Monodisperse spherical micro / nano silicon dioxide as well as preparation method and application thereof
By combining high-concentration sodium silicate and crown ether, micro/nano silica with high sphericity and good dispersion is prepared using chemical precipitation method, which solves the problem of poor dispersion of micro/nano silica preparation methods in the existing technology. and the problem of high cost, it achieves high-performance and low-cost preparation effects, and is suitable for multiple high-end fields.
Patent Information
- Application Number
- CN202410841109.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-27
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2044-06-27
AI Technical Summary
Existing micro/nano silica preparation methods have problems such as poor product dispersion, poor performance, high cost, waste of resources, and environmental pollution, making it difficult to meet the needs of high-end applications.
Using high-concentration and cheap sodium silicate as the silicon source, the chemical precipitation method is combined with crown ether and sulfuric acid to adjust the pH value, and organic extraction and composite liquid precipitation reactions are used to prepare monodisperse spherical microorganisms with uniform particles, high sphericity, and good dispersion. /Nano silica.
It achieves the preparation of micro/nano silica with good particle size uniformity, reduces manufacturing costs, improves product dispersion and performance, and is suitable for aerospace, biomedicine, electronic packaging and other fields, with simple process and low cost. , suitable for mass production.
Smart Images

Figure CN118754140A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of inorganic non-metallic materials and nanometer materials, and in particular to monodisperse spherical micro / nano silicon dioxide and a preparation method and application thereof. Background Art
[0002] Silicon dioxide (SiO2) is a non-toxic, odorless, and pollution-free inorganic non-metallic material. Due to its low thermal expansion coefficient and excellent properties such as high heat resistance, high moisture resistance, high filling content, low dielectric constant, and low friction coefficient, it has broad application prospects in many fields such as aerospace, biomedicine, electronics, and electrical appliances.
[0003] At present, the commonly used preparation methods of micro / nano SiO2 include gas phase method, sol-gel method, microemulsion method and chemical precipitation method. The gas phase method mainly uses silicon tetrachloride as raw material to prepare SiO2. This method has the disadvantages of high reaction temperature, high equipment requirements, expensive raw materials and harsh operating conditions. The sol-gel method uses silicate as raw material and uses ammonia water as catalyst to synthesize SiO2 particles with good dispersibility (particle size 50-1000nm) in an ethanol-water binary solvent system. This method also has some disadvantages and problems, such as expensive raw materials, large-scale use of organic solvents, long preparation time, and unsuitability for large-scale production. The microemulsion method uses two immiscible solvents to form a microemulsion under the action of a surfactant, and prepares nano SiO2 in the oil phase of the microemulsion by controlling the reaction conditions. This method requires the consumption of a large amount of organic solvents, and the preparation process is relatively complicated. The chemical precipitation method mainly uses sodium silicate and inorganic acid as raw materials, and the silicate ions are precipitated by adjusting the pH value of the solution, and nano SiO2 is obtained through filtering, washing, drying and other steps. The advantages of this method are simple process, cheap raw materials and wide sources, but it also has disadvantages such as difficult to control product morphology and particle size, wide pore size distribution, easy formation of aggregated particles, etc. In addition, the concentration of a single batch of nanoparticles is low, resulting in high energy consumption for subsequent concentration.
[0004] In recent years, the research on the preparation of micro / nano SiO2 materials using sodium silicate as raw material has made great progress. Various compounds have been continuously applied to the preparation of micro / nano SiO2. The research direction is mainly focused on the morphology / morphology control, modification, selection of low-cost template agents, and simplification of synthesis methods of micro / nano SiO2. As described in Chinese patent CN113880098A, sodium silicate is sequentially removed from sodium ions by strong acid cation exchange resin and weak base anion exchange resin, and then hydrophobic trifluoromethanesulfonic acid anions are introduced to destroy the double electric layer structure to increase the crystallization activity of the colloid particle surface, and then the silicate polymerization rate of large particle size colloid particles is increased through secondary growth, and finally silicon micropowder is prepared. For example, Chinese patent CN104058415A discloses a method for preparing highly dispersed nano SiO2. By using surfactant sodium carboxymethyl cellulose and microporous membrane, the shortcomings of high surface energy of SiO2 and easy polymerization of silanol groups are overcome, and the dispersibility of the product is improved. Although the specific surface area of SiO2 prepared by this method is 80 to 300 m 2 / g, particle size is 10-35nm, but the dispersibility is poor, and still can not achieve a good application effect. Chinese patent CN111196606A uses oxidized polyethylene wax and polyethylene glycol as modifiers to modify SiO2 in turn, reducing the degree of polymerization between silicon dioxide to make it more evenly dispersed. Chinese patent CN1715183A uses cationic and nonionic surfactants as dual templates, and the obtained SiO2 particle size is 1-5μm, and the specific surface area is 800-1400m 2 / g, pore size is 2~5nm.
[0005] In summary, there are many methods for preparing micro / nano silica, but there are more or less problems such as poor product dispersibility, poor performance, and failure to meet high-end application requirements. In addition, the templates, dispersants, modifiers and other external reagents used or introduced in the current preparation methods are not only expensive, difficult to remove, and cannot be reused, but also cause waste of resources and environmental pollution. Summary of the invention
[0006] The main purpose of the present invention is to solve the above problems existing in the prior art and provide a new method for preparing monodisperse spherical micro / nano silicon dioxide. The method uses a high-concentration, cheap raw material, sodium silicate, as a silicon source and adopts a chemical precipitation method to prepare micro / nano-grade SiO2 with uniform particles, high sphericity, good dispersibility and controllable size, which completely solves the common problem of the difficulty in balancing the manufacturing cost and product quality of micro / nano SiO2, and ensures its wide application prospects in high-end fields such as aerospace, biomedicine, and electronic packaging.
[0007] In order to achieve the above-mentioned purpose and effect, the technical solution adopted by the present invention is as follows:
[0008] The invention provides a method for preparing monodisperse spherical micro / nano silicon dioxide, comprising: mixing a crown ether with a sodium silicate solution for reaction, extracting the obtained mixture with an organic extractant to obtain an aqueous phase and an organic phase, taking a portion of the aqueous phase and adjusting its pH to acidity as a base liquid, taking another portion of the aqueous phase and mixing it with an organic solvent as a composite liquid, mixing the base liquid and the composite liquid for precipitation reaction, and finally obtaining monodisperse spherical micro / nano silicon dioxide.
[0009] Specifically, the crown ether is selected from at least one of 21-crown-7, 18-crown-6, 15-crown-5 or their derivatives, wherein the derivatives include benzo-15-crown-5, R-benzo-15-crown-5, wherein R=CH3, NH2, NO2, etc., specifically Figure 1 shown.
[0010] Specifically, the modulus of the sodium silicate is 1.5-3.5. The larger the modulus of the sodium silicate, the more silicon dioxide content, the weaker the alkalinity, and the less inorganic acid consumed; conversely, the smaller the modulus of the sodium silicate, the stronger the alkalinity, and the more inorganic acid consumed.
[0011] Specifically, the molar ratio of crown ether to sodium silicate during mixing is 0.05 to 1:1.
[0012] More specifically, the specific process of the mixed reaction of crown ether and sodium silicate solution is as follows: prepare sodium silicate aqueous solution and crown ether aqueous solution respectively, then add the crown ether aqueous solution to the sodium silicate aqueous solution under stirring, and the resulting mixture is reacted at 20-80°C for 0.1-2h, and then the pH of the mixture is adjusted to 10.5-11.5 by dropping sulfuric acid solution, and the stirring reaction is continued for 1-2h.
[0013] More specifically, the mass fraction of the prepared sodium silicate aqueous solution is 3%-20%, and the concentration of the prepared crown ether aqueous solution is 1-32 mol / L.
[0014] Specifically, the organic extractant is selected from at least one of solvents such as dichloromethane, chloroform, ethyl acetate, ether, toluene, and xylene.
[0015] Specifically, a sulfuric acid solution is added dropwise to the aqueous phase obtained by extraction, and the pH of the mixture is adjusted to 8.5-10.5 to obtain a bottom liquid.
[0016] More specifically, the mass fraction of the sulfuric acid solution is 0.5%-39%.
[0017] Specifically, the organic solvent is an alcohol solvent, selected from at least one of methanol, ethanol, propanol and isopropanol.
[0018] Specifically, when preparing the composite liquid, the volume ratio of the aqueous phase to the organic solvent is 1-10:1.
[0019] Specifically, the volume ratio of the base liquid to the composite liquid when mixed is 1:8-16.
[0020] Specifically, the reaction temperature after the base liquid and the composite liquid are mixed is 20-80°C, the reaction time is 1-3h, the supernatant is removed by centrifugation after the reaction, the obtained solid precipitate is washed with water until the supernatant is neutral, and then dried and baked to obtain monodisperse spherical micro / nano SiO2.
[0021] Specifically, the crown ether in the organic phase obtained by extraction is recovered and reused. The specific process is as follows: the organic phase is placed in a closed container and heated to 35-100° C., and the organic extractant is removed by vacuum distillation (recovered and reused after cooling), the obtained solid is dissolved in water and then adsorbed with a cation exchange resin, and the crown ether aqueous solution thus obtained is mixed with a sodium silicate solution for reaction again.
[0022] The present invention also provides a monodisperse spherical micro / nano silicon dioxide prepared according to the above method, which has a size of 20nm-1300nm and a specific surface area of 50-600m 2 / g.
[0023] In addition, the present invention also provides the application of the above-mentioned monodisperse spherical micro / nano silicon dioxide in the fields of aerospace, biomedicine, electronic packaging, etc. Compared with traditional brake materials, silicon dioxide has higher heat resistance, wear resistance and processing performance. It is widely used in aircraft brake systems in the field of aerospace, and can significantly improve the reliability and life of brakes. In the field of biomedicine, silicon dioxide microspheres can be used for drug delivery, diagnosis, biomarkers, imaging agents, nanocarriers, etc., providing more help for the diagnosis and treatment of diseases. In the field of electronic packaging, high-purity spherical micro / nano SiO2 has superior properties such as high dielectric, low expansion, and low friction coefficient, and is the main raw material required for large-scale and ultra-large-scale integrated circuit packaging. At present, most electronic packaging materials at home and abroad are polymers, among which epoxy resin is the most widely used, but the high water absorption and viscosity of epoxy resin limit its application in ultra-large-scale integrated circuits. Studies have shown that adding 70% to 90% of high-purity silicon dioxide powder to epoxy resin can effectively reduce the thermal expansion coefficient, water absorption, internal stress, shrinkage rate of the plastic packaging material and improve its thermal conductivity.
[0024] The principle of the present invention is as follows: sodium silicate is used as a raw material, and the pH value of the system is adjusted by using an inorganic acid. After adding a macrocyclic crown ether compound, it selectively forms a complex with the sodium ions in the solution. After a simple solvent extraction, the sodium ions can be transferred from the aqueous phase to the organic phase. The crown ether in the organic phase can be recycled and reused through subsequent processes. The obtained aqueous phase is divided into two parts. A portion of the aqueous phase solution is taken to continue to add an appropriate amount of inorganic acid. The resulting silicic acid solution (this is the seed solution) can be polymerized and grown into primary nanoparticles, which is used as a base liquid for the subsequent preparation of larger nanoparticles. A suitable organic solvent is added to the other part of the aqueous phase to prepare a composite liquid, and the composite liquid is added to the base liquid. The silicate concentration in the system is regulated by controlling the volume ratio of the composite liquid to the base liquid to avoid secondary / multiple nucleation in the system, and finally a monodisperse spherical micro / nano silica with good particle size uniformity is prepared. The reactions involved in the process are as follows:
[0025] Na2·nSiO2+H + →2Na + +nSiO2+H2O
[0026] The present invention gives full play to the inherent advantages of the chemical precipitation method, such as low raw material prices, and selects organic macrocyclic compound crown ether as a complexing agent to control the solution ion strength and stabilize nano micelles, thereby solving the problems commonly existing in the chemical precipitation method, such as difficult control of product morphology and particle size, easy formation of aggregate particles, and low concentration leading to high energy consumption for subsequent concentration, thereby realizing the preparation of low-cost, high-quality silicon dioxide micro / nano particles. The SiO2 micro / nano particles prepared according to the method of the present invention have many advantages, such as high production intensity, high sphericity, uniform particle size, good dispersibility, etc., and have high economic and practical value in many fields such as aerospace, biomedicine, and electronic packaging.
[0027] The present invention comprehensively considers the influence of sodium silicate solution nucleation, growth mechanism, solution ion strength and other factors on the growth of spherical particles, as well as the dispersibility of SiO2 in different solvents, and proposes a new method for preparing monodisperse spherical SiO2 micro / nano particles using organic macrocyclic compounds as complexing agents and high-concentration and cheap sodium silicate as raw materials. The particle size of the product is between 20-1300nm and is adjustable and controllable. The present invention utilizes the complexation of organic macrocyclic compounds and sodium ions to avoid the destruction of the double electric layer on the surface of silicon microspheres by excessive free sodium ions, reduces the collision and adhesion phenomenon between particles, thereby promoting the growth of spherical particles, and can also greatly increase the concentration of raw material sodium silicate in a single feed.
[0028] Compared with the prior art, the present invention has achieved the following beneficial technical effects:
[0029] (1) The present invention can prepare micro / nano-scale SiO2 using high-concentration and low-cost sodium silicate (single feed concentration up to 20%) as a silicon source, and the product has uniform particle size, high sphericity, good dispersibility, and the particle size is flexibly adjustable within the range of 20 to 1300 nm;
[0030] (2) The present invention proposes for the first time to adjust the ionic strength of the reaction system by adding an organic complexing agent, thereby accurately controlling the growth of spherical SiO2 particles, and the added complexing agent can be recycled and reused after simple chemical treatment;
[0031] (3) The method of the present invention has stable process conditions, does not involve high temperature, high pressure and expensive equipment, and has many advantages such as simple production process, easy operation, low cost, high yield, and easy large-scale industrial production. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 Schematic diagram of the chemical structure of each crown ether in the present invention.
[0033] Figure 2 This is a transmission electron microscope (TEM) photograph of the spherical silica nanoparticles prepared in Example 11.
[0034] Figure 3 This is a dynamic light scattering (DLS) photograph of the spherical silica nanoparticles prepared in Example 12.
[0035] Figure 4 This is a DLS photograph of the spherical silica nanoparticles prepared in Example 14.
[0036] Figure 5 This is a scanning electron microscope (SEM) photograph of the spherical silica nanoparticles prepared in Example 15.
[0037] Figure 6 This is a SEM photograph of spherical silica nanoparticles prepared in Example 16. DETAILED DESCRIPTION
[0038] In order to enable ordinary technicians in the field to fully understand the technical solutions and beneficial effects of the present invention, the following is further described in conjunction with specific embodiments and drawings. It should be noted that the following embodiments are only partial implementation methods of the present invention, and other implementation methods derived on the basis of not departing from the main purpose of the present invention should fall within the scope of protection of the present invention.
[0039] Example 1
[0040] (1) A certain amount of sodium silicate is dissolved in 100 mL of deionized water to obtain a sodium silicate solution with a mass fraction of 15%. 0.04 mol of 15-crown ether-5 is dissolved in 5 mL of water to obtain a crown ether aqueous solution with a concentration of 8 mol / L. The prepared crown ether aqueous solution is added to the sodium silicate solution under stirring (110-120 r / min), and reacted at 20° C. for 1 h to obtain a first solution.
[0041] (2) The first solution was transferred to a round-bottom flask, the stirring speed (110-120 r / min) and the reaction temperature (20°C) were kept constant, and an appropriate amount of sulfuric acid solution (mass fraction of 25%) was added to the flask, and the pH value of the system was controlled to be maintained in the range of 10.5-11.5. After reacting for 2 hours, a second solution was obtained. 25 mL of dichloromethane was added to the second solution and stirred evenly. After standing for stratification, the liquids were separated to obtain an aqueous phase solution and an organic phase solution, respectively.
[0042] (3) Measure 10 mL of the aqueous phase solution and add it to a round-bottom flask. Add sulfuric acid solution (mass fraction 6.5%) to the flask while stirring (290-300 r / min). Control the pH of the system to be maintained in the range of 9.5-10.5. React at 20°C for 30 min to obtain a base solution. Measure 80 mL of the aqueous phase solution and 10 mL of anhydrous methanol and mix them evenly to obtain a composite solution. Add all of the composite solution to the base solution, stir and react at 20°C for 1 h to obtain a nano-SiO2 dispersion.
[0043] (4) The nano-SiO2 dispersion was centrifuged, the supernatant was removed and then repeatedly washed with water until the supernatant was neutral, and then the solid precipitate was dried and baked in a step-by-step manner to obtain monodisperse spherical nano-SiO2. The test results showed that the average particle size was 212 nm.
[0044] (5) The organic phase solution obtained by the extraction and separation in step (2) is placed in a sealed container, heated to 45° C. and distilled under reduced pressure to remove dichloromethane. The obtained product is dispersed with water and then passed through a cation exchange resin to obtain a regenerated crown ether aqueous solution, which can be reused in step (1) after adjusting the solution concentration, thereby achieving a cycle.
[0045] Embodiment 2-9
[0046] With reference to the preparation method of Example 1, Examples 2-9 were carried out by changing key conditions such as the type of crown ether and the feed ratio of crown ether to sodium silicate. The specific conditions are shown in Table 1 below.
[0047] Table 1 Comparison of process conditions for Examples 2-9
[0048]
[0049] Examples 1-9 show that nano-silica of different sizes can be prepared by introducing different types of crown ethers. The particle size of nano-silica can be controlled by adjusting the feed ratio of crown ether to sodium silicate and temperature-related parameters, and the particle size range is 100-600 nm.
[0050] Example 10
[0051] (1) A certain amount of sodium silicate is dissolved in 100 mL of deionized water to obtain a sodium silicate solution with a mass fraction of 3%. 0.012 mol of 21-crown ether-7 is dissolved in 5 mL of water to obtain a crown ether aqueous solution with a concentration of 2.4 mol / L. The prepared crown ether aqueous solution is added to the sodium silicate solution under stirring (110-120 r / min), and reacted at 80° C. for 30 min to obtain a first solution.
[0052] (2) The first solution was transferred to a round-bottom flask, the stirring speed (110-120 r / min) and the reaction temperature (80°C) were kept constant, and an appropriate amount of sulfuric acid solution (mass fraction of 25%) was added to the flask, and the pH value of the system was controlled to be maintained in the range of 10.5-11.5. After reacting for 2 hours, a second solution was obtained. 25 mL of dichloromethane was added to the second solution and stirred evenly. After standing for stratification, the liquids were separated to obtain an aqueous phase solution and an organic phase solution, respectively.
[0053] (3) 10 mL of the aqueous phase solution was measured and added to a round-bottom flask. Sulfuric acid solution (mass fraction: 6.5%) was added dropwise to the flask while stirring (290-300 r / min). The pH of the system was controlled to be maintained in the range of 9.5-10.5. The mixture was reacted at 80°C for 1 h to obtain a base solution. 80 mL of the aqueous phase solution and 10 mL of anhydrous methanol were measured and mixed uniformly to obtain a composite solution. The composite solution was added to the base solution, and the mixture was stirred and reacted at 80°C for 2 h to obtain a nano-SiO2 dispersion.
[0054] (4) The nano-SiO2 dispersion was centrifuged, the supernatant was removed and then repeatedly washed with water until the supernatant was neutral, and then the solid precipitate was dried and baked in a step-by-step manner to obtain monodisperse spherical nano-SiO2. The test results showed that the average particle size was 30 nm.
[0055] (5) The organic phase solution obtained by extraction and separation in step (2) is placed in a sealed container, heated to 45° C. and distilled under reduced pressure to remove dichloromethane, the obtained product is dissolved in water and passed through a cation exchange resin to obtain a regenerated crown ether aqueous solution, and the solution concentration is adjusted and reused in step (1), thereby achieving a cycle.
[0056] Examples 11-14
[0057] With reference to the preparation method of Example 10, Examples 11-14 were carried out by changing key conditions such as the type of crown ether and the concentration of sodium silicate. The specific conditions are shown in Table 2 below.
[0058] Table 2 Comparison of process conditions for Examples 11-14
[0059]
[0060] Examples 10-14 show that, under the same other conditions, by adjusting the crown ether type, sodium silicate mass fraction (1-5%), reaction time and other related parameters, small-particle nano-SiO2 with good dispersibility and high particle size uniformity can be prepared. The particle size of these particles is between 20-200nm. Figure 2-4 shown.
[0061] Embodiment 15
[0062] (1) A certain amount of sodium silicate is dissolved in 100 mL of deionized water to obtain a sodium silicate solution with a mass fraction of 20%. 0.12 mol of 15-crown-5 is dissolved in 5 mL of water to obtain a crown ether aqueous solution with a concentration of 24 mol / L. The prepared crown ether aqueous solution is added to the sodium silicate solution under stirring (110-120 r / min), and reacted at 50° C. for 30 min to obtain a first solution.
[0063] (2) The first solution was transferred to a round-bottom flask, the stirring speed (110-120 r / min) and the reaction temperature (50°C) were kept constant, and an appropriate amount of sulfuric acid solution (mass fraction of 25%) was added to the flask, and the pH value of the system was controlled to be maintained in the range of 10.5-11.5. After reacting for 2 hours, a second solution was obtained. 25 mL of ethyl acetate was added to the second solution and stirred evenly. After standing for stratification, the liquids were separated to obtain an aqueous phase solution and an organic phase solution, respectively.
[0064] (3) Measure 10 mL of the aqueous phase solution and add it to a round-bottom flask. Add sulfuric acid solution (mass fraction: 39%) to the flask while stirring (290-300 r / min). Control the pH of the system to be maintained in the range of 9.5-10.5. React at 50°C for 1 h to obtain a base solution. Measure 80 mL of the aqueous phase solution and 30 mL of isopropanol and mix them evenly to obtain a composite solution. Add all of the composite solution to the base solution, stir and react at 50°C for 3 h to obtain a nano-SiO2 dispersion.
[0065] (4) The nano-SiO2 dispersion is centrifuged, the supernatant is removed, and the mixture is repeatedly washed with water until the supernatant is neutral. The solid precipitate is then dried and baked in a stepwise manner to obtain monodisperse spherical nano-SiO2.
[0066] (5) The organic phase solution obtained by extraction and separation in step (2) is placed in a sealed container, heated to 45° C. and distilled under reduced pressure to remove dichloromethane, the obtained product is dissolved in water and passed through a cation exchange resin to obtain a regenerated crown ether aqueous solution, and the solution concentration is adjusted and reused in step (1), thereby achieving a cycle.
[0067] The SEM photo of the nano-SiO2 prepared in this embodiment is as follows: Figure 5 As shown in the figure, it can be seen that the SiO2 particles are regular spherical, without obvious agglomeration, and the average particle size of the particles is 620nm.
[0068] Example 16
[0069] (1) A certain amount of sodium silicate is dissolved in 100 mL of deionized water to obtain a sodium silicate solution with a mass fraction of 15%. 0.12 mol of 18-crown-6 is dissolved in 5 mL of water to obtain a crown ether aqueous solution with a concentration of 24 mol / L. The prepared crown ether aqueous solution is added to the sodium silicate solution under stirring (110-120 r / min), and reacted at 50° C. for 30 min to obtain a first solution.
[0070] (2) The first solution was transferred to a round-bottom flask, the stirring speed (110-120 r / min) and the reaction temperature (50°C) were kept constant, and an appropriate amount of sulfuric acid solution (mass fraction of 25%) was added to the flask, and the pH value of the system was controlled to be maintained in the range of 10.5-11.5. After reacting for 2 hours, a second solution was obtained. 25 mL of ethyl acetate was added to the second solution and stirred evenly. After standing for stratification, the liquids were separated to obtain an aqueous phase solution and an organic phase solution, respectively.
[0071] (3) Measure 10 mL of the aqueous phase solution and add it to a round-bottom flask. Add sulfuric acid solution (mass fraction 39%) to the flask while stirring (290-300 r / min). Control the pH of the system to be kept in the range of 8.5-9.5. React at 50°C for 1 h to obtain a base solution. Measure 80 mL of the aqueous phase solution and 30 mL of isopropanol and mix them evenly to obtain a composite solution. Add all of the composite solution to the base solution, stir and react at 50°C for 3 h to obtain a nano-SiO2 dispersion.
[0072] (4) The nano-SiO2 dispersion is centrifuged, the supernatant is removed, and the mixture is repeatedly washed with water until the supernatant is neutral. The solid precipitate is then dried and baked in a stepwise manner to obtain monodisperse spherical nano-SiO2.
[0073] (5) The organic phase solution obtained by extraction and separation in step (2) is placed in a sealed container, heated to 45° C. and distilled under reduced pressure to remove dichloromethane, the obtained product is dissolved in water and passed through a cation exchange resin to obtain a regenerated crown ether aqueous solution, and the solution concentration is adjusted and reused in step (1), thereby achieving a cycle.
[0074] The SEM photo of the monodisperse spherical nano-SiO2 prepared in this example is as follows: Figure 6 As shown in the figure, it can be seen that the SiO2 particles are regular spherical, without obvious agglomeration, and the average particle size of the particles is 1134 μm.
Claims
1. A method for preparing monodisperse spherical micro / nano silicon dioxide, Features The method is specifically as follows: crown ether and sodium silicate solution are mixed for reaction, the obtained mixture is extracted with an organic extractant to obtain an aqueous phase and an organic phase, a portion of the aqueous phase is taken to adjust its pH to acidity to obtain a base liquid, another portion of the aqueous phase is taken and mixed with an organic solvent to obtain a composite liquid, the base liquid and the composite liquid are mixed for precipitation reaction, and solid-liquid separation is performed to obtain monodisperse spherical micro / nano silica.
2. The preparation method according to claim 1, Features: The crown ether is selected from at least one of 21-crown-7, 18-crown-6, 15-crown-5 or derivatives thereof, and the derivatives include benzo-15-crown-5, R-benzo-15-crown-5, wherein R=CH 3 NH 2 、NO 2 The organic extractant used in the extraction is selected from at least one of dichloromethane, chloroform, ethyl acetate, ether, toluene, and xylene, and the organic solvent used in the preparation of the composite liquid is specifically an alcohol solvent, selected from at least one of methanol, ethanol, propanol, and isopropanol.
3. The preparation method according to claim 1, Features: The modulus of the sodium silicate is 1.5-3.5, and the molar ratio of the crown ether to the sodium silicate during mixing is 0.05-1:
1.
4. The preparation method according to claim 1, Features The specific process of the mixed reaction of the crown ether and the sodium silicate solution is as follows: prepare a sodium silicate aqueous solution and a crown ether aqueous solution respectively, then add the crown ether aqueous solution to the sodium silicate aqueous solution under stirring, and the resulting mixture is fully reacted at 20-80° C., then sulfuric acid solution is added dropwise to adjust the pH of the mixture to 10.5-11.5, and the stirring reaction is continued.
5. The preparation method according to claim 4, Features: The mass fraction of the prepared sodium silicate aqueous solution is 3%-20%, and the concentration of the prepared crown ether aqueous solution is 1-32 mol / L.
6. The preparation method according to claim 1, Features: A sulfuric acid solution is added dropwise to the aqueous phase obtained by extraction, and the pH of the mixture is adjusted to 8.5-10.5 to obtain a base liquid; when preparing the composite liquid, the volume ratio of the aqueous phase to the organic solvent is 1-10:
1.
7. The preparation method according to claim 1, Features: The volume ratio of the base liquid to the composite liquid is 1:8-16, and the reaction temperature after mixing is 20-80°C. After the reaction, the solid obtained by centrifugation is washed with water until neutral, and then dried and baked to obtain monodispersed spherical micro / nano SiO 2 .
8. The preparation method according to claim 1, Features: The organic phase obtained by extraction is placed in a sealed container, heated to 35-100°C and distilled under reduced pressure to recover the organic extractant. The obtained solid is dissolved in water and then adsorbed by a cation exchange resin. The obtained crown ether aqueous solution is mixed with a sodium silicate solution for reaction again.
9. A monodisperse spherical micro / nano silica, Features: The size of the silica is 20nm-1300nm and the specific surface area is 50-600m 2 / g.
10. Application of the monodisperse spherical micro / nano silicon dioxide according to claim 9 in aerospace, biomedicine, and electronic packaging.
Citation Information
Patent Citations
Large-pore-wall cage-shaped silica hollow sphere and preparation method thereof
CN102381715A
Monodisperse silica nanoparticles and preparation method thereof
CN103896284A
Silica macropore particle, method for producing the same, and application thereof
JP2006273667A
Crown ether functionalized silica, manufacturing method thereof, use as lithium ion adsorbent and collecting method for lithium ions using same