Lithium manganese iron phosphate material and preparation method thereof

The carbon layer is repaired and the lithium ion conductor is fused through the secondary coating process, which solves the problem of battery performance degradation caused by low conductivity of lithium iron manganese phosphate and manganese dissolution, and significantly improves the battery's ionic conductivity and rate performance.

CN118754081APending Publication Date: 2024-10-11CHANGSHU INSTITUTE OF TECHNOLOGY
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202410906338.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-08
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

The conductivity of lithium iron manganese phosphate is low and the battery performance is degraded due to manganese dissolution during the charge and discharge process.

Method used

The secondary coating process is used to repair the carbon layer on the surface of the material, and the small particles of powder are combined into large particles through granulation, thereby reducing the contact between the lithium iron manganese phosphate body and the electrolyte, improving the ionic conductivity, and through the secondary carbon coating Lithium ion conductors and lithium iron manganese phosphate are integrated into microspheres to improve the compaction performance of the material.

Benefits of technology

It significantly improves the ionic conductivity of the material, reduces the oxygen release from the material and battery gas production, improves the Ginger-Taylor effect, and improves the rate performance and discharge capacity of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118754081A_ABST
    Figure CN118754081A_ABST
Patent Text Reader

Abstract

The invention discloses a lithium manganese iron phosphate material and a preparation method thereof. The preparation method comprises the following steps: S1, performing wet grinding and mixing on raw materials such as an iron source, a manganese source, a phosphorus source, a lithium source, a carbon source and an additive by using a grinding machine, and drying and granulating to prepare a lithium manganese iron phosphate precursor; s2, sintering the precursor in an inert or reducing atmosphere according to a first sintering schedule, discharging, and crushing to obtain a lithium manganese iron phosphate material; and S3, mixing, coating and granulating the lithium manganese iron phosphate, a lithium ion conductor and a binder into particles of 2-20 microns, sintering in an inert or reducing atmosphere according to a second sintering schedule, and sieving the discharged material to obtain the finished product pitaya structure-like lithium manganese iron phosphate material. The lithium manganese iron phosphate material prepared by the invention has the characteristics of low gas production, high compaction, high capacity, high magnification and long cycle.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of battery materials and relates to a lithium manganese iron phosphate material and a preparation method thereof. Background Art

[0002] Lithium iron manganese phosphate is a commonly used positive electrode material for lithium-ion batteries. It has the advantages of low cost, wide source of raw materials, and environmental friendliness. Lithium iron manganese phosphate has an olivine structure, and its structure does not change during the process of ion insertion and extraction. It is considered to be an upgraded version of lithium iron phosphate. However, compared with lithium iron phosphate, lithium iron manganese phosphate has lower conductivity, which limits the actual capacity and rate performance of the material. In addition, the dissolution of manganese due to the Jan-Taylor effect further limits the practical application of lithium iron manganese phosphate.

[0003] Conventional lithium manganese iron phosphate only uses a single sintering process. After the sintered material is crushed by the air flow mill, the high-intensity air flow impact can easily cause the coated carbon layer to fall off, exposing the lithium manganese iron phosphate matrix. In addition, the particle size of the product of the single sintering process is small, and the contact with the electrolyte increases, resulting in serious side reactions and increased gas production. Summary of the invention

[0004] Purpose of the invention: The purpose of the present invention is to solve the problem that the conductivity of lithium manganese iron phosphate is low and the battery performance is reduced due to manganese dissolution during charging and discharging, and to provide a lithium manganese iron phosphate material and a preparation method thereof.

[0005] Technical solution: A method for preparing a lithium manganese iron phosphate material of the present invention comprises the following steps:

[0006] S1, the iron source, manganese source, phosphorus source, lithium source, carbon source and additives are wet-grinded and mixed to 0.05-0.8 μm by a grinder, and then dried and granulated to obtain a lithium manganese iron phosphate precursor;

[0007] S2, sintering the lithium iron manganese phosphate precursor obtained in S1 in an inert or reducing atmosphere according to a first sintering system, and crushing it after it comes out of the furnace to obtain a lithium iron manganese phosphate material;

[0008] S3, mixing the lithium manganese iron phosphate material obtained in S2 with a lithium ion conductor and a binder, coating and granulating them into particles of 2 to 20 μm, and sintering them in an inert or reducing atmosphere according to a second sintering system, and sieving the material out of the furnace to obtain the target product, the lithium manganese iron phosphate material with a pitaya structure;

[0009] The chemical formula of the pitaya-like lithium iron manganese phosphate material is LiMn x Fe y PO4 / C, where x+y=1, 0.5≤x≤1, 0≤y≤0.5.

[0010] Furthermore, the LiMn x Fe y In PO4 / C, Li / (Mn+Fe)=1.02-1.10, the LiMn x Fe y The C content in PO4 / C is 0.5-5%.

[0011] Furthermore, the iron source in step S1 includes one or more of ferrous oxalate, ferric phosphate, manganese iron oxide, and manganese iron phosphate; the manganese source includes one or more of manganese carbonate, manganese dioxide, manganese tetraoxide, manganese iron oxide, manganese iron phosphate, and manganese oxalate; the phosphorus source includes one or more of ferric phosphate, manganese iron phosphate, lithium dihydrogen phosphate, ammonium dihydrogen phosphate, diammonium hydrogen phosphate, and phosphoric acid; the lithium source includes one or more of lithium carbonate, lithium hydroxide, and lithium nitrate; the carbon source includes one or more of sucrose, glucose, fructose, citric acid, phenolic resin, polyvinyl alcohol, polyethylene glycol, starch, urea, carbon black, acetylene black, graphite, graphene, and conductive carbon tubes; the additive includes an oxide of one or more elements selected from Mg, Zn, Ni, Co, V, Ti, Zr, W, La, Al, Y, Sr, and F.

[0012] Furthermore, the wet grinding particle size D in S1 is 50 It is 0.05~0.8μm.

[0013] Furthermore, the drying and granulation method includes one of centrifugal spray drying, two / four-fluid spray drying, fluidized bed drying, and freeze drying; the sintering kiln includes one or more of a tubular furnace, a box furnace, a push-plate furnace, a roller furnace, and a rotary furnace.

[0014] Furthermore, the lithium ion conductor in step S3 includes Li2ZrO3, LiNbO3, Li4Ti5O 12 , one or more of Li2TiO3, Li3VO4, LiSnO3, Li2SiO3, LiAlO2, Li3PO4, LLZO, LLTO and LATP, etc.; the binder includes one or more of asphalt powder, resin, PVDF, PTFE, PAA, PAN, etc.

[0015] Furthermore, the first sintering schedule in S2 is to heat the material to 500-700°C at a heating rate of 0.5-5°C / min and keep the temperature for 2-6 hours; the second sintering schedule in S3 is to heat the material to 600-800°C at a heating rate of 0.5-5°C / min and keep the temperature for 4-12 hours.

[0016] Furthermore, the coating granulation in S3 is achieved by a mechanical fusion machine or a VC mixer.

[0017] Provided is a lithium manganese iron phosphate material prepared by the preparation method.

[0018] Provided is a battery positive electrode plate made from the lithium manganese iron phosphate material.

[0019] Beneficial effects: Compared with the prior art, the present invention has the following significant advantages: 1. The carbon layer on the surface of the material is repaired by secondary coating, and small-particle powder is combined into large-particle secondary balls by granulation, which helps to reduce the specific surface area of ​​the material, reduce the contact between the lithium iron manganese phosphate body and the electrolyte, reduce the oxygen release of the material and the gas production of the battery, and improve the Jiang-Taylor effect; 2. The lithium ion conductor and lithium iron manganese phosphate are simultaneously integrated into the microspheres by secondary carbon coating, which improves the ionic conductivity of the material; 3. LiMn of different particle sizes can be obtained by secondary carbon coating. x Fe y PO4 / C materials can be graded by particles of different sizes to improve the compaction performance of the material. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 The present invention is a flow chart of the method for preparing lithium manganese iron phosphate material.

[0021] Figure 2 This is the charge and discharge curve of the lithium manganese iron phosphate material prepared in Example 1 of the present invention at 0.2C. DETAILED DESCRIPTION

[0022] The technical solution of the present invention is further described below in conjunction with the accompanying drawings. The equipment and raw materials used can be purchased from the market or are commonly used in the art.

[0023] Example 1

[0024] S1. 603.28g of iron phosphate, 689.70g of manganese carbonate, 162.56g of lithium carbonate, 633.97g of lithium dihydrogen phosphate, 90g of glucose, and 15g of titanium dioxide were wet-ground and mixed by a sand mill to 0.3 μm, and granulated by a centrifugal spray dryer to obtain a lithium manganese iron phosphate precursor;

[0025] S2. The precursor was heated to 600°C in a nitrogen atmosphere at a heating rate of 0.8°C / min and kept warm for 4h, and then crushed to obtain lithium manganese iron phosphate material;

[0026] S3. The above 1500g lithium iron manganese phosphate, 10g LATP and 20g low-temperature asphalt are mixed and coated in a mechanical fusion machine to form 3μm particles, and the temperature is increased to 700℃ in a nitrogen atmosphere at a heating rate of 1.2℃ / min for 8h for sintering. The material is sieved to obtain the finished product of pitaya structure lithium iron manganese phosphate material LiMn 0.6 Fe0.4 PO4 / C.

[0027] Example 2

[0028] S1. 1500g of ferromanganese phosphate, 363.30g of lithium carbonate, 110g of glucose and 8g of vanadium pentoxide were wet-ground and mixed by a sand mill to 0.2 μm, and granulated by a centrifugal spray dryer to obtain a lithium ferromanganese phosphate precursor;

[0029] S2. The precursor was heated to 580°C in a nitrogen atmosphere at a heating rate of 1.2°C / min and kept warm for 5h, and then crushed to obtain a lithium manganese iron phosphate material;

[0030] S3. The above 1000g lithium iron manganese phosphate, 6.3g LiAlO2 and 12g phenolic resin were mixed and coated in a VC mixer to form 5μm particles, and the temperature was raised to 690℃ in a nitrogen atmosphere at a heating rate of 1.0℃ / min for 10h for sintering. The material was sieved to obtain a finished product of a pitaya structure lithium iron manganese phosphate material LiMn 0.65 Fe 0.35 PO4 / C.

[0031] Example 3

[0032] S1.300g of iron phosphate, 695.52g of manganese dioxide, 94.757g of lithium carbonate, 852.23g of lithium dihydrogen phosphate, 150g of glucose, and 7.5g of tungsten trioxide were wet-ground and mixed by a sand mill to 0.1 μm, and granulated by a centrifugal spray dryer to obtain a lithium manganese iron phosphate precursor;

[0033] S2. The precursor was heated to 600°C in a nitrogen atmosphere at a heating rate of 1.3°C / min and kept warm for 3h, and then crushed to obtain lithium manganese iron phosphate material;

[0034] S3. The above 800g lithium iron manganese phosphate, 4.7g LATP and 12.7g low-temperature asphalt are mixed and coated in a mechanical fusion machine to form 2μm particles, and the temperature is increased to 680℃ in a nitrogen atmosphere at a heating rate of 0.9℃ / min for 8h for sintering. The material is sieved to obtain the finished product of pitaya structure lithium iron manganese phosphate material LiMn 0.8 Fe 0.2 PO4 / C.

[0035] Example 4

[0036] S1. 603.28g of iron phosphate, 689.70g of manganese carbonate, 162.56g of lithium carbonate, 633.97g of lithium dihydrogen phosphate, 90g of glucose, and 15g of titanium dioxide were wet-ground and mixed by a sand mill to 0.3 μm, and granulated by a centrifugal spray dryer to obtain a lithium manganese iron phosphate precursor;

[0037] S2. The above precursor was heated to 700°C in a nitrogen atmosphere at a heating rate of 5°C / min and kept warm for 3h, and then crushed to obtain lithium manganese iron phosphate material;

[0038] S3. The above 1500g lithium iron manganese phosphate, 10g LATP and 20g low-temperature asphalt are mixed and coated in a mechanical fusion machine to form 3μm particles, and the temperature is increased to 800℃ in a nitrogen atmosphere at a heating rate of 5℃ / min for 8h for sintering. The material is sieved to obtain the finished product of the pitaya structure lithium iron manganese phosphate material LiMn 0.6 Fe 0.4 PO4 / C.

[0039] Comparative Example 1

[0040] The steps are the same as those in Example 1, except that only a single sintering is performed and the lithium manganese iron phosphate material is obtained after crushing.

[0041] Comparative Example 2

[0042] The steps are the same as those in Example 1, except that no lithium ion conductor is added for secondary sintering in step S3.

[0043] In order to verify the progress of the embodiments of the present application, the following performance tests were conducted on the above embodiments 1-3: the above materials were mixed with SP, PVDF, and carbon nanotubes in a ratio of 96:0.5:3:0.5 to prepare positive electrode sheets, and metal lithium was used as the negative electrode sheet. Half-cells were assembled in a conventional manner, and then the half-cells were tested using the Xinwei half-cell test system. The charge and discharge test voltage was 2.0 to 4.5 V. The test results are shown in the following table:

[0044]

[0045] According to the above results, it can be seen that the positive electrode material prepared by the present invention has the characteristics of high discharge capacity, excellent rate performance and low internal resistance. The electrochemical performance of comparative example 1-2 is significantly inferior to that of embodiment 1-4, indicating that the present invention, on the basis of single sintering, is crushed into appropriate particle size, and then the material and lithium ion conductor and adhesive are subjected to secondary carbon coating and lithium ion conductor are introduced by secondary sintering to form a pitaya-like structure. On the one hand, the secondary sintering repairs the carbon coating layer damaged by air flow crushing, and on the other hand, the particles become larger after granulation to reduce the direct contact between lithium iron manganese phosphate and electrolyte. The lithium ion conductor and lithium iron manganese phosphate are simultaneously fused into the microspheres through secondary carbon coating, which improves the ionic conductivity of the material and solves the problem that the conductivity of lithium iron manganese phosphate is low and the battery performance is reduced due to manganese dissolution during charging and discharging.

Claims

1. A method for preparing lithium manganese iron phosphate material, characterized in that: The following steps are involved: S1, iron source, manganese source, phosphorus source, lithium source, carbon source and additives are wet-grinded and mixed by a grinder, and then dried and granulated to obtain lithium manganese iron phosphate precursor; S2, sintering the lithium iron manganese phosphate precursor obtained in S1 in an inert or reducing atmosphere according to a first sintering system, and crushing it after it comes out of the furnace to obtain a lithium iron manganese phosphate material; S3, mixing the lithium manganese iron phosphate material obtained in S2 with a lithium ion conductor and a binder, coating and granulating them into particles of 2 to 20 μm, and sintering them in an inert or reducing atmosphere according to a second sintering system, and sieving the material out of the furnace to obtain the target product, the lithium manganese iron phosphate material with a pitaya structure; The chemical formula of the pitaya-like lithium iron manganese phosphate material is LiMn x Fe y PO4 / C, where x+y=1, 0.5≤x≤1, 0≤y≤0.

5.

2. The method for preparing lithium iron manganese phosphate material according to claim 1, characterized in that: The LiMn x Fe y In PO4 / C, Li / (Mn+Fe)=1.02-1.10, the LiMn x Fe y The C content in PO4 / C is 0.5-5%.

3. The method for preparing lithium iron manganese phosphate material according to claim 1, characterized in that: The iron source in step S1 includes one or more of ferrous oxalate, ferric phosphate, manganese iron oxide, and manganese iron phosphate; the manganese source includes one or more of manganese carbonate, manganese dioxide, manganese tetraoxide, manganese iron oxide, manganese iron phosphate, and manganese oxalate; the phosphorus source includes one or more of ferric phosphate, manganese iron phosphate, lithium dihydrogen phosphate, ammonium dihydrogen phosphate, diammonium hydrogen phosphate, and phosphoric acid; the lithium source includes one or more of lithium carbonate, lithium hydroxide, and lithium nitrate; the carbon source includes one or more of sucrose, glucose, fructose, citric acid, phenolic resin, polyvinyl alcohol, polyethylene glycol, starch, urea, carbon black, acetylene black, graphite, graphene, and conductive carbon tubes; the additive includes an oxide of one or more elements selected from Mg, Zn, Ni, Co, V, Ti, Zr, W, La, Al, Y, Sr, and F.

4. The method for preparing lithium iron manganese phosphate material according to claim 1, characterized in that: The wet grinding particle size D in S1 50 It is 0.05~0.8μm.

5. The method for preparing lithium iron manganese phosphate material according to claim 1, characterized in that: The drying and granulation method includes one of centrifugal spray drying, two / four-fluid spray drying, fluidized bed drying, and freeze drying; the sintering kiln includes one or more of a tube furnace, a box furnace, a push plate furnace, a roller furnace, and a rotary furnace.

6. The method for preparing lithium iron manganese phosphate material according to claim 1, characterized in that: The lithium ion conductor in step S3 includes Li2ZrO3, LiNbO3, Li4Ti5O 12 , one or more of Li2TiO3, Li3VO4, LiSnO3, Li2SiO3, LiAlO2, Li3PO4, LLZO, LLTO and LATP, etc.; the binder includes one or more of asphalt powder, resin, PVDF, PTFE, PAA, PAN, etc.

7. The method for preparing lithium iron manganese phosphate material according to claim 1, characterized in that: The first sintering schedule in S2 is to heat the material to 500-700°C at a heating rate of 0.5-5°C / min and keep the temperature for 2-6 hours; the second sintering schedule in S3 is to heat the material to 600-800°C at a heating rate of 0.5-5°C / min and keep the temperature for 4-12 hours.

8. The method for preparing lithium iron manganese phosphate material according to claim 1, characterized in that: The coating granulation in S3 is achieved by a mechanical fusion machine or a VC mixer.

9. A lithium manganese iron phosphate material, characterized in that: Prepared by the preparation method according to any one of claims 1 to 8.

10. A positive electrode plate for a battery, characterized in that: Made from the lithium manganese iron phosphate material described in claim 9.

Citation Information

Patent Citations

  • Lithium battery composite positive electrode material with core-shell structure and preparing method of lithium battery composite positive electrode material

    CN108054378A

  • Lithium iron manganese phosphate cathode material and preparation method thereof

    CN111564622A

  • Carbon-coated lithium aluminum titanium phosphate solid electrolyte as well as preparation method and application thereof

    CN116914237A

  • Preparation method of high-conductivity super-ionic conductor composite lithium manganese iron phosphate positive electrode material

    CN117049495A

  • Modified lithium iron manganese phosphate positive electrode material, preparation method thereof, positive plate and battery

    CN117936742A