Method for producing aluminum oxide in reverse two stages and aluminum oxide

Through the reverse two-stage production of alumina, through the reaction and adsorption treatment of saturated sodium aluminate semen and aluminum hydroxide, the problems of high wear index and low decomposition rate of alumina products are solved, and high strength, low wear and high Alumina products with high decomposition rate are suitable for aluminum electrolysis raw materials.

CN118754175APending Publication Date: 2024-10-11ZHENGZHOU NON FERROUS METALS RES INST CO LTD OF CHALCO
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411014445.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-26
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

In the current alumina production technology, the abrasion index of alumina products is high, which affects its strength and fine particle content during transportation and loading. Moreover, the decomposition rate of aluminum hydroxide is insufficient, making it difficult to increase the particle size and strength in a short time.

Method used

Adopting a reverse two-stage method to produce alumina, through the seed growth reaction of saturated sodium aluminate semen and crude aluminum hydroxide seeds and the seed adsorption reaction of fine aluminum hydroxide seeds, separation and washing, and combined roasting to obtain High-strength, coarse-grained alumina products control the particle size distribution and impurity content, and extend the decomposition time to increase the decomposition rate.

Benefits of technology

Significantly reduce the wear index of alumina products, increase the decomposition rate and particle size of aluminum hydroxide, and ensure the high strength and low wear characteristics of alumina products. It is suitable for aluminum electrolysis raw materials and has large specific surface area, small dust, good dissolution performance and energy saving. and other characteristics.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118754175A_ABST
    Figure CN118754175A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of aluminum oxide production, in particular to a method for producing aluminum oxide in a reverse two-stage mode and aluminum oxide. The method comprises the following steps: carrying out a seed crystal growth reaction on saturated sodium aluminate fine liquid and coarse aluminum hydroxide seed crystal, and then separating to obtain a coarse aluminum hydroxide filter cake and a coarse aluminum hydroxide separation liquid; washing part of the coarse aluminum hydroxide filter cake to obtain a first aluminum hydroxide product; carrying out an adsorption reaction on the coarse aluminum hydroxide separation liquid and the fine aluminum hydroxide seed crystal, and then grading to obtain an underflow product and an overflow product; separating and washing the underflow product to obtain a second aluminum hydroxide product; combining the two aluminum hydroxide products, and roasting to obtain an aluminum oxide product; and filtering the overflow product to obtain the overflow fine seed crystal. According to the method, a seed crystal growth reaction is used as a first stage to reduce the wear index of aluminum oxide, and a seed crystal adsorption reaction is used as a second stage, so that the impurity content in a production system can be reduced, and the seed crystal decomposition rate is increased.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of alumina production, and in particular to a method for producing alumina in two stages and alumina. Background Art

[0002] Industrially produced alumina needs to have certain physical properties, such as specific surface area, α-A12O3 content, angle of repose, particle size and wear index. Among these physical properties, specific surface area, α-A12O3 content and angle of repose mainly depend on the roasting conditions, while particle size and wear index mainly depend on the particle size and strength of the original aluminum hydroxide. Therefore, in order to improve the particle size and strength of alumina, it is necessary to first obtain aluminum hydroxide raw materials with coarser particle size and greater strength. At this stage, the raw materials of aluminum hydroxide mainly come from the decomposition of sodium aluminate solution. After roasting, the aluminum hydroxide obtained by these decompositions can remove the attached water and crystal water of aluminum hydroxide. In addition, aluminum hydroxide will also undergo a certain degree of crystal transformation, and the particle size and strength of the alumina product will also change. The greater the strength of alumina, the smaller the wear index of alumina. The alumina with a small wear index will have less fine particle content due to impact and wear during transportation and loading and unloading.

[0003] At present, the alumina production technology mainly includes one-stage sand-like alumina production technology and two-stage sand-like alumina production technology. Although both methods can produce coarse-grained sand-like alumina, the decomposition time of these two methods is about 45 hours. During the long decomposition process, the alumina seeds will be broken and severely corroded in the later stage of decomposition, which will significantly reduce the strength of the alumina product and increase the wear index of the alumina product. For example, the wear index of the traditional one-stage sand-like alumina is as high as 20% to 25%, and the wear index of the traditional two-stage sand-like alumina is as high as 15% to 20%; however, if the decomposition time is directly shortened, it is not conducive to improving the decomposition rate of aluminum hydroxide. Summary of the invention

[0004] The present application provides a method for producing alumina in two stages and alumina to solve the following technical problem: how to reduce the wear index of alumina products while increasing the decomposition rate of aluminum hydroxide.

[0005] In a first aspect, the present application provides a method for producing alumina in two stages, the method comprising:

[0006] Carrying out a seed growth reaction between saturated sodium aluminate concentrate and crude aluminum hydroxide seed crystals to obtain an aluminum hydroxide slurry having a first preset solid content;

[0007] Separating the aluminum hydroxide slurry having a first preset solid content to obtain a crude aluminum hydroxide filter cake and a crude aluminum hydroxide separated liquid, respectively;

[0008] washing a portion of the crude aluminum hydroxide filter cake to obtain a first aluminum hydroxide product;

[0009] The crude aluminum hydroxide separated liquid is subjected to a seed adsorption reaction with fine aluminum hydroxide seed crystals to obtain an aluminum hydroxide slurry having a second preset solid content;

[0010] Performing cyclone classification on the aluminum hydroxide slurry having a second preset solid content to obtain an underflow product and an overflow product respectively;

[0011] Separating and washing the underflow product to obtain a second aluminum hydroxide product;

[0012] Combining the first aluminum hydroxide product and the second aluminum hydroxide product to obtain a crude aluminum hydroxide product;

[0013] calcining the crude aluminum hydroxide product to obtain an aluminum oxide product;

[0014] filtering the overflow product to obtain overflow fine seeds;

[0015] Wherein, the fine aluminum hydroxide seeds include the overflow fine seeds, and the coarse aluminum hydroxide seeds include the remaining coarse aluminum hydroxide filter cake;

[0016] The mass ratio of the content of aluminum hydroxide seeds with a particle size of less than 45 μm in the crude aluminum hydroxide seeds to the crude aluminum hydroxide seeds is ≤0.15; the mass ratio of the content of aluminum hydroxide seeds with a particle size of less than 45 μm in the fine aluminum hydroxide seeds to the fine aluminum hydroxide seeds is ≤0.40; the mass ratio of part of the crude aluminum hydroxide filter cake to the remaining crude aluminum hydroxide filter cake is 1:(5-10); the mass ratio of the seeds in the underflow product to the seeds in the overflow product is 1:(2-5); the mass ratio of the first aluminum hydroxide product to the second aluminum hydroxide product is (3-8):1.

[0017] Optionally, the first preset solid content is 600 g / L to 900 g / L, and the second preset solid content is 150 g / L to 350 g / L.

[0018] Optionally, the time for the seed crystal growth reaction is 25 h to 35 h, and the time for the seed crystal adsorption reaction is 15 h to 20 h.

[0019] Optionally, the molecular ratio of the saturated sodium aluminate semen is 1.40-1.50.

[0020] Optionally, the molecular ratio of the endpoint solution of the seed crystal growth reaction is 2.4 to 2.6, and the molecular ratio of the endpoint solution of the seed crystal adsorption reaction is 2.8 to 3.2.

[0021] Optionally, the end point temperature T2 of the seed growth reaction satisfies:

[0022] T2 = T1 - t1,

[0023] Wherein, T1 is the initial temperature of the seed growth reaction, and t1 is the first temperature drop amplitude;

[0024] The initial temperature of the seed crystal growth reaction is 58°C to 65°C, and the first temperature reduction range is 10°C to 15°C.

[0025] Optionally, the end point temperature T3 of the seed adsorption reaction satisfies:

[0026] T3 = T2 - t2,

[0027] Wherein, T2 is the end temperature of the seed growth reaction, and t2 is the second temperature reduction amplitude;

[0028] The second temperature reduction range is 1°C to 2°C.

[0029] Optionally, the mass ratio of the content of oxalate in the aluminum hydroxide product to the aluminum hydroxide is less than 0.0005;

[0030] The mass ratio of the content of aluminum hydroxide with a particle size of less than 45 μm in the aluminum hydroxide product to the aluminum hydroxide product is less than 0.08.

[0031] In a second aspect, the present application provides an aluminum oxide, which is prepared by the method described in the first aspect, and the morphology of the aluminum oxide is an agglomerated mosaic aluminum oxide.

[0032] Optionally, the mass ratio of the content of alumina with a particle size of less than 45 μm in the alumina product to the alumina product is less than 0.10;

[0033] The wear index of the aluminum oxide is ≤12%.

[0034] The above technical solution provided by the embodiment of the present application has the following advantages compared with the prior art:

[0035] The present application provides a method for producing aluminum oxide in two stages, the method comprising:

[0036] A saturated sodium aluminate concentrate and crude aluminum hydroxide seeds are subjected to a seed growth reaction to obtain an aluminum hydroxide slurry with a first preset solid content; the aluminum hydroxide slurry with the first preset solid content is separated to obtain a crude aluminum hydroxide filter cake and a crude aluminum hydroxide separated liquid, respectively; a portion of the crude aluminum hydroxide filter cake is washed to obtain a first aluminum hydroxide product; the crude aluminum hydroxide separated liquid is subjected to a seed adsorption reaction with fine aluminum hydroxide seeds to obtain an aluminum hydroxide slurry with a second preset solid content; the aluminum hydroxide slurry with the second preset solid content is subjected to cyclone classification to obtain an underflow product and an overflow product, respectively; the underflow product is separated and washed to obtain a second aluminum hydroxide product; the first aluminum hydroxide product and the second aluminum hydroxide product are combined to obtain a coarse aluminum hydroxide product; the coarse aluminum hydroxide product The product is roasted to obtain an alumina product; the overflow product is filtered to obtain overflow fine seeds; wherein the fine aluminum hydroxide seeds include the overflow fine seeds, and the coarse aluminum hydroxide seeds include the remaining coarse aluminum hydroxide filter cake; the mass ratio of the aluminum hydroxide seeds with a particle size of less than 45 μm in the coarse aluminum hydroxide seeds to the coarse aluminum hydroxide seeds is ≤0.15; the mass ratio of the aluminum hydroxide seeds with a particle size of less than 45 μm in the fine aluminum hydroxide seeds to the fine aluminum hydroxide seeds is ≤0.40; the mass ratio of part of the coarse aluminum hydroxide filter cake to the remaining coarse aluminum hydroxide filter cake is 1:(5-10); the mass ratio of the seeds in the underflow product to the seeds in the overflow product is 1:(2-5); the mass ratio of the first aluminum hydroxide product to the second aluminum hydroxide product is (3-8):1. 。The method is based on a sand-like aluminum oxide production technology, uses coarse aluminum hydroxide seeds and saturated sodium aluminate concentrate to carry out a seed growth reaction, and the content of aluminum hydroxide seeds with a particle size of less than 45 μm in the coarse aluminum hydroxide seeds and the mass ratio of the coarse aluminum hydroxide seeds are ≤0.15, so that the coarse aluminum oxide seeds can overcome the interfacial tension between the saturated sodium aluminate solution and the aluminum hydroxide crystals, thereby promoting aluminum hydroxide in the saturated sodium aluminate concentrate to be continuously precipitated and adsorbed on the periphery of the coarse aluminum hydroxide seeds, thereby obtaining a high-strength and coarse-grained aluminum hydroxide product, and then uses fine aluminum hydroxide seeds to carry out a seed adsorption reaction on impurities in the aluminum hydroxide raw material solution, and the content of aluminum hydroxide seeds with a particle size of less than 45 μm in the fine aluminum hydroxide seeds and the mass ratio of the fine aluminum hydroxide seeds are ≤0.40, so that impurities can be prevented from entering the aluminum hydroxide product, and the seed adsorption reaction will delay the reaction. The decomposition time of the whole aluminum hydroxide is prolonged, thereby improving the decomposition rate of the system; in addition, the coarse aluminum hydroxide seeds include the remaining coarse aluminum hydroxide filter cake, and the mass ratio of part of the coarse aluminum hydroxide filter cake and the remaining coarse aluminum hydroxide filter cake is 1: (5-10), so as to promote the seed growth reaction to have sufficient coarse aluminum hydroxide seeds, and at the same time promote the recycling of saturated sodium aluminate semen, so as to improve the decomposition rate of the system; in addition, the fine aluminum hydroxide seeds include overflow fine seeds, and the mass ratio of the seeds in the underflow product and the overflow product is 1: (2-5), so as to promote the seed adsorption reaction to have sufficient fine aluminum hydroxide seeds, and at the same time promote the recycling of saturated sodium aluminate semen, so as to improve the decomposition rate of the system; in addition, the mass ratio of the first aluminum hydroxide product and the second aluminum hydroxide product is (3-8): 1, which can promote uniform particle size distribution in the aluminum hydroxide product, so as to increase the proportion of large particles in the aluminum hydroxide product. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate embodiments consistent with the present application and, together with the description, serve to explain the principles of the present application.

[0038] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative labor.

[0039] Figure 1 A schematic flow chart of a method for producing aluminum oxide in two stages provided in an embodiment of the present application;

[0040] Figure 2 A schematic diagram of the actual process of a method for producing aluminum oxide in two stages provided in an embodiment of the present application;

[0041] Figure 3A schematic flow chart of a method for producing aluminum oxide by a one-stage decomposition process provided in Comparative Example 1 of the present application;

[0042] Figure 4 A schematic diagram of the characterization structure of aluminum oxide provided in Example 1 of the present application;

[0043] Figure 5 A schematic diagram of the characterization structure of aluminum oxide provided for Comparative Example 1 of the present application. DETAILED DESCRIPTION

[0044] In order to make the purpose, technical solution and advantages of the embodiments of the present application clearer, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of this application.

[0045] Various embodiments of the present application may be presented in the form of a range; it should be understood that the description in the form of a range is only for convenience and brevity and should not be understood as a rigid limitation on the scope of the present application; therefore, it should be considered that the range description has specifically disclosed all possible sub-ranges and single numerical values ​​within the range; for example, it should be considered that the range description from 1 to 6 has specifically disclosed sub-ranges, such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., as well as single numbers within the range, such as 1, 2, 3, 4, 5 and 6, which applies regardless of the range; in addition, whenever a numerical range is indicated in this document, it is meant to include any cited numbers (fractions or integers) within the indicated range.

[0046] In this document, the terms including "including" and "including" mean "including but not limited to". Relational terms such as "first" and "second" are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. "And / or" describes the association relationship of associated objects, indicating that there can be three relationships. For example, A and / or B can mean: A exists alone, A and B exist at the same time, and B exists alone; where A and B can be singular or plural. "At least one" means one or more, and "plurality" means two or more; "at least one", "at least one of the following" or similar expressions refer to any combination of these items, including any combination of single or plural items; for example, "at least one of a, b, or c", or "at least one of a, b, and c" can all mean: a, b, c, ab (i.e., a and b), ac, bc, or abc, where a, b, and c can be single or multiple. Unless otherwise specified, various raw materials, reagents, instruments and equipment used in this application can be purchased from the market or prepared by existing methods.

[0047] It should be noted that the inventors of the present application have discovered that with the development of the modern electrolytic aluminum industry, alumina products with a low wear index, coarse particle size and uniform particle distribution, when used as raw materials for aluminum electrolysis, have the characteristics of large specific surface area, small dust, good solubility and fluidity, and energy saving. Therefore, how to increase the particle size and strength of aluminum hydroxide and transform the morphology of aluminum hydroxide into densely embedded particles has been a technical problem that the alumina industry has been trying to overcome.

[0048] Figure 1 A schematic flow chart of a method for producing aluminum oxide in two stages provided in an embodiment of the present application is shown by way of example;

[0049] Figure 2 An actual flow diagram of a method for producing aluminum oxide in two stages provided in an embodiment of the present application is shown by way of example;

[0050] like Figure 1 As shown, the embodiment of the present application provides a method for producing aluminum oxide in two stages, the method comprising:

[0051] S1. The saturated sodium aluminate semen and the crude aluminum hydroxide seed crystals are subjected to a seed growth reaction to obtain an aluminum hydroxide slurry having a first preset solid content;

[0052] S2. separating the aluminum hydroxide slurry having a first preset solid content to obtain a crude aluminum hydroxide filter cake and a crude aluminum hydroxide separated liquid;

[0053] S3. washing a portion of the crude aluminum hydroxide filter cake to obtain a first aluminum hydroxide product;

[0054] S4. performing a seed adsorption reaction on the crude aluminum hydroxide separated liquid and the fine aluminum hydroxide seed crystals to obtain an aluminum hydroxide slurry having a second preset solid content;

[0055] S5. performing cyclone classification on the aluminum hydroxide slurry having a second preset solid content to obtain an underflow product and an overflow product, respectively;

[0056] S6. Separating and washing the underflow product to obtain a second aluminum hydroxide product;

[0057] S7. combining the first aluminum hydroxide product and the second aluminum hydroxide product to obtain a coarse aluminum hydroxide product;

[0058] S8. roasting the crude aluminum hydroxide product to obtain an alumina product;

[0059] S9. The overflow product is filtered to obtain overflow fine seeds;

[0060] Wherein, the fine aluminum hydroxide seeds include the overflow fine seeds, and the coarse aluminum hydroxide seeds include the remaining coarse aluminum hydroxide filter cake;

[0061] The mass ratio of the content of aluminum hydroxide seeds with a particle size of less than 45 μm in the crude aluminum hydroxide seeds as the numerator and the crude aluminum hydroxide seeds as the denominator is ≤0.15; the mass ratio of the content of aluminum hydroxide seeds with a particle size of less than 45 μm in the fine aluminum hydroxide seeds as the numerator and the fine aluminum hydroxide seeds as the denominator is ≤0.40; the mass ratio of part of the crude aluminum hydroxide filter cake as the numerator and the remaining crude aluminum hydroxide filter cake as the denominator is 1:(5~10); the mass ratio of the seeds in the underflow product as the numerator and the seeds in the overflow product as the denominator is 1:(2~5); the mass ratio of the first aluminum hydroxide product as the numerator and the second aluminum hydroxide product as the denominator is (3~8):1.

[0062] The mass ratio of the portion of crude aluminum hydroxide filter cake as the numerator and the remaining crude aluminum hydroxide filter cake as the denominator can be 1:5, 1:6, 1:7, 1:8, 1:9 or 1:10;

[0063] The mass ratio of the seed crystals in the underflow product as the numerator and the seed crystals in the overflow product as the denominator can be 1:2, 1:3, 1:4 or 1:5.

[0064] The mass ratio of the first aluminum hydroxide product as the numerator and the second aluminum hydroxide product as the denominator can be 3:1, 4:1, 5:1, 6:1, 7:1 or 8:1.

[0065] It should be noted that the aluminum hydroxide product slurry discharged during the seed growth reaction does not need to be graded. A portion of the aluminum hydroxide slurry is directly used as an aluminum hydroxide product solution for filtration, separation and washing to obtain coarse-grained aluminum hydroxide seeds, and another portion of the aluminum hydroxide slurry is subjected to coarse seed filtration to obtain a filtrate, which is then used as an aluminum hydroxide raw material solution for a seed adsorption reaction. The filter cakes obtained from these filtration stages of the aluminum hydroxide slurries can be returned to the seed growth as a raw material.

[0066] It should be noted that the fine aluminum hydroxide seeds in the adsorption process need to enter the cyclone for classification, the underflow is sent to the flat disc filter as the aluminum hydroxide product for filtration, separation and washing, the overflow is sent to the fine seed disc filter for filtration and use as fine-grained aluminum hydroxide seeds, the filtrate goes to the evaporation process, and the filter cake returns to the first tank of the adsorption section of the seed adsorption reaction for recycling.

[0067] It should be noted that a portion of the aluminum hydroxide slurry with the first preset solid content is used as coarse aluminum hydroxide seed crystals for cyclic decomposition.

[0068] It should be noted that a portion of the aluminum hydroxide slurry with the second preset solid content is used as fine aluminum hydroxide seeds for cyclic decomposition.

[0069] It should be noted that the difference in composition between the coarse aluminum hydroxide and the fine aluminum hydroxide lies in the different particle size distribution of aluminum hydroxide and the different impurity content.

[0070] In some optional embodiments, the first preset solid content is 600 g / L to 900 g / L, and the second preset solid content is 150 g / L to 350 g / L;

[0071] In these embodiments, the interfacial tension between the saturated sodium aluminate solution and the aluminum hydroxide crystals is relatively large, and the surface energy actually provided by the saturated sodium aluminate solution during the decomposition process is relatively low. Therefore, a certain amount of aluminum hydroxide seeds need to be added to the saturated sodium aluminate solution to overcome the interfacial tension between the saturated sodium aluminate solution and the aluminum hydroxide crystals, thereby promoting the precipitation of aluminum hydroxide crystals in the saturated sodium aluminate solution, and the first preset solid content can be 600g / L to 900g / L, which can provide higher aluminum hydroxide seed activity in the seed growth reaction stage, which is beneficial to increase the agglomeration and growth rate of aluminum hydroxide crystals, thereby obtaining a sufficient amount of high-strength and coarse-grained aluminum hydroxide product; in addition, the second preset solid content can be 150g / L to 350g / L, which can promote the solid content of the seed adsorption reaction process to be at a lower level, so as to reduce the risk of collision between aluminum hydroxide crystals, thereby inhibiting the rupture of aluminum hydroxide crystals in the later stage of the decomposition process of saturated sodium aluminate semen, so as to improve the decomposition efficiency of the decomposition process of saturated sodium aluminate semen.

[0072] The first preset solid content may be 600 g / L, 650 g / L, 700 g / L, 750 g / L, 800 g / L, 850 g / L or 900 g / L.

[0073] The second preset solid content may be 150 g / L, 200 g / L, 250 g / L, 300 g / L or 350 g / L.

[0074] It should be noted that the first preset solid content and the second preset solid content are used to describe the states of different solid contents in the sodium aluminate solution.

[0075] In some optional embodiments, the time of the seed crystal growth reaction is 25h to 35h, and the time of the seed crystal adsorption reaction is 15h to 20h;

[0076] In these embodiments, the time of the seed growth reaction can be 25h to 35h, and the time of the seed adsorption reaction can be 15h to 20h, which can promote the decomposition process of the saturated sodium aluminate semen to be split into two parts: the seed growth reaction and the seed adsorption reaction, so that the seed growth reaction includes the early and middle stages of the decomposition of the saturated sodium aluminate semen, and the seed adsorption reaction includes the late stage of the decomposition of the saturated sodium aluminate semen, the seed growth reaction including the early and middle stages of the decomposition of the saturated sodium aluminate semen can have enough time to obtain a sufficient amount of high-strength and coarse-grained aluminum hydroxide product, and the seed adsorption reaction including the late stage of the decomposition of the saturated sodium aluminate semen can have enough time to improve the decomposition efficiency of the saturated sodium aluminate semen.

[0077] The seed growth reaction time can be 25h, 26h, 27h, 28h, 29h, 30h, 31h, 32h, 33h, 34h or 35h.

[0078] The time for the seed adsorption reaction can be 15 h, 16 h, 17 h, 18 h, 19 h or 20 h.

[0079] It should be noted that in the early stage of decomposition of saturated sodium aluminate semen, the decomposition temperature is relatively high, but the supersaturation of the saturated sodium aluminate semen itself is relatively high, resulting in a strong agglomeration and growth ability of aluminum hydroxide crystals; in the middle stage of decomposition of saturated sodium aluminate semen, the supersaturation of the saturated sodium aluminate semen itself is reduced, but because the decomposition process of saturated sodium aluminate semen is a cooling process, the supersaturation of the saturated sodium aluminate semen will be strengthened in the intermediate cooling stage of the decomposition of saturated sodium aluminate semen, and the agglomeration and growth ability of aluminum hydroxide crystals is still strong; in the late stage of decomposition of saturated sodium aluminate semen, the supersaturation of the saturated sodium aluminate semen itself will decrease, and at the same time, its temperature will decrease and its viscosity will increase, resulting in a decrease in the growth rate of aluminum hydroxide crystals. In addition, after long-term stirring in the late stage of decomposition, the probability of breakage and abrasion of aluminum hydroxide crystals can be increased, which is not conducive to the improvement of the particle size and strength of aluminum hydroxide seed crystals.

[0080] In some optional embodiments, the molecular ratio of the saturated sodium aluminate semen is 1.40 to 1.50;

[0081] In these embodiments, the molecular ratio of the saturated sodium aluminate semen can be 1.40-1.50, which can provide a higher supersaturation for the sodium aluminate semen, and is beneficial to the decomposition of the seed in the subsequent seed growth reaction stage.

[0082] The molecular ratio of the saturated sodium aluminate semen can be 1.40, 1.41, 1.42, 1.43, 1.44, 1.45, 1.46, 1.47, 1.48, 1.49 or 1.50.

[0083] In some optional embodiments, the molecular ratio of the endpoint solution of the seed crystal growth reaction is 2.4-2.6, and the molecular ratio of the endpoint solution of the seed crystal adsorption reaction is 2.8-3.2.

[0084] In these embodiments, the molecular ratio of the endpoint solution of the seed growth reaction can be 2.4-2.6, which can obtain a sufficient amount of high-strength and coarse-grained aluminum hydroxide product; in addition, the molecular ratio of the endpoint solution of the seed adsorption reaction can be 2.8-3.2, which can improve the system decomposition rate.

[0085] The molecular ratio of the endpoint solution of the seed growth reaction can be 2.4, 2.5 or 2.6.

[0086] The molecular ratio of the endpoint solution of the adsorption reaction can be 2.8, 2.9, 3.0, 3.1 or 3.2.

[0087] In some optional embodiments, the end point temperature T2 of the seed growth reaction satisfies:

[0088] T2 = T1 - t1,

[0089] Wherein, T1 is the initial temperature of the seed growth reaction, and t1 is the first temperature drop amplitude;

[0090] The initial temperature of the seed growth reaction is 58°C to 65°C, and the first temperature reduction range is 10°C to 15°C;

[0091] In these embodiments, the terminal temperature T2 of the seed growth reaction can satisfy: T2=T1-t1, and the initial temperature of the seed growth reaction can be 58°C~65°C, and the first temperature reduction amplitude can be 10°C~15°C, which can promote the seed growth reaction including the early and middle stages of the decomposition of the saturated sodium aluminate semen to effectively enhance the supersaturation of the saturated sodium aluminate semen, so as to improve the agglomeration and growth ability of aluminum hydroxide grains, thereby facilitating the improvement of the particle size and strength of aluminum hydroxide.

[0092] The initial temperature of the seed growth reaction can be 58°C, 59°C, 60°C, 61°C, 62°C, 63°C, 64°C or 65°C.

[0093] The first temperature reduction amplitude may be 10°C, 11°C, 12°C, 13°C, 14°C or 15°C.

[0094] It should be noted that the decomposition temperature of saturated sodium aluminate semen is high, and the viscosity of saturated sodium aluminate semen will decrease, which will increase the diffusion rate of aluminate ions in the saturated sodium aluminate semen to improve the mass transfer effect of the saturated sodium aluminate semen, which can be beneficial to the agglomeration and growth of aluminum hydroxide crystals, and then to the coarsening of the aluminum hydroxide particle size. However, if the decomposition temperature is too high, the supersaturation of the saturated sodium aluminate semen will decrease, which is not conducive to the improvement of the strength of the aluminum hydroxide crystals, and thus will ultimately increase the wear index of alumina.

[0095] In some optional embodiments, the end point temperature T3 of the seed adsorption reaction satisfies:

[0096] T3 = T2 - t2,

[0097] Wherein, T2 is the end temperature of the seed growth reaction, and t2 is the second temperature reduction amplitude;

[0098] The first temperature reduction range is 1°C to 2°C;

[0099] In these embodiments, the terminal temperature T3 of the seed adsorption reaction can satisfy T3=T2-t2, and the second temperature reduction amplitude can be 1°C~2°C, which can promote the seed adsorption reaction to proceed at room temperature, so as to effectively prolong the decomposition time of the saturated sodium aluminate semen, thereby improving the decomposition rate of the saturated sodium aluminate semen.

[0100] In some optional embodiments, the mass ratio of the content of oxalate in the aluminum hydroxide product to the aluminum hydroxide is less than 0.0005;

[0101] The mass ratio of the content of aluminum hydroxide with a particle size of less than 45 μm in the aluminum hydroxide product to the aluminum hydroxide product is less than 0.08;

[0102] In these embodiments, since oxalate impurities (especially sodium oxalate impurities) in the saturated sodium aluminate semen will adhere to the surface of the precipitated crystals after crystallization and precipitation on the surface of the aluminum hydroxide seed crystals, it will hinder the agglomeration and growth of the aluminum hydroxide seed crystals, thereby causing serious defects in the aluminum hydroxide seed crystals, and also reduce the strength of the aluminum hydroxide crystals to refine the particle size of the aluminum hydroxide crystals; when the oxalate content in the aluminum hydroxide product and the mass ratio of aluminum hydroxide are less than 0.0005, it means that the oxalate content in the filtrate after the seed adsorption reaction is the minimum, which is conducive to ensuring that the aluminum hydroxide content with a particle size of less than 45 μm in the aluminum hydroxide product and the mass ratio of the aluminum hydroxide product are less than 0.08, so as to finally obtain an alumina product with coarse particle size and low wear index.

[0103] Based on a general inventive concept, an embodiment of the present application provides an aluminum oxide, wherein the aluminum oxide is prepared by the method described in the first aspect, and the morphology of the aluminum oxide is an agglomerated mosaic aluminum oxide.

[0104] The aluminum oxide is realized based on the above method, and the specific steps of the method can refer to the above embodiment. Since the aluminum oxide adopts part or all of the technical solutions of the above embodiment, it has at least all the beneficial effects brought by the technical solutions of the above embodiment, which will not be described one by one here.

[0105] It should be noted that the decomposition rate of saturated sodium aluminate semen in the alumina production process is 48% to 55%.

[0106] In some optional embodiments, the mass ratio of the content of alumina with a particle size of less than 45 μm in the alumina product to the alumina product is less than 0.10;

[0107] The wear index of the aluminum oxide is ≤12%;

[0108] In these embodiments, the mass ratio of the alumina content with a particle size of less than 45 μm in the alumina product to the alumina product is less than 0.10, and the wear index of the alumina can be ≤12%, which can indicate that the high-strength agglomerated mosaic alumina crystals have been fully developed, and the structural symmetry of the alumina is better, the overall alumina grains are densely inlaid, and the gaps on the outside of the alumina product are filled with small grains, which makes the main dehydration trajectory in the subsequent process the gaps between the fine alumina particles, so that alumina particles with no obvious cracks in the crystal morphology can be obtained, and the overall alumina exhibits a low wear index.

[0109] The present application is further described below in conjunction with specific examples. The experimental methods in the following examples that do not specify specific conditions are usually measured according to industry standards; if there are no corresponding industry standards, they are carried out according to common international standards, conventional conditions, or conditions recommended by the manufacturer.

[0110] Example 1

[0111] The saturated sodium aluminate concentrate of an alumina enterprise was selected, the caustic soda concentration of which was 155 g / L and the molecular ratio of which was 1.46.

[0112] like Figure 1 and Figure 2 As shown, a method for producing aluminum oxide in two stages, comprising:

[0113] S1. The saturated sodium aluminate semen and the crude aluminum hydroxide seed crystals are subjected to a seed growth reaction to obtain an aluminum hydroxide slurry having a first preset solid content;

[0114] S2. separating the aluminum hydroxide slurry having a first preset solid content to obtain a crude aluminum hydroxide filter cake and a crude aluminum hydroxide separated liquid;

[0115] S3. washing a portion of the crude aluminum hydroxide filter cake to obtain a first aluminum hydroxide product;

[0116] S4. The crude aluminum hydroxide separated liquid is subjected to a seed adsorption reaction with fine aluminum hydroxide seed crystals to obtain an aluminum hydroxide slurry having a second preset solid content;

[0117] S5. Performing cyclone classification on the aluminum hydroxide slurry having a second preset solid content to obtain an underflow product and an overflow product, respectively;

[0118] S6. Separating and washing the underflow product to obtain a second aluminum hydroxide product;

[0119] S7. combining the first aluminum hydroxide product and the second aluminum hydroxide product to obtain a coarse aluminum hydroxide product;

[0120] S8. The crude aluminum hydroxide product is roasted to obtain an alumina product;

[0121] S9. Filtering the overflow product to obtain overflow fine seeds respectively;

[0122] Wherein, the fine aluminum hydroxide seeds include overflow fine seeds, and the coarse aluminum hydroxide seeds include remaining coarse aluminum hydroxide filter cake;

[0123] The mass ratio of part of the crude aluminum hydroxide filter cake as the numerator and the remaining crude aluminum hydroxide filter cake as the denominator is 1:8; the mass ratio of the seed crystals in the underflow product as the numerator and the seed crystals in the overflow product as the denominator is 1:4; the mass ratio of the first aluminum hydroxide product as the numerator and the second aluminum hydroxide product as the denominator is 6:1.

[0124] In the aluminum hydroxide product, the mass ratio of the crude aluminum hydroxide to the fine aluminum hydroxide is 9:1.

[0125] The first preset solid content is 800 g / L, and the second preset solid content is 300 g / L.

[0126] The time for the seed growth reaction is 30 h, and the time for the seed adsorption reaction is 15 h.

[0127] The molecular ratio of the end point solution of the seed growth reaction was 2.5, the molecular ratio of the end point solution of the seed adsorption reaction was 3.0, and the system decomposition rate was 52%.

[0128] The end temperature T2 of the seed growth reaction satisfies:

[0129] T2 = T1 - t1,

[0130] Where T1 is the initial temperature of the seed growth reaction, and t1 is the first temperature drop amplitude;

[0131] The initial temperature of the seed growth reaction was 65°C, and the first temperature drop was 10°C.

[0132] The end point temperature T3 of the seed adsorption reaction satisfies:

[0133] T3 = T2 - t2,

[0134] Where, T2 is the end temperature of the seed growth reaction, and t2 is the second temperature drop amplitude;

[0135] The second temperature reduction is 1°C.

[0136] The mass ratio of the content of oxalate in the aluminum hydroxide product to the aluminum hydroxide is 0.0003; the mass ratio of the content of particles below 45 μm in the aluminum hydroxide product to the aluminum hydroxide product is 0.05.

[0137] After aluminum hydroxide was statically calcined at 900°C for 20 minutes, the mass ratio of the aluminum oxide content with a particle size of less than 45 μm in the aluminum oxide product to the aluminum oxide product was 0.06; the wear index of the aluminum oxide was 9%;

[0138] Example 2

[0139] Based on the contents disclosed in Example 1, the following modifications are further made:

[0140] The first preset solid content is 600 g / L, and the second preset solid content is 300 g / L.

[0141] The molecular ratio of the end point solution of the seed growth reaction is 2.5, the molecular ratio of the end point solution of the seed adsorption reaction is 2.9, and the system decomposition rate is 50%.

[0142] The end temperature T2 of the seed growth reaction satisfies:

[0143] T2 = T1 - t1,

[0144] Where T1 is the initial temperature of the seed growth reaction, and t1 is the first temperature drop amplitude;

[0145] The mass ratio of the content of oxalate in the aluminum hydroxide product to the aluminum hydroxide is 0.0004; the mass ratio of the content of aluminum hydroxide with a particle size of less than 45 μm in the aluminum hydroxide product to the aluminum hydroxide product is 0.07.

[0146] After aluminum hydroxide is statically calcined at 900°C for 20 minutes, the mass ratio of the aluminum oxide content with a particle size of less than 45 μm in the aluminum oxide product to the aluminum oxide product is 0.09; the wear index of the aluminum oxide is 10%;

[0147] Example 3

[0148] Based on the contents disclosed in Example 1, the following modifications are further made:

[0149] The time for the seed growth reaction is 35 h, and the time for the seed adsorption reaction is 20 h.

[0150] The molecular ratio of the end point solution of the seed growth reaction was 2.6, the molecular ratio of the end point solution of the seed adsorption reaction was 3.2, and the system decomposition rate was 54%.

[0151] The mass ratio of the content of oxalate in the aluminum hydroxide product to the aluminum hydroxide is 0.0004; the mass ratio of the content of aluminum hydroxide with a particle size of less than 45 μm in the aluminum hydroxide product to the aluminum hydroxide product is 0.07.

[0152] After aluminum hydroxide was statically calcined at 900°C for 20 minutes, the mass ratio of the aluminum oxide content with a particle size of less than 45 μm in the aluminum oxide product to the aluminum oxide product was 0.08; the wear index of the aluminum oxide was 11%;

[0153] Example 4

[0154] Based on the contents disclosed in Example 1, the following modifications are further made:

[0155] The time for the seed growth reaction is 25 h, and the time for the seed adsorption reaction is 15 h.

[0156] The molecular ratio of the endpoint solution of the seed growth reaction is 2.4, the molecular ratio of the endpoint solution of the seed adsorption reaction is 2.8, and the system decomposition rate is 48%.

[0157] The mass ratio of the content of oxalate in the aluminum hydroxide product to the aluminum hydroxide is 0.0002; the mass ratio of the content of aluminum hydroxide with a particle size below 45 μm in the aluminum hydroxide product to the aluminum hydroxide product is 0.04.

[0158] After aluminum hydroxide is statically calcined at 900°C for 20 minutes, the content of aluminum oxide with a particle size below 45 μm in the aluminum oxide product and the mass ratio of the aluminum oxide product are 0.05; the wear index of the aluminum oxide is 8%.

[0159] Example 5

[0160] Based on the contents disclosed in Example 1, the following modifications are further made:

[0161] The molecular ratio of the end point solution of the seed growth reaction is 2.6, the molecular ratio of the end point solution of the seed adsorption reaction is 3.1, and the system decomposition rate is 53%.

[0162] The end temperature T2 of the seed growth reaction satisfies:

[0163] T2 = T1 - t1,

[0164] Where T1 is the initial temperature of the seed growth reaction, and t1 is the first temperature drop amplitude;

[0165] The initial temperature of the seed growth reaction was 58°C, and the first temperature drop was 10°C.

[0166] The end point temperature T3 of the seed adsorption reaction satisfies:

[0167] T3 = T2 - t2,

[0168] Where, T2 is the end temperature of the seed growth reaction, and t2 is the second temperature drop amplitude;

[0169] The first temperature reduction is 1°C.

[0170] The mass ratio of the content of oxalate in the aluminum hydroxide product to the aluminum hydroxide is 0.0003; the mass ratio of the content of aluminum hydroxide with a particle size of less than 45 μm in the aluminum hydroxide product to the aluminum hydroxide product is 0.06.

[0171] After aluminum hydroxide was statically calcined at 900°C for 20 minutes, the mass ratio of the aluminum oxide content with a particle size of less than 45 μm in the aluminum oxide product to the aluminum oxide product was 0.07; the wear index of the aluminum oxide was 11%.

[0172] Comparative Example 1

[0173] Based on the contents disclosed in Example 1, the following modifications are further made:

[0174] Figure 3 A schematic flow chart of a method for producing aluminum oxide by a one-stage decomposition process provided in Comparative Example 1 of the present application is shown by way of example;

[0175] like Figure 3 As shown, a traditional one-stage decomposition process is used: saturated sodium aluminate semen is directly decomposed continuously to obtain an aluminum hydroxide product, wherein the solid content of the saturated sodium aluminate semen is 800 g / L, the initial temperature of the continuous decomposition is 62°C, the terminal temperature of the continuous decomposition is 50°C, and the continuous decomposition time is 45 h.

[0176] The end point solution molecular ratio of the decomposition reaction is 2.9, and the system decomposition rate is 50%.

[0177] The mass ratio of the content of oxalate in the aluminum hydroxide product to the aluminum hydroxide is 0.0011; the mass ratio of the content of aluminum hydroxide with a particle size of less than 45 μm in the aluminum hydroxide product to the aluminum hydroxide product is 0.15.

[0178] After aluminum hydroxide is statically calcined at 900°C for 20 minutes, the mass ratio of the aluminum oxide content with a particle size of less than 45 μm in the aluminum oxide product to the aluminum oxide product is 0.16; the wear index of the aluminum oxide is 20%.

[0179] Comparative Example 2

[0180] Based on the contents disclosed in Example 1, the following modifications are further made:

[0181] The first preset solid content is 500 g / L, and the second preset solid content is 100 g / L.

[0182] The molecular ratio of the end point solution of the seed growth reaction was 2.3, the molecular ratio of the end point solution of the seed adsorption reaction was 2.6, and the system decomposition rate was 45%.

[0183] The mass ratio of the content of oxalate in the aluminum hydroxide product to the aluminum hydroxide is 0.0004; the mass ratio of the content of aluminum hydroxide with a particle size of less than 45 μm in the aluminum hydroxide product to the aluminum hydroxide product is 0.07.

[0184] After aluminum hydroxide is statically calcined at 900°C for 20 minutes, the mass ratio of the aluminum oxide content with a particle size of less than 45 μm in the aluminum oxide product to the aluminum oxide product is 0.08; the wear index of the aluminum oxide is 9%.

[0185] Comparative Example 3

[0186] Based on the contents disclosed in Example 1, the following modifications are further made:

[0187] The first preset solid content is 1000 g / L, and the second preset solid content is 400 g / L.

[0188] The molecular ratio of the end point solution of the seed growth reaction was 2.6, the molecular ratio of the end point solution of the seed adsorption reaction was 3.0, and the system decomposition rate was 51%.

[0189] The mass ratio of the content of oxalate in the aluminum hydroxide product to the aluminum hydroxide is 0.0004; the mass ratio of the content of aluminum hydroxide with a particle size of less than 45 μm in the aluminum hydroxide product to the aluminum hydroxide product is 0.013.

[0190] After aluminum hydroxide is statically calcined at 900°C for 20 minutes, the content of aluminum oxide with a particle size of less than 45 μm in the aluminum oxide product and the mass ratio of the aluminum oxide product are 0.15; the wear index of the aluminum oxide is 15%.

[0191] Comparative Example 4

[0192] Based on the contents disclosed in Example 1, the following modifications are further made:

[0193] The time for the seed growth reaction is 20 h, and the time for the seed adsorption reaction is 10 h.

[0194] The molecular ratio of the end point solution of the seed growth reaction was 2.3, the molecular ratio of the end point solution of the seed adsorption reaction was 2.6, and the system decomposition rate was 43%.

[0195] The mass ratio of the content of oxalate in the aluminum hydroxide product to the aluminum hydroxide is 0.0004; the mass ratio of the content of aluminum hydroxide with a particle size of less than 45 μm in the aluminum hydroxide product to the aluminum hydroxide product is 0.07.

[0196] After aluminum hydroxide is statically calcined at 900°C for 20 minutes, the mass ratio of the aluminum oxide content with a particle size of less than 45 μm in the aluminum oxide product to the aluminum oxide product is 0.08; the wear index of the aluminum oxide is 7%.

[0197] Comparative Example 5

[0198] Based on the contents disclosed in Example 1, the following modifications are further made:

[0199] The time for the seed growth reaction is 40 h, and the time for the seed adsorption reaction is 25 h.

[0200] The molecular ratio of the end point solution of the seed growth reaction was 2.6, the molecular ratio of the end point solution of the seed adsorption reaction was 3.2, and the system decomposition rate was 54%.

[0201] The mass ratio of the content of oxalate in the aluminum hydroxide product to the aluminum hydroxide is 0.0004; the mass ratio of the content of aluminum hydroxide with a particle size of less than 45 μm in the aluminum hydroxide product to the aluminum hydroxide product is 0.07.

[0202] After aluminum hydroxide is statically calcined at 900°C for 20 minutes, the content of aluminum oxide with a particle size of less than 45 μm in the aluminum oxide product and the mass ratio of the aluminum oxide product are 0.09; the wear index of the aluminum oxide is 18%.

[0203] Comparative Example 6

[0204] Based on the contents disclosed in Example 1, the following modifications are further made:

[0205] The initial temperature of the seed growth reaction was 50°C, and the first temperature drop was 10°C.

[0206] The molecular ratio of the end point solution of the seed growth reaction was 2.6, the molecular ratio of the end point solution of the seed adsorption reaction was 3.1, and the system decomposition rate was 53%.

[0207] The mass ratio of the content of oxalate in the aluminum hydroxide product to the aluminum hydroxide is 0.0004; the mass ratio of the content of aluminum hydroxide with a particle size of less than 45 μm in the aluminum hydroxide product to the aluminum hydroxide product is 0.13.

[0208] After aluminum hydroxide is statically calcined at 900°C for 20 minutes, the mass ratio of the content of aluminum oxide with a particle size of less than 45 μm in the aluminum oxide product to the aluminum oxide product is 0.15; the wear index of the aluminum oxide is 13%.

[0209] Comparative Example 7

[0210] Based on the contents disclosed in Example 1, the following modifications are further made:

[0211] The initial temperature of the seed growth reaction was 70°C, and the first temperature drop was 20°C.

[0212] The molecular ratio of the end point solution of the seed growth reaction was 2.2, the molecular ratio of the end point solution of the seed adsorption reaction was 2.6, and the system decomposition rate was 44%.

[0213] The mass ratio of the content of oxalate in the aluminum hydroxide product to the aluminum hydroxide is 0.0004; the mass ratio of the content of aluminum hydroxide with a particle size of less than 45 μm in the aluminum hydroxide product to the aluminum hydroxide product is 0.06.

[0214] After aluminum hydroxide was statically calcined at 900°C for 20 minutes, the mass ratio of the aluminum oxide content with a particle size of less than 45 μm in the aluminum oxide product to the aluminum oxide product was 0.07; the wear index of the aluminum oxide was 15%;

[0215] Related experiments and effect data:

[0216] Figure 4 The schematic diagram of the characterization structure of an aluminum oxide provided in Example 1 of the present application is shown as an example;

[0217] Figure 5 The schematic diagram of the characterization structure of an aluminum oxide provided in Comparative Example 1 of the present application is shown as an example;

[0218] 1. The alumina products obtained in Example 1 and Comparative Example 1 were collected and characterized. The results were as follows: Figure 4 and Figure 5 As shown, Figure 4 The results show that the alumina product obtained in Example 1 has an agglomerated mosaic morphology. Figure 5 It shows that the alumina product morphology obtained in Comparative Example 1 is a single crystal radially elongated type.

[0219] 2. The decomposition rates of the embodiments and comparative examples in the decomposition process of the saturated sodium aluminate concentrate were counted respectively, and the content of fine-grained alumina with a particle size of less than 45 μm in the produced alumina products, as well as the wear index of alumina were counted. The results are shown in Table 1.

[0220] Table 1 Decomposition rate, content of alumina with a particle size of less than 45 μm in alumina and wear index of each embodiment and comparative example

[0221]

[0222]

[0223] As can be seen from Table 1, the method for producing alumina in a two-stage reverse manner provided in the embodiment of the present application is simple and easy to implement as a whole. Under the premise that the decomposition rate of saturated sodium aluminate semen is not reduced, it can not only comprehensively inhibit the precipitation of sodium oxalate impurities in the sodium aluminate semen through the seed growth reaction and the seed adsorption reaction to coarsen the particle size of the final alumina, but also can improve the strength of the alumina and optimize the crystal structure of the alumina, thereby comprehensively reducing the wear index of the alumina.

[0224] However, in the method for producing alumina in two stages provided in the embodiments of the present application, when one of the process parameters is out of the process parameter range provided in the embodiments of the present application, the quality of the obtained alumina product is poor. However, when all the parameters are within the process parameter range provided in the embodiments of the present application, the particle size and wear index of the obtained alumina are significantly better.

[0225] In addition, an embodiment of the present application provides an alumina product, in which the mass ratio of the alumina content with a particle size below 45 μm to the alumina product is less than 0.10, and the wear index of the alumina is ≤12%, and the obtained alumina morphology is an agglomerated mosaic type.

[0226] The above is only a specific implementation of the present application, so that those skilled in the art can understand or implement the present application. It will be apparent to those skilled in the art that various modifications to these embodiments are possible, and the general principles defined in the present application can be implemented in other embodiments without departing from the spirit or scope of the present application. Therefore, the present application will not be limited to these embodiments shown in the present application, but will conform to the widest scope consistent with the principles and novel features applied for by the present application.

Claims

1. A method for producing aluminum oxide in two stages, It is characterized in that The method comprises: Carrying out a seed growth reaction between saturated sodium aluminate concentrate and crude aluminum hydroxide seed crystals to obtain an aluminum hydroxide slurry having a first preset solid content; Separating the aluminum hydroxide slurry having a first preset solid content to obtain a crude aluminum hydroxide filter cake and a crude aluminum hydroxide separated liquid, respectively; washing a portion of the crude aluminum hydroxide filter cake to obtain a first aluminum hydroxide product; The crude aluminum hydroxide separated liquid is subjected to a seed adsorption reaction with fine aluminum hydroxide seed crystals to obtain an aluminum hydroxide slurry having a second preset solid content; Performing cyclone classification on the aluminum hydroxide slurry having a second preset solid content to obtain an underflow product and an overflow product respectively; Separating and washing the underflow product to obtain a second aluminum hydroxide product; Combining the first aluminum hydroxide product and the second aluminum hydroxide product to obtain a crude aluminum hydroxide product; calcining the crude aluminum hydroxide product to obtain an aluminum oxide product; filtering the overflow product to obtain overflow fine seeds respectively; Wherein, the fine aluminum hydroxide seeds include the overflow fine seeds, and the coarse aluminum hydroxide seeds include the remaining coarse aluminum hydroxide filter cake; The mass ratio of the content of aluminum hydroxide seeds with a particle size of less than 45 μm in the crude aluminum hydroxide seeds to the crude aluminum hydroxide seeds is ≤0.15; the mass ratio of the content of aluminum hydroxide seeds with a particle size of less than 45 μm in the fine aluminum hydroxide seeds to the fine aluminum hydroxide seeds is ≤0.40; the mass ratio of part of the crude aluminum hydroxide filter cake to the remaining crude aluminum hydroxide filter cake is 1:(5-10); the mass ratio of the seeds in the underflow product to the seeds in the overflow product is 1:(2-5); the mass ratio of the first aluminum hydroxide product to the second aluminum hydroxide product is (3-8):

1.

2. The method according to claim 1, It is characterized in that The first preset solid content is 600 g / L to 900 g / L, and the second preset solid content is 150 g / L to 350 g / L.

3. The method according to claim 1, It is characterized in that The time for the seed crystal growth reaction is 25h to 35h, and the time for the seed crystal adsorption reaction is 15h to 20h.

4. The method according to claim 1, It is characterized in that The molecular ratio of the saturated sodium aluminate semen is 1.40-1.

50.

5. The method according to claim 1, It is characterized in that The molecular ratio of the end point solution of the seed crystal growth reaction is 2.4 to 2.6, and the molecular ratio of the end point solution of the seed crystal adsorption reaction is 2.8 to 3.

2.

6. The method according to claim 1, It is characterized in that The end point temperature T of the seed growth reaction 2 satisfy: T 2 =T 1 -t 1 , Where, T 1 is the initial temperature of the seed growth reaction, t 1 is the first temperature reduction range; The initial temperature of the seed crystal growth reaction is 58°C to 65°C, and the first temperature reduction range is 10°C to 15°C.

7. The method according to claim 6, It is characterized in that The end point temperature T of the seed adsorption reaction 3 satisfy: T 3 =T 2 -t 2 , Where, T 2 is the end temperature of the seed growth reaction, t 2 is the second cooling range; The second temperature reduction range is 1°C to 2°C.

8. The method according to claim 1, It is characterized in that The mass ratio of the content of oxalate in the aluminum hydroxide product to the aluminum hydroxide is less than 0.0005; The mass ratio of the content of aluminum hydroxide with a particle size of less than 45 μm in the aluminum hydroxide product to the aluminum hydroxide product is less than 0.

08.

9. Aluminium oxide, It is characterized in that The aluminum oxide is prepared by the method according to any one of claims 1 to 8, and the morphology of the aluminum oxide is agglomerated mosaic aluminum oxide.

10. Aluminum oxide according to claim 9, It is characterized in that The mass ratio of the content of alumina with a particle size of less than 45 μm in the alumina product to the alumina product is less than 0.10; The wear index of the aluminum oxide is ≤12%.