Method for manufacturing large-area graphene heat dissipation film through two-step method

Preparing graphene oxide films through a two-step method and using laser processing solves the problems of long preparation time and low efficiency of graphene films in the existing technology, and achieves the preparation of high-quality, low-cost large-area graphene films with excellent thermal conductivity and commercialization prospects.

CN118754113AActive Publication Date: 2024-10-11SHANDONG UNIV SHENZHEN RES INST
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202410935149.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-12
Publication Date
2024-10-11
Estimated Expiration
2044-07-12

AI Technical Summary

Technical Problem

It is difficult to prepare large-area graphene heat dissipation films with low defects quickly, efficiently and on a large scale using existing technology, which limits its application in electronic and electrical equipment.

Method used

A two-step preparation method is adopted: first, a graphene oxide film is prepared through low-temperature demoulding treatment, and then laser scanning is used to remove oxygen-containing groups and repair structural defects to obtain a high-quality graphene film.

Benefits of technology

The preparation of low-cost, low-defect large-area graphene films has been achieved. The thermal conductivity reaches 1801.07W/(m·K), which is much higher than that of common metals. It is suitable for industrial production and flexible electronic products.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118754113A_ABST
    Figure CN118754113A_ABST
Patent Text Reader

Abstract

The invention relates to a method for manufacturing a large-area graphene heat dissipation film through a two-step method. The method comprises the two continuous steps of preparation of a graphene oxide film and reduction of graphene oxide through laser treatment. The method comprises the following steps: taking a graphene oxide solution as an initial raw material, then placing the graphene oxide solution on a template to form a film, carrying out lossless demolding on the film by using liquid nitrogen, and finally carrying out selective laser treatment on the obtained graphene oxide film, so as to obtain the ultra-thin micron-sized large-area graphene film with good flexibility. And the material has a huge application prospect in transparent conductive films, flexible devices, heat dissipation films and electromagnetic shielding. The method for preparing the graphene film through the two-step method is easy to operate, low in cost, high in operability and good in repeatability, the thermal conductivity obtained through calculation is far higher than that of common metal copper, aluminum and silver, and the method can be used for large-scale industrial production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for preparing an ultra-thin flexible large-area graphene film by a simple two-step method, and belongs to the technical field of film materials. Background Art

[0002] With the rapid development of science and technology, electronic and electrical equipment is gradually developing towards thinness, miniaturization and flexibility. The power density of integrated circuit chips and electronic components inside them is increasing rapidly. Small space and high power will inevitably generate a lot of heat accumulation, which seriously affects the performance and service life of electronic and electrical equipment and brings safety hazards. Therefore, it is particularly important to find a low-density and high-thermal conductivity heat dissipation material. Graphene is a two-dimensional carbon allotrope, which is composed of a single layer of sp 2 The hexagonal honeycomb two-dimensional structure composed of hybrid carbon atoms has a unique stable structure that gives graphene many excellent properties. Among them, graphene's high thermal conductivity (~5300W·m -1 ·K -1 ) shows great application prospects in the field of thermal management of electronic devices. In particular, large-sized graphene flakes, complete interlayer structures and orderly interlayer arrangements all have a positive effect on the thermal conductivity of graphene-based heat dissipation materials. Although there are many methods for preparing graphene heat dissipation films, there are problems such as long preparation time and low efficiency, limited size, and high process parameter requirements, which make it difficult to apply industrially, limiting the commercial application of graphene heat dissipation films. Therefore, it is particularly important to develop a method that is environmentally friendly, low-cost, and can be used to prepare large-area and low-defect graphene-based films on a large scale. Summary of the invention

[0003] In view of the shortcomings of the prior art, the present invention provides a method for preparing a large-area graphene heat dissipation film by a two-step method. The method is mainly divided into two steps: preparation of a graphene oxide film and laser treatment to obtain a graphene film. First, a graphene oxide film is prepared by a simple and pollution-free method, and demolding treatment is performed at low temperature. Then, the graphene oxide film is treated by laser reduction to remove oxygen-containing functional groups and repair structural defects, thereby obtaining a large-area low-defect graphene functional film, which can be widely used in device heat dissipation, electromagnetic shielding, flexible electronic products and other fields.

[0004] The technical solution of the present invention is:

[0005] A two-step method for manufacturing a large-area graphene heat dissipation film comprises:

[0006] Preparation of graphene oxide film: preparing a graphene oxide dispersion, placing the prepared graphene oxide dispersion in a mold, and performing demoulding treatment at low temperature;

[0007] Preparation of graphene film: pre-annealing the graphene oxide film; and further treating the pre-annealed graphene oxide film using laser scanning to remove oxygen-containing groups, restore the conjugated structure of graphene, and obtain a low-defect graphene film;

[0008] The obtained graphene film is pressed to obtain a large-area graphene heat dissipation film.

[0009] According to the preferred embodiment of the present invention, the demoulding process is performed at low temperature; comprising:

[0010] The mold containing the graphene oxide dispersion is dried on an electric furnace to form a film, and then liquid nitrogen is slowly poured into the mold to separate the graphene oxide film from the substrate.

[0011] Preferably according to the present invention, the heating temperature of the electric furnace is 50-100°C.

[0012] Preferably according to the present invention, after the graphene oxide film is prepared, the substrate is cleaned with isopropanol and ethanol and dried.

[0013] Preferably according to the present invention, the temperature for pre-annealing the graphene oxide film is 1000°C.

[0014] Preferably according to the present invention, a laser light source with a laser aperture of 50 micrometers is used to perform laser scanning processing on the obtained graphene oxide film, the laser power density is 1-20W, and the laser scanning speed is 0.8-2.0m / s.

[0015] The beneficial effects of the present invention are:

[0016] 1. The method for preparing a graphene film provided by the present invention is simple to operate and mainly consists of two steps, namely, the preparation of a graphene oxide film and a laser reduction treatment. The operation cost is low, the operability is strong, the repeatability is good, and it is very suitable for the preparation of large-area graphene-based films of different thicknesses. The prepared graphene-based films have very good flexibility and can be applied to industrial production.

[0017] 2. In the process of preparing graphene oxide film, the present invention changes the traditional film preparation process, pours the graphene-based dispersion into the mold to dry and form a film, and uses liquid nitrogen to achieve non-destructive demoulding of the graphene oxide film. After the film is separated from the substrate, the mold can be recycled and reused, which greatly reduces the cost. In addition, templates of different properties can be selected as needed, which is conducive to further functionalization of the film.

[0018] 3. The present invention uses laser to process graphene oxide film, which has the characteristics of higher selectivity, higher efficiency and lower cost. The laser not only removes a large number of oxygen-containing groups on the surface of graphene oxide through high temperature and chemical reaction, but also destroys chemical bonds for reorganization to form sp2 The conjugated graphene plane hexagonal structure further reduces impurities and defects inside the film, effectively improving the quality and performance of the graphene film. The thermal conductivity of the 10μm graphene heat dissipation film obtained by the present invention is 1801.07W / (m·K). The thermal conductivity is much higher than that of common metals Cu (400W / (m·K)), Al (237W / (m·K)) and Ag (429W / (m·K)). It has very good commercial prospects. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 This is a schematic diagram of a graphene oxide film photo;

[0020] Figure 2 This is a photo schematic of a graphene film that has been laser processed and pressed. DETAILED DESCRIPTION

[0021] The present invention will be further described below in conjunction with the embodiments and the accompanying drawings, but is not limited thereto.

[0022] Example 1

[0023] A two-step method for manufacturing a large-area graphene heat dissipation film comprises:

[0024] Preparation of graphene oxide film: preparing a graphene oxide dispersion, placing the prepared graphene oxide dispersion in a mold of a certain shape, and performing demoulding treatment at low temperature;

[0025] Preparation of graphene film: pre-annealing the graphene oxide film; and further treating the pre-annealed graphene oxide film using laser scanning to remove oxygen-containing groups, restore the conjugated structure of graphene, and obtain a low-defect graphene film;

[0026] The obtained graphene film is pressed to obtain a large-area graphene heat dissipation film.

[0027] Example 2

[0028] The two-step method for manufacturing a large-area graphene heat dissipation film according to Example 1 is different in that:

[0029] The preparation of the graphene oxide solution comprises: adding a certain volume of concentrated sulfuric acid into a beaker, cooling in an ice water bath, sequentially adding graphite, sodium nitrate and potassium permanganate, controlling the reaction temperature, and finally adding 30% hydrogen peroxide to terminate the reaction after the reaction is completed, followed by precipitation, washing and other operations to obtain a graphene oxide colloidal solution;

[0030] In this embodiment, a certain volume of concentrated sulfuric acid is poured into a beaker, the beaker is placed in an ice water bath to cool, then expanded graphite and sodium nitrate are added, and after stirring for a period of time, potassium permanganate is added, and the temperature is controlled at 0-8°C, and the reaction time is 1h; specifically, the amount of concentrated sulfuric acid is 400mL, the mass of graphite is 10g, the mass of sodium nitrate is 7.5g, and the mass of potassium permanganate is 30g. Subsequently, it is heated at 30-45°C for 1h; 600-1200mL of dilute sulfuric acid with a mass fraction of 5% is added to the solution, and the reaction is continued at 90-99°C for 1h. Finally, 20-50mL of hydrogen peroxide (30%) is added to terminate the reaction. The solution is placed at room temperature to sink, and washed with deionized water to neutrality to obtain a graphene oxide colloidal solution.

[0031] The preparation of graphene oxide dispersion includes: dispersing graphene oxide colloidal solution into deionized water, and obtaining uniform large-scale graphene oxide solution after ultrasonic treatment;

[0032] Use low temperature for demoulding; including:

[0033] The mold containing graphene oxide dispersion is dried on an electric furnace to form a film, and then liquid nitrogen is slowly poured into the mold to separate the graphene oxide film from the substrate. Specifically, it includes:

[0034] Assemble the mold (made of aluminum plate), then clean and dry the mold with isopropanol and ethanol in turn, then add 10-50mL of solution to the pre-heated mold at a heating temperature of 50-100°C. After the solution forms a film, remove the mold from the electric heating table, cool it to room temperature, add liquid nitrogen, wait for the thin substrate to detach, and remove it. Figure 1 The graphene oxide film with good flexibility is shown. The metal mold can not only act as a substrate, but also play a role in the initial reduction of the graphene oxide film. The side in direct contact with the metal substrate has obvious metallic luster.

[0035] The material of the mold of a certain shape can be metal, plastic or other materials. Metal materials (such as copper, zinc and aluminum, etc.) have certain reducing properties, and can perform preliminary reduction of graphene oxide, and dope certain metal ions in the obtained film, so as to prepare a composite graphene film. If plastic materials are used, a pure graphene-based film can be prepared.

[0036] The size and shape of the mold can be selected according to different application fields, so as to prepare graphene functional films of different sizes and shapes. In addition, there is no strict requirement for the thickness of the mold. For example, in a metal mold, either a thick aluminum plate or a thin aluminum foil can be used.

[0037] After the graphene oxide film is prepared, the substrate is cleaned with isopropanol and ethanol and dried. It can be used for the preparation of the next film, realizing the recycling of the substrate.

[0038] Preparation of graphene film, including:

[0039] The obtained film was pretreated by annealing at 1000°C for 2h in an Ar / H2 atmosphere, and then the graphene oxide film was laser treated using ReniShaw RenAM 500E. The laser power used was 1-20W and the laser scanning speed was 0.8-2.0m / s. By changing the number of scans, the graphene oxide film was deoxygenated, the conjugated structure of graphene was restored, and the deep reduction of graphene was achieved. Figure 2 This is a photo of a graphene film that has been laser treated and pressed.

[0040] The obtained film was hydraulically treated to eliminate internal bubbles. The thermal diffusivity of three films with different thicknesses was tested by laser flash method, and the calculated thermal conductivity is shown in Table 1 below.

[0041] Table 1

[0042]

[0043] When the film thickness is 20 and 10 microns, the measured thermal conductivity is much higher than that of common metals Cu (400W / (m·K)), Al (237W / (m·K)) and Ag (429W / (m·K)). Moreover, the prepared film has very good flexibility. This method is very simple to operate, and the size of the substrate can be changed as needed. Large-area films can be prepared, and the substrate used can be recycled repeatedly. It has a high degree of industrialization and shows great application prospects in the fields of heat dissipation, electromagnetic shielding and flexible electronic devices.

Claims

1. A two-step method for preparing a large-area graphene heat dissipation film, characterized in that: include: Preparation of graphene oxide film: preparing a graphene oxide dispersion, placing the prepared graphene oxide dispersion in a mold, and performing demoulding treatment at low temperature; Preparation of graphene film: pre-annealing the graphene oxide film; and further treating the pre-annealed graphene oxide film using laser scanning to remove oxygen-containing groups, restore the conjugated structure of graphene, and obtain a low-defect graphene film; The obtained graphene film is pressed to obtain a large-area graphene heat dissipation film.

2. The method for preparing a large-area graphene heat dissipation film by a two-step method according to claim 1, characterized in that: Use low temperature for demoulding; including: The mold containing the graphene oxide dispersion is dried on an electric furnace to form a film, and then liquid nitrogen is slowly poured into the mold to separate the graphene oxide film from the substrate.

3. The two-step method for preparing a large-area graphene heat dissipation film according to claim 2, characterized in that: The heating temperature of the electric furnace is 50-100°C.

4. The method for preparing a large-area graphene heat dissipation film by two steps according to claim 1, characterized in that: After the graphene oxide film was prepared, the substrate was cleaned with isopropanol and ethanol and dried.

5. The two-step method for preparing a large-area graphene heat dissipation film according to claim 1, characterized in that: The graphene oxide film is pre-annealed at a temperature of 1000°C.

6. A two-step method for preparing a large-area graphene heat dissipation film according to any one of claims 1 to 5, characterized in that: The obtained graphene oxide film is subjected to laser scanning treatment using a laser light source with a laser aperture of 50 microns, the laser power density is 1-20 W, and the laser scanning speed is 0.8-2.0 m / s.

Citation Information

Patent Citations

  • Graphene thin film, graphene super capacitor and preparation method of graphene thin film and graphene super capacitor

    CN104944414A

  • Method for preparing functional graphene film with heterostructure through one-step laser reduction

    CN107161990A

  • Laser reduced graphene film and preparation method thereof

    CN110723726A

  • Preparation method of ultrathin flexible graphene film

    CN114702030A

  • Method for manufacturing of graphene layer, method for manufacturing of touch device using the same

    KR1020130055111A