximized. In particular, when a metal oxide is used as a dechlorinating agent, the binding performance with a plurality of primary particles is very good, and aggregation can occur more stably, which is preferred. Specifically, the dechlorinating agent can be calcium oxide, magnesium oxide, sodium oxide or potassium oxide, preferably calcium oxide.

[0047] In one embodiment, the dechlorinating agent can be a binder powder further containing water, and can be combined with multiple primary particles. Due to the use of a binder powder containing water, the cohesive force between multiple primary particles is improved, thereby forming a stable aggregate. In addition, the chlorine separated from the waste plastics will be collected by the water, thereby improving the adsorption effect of chlorine. Specifically, relative to 100 parts by weight of the dechlorinating agent, the water content can be 0.1-5 parts by weight. When the water content is within the above-mentioned appropriate range, the improvement of the cohesive force of the aggregate can be effectively achieved. More specifically, relative to 100 parts by weight of the dechlorinating agent, the water content can be 0.5-2 parts by weight.

[0048] In one embodiment, the weight content of the slag in the promoter may be greater than the weight of the dechlorinating agent. Since the weight content of the slag is greater than the weight of the dechlorinating agent, the adsorption effect of chlorine can be further improved. Specifically, the weight ratio of the slag to the dechlorinating agent may be 100:10-100:40. Since the slag and the dechlorinating agent are contained in the above-mentioned weight ratio, the physical adsorption effect of chlorine through the pores formed on the surface of the slag is very good, which is preferred. Specifically, the weight ratio may be 100:10-100:30, and more specifically, it may be 100:10-100:25.

[0049] The average size of the slag can be 0.1-5 mm. Within the above size range, the dechlorinating agent can be effectively aggregated. Specifically, the average particle size can be 0.1-3 mm.

[0050] The second step is to pyrolyze the waste plastic raw material and recover the pyrolysis oil. The pyrolysis product may include pyrolysis gas and solid by-products. After the pyrolysis gas is discharged from the reactor, the pyrolysis gas can be cooled and liquefied to recover the liquid pyrolysis oil.

[0051] Relative to the total weight of the waste plastic raw materials, the pyrolysis gas may include 5-35 wt % of naphtha (boiling point (bp) to 150°C), 10-60 wt % of kerosene (Kero) (boiling point 150-265°C), 20-40 wt % of light gas oil (LGO) (boiling point 265-380°C) and 5-40 wt % of UCO-2 / AR (boiling point from 380°C). Specifically, relative to the total weight of the waste plastic raw materials, it may include 5-30 wt % of naphtha (boiling point to 150°C), 15-50 wt % of Kero (boiling point 150-265°C), 20-35 wt % of LGO (boiling point 265-380°C) and 10-40 wt % of UCO-2 / AR (boiling point from 380°C). In addition, the pyrolysis gas may include a residual amount of low-boiling hydrocarbon compounds, such as methane (CH4), ethane (C2H6) and propane (C3H8).

[0052] The third step is a step of recovering a promoter from the reactor, and the promoter can be recovered from the solid byproducts remaining in the reactor after the pyrolysis gas is discharged. In the related art, in the case where the waste plastic pyrolysis process is carried out by adding a dechlorinating agent, the residual amount of the dechlorinating agent in the recovered liquid pyrolysis oil is generally 5-10% by weight. On the other hand, in the present invention, the dechlorinating agent remains in the solid byproduct in the form of an aggregate, wherein the dechlorinating agent and the coke residue are aggregated together, so high-quality pyrolysis oil can be recovered, and the additional post-processing process of treating the dechlorinating agent remaining in the pyrolysis oil can be omitted. In the method for recovering the promoter, the promoter can be recovered by the pyrolysis oil refining device described below.

[0053] In one embodiment, the method may further include a fourth step of resupplying the promoter recovered in the third step to the first step. The byproduct slag and dechlorinating agent generated in the pyrolysis process are recovered as promoters in the form of aggregates, which can achieve waste resource utilization and obtain the above-mentioned chlorine adsorption effect.

[0054] In one embodiment, the fourth step may include: a step of washing the accelerator recovered in the third step with alcohol; a step of supplementing the accelerator and dechlorinating agent washed with alcohol to prepare the accelerator; and a step of resupplying the prepared accelerator to the first step. Specifically, the recovered accelerator has adsorbed chlorine in the pyrolysis process and converted into metal chloride, so it may be in an inactivated state. The accelerator containing the inactivated metal chloride is washed with alcohol, so that the metal chloride with high solubility in alcohol can be leached and removed, the unreacted dechlorinating agent (such as calcium oxide) with relatively low solubility in alcohol can be retained, and the residual dechlorinating agent can be combined with multiple primary particles containing slag to form aggregates. The alcohol can be a fatty alcohol, specifically, it can be a mixture of one or more selected from methanol, ethanol, propanol, isopropanol, butanol and 2-ethylhexanol, but this is only an example, and the alcohol is not limited to this. Through a series of processes such as washing the recovered accelerator, supplementing the dechlorinating agent to improve the activity of the accelerator, and resupplying the accelerator to the first step, the utilization of waste resources and the adsorption effect of chlorine can be met at the same time.

[0055] In one embodiment, the first step can be performed at a temperature of 300-600° C. When the pyrolysis process is performed within the above temperature range, the fusion of the waste plastic can be prevented, the aggregation of the char and the dechlorination agent can be improved, and the adsorption efficiency of the chlorine dissociated from the waste plastic to the promoter can be increased. Specifically, the temperature can be 300-550° C., more specifically, 350-500° C.

[0056] In one embodiment, the first step can be carried out in a non-oxidizing atmosphere. A non-oxidizing atmosphere refers to an atmosphere in which the waste plastic does not burn. In order to make the slag aggregate, combustion should be prevented by heating without providing oxygen. For example, the non-oxidizing atmosphere can be an atmosphere in which the oxygen concentration is adjusted to less than 1% by volume, or an atmosphere of an inert gas such as nitrogen, water vapor, carbon dioxide or argon. The pyrolysis process can be stably carried out in the above atmosphere.

[0057] The first step can be carried out in a non-oxidizing atmosphere for 150-350 minutes. When the retention time is met, the components in the non-oxidizing atmosphere can be activated and the slag and the dechlorinating agent can be fully aggregated. Specifically, the retention time can be 170-330 minutes, more specifically, it can be 200-300 minutes.

[0058] In one embodiment, the method may further include a step of heat treating the recovered promoter at 500-1,000° C. The promoter may be activated by a pretreatment process of heating the promoter at the above temperature, and the chlorine adsorption activity may be improved. The heating may be performed in a non-oxidizing atmosphere, specifically, the temperature may be 500-900° C., more specifically, 600-800° C.

[0059] The first step may further include a step of drying the waste plastic raw material with hot air. In order to improve the pyrolysis efficiency, the waste plastic raw material may be dried with hot air, and the drying may be performed before the pyrolysis process, or the drying and pyrolysis processes may be performed simultaneously. For example, when hot air is blown during the pyrolysis of the first step, the drying of the waste plastic and the activation of the accelerator may be achieved simultaneously, thereby further improving the adsorption effect of chlorine.

[0060] The pyrolysis oil recovered in the third step may include an oil layer and a water layer. Oil-water separation is performed in the liquid pyrolysis oil to form an oil layer and a water layer in the liquid pyrolysis oil. After the oil layer and the water layer are separated, the oil layer is immediately recovered or the water layer is discharged to recover the remaining oil layer after adsorption, so that the waste plastic pyrolysis oil can be recovered, which is an oil layer with minimized chlorine content.

[0061] The chlorine content in the recovered oil layer (pyrolysis oil) can be less than 300 ppm. As described above, adding slag to the waste plastic pyrolysis process can effectively reduce the chlorine content in the produced waste plastic pyrolysis oil. In particular, when the aggregate of slag and dechlorinating agent is used as a promoter, the adsorption effect of chlorine can be further improved, so the chlorine content in the pyrolysis oil can be less than 150 ppm, more specifically, less than 100 ppm.

[0062] An electric field may be applied to effectively separate the oil layer and the water layer, and due to the application of the electric field, the oil layer and the water layer may be separated in a short time by electrostatic adhesion. In addition, additives may be added as needed to improve the oil-water separation efficiency, and the additives may be conventional demulsifiers known in the art.

[0063] When the water layer is discharged and adsorbed, a density profiler is used to detect the density, which can prevent the oil layer from being adsorbed together with the water layer when the water layer is adsorbed, and only the water layer can be effectively adsorbed.

[0064] In addition, one embodiment of the present invention provides an apparatus for producing waste plastic pyrolysis oil with reduced chlorine content, the apparatus comprising a reactor, in which waste plastic raw materials and a promoter containing slag are loaded and a pyrolysis process is carried out; and a storage tank, in which the pyrolysis oil is recovered from the reactor.

[0065] The reactor can be a batch reactor or a continuous reactor. For a batch reactor, any type of batch reactor capable of stirring and controlling temperature rise can be used, for example, a rotary kiln type batch reactor can be used. For a continuous reactor, a fixed bed continuous reactor can be used.

[0066] As pyrolysis proceeds, pyrolysis gas is discharged through a first outlet located at the top of the reactor. The discharged pyrolysis gas may enter a condenser. The condenser may include a region through which a coolant flows, and the pyrolysis gas introduced into the condenser may be liquefied by the coolant and converted into pyrolysis oil. The cooling temperature may be 80-180° C., specifically, 100-150° C. When the liquid pyrolysis oil produced in the condenser rises to a predetermined level, the liquid pyrolysis oil may be transferred and recovered to a storage tank.

[0067] A heat exchanger may be further arranged between the condenser and the storage tank. The uncondensed pyrolysis gas in the condenser is introduced into the heat exchanger and condensed again, and the generated pyrolysis oil may be recycled into the storage tank. The uncondensed pyrolysis gas is recycled again, thereby increasing the reaction yield.

[0068] In one embodiment, the device may further include a recovery tank for recovering the promoter from the reactor; and a recycle line for resupplying the promoter from the recovery tank to the reactor. The solid byproduct containing the promoter may be discharged through a second outlet located at the bottom of the reactor, and the discharged solid byproduct may be introduced into the recovery tank.

[0069] The recovery tank may include an alcohol supply unit. The solid byproduct may include unreacted promoter, promoter containing deactivated metal chloride and other impurities (such as copper impurities), and impurities other than the unreacted promoter may be removed by washing the solid byproduct with the alcohol supply unit.

[0070] The recovery tank may further include a dechlorinating agent supply unit. The dechlorinating agent supply unit supplies the dechlorinating agent to the cleaned accelerator, thereby increasing the activity of the accelerator.

[0071] The recovery tank may further include a classifier. Since the classifier is further included in the recovery zone, the promoter can be classified according to the particle size. For example, particles with a particle size of 1 mm or more and particles with a particle size of less than 1 mm can be classified by a screening device. In particular, since coke residue and dechlorinating agent are gathered in the promoter, large particles can be selectively recovered by particle size classification, thereby recovering the promoter with a higher yield. Fine particle carbides may cause problems such as reactor blockage and reduced process efficiency, so it is preferred to selectively recover only large particles without recovering fine particle carbides. The recovered promoter can be resupplied to the reactor through a recirculation line.

[0072] The removed impurities and fine carbides can be used as a fuel source for the batch reactor, thereby helping to save fuel.

[0073] For the contents of the device for refining waste plastic pyrolysis oil that are not further described, reference may be made to the description of the method for refining waste plastic pyrolysis oil described above.

[0074] Preferred examples and comparative examples of the embodiments of the present invention will be described below. However, the following examples are merely preferred examples of the present invention, and the present invention is not limited to the following examples.

[0075] Example 1

[0076] A household mixed plastic including more than 3 wt% of PVC, PE and PP was extruded at 250° C. to prepare 400 g of household waste plastic pellets. The chlorine content in the household waste plastic pellets was 4,000 ppm. The inside of the batch reactor was purged with nitrogen to generate a non-oxidizing atmosphere.

[0077] 400g of household waste plastic particles and 100g of char residue were placed in a batch reactor and then pyrolyzed at 400°C for 250 minutes while continuously supplying fuel. The generated pyrolysis products were transferred to a classification tank, and the pyrolysis gas was recovered from the second outlet located at the top of the classification tank. The recovered pyrolysis gas was collected in a condenser, and the waste plastic pyrolysis oil was finally recovered in a storage tank, and then the solid by-products were recovered from the second outlet located at the bottom of the reactor to the recovery tank.

[0078] The slag produced in the following process was used as the slag. The waste plastic was uniformly cut into a size of 150-200 meshes, and then the cut waste plastic was placed in a U-shaped reactor. Then, using a proportional-integral-differential (PID) controller, nitrogen was continuously introduced at a flow rate of 50 ml / min at 600° C. to perform pyrolysis for 2 hours. As a result, 100 g of slag produced as a solid by-product was recovered and used.

[0079] Example 2

[0080] The reaction was carried out under the same conditions as in Example 1 to recover the waste plastic pyrolysis oil, except that 110 g of slag and calcium oxide aggregates were added instead of using slag alone. When preparing the aggregates, 100 g of slag and 10 g of calcium oxide were used.

[0081] Example 3

[0082] The reaction was carried out under the same conditions as in Example 1 to recover the waste plastic pyrolysis oil, except that the solid by-products contained in the pyrolysis products of Example 2 were recovered instead of the slag, and the recovered solid by-products were reused. Specifically, in Example 2, the solid by-products were recovered from the second outlet at the bottom of the reactor to the recovery tank, and then the recovered solid by-products were reused as the slag in Example 1.

[0083] Example 4

[0084] In Example 3, ethanol was supplied at a flow rate of 50 ml / min for 30 minutes through the ethanol supply unit of the recovery tank to remove impurities contained in the solid by-products. After that, only aggregates with a size of 1 mm or more were recovered by the screening device, and 10 g of calcium oxide was additionally supplied to the recovered aggregates to polymerize and increase activity, and then these aggregates were reused as the slag in Example 1.

[0085] Comparative Example 1

[0086] The reaction was carried out under the same conditions as in Example 1 to recover the waste plastic pyrolysis oil, except that no coke residue was added.

[0087] Comparative Example 2

[0088] The reaction was carried out under the same conditions as in Example 1 to recover the waste plastic pyrolysis oil, except that the reaction was carried out by adding only calcium oxide without adding coke residue.

[0089] Evaluation example

[0090] The chlorine content (ppm) in the recycled waste plastic pyrolysis oil was measured by ICP and XRF analysis.

[0091] Measures the amount of fuel consumed in the pyrolysis process.

[0092] [Table 1]

[0093]

[0094] According to Example 1, the pyrolysis process was carried out in the presence of coke residue, and it was confirmed that the chlorine content in the pyrolysis oil was 270 ppm, which was significantly lower than the chlorine content in the waste plastic raw material (chlorine content was 4,000 ppm). In Example 2, it was confirmed that the chlorine content in the pyrolysis oil was further reduced to 160 ppm due to the use of the aggregate of coke residue and calcium oxide.

[0095] Furthermore, according to Example 3, in the case where the solid byproducts included in the pyrolysis product of Example 2 were recovered and the recovered solid byproducts were reused as slag, it was confirmed that the chlorine content in the pyrolysis oil was 290 ppm, which was significantly lower than the chlorine content in the waste plastic raw material. In particular, according to Example 4, in the case where the recovered solid byproducts were washed with ethanol, calcium oxide was additionally added to increase the activity, and then it was reused as slag, it was confirmed that the chlorine content in the pyrolysis oil was 150 ppm, which was the largest reduction compared to the chlorine content in the waste plastic raw material.

[0096] On the other hand, according to Comparative Example 1, when the pyrolysis process was performed without adding slag, it was confirmed that the chlorine content in the pyrolysis oil was 970 ppm, indicating that the chlorine content was too high. According to Comparative Example 2, even when only calcium oxide was added without adding slag, it was confirmed that the chlorine content in the pyrolysis oil was 370 ppm, indicating that the amount of chlorine present was large.

[0097] In addition, in the case of Examples 1 to 4, the fuel consumed in the pyrolysis process was about 51 g or less. On the other hand, in the case of Comparative Examples 1 and 2, it can be confirmed that about 60 g of fuel was consumed, which shows that the slag as a heat carrier effectively saves fuel consumption.

[0098] Although embodiments of the present invention have been described, the present invention is not limited to the embodiments, but can be implemented in various forms. For those skilled in the art to which the present invention relates, it is obvious that embodiments of the present invention can be implemented in other specific forms without departing from the spirit or essential features of the present invention. Therefore, it should be understood that the embodiments described herein are illustrative in all aspects and not restrictive.

Claims

1. A method for producing pyrolysis oil of waste plastics with reduced chlorine content, the method comprising The first step is to charge the waste plastic raw material and the accelerator containing char into the reactor; A second step of pyrolyzing the waste plastic feedstock in a reactor and recovering pyrolysis oil; and A third step is to recover the promoter from the reactor.

2. The method according to claim 1, wherein the accelerator in the first step is loaded into the reactor in an amount of 5-30 parts by weight relative to 100 parts by weight of the waste plastic raw material.

3. The method according to claim 1, wherein the promoter further contains one or more dechlorinating agents selected from the group consisting of metal oxides, metal hydroxides and metal carbonates. The method according to claim 3 , wherein the dechlorinating agent is a metal oxide.

5. The method according to claim 3, wherein the promoter is an aggregate in which a plurality of primary particles containing coke residue are combined and aggregated together by the dechlorination agent.

6. The method according to claim 5, wherein the dechlorination agent is a binder powder further containing moisture and combining a plurality of primary particles. 7 . The method according to claim 3 , wherein the coke residue is contained in the accelerator in an amount greater than the weight of the dechlorination agent.

8. The method according to claim 3, further comprising a fourth step of resupplying the promoter recovered in the third step to the first step.

9. The method according to claim 8, wherein the fourth step comprises A step of washing the promoter recovered in the third step with alcohol; a step of supplementing the accelerator and the dechlorinating agent washed with alcohol to prepare an accelerator; and A step of resupplying the prepared accelerator to the first step.

10. The method according to claim 1, wherein the second step is performed at a temperature of 300-600°C.

11. The method according to claim 1, wherein the second step is performed in a non-oxidizing atmosphere.

12. The method according to claim 9, further comprising the step of additionally heating the prepared accelerator at a temperature of 500-1,000°C to increase the activity of the accelerator before the step of resupplying the prepared accelerator to the first step.

13. A device for producing pyrolysis oil of waste plastics with reduced chlorine content, the device include: A reactor, wherein the waste plastic raw material and the accelerator containing the coke residue are loaded into the reactor and a pyrolysis process is performed therein; as well as Storage tank where the pyrolysis oil is recovered from the reactor.

14. The device according to claim 13, further comprising a recovery tank for recovering the promoter from the reactor; and The promoter is re-supplied from the recovery tank to the recycle line of the reactor.