Mobile phone rear cover with liquid crystal and optical texture combination and preparation method thereof
By using a grayscale diaphragm with a textured structure and a UV curing and optical coating layer of a semi-solid liquid crystal film in the back cover of the mobile phone, the problem of single pattern color in the existing technology is solved, and a colorful and three-dimensional effect is achieved. , to meet users’ aesthetic needs.
Patent Information
- Application Number
- CN202410855157.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-28
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2044-06-28
AI Technical Summary
The pattern and color of the existing mobile phone back cover is relatively single, which cannot meet the user's pursuit of beauty. The liquid crystal film is self-oriented, resulting in consistent colors and lack of richness and three-dimensionality.
A gray-scale diaphragm with a textured structure is laminated to a semi-solid liquid crystal film and then UV cured to form pitch differences in different light transmittance areas, making the liquid crystal film appear in multiple colors, and the corresponding texture is transferred to the surface of the liquid crystal film. layer, combined with the optical coating layer, to achieve the superposition of textured liquid crystal and optical texture.
Through the difference in pitch of different areas on the liquid crystal film and the influence of the optical texture layer, rich pattern colors and three-dimensional effects are produced to satisfy users' pursuit of beauty, and the pattern colors are richer and three-dimensional and vivid.
Smart Images

Figure CN118752885A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of mobile phone back covers, and in particular relates to a mobile phone back cover with a combination of liquid crystal and optical textures and a preparation method thereof. Background Art
[0002] In the design and manufacture of mobile phone back covers, PMMA / PC composite boards or glass fiber composite materials are often used as substrates in pursuit of lightness and thinness. At the same time, in order to achieve a unique visual appearance, a process combining UV transfer, PVD (optical plating) and liquid crystal film has emerged. The optical texture formed by UV transfer can introduce some light and shadow (dynamic effect), PVD can increase color and gloss, and the liquid crystal film can present a colorful and flowing effect.
[0003] The steps of the above process are usually: attaching a liquid crystal film to one surface of the plate, and then forming an optical texture, a PVD layer, and a cover bottom layer on the surface of the liquid crystal film in sequence, and then performing high pressure molding, spray coating, and CNC cutting in sequence; in addition, the steps of the above process can also be: forming an optical texture, a PVD layer, and a cover bottom layer on one surface of the plate in sequence, and then attaching a liquid crystal film to the other surface of the plate, and then forming an optical texture on the surface of the liquid crystal film, and finally cutting. However, since the liquid crystal film is self-oriented, the entire liquid crystal film presents a consistent color, so the pattern color of the back cover of the mobile phone is relatively single, which cannot meet the user's pursuit of beauty.
[0004] Therefore, there is an urgent need for a new mobile phone back cover with a combination of liquid crystal and optical texture and a preparation method thereof to solve the shortcomings of the existing technical problems. Summary of the invention
[0005] In view of the above problems, the purpose of the present invention is to provide a new mobile phone back cover with a combination of liquid crystal and optical texture and a preparation method thereof. The mobile phone back cover has superimposed textured liquid crystal and optical texture, and the textured liquid crystal formed on the liquid crystal film is highly consistent with the optical texture, so that the pattern of the mobile phone back cover is richer in color, more three-dimensional and vivid, satisfying the user's pursuit of beauty.
[0006] To achieve the above objectives, the first aspect of the present invention provides a method for preparing a mobile phone back cover having a combination of liquid crystal and optical texture, the steps comprising:
[0007] (1) applying a liquid crystal coating on a substrate, and then baking the liquid crystal coating to form a semi-solid liquid crystal film;
[0008] (2) Laminating the grayscale film with the texture structure with the semi-solid liquid crystal film and then UV curing;
[0009] (3) peeling off the grayscale film to obtain a liquid crystal film, on which a textured liquid crystal corresponding to the texture structure is formed; (4) bonding the liquid crystal film to the transparent composite plate using an adhesive;
[0010] (5) A first texture layer corresponding to the textured liquid crystal is formed by transfer printing on the surface of the liquid crystal film; or a first texture layer corresponding to the textured liquid crystal is formed by transfer printing on the surface of the transparent composite plate facing away from the liquid crystal film.
[0011] Compared with the prior art, the present invention laminates a grayscale film with a texture structure with a semi-solid liquid crystal film and then performs UV curing. The presence of the texture structure causes the grayscale film to have high transmittance areas and low transmittance areas. The parts of the semi-solid liquid crystal film corresponding to the high transmittance areas will receive more UV light energy and thus have a high degree of curing reaction, while those semi-solid liquid crystal films corresponding to the low transmittance areas receive less UV light energy, resulting in a low degree of curing reaction. Therefore, the parts of the liquid crystal film corresponding to the high transmittance areas and the parts corresponding to the low transmittance areas have different pitches, so that different areas of the liquid crystal film present different colors, thereby presenting graphic liquid crystal (i.e., textured liquid crystal). The graphic liquid crystal corresponds to the texture structure on the grayscale film, which can make the pattern color of the liquid crystal richer. At the same time, the present invention also transfers on the surface of the liquid crystal film to form a first texture layer (i.e., optical texture) corresponding to the textured liquid crystal; or transfers on the surface of the transparent composite plate away from the liquid crystal film to form a first texture layer (i.e., optical texture) corresponding to the textured liquid crystal. The first texture layer can further affect the reflection, refraction or interference of light, producing a visual sense of depth and rich color effects; therefore, the present invention superimposes the textured liquid crystal and the optical texture and ensures that the textured liquid crystal is highly consistent with the optical texture, so that the pattern color of the back cover of the mobile phone is richer, more three-dimensional and vivid, satisfying the user's pursuit of beauty.
[0012] Furthermore, step (4) of the present invention includes: using an adhesive to bond the liquid crystal film to the transparent composite plate and then peeling off the substrate. Specifically, the thickness of the adhesive is 12-18 μm, and the adhesive can be UV glue.
[0013] Furthermore, the preparation of the grayscale membrane with a texture structure of the present invention includes: generating a grayscale image using a texture design file and producing the grayscale membrane by offset printing or printing.
[0014] Furthermore, step (5) of the present invention includes: forming a first texture layer corresponding to the textured liquid crystal by transfer printing on the surface of the liquid crystal film, and then forming an optical coating layer and a cover bottom layer in sequence on the surface of the first texture layer. Specifically, the first texture layer corresponding to the textured liquid crystal is formed by UV transfer printing; metal, metal oxide or other inorganic substances are plated on the surface of the first texture layer by PVD to form an optical coating layer, and the optical coating layer can achieve a bright silver effect; and the cover bottom layer is formed by silk screen printing or spraying ink.
[0015] Furthermore, step (5) of the present invention includes: forming a first texture layer corresponding to the textured liquid crystal by transfer printing on the surface of the liquid crystal film, and then forming a second texture layer by transfer printing on the surface of the transparent composite plate away from the liquid crystal film, and forming an optical coating layer and a cover bottom layer on the surface of the second texture layer in sequence. Specifically, the first texture layer corresponding to the textured liquid crystal is formed by UV transfer printing; the optical coating layer is formed by coating the surface of the second texture layer with metal, metal oxide or other inorganic substances by PVD; and the cover bottom layer is formed by silk screen printing or ink spraying.
[0016] Furthermore, step (5) of the present invention includes: forming a first texture layer corresponding to the textured liquid crystal by transfer printing on the surface of the transparent composite plate facing away from the liquid crystal film, and then forming a second texture layer by transfer printing on the surface of the liquid crystal film, and forming an optical coating layer and a cover bottom layer on the surface of the second texture layer in sequence. Specifically, the first texture layer and the second texture are formed by UV transfer printing; metal, metal oxide or other inorganic substances are plated on the surface of the second texture layer by PVD to form an optical coating layer; and the cover bottom layer is formed by silk screen printing or ink spraying.
[0017] Furthermore, the optical coating layer of the present invention has a thickness of 30 to 400 nm, the cover layer has a thickness of 30 to 40 μm, and the thicknesses of the first texture layer and the second texture layer are independently 12 to 30 μm.
[0018] Furthermore, the thickness of the liquid crystal film of the present invention is 2-3 μm.
[0019] Furthermore, the transparent composite plate of the present invention is a PMMA / PC plate. The thickness of the transparent composite plate is 0.4-0.6 mm.
[0020] Furthermore, the liquid crystal coating of the present invention comprises cholesteric liquid crystal, UV resin and solvent.
[0021] Further, the UV resin of the present invention comprises 20-80 parts of UV oligomer, 10-60 parts of UV dilution monomer, 0.1-5 parts of photoinitiator, and 0.1-5 parts of auxiliary agent by weight. The UV oligomer may be, but not limited to, polyurethane-modified acrylate, polyester-modified acrylate, polyether-modified acrylate, and pure acrylate; the UV dilution monomer may be, but not limited to, monofunctional acrylate monomer, difunctional acrylate monomer, and trifunctional acrylate monomer; the photoinitiator may be, but not limited to, at least one of free radical initiator, free radical thermal initiator, and cationic initiator; the auxiliary agent may be, but not limited to, at least one of KH550, KH560, and KH570. The solvent is a ketone solvent, such as the solvent may be, but not limited to, at least one of methyl ethyl ketone, cyclohexanone, and cyclopentanone.
[0022] Furthermore, the substrate of the present invention is a PET substrate. The PET substrate has good supporting capacity and is convenient for coating liquid crystal coating.
[0023] Correspondingly, the second aspect of the present invention further provides a mobile phone back cover having a combination of liquid crystal and optical texture, which is prepared by the above-mentioned method for preparing a mobile phone back cover having a combination of liquid crystal and optical texture.
[0024] Compared with the prior art, the mobile phone back cover of the present invention has superimposed textured liquid crystal and optical texture, and the textured liquid crystal is highly consistent with the optical texture. Therefore, the pattern of the mobile phone back cover of the present invention is richer in color, more three-dimensional and vivid, thereby satisfying the user's pursuit of beauty. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 The present invention is a flow chart of a method for preparing a mobile phone back cover with a combination of liquid crystal and optical texture.
[0026] Figure 2 It is a schematic diagram of the structure of cholesteric liquid crystal in the liquid crystal coating of the present invention.
[0027] Figure 3 Schematic diagram of the structure of the texture of the grayscale film in Examples 1 to 3 of the present invention.
[0028] Figure 4 Schematic diagram of the structure of the textured liquid crystal of the liquid crystal film in Examples 1 to 3 of the present invention.
[0029] Figure 5 This is a schematic structural diagram of the mobile phone back cover according to Embodiment 1 of the present invention.
[0030] Figure 6 This is a diagram showing the effect of the superposition of the textured liquid crystal and the first texture layer in the back cover of the mobile phone according to Example 1 of the present invention.
[0031] Figure 7 This is a schematic structural diagram of the back cover of a mobile phone according to Embodiment 2 of the present invention.
[0032] Figure 8 This is a schematic structural diagram of the back cover of a mobile phone according to Embodiment 3 of the present invention. DETAILED DESCRIPTION
[0033] In order to better illustrate the purpose, technical scheme and beneficial effects of the present invention, the present invention will be further described below in conjunction with specific embodiments and drawings. It should be noted that the following implementation method is a further explanation of the present invention and should not be used as a limitation of the present invention.
[0034] Please see Figure 1 The present invention provides a method for preparing a mobile phone back cover having a combination of liquid crystal and optical texture, the steps comprising:
[0035] (1) applying a liquid crystal coating 11 on a substrate 12, and then baking the liquid crystal coating 11 to form a semi-solid liquid crystal film 111;
[0036] (2) Laminating the grayscale film 13 with a texture structure with the semi-solid liquid crystal film 111, and then UV curing;
[0037] (3) peeling off the grayscale film 13 to obtain a liquid crystal film 112, on which a textured liquid crystal corresponding to the texture structure is formed;
[0038] (4) Adhesive 14 is used to bond the liquid crystal film 112 to the transparent composite plate 15;
[0039] (5) The first texture layer 16 corresponding to the textured liquid crystal is formed by transfer printing on the surface of the liquid crystal film 112 ; or the first texture layer 16 corresponding to the textured liquid crystal is formed by transfer printing on the surface of the transparent composite board 15 away from the liquid crystal film 112 .
[0040] Please continue to see Figure 1 Step (4) further includes: using an adhesive 14 to bond the liquid crystal film 112 to the transparent composite plate 15 and then peeling off the substrate 12.
[0041] Please continue to see Figure 1 Step (5) further includes: transferring a first texture layer 16 corresponding to the textured liquid crystal on the surface of the liquid crystal film 112, and then sequentially forming an optical coating layer 17 and a cover layer 18 on the surface of the first texture layer 16.
[0042] Please continue to see Figure 1 Step (5) further includes: transferring a first texture layer 16 corresponding to the textured liquid crystal on the surface of the liquid crystal film 112, and then transferring a second texture layer 19 on the surface of the transparent composite board 15 away from the liquid crystal film 112, and forming an optical coating layer 17 and a cover layer 18 on the surface of the second texture layer 19 in sequence.
[0043] Please continue to see Figure 1 Step (5) of the present invention further includes: transferring a first texture layer 16 corresponding to the textured liquid crystal on the surface of the transparent composite plate 15 facing away from the liquid crystal film 112, then transferring a second texture layer 19 on the surface of the liquid crystal film 112, and sequentially forming an optical coating layer 17 and a cover layer 18 on the surface of the second texture layer 19.
[0044] Specifically, in the above step (1): the liquid crystal coating is applied and baked, so that the liquid crystal coating is transformed from a liquid state into a semi-solid liquid crystal film. During the baking process, the liquid crystals in the liquid crystal coating begin to align and orient. This step provides a basis for the subsequent formation of textured liquid crystals corresponding to the texture structure on the liquid crystal film.
[0045] Specifically, in the above step (2): a grayscale film with a preset texture structure is laminated to the semi-solid liquid crystal film, and a photocuring reaction is initiated by ultraviolet curing technology.
[0046] Specifically, in the above step (3): since the liquid crystal molecules are photocured to different degrees according to the areas of the grayscale film during the curing process, the pitches of the periodic arrangement of the liquid crystal molecules are different, thereby presenting different colors, that is, presenting a texture (pattern).
[0047] The following combination Figure 2 , the reasons why the liquid crystal film of the present invention presents different colors are further explained. The cholesteric phase liquid crystal of the present invention has a spiral structure, which can be divided into two chiralities, left-handed and right-handed. When the incident light enters, half of the incident light (circularly polarized light) will enter along the spiral structure, and the other half will be reflected due to the reverse rotation, wherein the director n of the liquid crystal molecule twists along the spiral axis X to form a layer and align. In the liquid crystal molecular structure, the distance that the director n of the liquid crystal molecule completes a 360-degree rotation is called the pitch d. The liquid crystal coating of the present invention is baked after coating, and the rod-shaped liquid crystal molecules can self-assemble to form a periodic spiral structure, thereby forming a one-dimensional soft photonic crystal with a gradient dielectric tensor, and present a unique spin-selective Bragg reflection, and then UV curing is performed, and the spiral structure will not be destroyed due to photopolymerization. The Bragg equation is: 2dSinθ=mλ; wherein d is the pitch of the cholesteric liquid crystal, θ is the incident angle, λ is the wavelength, and m is an integer. When the pitch and a specific wavelength in the visible light satisfy the above-mentioned Bragg equation, a portion of the visible light is diffracted, thereby reflecting its complementary color, which is why the liquid crystal film presents color. In other words, the present invention can produce different reflection band effects by adjusting the size of the pitch of the liquid crystal film, that is, different areas on the liquid crystal film present different colors. Specifically, the presence of the texture structure of the present invention makes the degree of curing different at different positions on the liquid crystal film during UV curing, which in turn leads to different torsional forces at different positions of the liquid crystal film. When the torsional force changes, the pitch of the liquid crystal film will also change, so that different areas on the liquid crystal film present different colors, thereby forming a texture (graphic).
[0048] The following is a detailed description of the preparation method of the mobile phone back cover with a combination of liquid crystal and optical texture of the present invention through specific examples. The liquid crystal coating used in Examples 1 to 3 includes 25 parts of cholesteric liquid crystal, 10 parts of UV resin and 65 parts of cyclohexanone; wherein the monomers of the cholesteric liquid crystal are RM82, RM257 and LC242, and their model is BS2D-SXH-C01, purchased from Shanghai Xianhuan High-tech New Materials Co., Ltd.; the UV resin includes 54 parts of polyurethane acrylate, 30 parts of isobornyl acrylate, 5 parts of tripropylene glycol diacrylate, 5 parts of 1,6-hexanediol diacrylate, 2 parts of photoinitiator 651, 3 parts of photoinitiator 184, and 0.5 parts of KH570; the optical coating layer is a ZrO (zirconium oxide) / SiO (silicon oxide) / NbO (niobium oxide) / SiO (silicon oxide) / NbO (niobium oxide) composite layer. At the same time, the texture structure of the grayscale film used in Examples 1 to 3 is as follows Figure 3 As shown, the textured liquid crystal structure of the liquid crystal film in Examples 1 to 3 is as follows Figure 4 shown.
[0049] Example 1
[0050] This embodiment provides a method for preparing a mobile phone back cover having a combination of liquid crystal and optical texture, the steps comprising:
[0051] (1) coating a liquid crystal coating on a PET substrate, and then baking the liquid crystal coating to form a semi-solid liquid crystal film;
[0052] (2) Laminating the grayscale film with the texture structure with the semi-solid liquid crystal film and then UV curing;
[0053] (3) peeling off the grayscale film to obtain a liquid crystal film, on which a textured liquid crystal corresponding to the texture structure is formed, wherein the thickness of the liquid crystal film is 2.5 μm;
[0054] (4) using an adhesive to bond the liquid crystal film to a transparent composite sheet with a thickness of 0.5 mm, and then peeling off the PET substrate, wherein the thickness of the adhesive is 15 μm, the adhesive is UV glue, and the transparent composite sheet is a PMMA / PC sheet;
[0055] (5) forming a first texture layer with a thickness of 18 μm corresponding to the textured liquid crystal on the surface of the liquid crystal film by UV transfer, and then forming an optical coating layer with a thickness of 100 nm and a cover layer with a thickness of 35 μm on the surface of the first texture layer in sequence;
[0056] (6) After step (5), high pressure forming, high gloss coating liquid and CNC cutting are performed in sequence to obtain the following Figure 5 The phone back cover shown has a combination of liquid crystal and optical texture.
[0057] The effect of the superposition of the textured liquid crystal and the first texture layer in the back cover of the mobile phone in this embodiment is as follows: Figure 6 As shown by Figure 6 It can be seen that the textured liquid crystal and the optical texture are superimposed and the textured liquid crystal and the optical texture are highly consistent.
[0058] Example 2
[0059] This embodiment provides a method for preparing a mobile phone back cover having a combination of liquid crystal and optical texture, the steps comprising:
[0060] (1) coating a liquid crystal coating on a PET substrate, and then baking the liquid crystal coating to form a semi-solid liquid crystal film;
[0061] (2) Laminating the grayscale film with the texture structure with the semi-solid liquid crystal film and then UV curing;
[0062] (3) peeling off the grayscale film to obtain a liquid crystal film, on which a textured liquid crystal corresponding to the texture structure is formed, wherein the thickness of the liquid crystal film is 3 μm;
[0063] (4) using an adhesive to bond the liquid crystal film to a transparent composite sheet with a thickness of 0.5 mm, and then peeling off the PET substrate, wherein the thickness of the adhesive is 18 μm, the adhesive is UV glue, and the transparent composite sheet is a PMMA / PC sheet;
[0064] (5) UV transfer is performed on the surface of the liquid crystal film to form a first texture layer with a thickness of 20 μm corresponding to the textured liquid crystal, and then transfer is performed on the surface of the transparent composite plate away from the liquid crystal film to form a second texture layer with a thickness of 20 μm, and an optical coating layer with a thickness of 200 nm and a cover layer with a thickness of 40 μm are sequentially formed on the surface of the second texture layer, and the second texture layer has a bullet head texture;
[0065] (6) After step (5), high pressure forming and CNC cutting are performed in sequence to obtain Figure 7 The phone back cover shown has a combination of liquid crystal and optical texture.
[0066] Example 3
[0067] This embodiment provides a method for preparing a mobile phone back cover having a combination of liquid crystal and optical texture, the steps comprising:
[0068] (1) coating a liquid crystal coating on a PET substrate, and then baking the liquid crystal coating to form a semi-solid liquid crystal film;
[0069] (2) Laminating the grayscale film with the texture structure with the semi-solid liquid crystal film and then UV curing;
[0070] (3) peeling off the grayscale film to obtain a liquid crystal film, on which a textured liquid crystal corresponding to the texture structure is formed, wherein the thickness of the liquid crystal film is 2 μm;
[0071] (4) using an adhesive to bond the liquid crystal film to a transparent composite sheet with a thickness of 0.5 mm, and then peeling off the PET substrate, wherein the thickness of the adhesive is 13 μm, the adhesive is UV glue, and the transparent composite sheet is a PMMA / PC sheet;
[0072] (5) a first texture layer with a thickness of 13 μm corresponding to the textured liquid crystal is formed on the surface of the transparent composite plate facing away from the liquid crystal film, and a second texture layer with a thickness of 22 μm is formed on the surface of the liquid crystal film, and an optical coating layer with a thickness of 300 nm and a cover layer with a thickness of 30 μm are formed on the surface of the second texture layer in sequence, and the second texture layer has a bullet head texture;
[0073] (6) After step (5), CNC cutting is performed to obtain Figure 8 The phone back cover shown has a combination of liquid crystal and optical texture.
[0074] In summary, the present invention laminates a grayscale film with a texture structure with a semi-solid liquid crystal film and then performs UV curing. During the curing process, the portion of the semi-solid liquid crystal film corresponding to the high transmittance area will receive more UV light energy, resulting in a high degree of curing reaction, while those semi-solid liquid crystal films corresponding to the low transmittance area receive less UV light energy, resulting in a low degree of curing reaction. Therefore, the portion of the liquid crystal film corresponding to the high transmittance area and the portion corresponding to the low transmittance area have different pitches, so that different areas of the liquid crystal film present different colors and thus present a pattern, which corresponds to the texture structure on the grayscale film, which can make the liquid crystal pattern color richer. At the same time, the present invention also transfers a first texture layer corresponding to the textured liquid crystal on the surface of the liquid crystal film; or transfers a first texture layer corresponding to the textured liquid crystal on the surface of the transparent composite plate away from the liquid crystal film. The first texture layer can further affect the reflection, refraction or interference of light, producing a visual sense of depth and rich color effects. Therefore, the present invention can make the pattern color of the back cover of the mobile phone richer, more three-dimensional and vivid by superimposing the textured liquid crystal and the optical texture and ensuring that the pattern formed on the liquid crystal film is highly consistent with the optical texture, thereby satisfying the user's pursuit of beauty.
[0075] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention is described in detail with reference to the preferred embodiments, it is not limited to those listed in the embodiments. Those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.
Claims
1. A method for preparing a mobile phone back cover with a combination of liquid crystal and optical texture, It is characterized in that the steps include: (1) applying a liquid crystal coating on a substrate, and then baking the liquid crystal coating to form a semi-solid liquid crystal film; (2) laminating the grayscale film with a texture structure with the semi-solid liquid crystal film, and then performing UV curing; (3) peeling off the grayscale film to obtain a liquid crystal film, on which a textured liquid crystal corresponding to the texture structure is formed; (4) bonding the liquid crystal film to the transparent composite plate using an adhesive; (5) A first texture layer corresponding to the textured liquid crystal is formed by transfer printing on the surface of the liquid crystal film; or a first texture layer corresponding to the textured liquid crystal is formed by transfer printing on the surface of the transparent composite plate facing away from the liquid crystal film.
2. The method for preparing a mobile phone back cover having a combination of liquid crystal and optical texture as claimed in claim 1, It is characterized in that The step (4) comprises: using an adhesive to bond the liquid crystal film to the transparent composite plate and then peeling off the substrate.
3. The method for preparing a mobile phone back cover having a combination of liquid crystal and optical texture as claimed in claim 1, It is characterized in that The step (5) comprises: transferring a first texture layer corresponding to the textured liquid crystal onto the surface of the liquid crystal film, and then sequentially forming an optical coating layer and a cover layer on the surface of the first texture layer.
4. The method for preparing a mobile phone back cover having a combination of liquid crystal and optical texture as claimed in claim 1, It is characterized in that The step (5) comprises: transferring a first texture layer corresponding to the textured liquid crystal on the surface of the liquid crystal film, then transferring a second texture layer on the surface of the transparent composite board facing away from the liquid crystal film, and sequentially forming an optical coating layer and a cover layer on the surface of the second texture layer.
5. The method for preparing a mobile phone back cover having a combination of liquid crystal and optical texture as claimed in claim 1, It is characterized in that The step (5) comprises: transferring a first texture layer corresponding to the textured liquid crystal on the surface of the transparent composite plate facing away from the liquid crystal film, then transferring a second texture layer on the surface of the liquid crystal film, and sequentially forming an optical coating layer and a cover layer on the surface of the second texture layer.
6. The method for preparing a mobile phone back cover having a combination of liquid crystal and optical texture as claimed in claim 1, It is characterized in that The thickness of the liquid crystal film is 2-3 μm.
7. The method for preparing a mobile phone back cover having a combination of liquid crystal and optical texture as claimed in claim 1, It is characterized in that The transparent composite plate is a PMMA / PC plate.
8. The method for preparing a mobile phone back cover having a combination of liquid crystal and optical texture as claimed in claim 1, It is characterized in that The liquid crystal coating comprises cholesteric liquid crystal and UV glue.
9. The method for preparing a mobile phone back cover having a combination of liquid crystal and optical texture as claimed in claim 1, It is characterized in that The substrate is a PET substrate.
10. A mobile phone back cover with a combination of liquid crystal and optical texture, It is characterized in that The mobile phone back cover having a combination of liquid crystal and optical texture is prepared by the preparation method of any one of claims 1 to 9.
Citation Information
Patent Citations
Diaphragm and preparation method thereof, shell and electronic device
CN113703210A
Shell, manufacturing method thereof and electronic equipment
CN115119432A
Production method of optical film having surface shape, polymerizable liquid crystal film, and polymerizable liquid crystal film having surface shape
JP2014174321A
Liquid cristal film, light source assembly including the same and liquid crystal display including the liquid crystal film
KR1020110116113A