Tannic acid modified molybdenum disulfide oxide, preparation method of tannic acid modified molybdenum disulfide oxide, tannic acid modified molybdenum disulfide oxide composite film and preparation method of tannic acid modified molybdenum disulfide oxide composite film

By introducing tannic acid-modified molybdenum disulfide oxide into the ultrafiltration membrane material, the pollution problem caused by the hydrophobicity of the existing ultrafiltration membrane material is solved, achieving higher anti-pollution performance and water flux, and improving the membrane's separation efficiency.

CN118754201APending Publication Date: 2024-10-11ENERGY RES INST OF JIANGXI ACAD OF SCI
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202410730366.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-06
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Existing ultrafiltration membrane materials such as polyethersulfone, polysulfone and polyimide are prone to adsorbing pollutants due to their hydrophobicity, resulting in a decrease in membrane separation performance and limiting their application.

Method used

Tannic acid-modified oxidized molybdenum disulfide (TA@O-MoS2) is used as the key component of the composite membrane. By mixing with high molecular polymers, polar organic solvents and porogens, a composite membrane with good hydrophilicity and negative charge is prepared. Anti-pollution performance of membrane surface.

Benefits of technology

It improves the anti-pollution performance and water flux of the membrane, enhances the rejection of pollutants in water, and improves the rejection rate and pure water flux of PEG20000.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118754201A_ABST
    Figure CN118754201A_ABST
Patent Text Reader

Abstract

The invention provides tannic acid modified molybdenum disulfide oxide and a preparation method thereof, and a tannic acid modified molybdenum disulfide oxide composite membrane and a preparation method thereof, and relates to the technical field of membrane separation. The tannic acid modified molybdenum disulfide oxide (marked as TA-atO-MoS2) prepared by the method shows good hydrophilicity and is negatively charged, and when the tannic acid modified molybdenum disulfide oxide is used for preparing a membrane material, the hydrophilicity and nuclear negative electricity performance of the membrane surface are enhanced, and a certain repulsive interaction is achieved on pollutants in water, so that the anti-pollution performance of the membrane surface is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of membrane separation, and in particular to a tannic acid modified oxidized molybdenum disulfide and a preparation method thereof, a tannic acid modified oxidized molybdenum disulfide composite membrane and a preparation method thereof. Background Art

[0002] Ultrafiltration membrane is a microporous filtration membrane with a consistent pore size structure and a pore size range of less than 100nm. By applying appropriate pressure on the liquid side of the membrane, solute particles smaller than the pore size can be retained to separate particles with a molecular weight greater than 500 Daltons and a particle size greater than 10nm.

[0003] The materials of ultrafiltration membranes usually include polyethersulfone, polysulfone and polyimide. These high molecular polymers have excellent comprehensive properties and are widely used. However, polyethersulfone, polysulfone and polyimide ultrafiltration membranes are highly hydrophobic. Pollutants are easily adsorbed on the membrane surface and in the membrane pores, causing pollution of the ultrafiltration membrane, resulting in a significant decrease in membrane separation performance, which greatly limits its application. Summary of the invention

[0004] The purpose of the present invention is to provide a tannic acid modified oxidized molybdenum disulfide and a preparation method thereof, a tannic acid modified oxidized molybdenum disulfide composite membrane and a preparation method thereof. The tannic acid modified oxidized molybdenum disulfide composite membrane provided by the present invention has good anti-pollution performance.

[0005] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0006] The present invention provides a method for preparing tannic acid modified oxidized molybdenum disulfide, comprising the following steps: mixing molybdenum disulfide and sodium nitrate to obtain a mixture;

[0007] mixing the mixture with concentrated sulfuric acid to obtain a dispersion;

[0008] The dispersion liquid is mixed with potassium permanganate to carry out an oxidation reaction, and the obtained oxidation liquid is subjected to impurity removal and solid-liquid separation to obtain oxidized molybdenum disulfide;

[0009] The molybdenum disulfide oxide, water and tannic acid are mixed and subjected to ultrasonic stripping to obtain a tannic acid-modified molybdenum disulfide oxide dispersion;

[0010] The tannic acid-modified molybdenum disulfide oxide dispersion is subjected to solid-liquid separation and solid drying to obtain tannic acid-modified molybdenum disulfide oxide.

[0011] Preferably, the oxidation reaction comprises: a first oxidation reaction and a second oxidation reaction are carried out in sequence; the temperature of the first oxidation reaction is 0 to 3°C, and the time is 0.2 to 1 h; the temperature of the second oxidation reaction is 33 to 37°C, and the time is 2.8 to 3.2 h.

[0012] Preferably, the mass ratio of molybdenum disulfide oxide to tannic acid is (11-13):(3-20); the power of the ultrasonic stripping is 300-600W, and the time is 2-48h.

[0013] The present invention provides tannic acid modified oxidized molybdenum disulfide prepared by the preparation method described in the above scheme.

[0014] Preferably, the particle size of the tannic acid modified oxidized molybdenum disulfide is 50 to 2000 nm.

[0015] The present invention provides a tannic acid modified oxidized molybdenum disulfide composite membrane, which is prepared from raw materials including the following mass percentages:

[0016] High molecular weight polymer 10-30%;

[0017] Polar organic solvent 47~89.99%;

[0018] 0.01-3% of the tannic acid-modified oxidized molybdenum disulfide according to claim 4 or 5;

[0019] Porogen 0.01~20%.

[0020] Preferably, the tannic acid modified oxidized molybdenum disulfide composite membrane has a thickness of 0.010 to 0.035 mm, an average pore size of 3.5 to 5 nm, a porosity of 45 to 75%, and a membrane surface water contact angle of 40° to 65°.

[0021] Preferably, the high molecular polymer is one or more of polyethersulfone, polysulfone and polyimide;

[0022] The porogen is one or more of polyethylene glycol, polyvinyl pyrrolidone, sodium lauryl sulfate, lithium chloride and water;

[0023] The polar organic solvent is one or more of N,N-dimethylformamide, N,N-dimethylacetamide and N-methylpyrrolidone.

[0024] The present invention provides a method for preparing the tannic acid modified oxidized molybdenum disulfide composite film described in the above scheme, comprising the following steps:

[0025] Mixing the prepared raw materials to obtain a film casting solution;

[0026] The casting solution is coated to form a film, and is placed in an air bath and a coagulation bath in sequence to obtain the tannic acid modified molybdenum disulfide oxide composite film.

[0027] Preferably, the temperature of the coagulation bath is 0-90° C., the time of the coagulation bath is 30-120 s; and the coagulation bath is water or an organic solvent-water mixed solution.

[0028] The invention provides a preparation method of tannic acid modified molybdenum disulfide oxide, comprising the following steps: mixing molybdenum disulfide and sodium nitrate to obtain a mixture; mixing the mixture with concentrated sulfuric acid to obtain a dispersion; mixing the dispersion with potassium permanganate, performing an oxidation reaction, removing impurities from the obtained oxidized liquid, and performing solid-liquid separation to obtain molybdenum disulfide oxide; mixing the molybdenum disulfide oxide, water and tannic acid, and performing ultrasonic stripping to obtain a tannic acid modified molybdenum disulfide oxide dispersion; performing solid-liquid separation and solid drying on the tannic acid modified molybdenum disulfide oxide dispersion to obtain tannic acid modified molybdenum disulfide oxide.

[0029] The tannic acid modified oxidized molybdenum disulfide (TA@O-MoS 2 ) exhibits good hydrophilicity and carries a negative charge. Using it to prepare membrane materials enhances the hydrophilicity and negative nuclear charge properties of the membrane surface, and has a certain repulsive effect on pollutants in the water, thereby improving the anti-pollution performance of the membrane surface.

[0030] In addition, the tannic acid modified molybdenum disulfide oxide composite film (TA@O-MoS 2 The composite membrane has a high PEG20000 retention rate and water flux. Experimental data show that the TA@O-MoS 2 The retention rate of the composite membrane for polyethylene glycol (PEG20000) is 82.0-91.5%, and the pure water flux of the membrane is 108.7-140.9 L·m -2 ·h -1 bar -1 , the molecular weight cutoff is 19000Da~28000Da. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 The schematic diagram of the preparation process of tannic acid modified oxidized molybdenum disulfide of the present invention;

[0032] Figure 2 TA@O-MoS prepared in Example 2 2 AFM (a) and thickness distribution (b-d) images;

[0033] Figure 3 TEM images of the cross sections of the films of Comparative Example 1 (a) and Example 2 (b);

[0034] Figure 4 The results of the characterization of the zeta potential of the membrane surface of Comparative Example 1 and Example 2;

[0035] Figure 5 It is the membrane flux recovery rate diagram of Comparative Example 1 and Example 2. DETAILED DESCRIPTION

[0036] The present invention provides a method for preparing tannic acid modified oxidized molybdenum disulfide, comprising the following steps: mixing molybdenum disulfide and sodium nitrate to obtain a mixture;

[0037] mixing the mixture with concentrated sulfuric acid to obtain a dispersion;

[0038] The dispersion liquid is mixed with potassium permanganate to carry out an oxidation reaction, and the obtained oxidation liquid is subjected to impurity removal and solid-liquid separation to obtain oxidized molybdenum disulfide;

[0039] The molybdenum disulfide oxide, water and tannic acid are mixed and subjected to ultrasonic peeling to obtain a tannic acid-modified molybdenum disulfide oxide dispersion;

[0040] The tannic acid-modified molybdenum disulfide oxide dispersion is subjected to solid-liquid separation and solid drying to obtain tannic acid-modified molybdenum disulfide oxide.

[0041] In the present invention, unless otherwise specified, the raw materials used are commercially available products well known in the art.

[0042] The present invention mixes molybdenum disulfide and sodium nitrate to obtain a mixture.

[0043] In the present invention, the mass ratio of molybdenum disulfide to sodium nitrate is preferably 2.7 to 3.3:1, more preferably 3:1. The present invention has no special limitation on the mixing, and the process well known to those skilled in the art is adopted to ensure that the molybdenum disulfide and sodium nitrate are fully mixed. In the present invention, the role of the sodium nitrate is to enhance the redox reaction.

[0044] After obtaining the mixture, the present invention mixes the mixture with concentrated sulfuric acid to obtain a dispersion.

[0045] In the present invention, the mass ratio of molybdenum disulfide to concentrated sulfuric acid is preferably 2.7-3.3 g:50 mL, more preferably 3 g:50 mL; the mass concentration of concentrated sulfuric acid is preferably 98%. In the present invention, the mixing is preferably carried out under stirring; the stirring speed is preferably 400-500 r / min, more preferably 450 r / min, and the time is preferably 11-13 h, more preferably 12 h.

[0046] After obtaining the dispersion, the present invention mixes the dispersion with potassium permanganate to carry out an oxidation reaction, removes impurities from the obtained oxidation liquid, separates the solid from the liquid, and obtains oxidized molybdenum disulfide.

[0047] In the present invention, the mass ratio of potassium permanganate to molybdenum disulfide is preferably 1.7 to 2.3: 1, more preferably 2: 1. In the present invention, the mixing preferably comprises: adding potassium permanganate to the dispersion under ice bath conditions.

[0048] In the present invention, the oxidation reaction preferably includes: a first oxidation reaction and a second oxidation reaction are carried out in sequence; the temperature of the first oxidation reaction is preferably 0-3°C, more preferably 0-1°C; the time of the first oxidation reaction is preferably 0.2-1h, more preferably 0.5-0.6h; the temperature of the second oxidation reaction is preferably 33-37°C, more preferably 35°C; the time of the second oxidation reaction is preferably 2.8-3.2h, more preferably 3h.

[0049] In the present invention, the first oxidation reaction is preferably carried out in an ice bath; the second oxidation reaction is preferably carried out in an oil bath, and the oil bath process is preferably carried out under stirring conditions. The present invention has no special limitation on the stirring, and the stirring can be carried out using a process well known to those skilled in the art. The present invention converts molybdenum disulfide into oxidized molybdenum disulfide through an oxidation reaction.

[0050] In the present invention, the impurity removal preferably includes: placing the oxidized liquid in an ice bath, adding deionized water to the oxidized liquid for dilution, then transferring the resulting diluted liquid to room temperature, continuing to add deionized water to the diluted liquid to control the temperature of the diluted liquid below 60°C, and finally adding hydrogen peroxide and hydrochloric acid.

[0051] In the present invention, the mass ratio of the total volume of the deionized water to molybdenum disulfide is preferably 148-152 mL:3 g, more preferably 150 mL:3 g; the amount of the deionized water for dilution is preferably 30-35% of the total amount of the deionized water. In the present invention, the dilution is preferably carried out under stirring.

[0052] In the present invention, the mass concentration of the hydrogen peroxide is preferably 28-32%, more preferably 30%; the mass ratio of the volume of the hydrogen peroxide to molybdenum disulfide is preferably 7.8-8.2 mL:3 g, more preferably 8 mL:3 g. In the present invention, the purpose of adding deionized water and hydrogen peroxide is to more effectively remove excess potassium permanganate in the oxidizing liquid. In the present invention, the mass concentration of the hydrochloric acid is preferably 0.08-1.2%, more preferably 0.1%; the mass ratio of the volume of the hydrochloric acid to molybdenum disulfide is preferably 248-252 mL:3 g, more preferably 250 mL:3 g. In the present invention, the purpose of adding the hydrochloric acid is to remove metal elements in the oxidizing liquid.

[0053] In the present invention, the solid-liquid separation method is preferably filtration.

[0054] After the solid-liquid separation is completed, the present invention preferably further comprises drying the obtained solid to obtain molybdenum disulfide oxide. The present invention has no special requirements for the drying, and a drying process well known in the art can be used.

[0055] After obtaining the molybdenum disulfide oxide, the present invention mixes the molybdenum disulfide oxide, water and tannic acid, and performs ultrasonic stripping to obtain a tannic acid-modified molybdenum disulfide oxide dispersion.

[0056] In the present invention, the mass ratio of the molybdenum disulfide oxide to the volume ratio of water is preferably 110-130 mg:70-90 mL, and more preferably 120 mg:80 mL; the mass ratio of the molybdenum disulfide oxide to tannic acid is preferably (11-13):(3-20), and more preferably 12:(3-20), and further preferably 12:(3-10).

[0057] In the present invention, the power of the ultrasonic glass is preferably 300-600 W, more preferably 350-500 W; the time of the ultrasonic glass is preferably 2-48 hours, more preferably 2-12 hours, and most preferably 3-5 hours. In the present invention, an ultrasonic crusher is preferably used for ultrasonic peeling.

[0058] After obtaining the tannic acid-modified oxidized molybdenum disulfide dispersion, the present invention performs solid-liquid separation and solid drying on the tannic acid-modified oxidized molybdenum disulfide dispersion to obtain the tannic acid-modified oxidized molybdenum disulfide.

[0059] In the present invention, the solid-liquid separation is preferably performed by filtration; the present invention preferably uses a polytetrafluoroethylene (PTFE) microfiltration membrane for the filtration.

[0060] After the solid-liquid separation, the present invention preferably further comprises washing the obtained solid with deionized water and then drying. The present invention has no special limitation on the drying, and the drying can be carried out using a process well known to those skilled in the art.

[0061] In the present invention, the preparation process of the tannic acid modified oxidized molybdenum disulfide is as follows: Figure 1 shown.

[0062] The present invention provides tannic acid-modified oxidized molybdenum disulfide prepared by the preparation method described in the above scheme; the particle size of the tannic acid-modified oxidized molybdenum disulfide is preferably 50 to 2000 nm, more preferably 100 to 800 nm, and further preferably 200 to 500 nm.

[0063] TA@O-MoS prepared by the present invention 2 It exhibits good hydrophilicity and carries a negative charge. Using it to prepare membrane materials enhances the hydrophilicity and nuclear negative charge properties of the membrane surface, has a certain repelling effect on pollutants in the water, and thus improves the anti-pollution performance of the membrane surface.

[0064] The present invention provides a tannic acid modified oxidized molybdenum disulfide composite membrane, which is prepared from raw materials including the following mass percentages:

[0065] High molecular weight polymer 10-30%;

[0066] Polar organic solvent 47~89.99%;

[0067] 0.01-3% of the tannic acid-modified oxidized molybdenum disulfide according to claim 4 or 5;

[0068] Porogen 0.01~20%.

[0069] In terms of mass percentage, the raw materials for preparing the tannic acid modified oxidized molybdenum disulfide composite membrane provided by the present invention include 10-30% of a polymer, preferably 13-25%, and more preferably 15-20%. In the present invention, the polymer is preferably one or more of polyethersulfone, polysulfone, and polyimide, more preferably polyethersulfone or polysulfone. The present invention has no particular limitation on the molecular weight of the polymer, and a polymer suitable for preparing a membrane material well known to those skilled in the art can be used.

[0070] The raw materials for preparing the tannic acid modified oxidized molybdenum disulfide composite membrane provided by the present invention include 0.01-3%, preferably 0.05-2%, and more preferably 0.1-0.5% of the tannic acid modified oxidized molybdenum disulfide. The present invention improves the hydrophilicity and electronegativity of the membrane surface by adding tannic acid modified oxidized molybdenum disulfide, thereby improving the anti-pollution ability of the membrane.

[0071] In terms of mass percentage, the raw materials for preparing the tannic acid modified oxidized molybdenum disulfide composite film provided by the present invention include 0.01-20% of a porogen, preferably 0.1-18%, and more preferably 2-15%. In the present invention, the porogen is preferably one or more of polyethylene glycol, polyvinyl pyrrolidone, sodium dodecyl sulfate, lithium chloride, and water, and more preferably one or more of polyethylene glycol, polyvinyl pyrrolidone, sodium dodecyl sulfate, and water. In the present invention, when there are multiple porogens, the present invention has no special restrictions on the dosage ratio of each porogen, and they can be mixed in any proportion. In an embodiment of the present invention, the porogen is polyvinyl pyrrolidone, and the model is PVP K30.

[0072] In terms of mass percentage, the raw materials for preparing the tannic acid modified oxidized molybdenum disulfide composite film provided by the present invention include 47-89.99% polar organic solvent, preferably 50-80%, and more preferably 60-70%. In the present invention, the polar organic solvent is preferably one or more of N,N-dimethylformamide, N,N-dimethylacetamide and N-methylpyrrolidone, more preferably N,N-dimethylacetamide and / or N,N-dimethylformamide. In the present invention, when the polar organic solvent is multiple, the present invention has no special limitation on the usage ratio of each polar organic solvent, and they can be mixed in any proportion.

[0073] In the present invention, the thickness of the tannic acid modified oxidized molybdenum disulfide composite membrane is preferably 0.010-0.035 mm, more preferably 0.03 mm; the average pore size is preferably 3.5-5 nm, more preferably 4.0-4.5 nm; the porosity is preferably 45-75%, more preferably 50-60%; and the water contact angle of the membrane surface is preferably 40°-65°.

[0074] The tannic acid modified oxidized molybdenum disulfide composite membrane provided by the invention has hydrophilicity and negative charge, so that the membrane is not easily contaminated during use.

[0075] The present invention provides a method for preparing the tannic acid modified oxidized molybdenum disulfide composite film described in the above scheme, comprising the following steps:

[0076] Mixing the prepared raw materials to obtain a film casting solution;

[0077] The casting solution is coated to form a film, and is placed in an air bath and a coagulation bath in sequence to obtain the tannic acid modified molybdenum disulfide oxide composite film.

[0078] The present invention mixes various prepared raw materials to obtain a film casting solution.

[0079] In the present invention, the mixing preferably includes: firstly mixing the porogen, tannic acid-modified molybdenum disulfide oxide and polar organic solvent to obtain a first mixed solution; and then mixing the first mixed solution with a high molecular polymer for a second time.

[0080] In the present invention, the temperature of the first mixing is preferably 45-60° C., more preferably 50-55° C. In the present invention, the first mixing is preferably performed under ultrasonic conditions. The present invention has no special requirements on the time of the first mixing. In the embodiment of the present invention, the first mixing is specifically performed for 2 hours.

[0081] The present invention preferably heats the mixture from room temperature to the first mixed temperature. The present invention has no particular limitation on the rate of heating to the first mixed temperature, and any heating rate known to those skilled in the art may be selected.

[0082] In the present invention, the temperature of the second mixing is preferably 60 to 80°C, more preferably 70 to 75°C.

[0083] The present invention preferably heats the mixture from the temperature of the first mixing to the temperature of the second mixing. The present invention has no particular limitation on the rate of heating to the temperature of the second mixing, and any heating rate known to those skilled in the art may be selected. In the present invention, the second mixing is preferably carried out under stirring. The present invention has no particular requirement on the time of the second mixing, and the mixing may be carried out until the polymer is completely dissolved to form a uniform casting solution.

[0084] After obtaining the casting solution, the present invention preferably applies the casting solution into a film, and sequentially places it in an air bath and a coagulation bath to obtain the tannic acid-modified molybdenum disulfide oxide composite film.

[0085] Before the coating, the present invention preferably also includes degassing the casting liquid, and the degassing is preferably static degassing or vacuum degassing; the static degassing time is preferably 4 hours; the vacuum degree of the vacuum degassing is preferably 0.3-0.6MPa, more preferably 0.4MPa; the vacuum degassing time is preferably 3-12h, more preferably 4-8h.

[0086] The present invention has no special requirements for the coating and film-forming process, and the coating and film-forming process known in the art can be used. In the embodiment of the present invention, the coating is specifically performed on the polyester non-woven fabric using a scraper.

[0087] In the present invention, the temperature of the air bath is preferably room temperature; the time of the air bath is preferably 5 to 10 seconds, more preferably 8 seconds. In the present invention, a dense skin layer is formed on the membrane surface by air bathing.

[0088] In the present invention, the temperature of the coagulation bath is preferably 0-90°C, more preferably 20-40°C; the time of the coagulation bath is preferably 30-120s, more preferably 40-60s. In the present invention, the coagulation bath is preferably water or an organic solvent-water mixed solution; the organic solvent is preferably one or more of N,N-dimethylformamide, N,N-dimethylacetamide and N-methylpyrrolidone; the present invention has no special requirements for the ratio of organic solvent to water in the organic solvent-water mixed solution, and the ratio well known in the art can be used.

[0089] The tannic acid modified oxidized molybdenum disulfide and its preparation method, the tannic acid modified oxidized molybdenum disulfide composite film and its preparation method provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be understood as limiting the scope of protection of the present invention.

[0090] Comparative Example 1

[0091] Table 1 Raw material formula in comparative example 1

[0092]

[0093]

[0094] 1) According to Table 1, PVP K30 and polyethersulfone (PES) were added to N,N-dimethylacetamide solvent (DMAC), and stirred at 60° C. until they were completely dissolved to form a uniform and stable casting solution; the casting solution was poured into a sealed conical flask, and vacuum degassed to obtain a degassed casting solution;

[0095] 2) Use a scraper to coat the polyester non-woven fabric support layer, control the scraper thickness to 100 μm, place in an air bath at 25° C. for 10 seconds, then immerse in a 25° C. coagulation bath (water) for phase inversion to obtain a membrane material, store in deionized water for 24 hours, and replace clean deionized water several times for standby use.

[0096] Example 1

[0097] Table 2 Raw material formula in Example 1

[0098] Components Mass percentage (%) Polyethersulfone 20 PVPK30 16 DMAC 63.95 <![CDATA[TA@O-MoS 2 ]]> 0.05

[0099] 1) Mix 3.0g of flake molybdenum disulfide and 1.0g of NaNO 3 The mixture was mixed with 50 mL of concentrated sulfuric acid having a mass concentration of 98%, and then stirred at a rate of 500 r / min for 12 h to obtain a dispersion; 6.0 g of KMnO was slowly added to the dispersion under ice bath conditions. 4 , the first oxidation reaction was carried out for 0.5h, then, it was switched to an oil bath at 35°C, and the second oxidation reaction was carried out at a stirring rate of 350r / min for 3h, and finally moved into an ice bath, and 50mL of deionized water was added, and after stirring for 30min, it was removed from the ice bath, and 100mL of deionized water was added until room temperature, and the temperature was controlled below 60°C; then, 8.0mL of hydrogen peroxide with a mass concentration of 30% was added, and then 250mL of hydrochloric acid with a mass concentration of 10% was added, and finally, after filtering and drying, oxidized molybdenum disulfide nanosheets were obtained; 120mg of oxidized molybdenum disulfide nanosheets were added to 80mL of deionized water, and then 50mg of tannic acid was added to the above solution for mixing, and a 500W ultrasonic crusher was used for crushing for 2h to obtain a tannic acid-modified oxidized molybdenum disulfide mixed solution, and the obtained mixed solution was filtered with a polytetrafluoroethylene (PTFE) microfiltration membrane, washed with deionized water several times, and dried to obtain tannic acid (TA) modified O-MoS 2 (denoted as TA@O-MoS 2 ).

[0100] 2) According to Table 2, TA@O-MoS was added to N,N-dimethylacetamide solvent (DMAC). 2 and PVP K30, ultrasonically crushed at 50°C for 2h, then polyethersulfone (PES) was added, stirred at 60°C for 4h to completely dissolve and form a uniform casting solution; the casting solution was poured into a sealed conical flask and vacuum degassed to obtain the degassed casting solution.

[0101] 3) Use a scraper to coat the polyester non-woven fabric support layer, control the scraper thickness to 100 μm, place in an air bath at 25° C. for 10 s, then immerse in a 25° C. coagulation bath (water) for phase inversion to obtain a membrane material, store in deionized water for 24 h, replace the deionized water several times, and keep aside.

[0102] Example 2

[0103] Table 3 Raw material formula in Example 2

[0104] Components Mass percentage (%) Polyethersulfone 20 PVPK30 16 DMAC 63.9 <![CDATA[TA@O-MoS 2 ]]> 0.1

[0105] 1)TA@O-MoS 2 Preparation: Same as Example 1, except that 50 mg of tannic acid is replaced by 32 mg of tannic acid.

[0106] 2) According to Table 3, add TA@O-MoS to DMAC 2 and PVP K30, ultrasonically crushed at 50°C for 2h, then polyethersulfone (PES) was added in proportion, and stirred at 70°C for complete dissolution for 5h to form a uniform casting liquid; the casting liquid was poured into a sealed conical flask and vacuum degassed to obtain the degassed casting liquid.

[0107] 3) Use a scraper to coat the polyester non-woven fabric support layer, control the scraper thickness to 100 μm, place in an air bath at 25° C. for 10 seconds, then immerse in a 25° C. coagulation bath (water) for phase inversion to obtain a membrane material, store in deionized water for 24 hours, and replace clean deionized water several times for standby use.

[0108] Example 3

[0109] Table 4 Raw material formula in Example 3

[0110]

[0111]

[0112] 1)TA@O-MoS 2 Preparation: Same as Example 1, except that 50 mg of tannic acid is replaced by 40 mg of tannic acid.

[0113] 2) Add TA@O-MoS to DMAC2 and PVP K30, ultrasonically crushed at 50°C for 2h, then polyethersulfone (PES) was added in proportion, and stirred at 60°C for 4h to completely dissolve and form a uniform casting liquid; the casting liquid was poured into a sealed conical flask and vacuum degassed to obtain the degassed casting liquid.

[0114] 3) Use a scraper to coat the polyester non-woven fabric support layer, control the scraper thickness to 100 μm, place in an air bath at 25° C. for 10 seconds, then immerse in a 25° C. coagulation bath (water) for phase inversion to obtain a membrane material, store in deionized water for 24 hours, and replace clean deionized water several times for standby use.

[0115] Example 4

[0116] Table 5 Raw material formula in Example 4

[0117] Components Mass percentage (%) Polyethersulfone 20 PVPK30 16 NMP 63.8 <![CDATA[TA@O-MoS 2 ]]> 0.2

[0118] 1)TA@O-MoS 2 Preparation: Same as Example 1, except that 50 mg of tannic acid is replaced by 100 mg of tannic acid.

[0119] 2) According to Table 5, TA@O-MoS was added to N-methylpyrrolidone (NMP). 2 and PVP K30, ultrasonically crushed at 50°C for 2h, then polyethersulfone (PES) was added in proportion, and stirred at 60°C for 4h to completely dissolve and form a uniform casting liquid; the casting liquid was poured into a sealed conical flask and vacuum degassed to obtain the degassed casting liquid.

[0120] 3) Use a scraper to coat the polyester non-woven fabric support layer, control the scraper thickness to 100 μm, place in an air bath at 25° C. for 10 seconds, then immerse in a 25° C. coagulation bath (water) for phase inversion to obtain a membrane material, store in deionized water for 24 hours, and replace clean deionized water several times for standby use.

[0121] Comparative Example 2

[0122] Table 6 Raw material formula in comparative example 2

[0123]

[0124]

[0125] 1) According to Table 6, PVP K30 and polysulfone (PSF) were added to NMP in proportion, and the mixture was stirred at 60° C. for 4 h to completely dissolve and form a uniform casting solution; the casting solution was poured into a sealed conical flask and vacuum degassed to obtain a degassed casting solution.

[0126] 2) Use a scraper to coat the polyester non-woven fabric support layer, control the scraper thickness to 100 μm, place in an air bath at 25° C. for 10 seconds, then immerse in a 25° C. coagulation bath (water) for phase inversion to obtain a membrane material, store it in deionized water, and replace the clean deionized water several times for standby use.

[0127] Example 5

[0128] Table 7 Raw material formula in Example 5

[0129] Components Mass percentage (%) Polysulfone 20 SDS 0.5 <![CDATA[H 2 The]]> 0.5 NMP 78.9 <![CDATA[TA@O-MoS 2 ]]> 0.1

[0130] 1)TA@O-MoS 2 Preparation: Same as Example 1, except that 50 mg of tannic acid is replaced by 32 mg of tannic acid.

[0131] 2) According to Table 7, TA@O-MoS was added to NMP in proportion. 2 , water and sodium dodecyl sulfate (SDS), ultrasonically crush at 50°C for 2h, then add polysulfone (PSF) in proportion, stir at 60°C for complete dissolution for 4h to form a uniform casting liquid; pour the casting liquid into a sealed conical flask, vacuum degassing, and obtain the degassed casting liquid.

[0132] 3) Use a scraper to coat the polyester non-woven fabric support layer, control the scraper thickness to 100 μm, place in an air bath at 25° C. for 10 seconds, then immerse in a 25° C. coagulation bath (water) for phase inversion to obtain a membrane material, store it in deionized water, and replace the clean deionized water several times for standby use.

[0133] Structure and performance characterization:

[0134] The performance indicators of the membrane materials prepared in Comparative Examples 1-2 and Examples 1-5 are shown in Table 8. In Table 8, the PEG20000 and BSA retention rates refer to the retention rates when the concentrations of PEG20000 and BSA are 1000 ppm.

[0135] Table 8 Performance indicators of membrane materials prepared in comparative examples and examples

[0136]

[0137] From the results in Table 8, it can be seen that compared with the polyethersulfone membrane in Comparative Example 1, the TA@O-MoS prepared in Examples 1 to 4 2 The retention rate of polyethersulfone composite membrane for PEG20000 is above 82.5%, showing good retention performance of PEG20000. In addition, it can be seen from Table 8 that TA-O-MoS 2The addition of high-density polymer polyethersulfone makes the membrane surface have better hydrophilicity and surface roughness, which is manifested by a decrease in water contact angle and an increase in roughness. The enhanced hydrophilicity is conducive to the formation of a water film on the membrane surface, which can alleviate the adhesion of pollutants on the surface of the membrane, thereby improving the anti-pollution performance of the membrane, and the increase in roughness is conducive to increasing the effective contact area of ​​the membrane, thereby increasing the permeation flux of the membrane. In addition, in order to test the change in the charge intensity of the membrane surface of Example 2 and Comparative Example 1, the present invention characterized the membrane surface zeta potential of the two membranes, and the results are as follows Figure 4 As shown, from Figure 4 It can be seen that compared with comparative example 1, the surface nuclear negative charge of example 2 is significantly enhanced. The enhanced nuclear negative charge of the composite membrane surface is beneficial to improving the repulsion of nuclear negatively charged pollutants on the membrane surface and enhancing the anti-pollution performance of the membrane surface. Among examples 1 to 4, compared with comparative example 1, the polyethersulfone composite membrane example 2 has the best pure water flux of 140.98 L·m -2 ·h -1 bar -1 , is the original membrane of Example 1 (75.16 L·m -2 ·h -1 bar -1 ) was 1.88 times that of TA-O-MoS, and the retention rate of PEG 20000 also increased from 74.8% to 91.0%. Similarly, by comparing Comparative Example 2 with Example 5 under the conditions of polysulfone polymer, it can be seen that TA-O-MoS 2 The flux and retention of the polysulfone composite membrane are higher than those of Comparative Example 2, wherein the flux of Example 5 is 323.4 L·m -2 ·h -1 bar -1 , which is 2.15 times the flux of Example 2, and the BSA retention rate also increased from 97.8% in Example 2 to 98.6%, showing that the additive TA-O-MoS 2 Excellent improvement performance for polysulfone composite membrane.

[0138] TA-O-MoS prepared in Example 2 2 Atomic force microscopy (AFM) characterization was performed and the results are shown in Figure 2 , Figure 2 In the figure, a is an AFM image, and b to d are partial TA-O-MoS in a. 2 The thickness distribution of the nanosheets. Figure 2 It can be seen that TA-O-MoS 2 The thickness range is 1.61nm~1.79nm.

[0139] The membrane materials prepared in Comparative Example 1 and Example 2 were observed by transmission electron microscopy. The results are as follows: Figure 3 As shown, compared with Comparative Example 1 ( Figure 3 a) and Example 2 ( Figure 3 It can be clearly seen in b) that the cross section of Example 2 has embedded TA-O-MoS 2 Nanosheet materials, this result shows that TA-O-MoS 2 The nanosheets are successfully embedded in the membrane. This helps to improve the hydrophilicity of the membrane surface and enhance the anti-fouling ability of the membrane surface. In addition, due to the presence of hydrophilic nanomaterials, the pressure resistance of the membrane is further enhanced, and the flux stability of the membrane during actual operation is improved.

[0140] The present invention utilizes 10g / L CaCl 2 The membrane cleaning and flux recovery experiments were carried out on Comparative Example 1 and Example 2 using a cross-flow experimental device under 0.1 MPa conditions. The specific operation was that the membrane of Comparative Example 1 and Example 2 were run in the simulated rare earth wastewater for 60 minutes under 0.1 MPa conditions, and then run in clean water for 60 minutes. The same operation was repeated three times. The results are as follows: Figure 5 As shown. Figure 5 It can be seen that the membrane of Example 2 shows a significantly better permeation flux than the membrane of Comparative Example 1. Among them, the third-pass flux recovery rate of the membrane of Comparative Example 1 is 59%, and the third-pass flux recovery rate of the membrane of Example 2 is 72%. This significant difference indicates that the modified membrane of Example 2 has a more excellent anti-fouling performance.

[0141] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for preparing tannic acid modified oxidized molybdenum disulfide, characterized in that: The following steps are involved: mixing molybdenum disulfide and sodium nitrate to obtain a mixture; mixing the mixture with concentrated sulfuric acid to obtain a dispersion; The dispersion liquid is mixed with potassium permanganate to carry out an oxidation reaction, and the obtained oxidation liquid is subjected to impurity removal and solid-liquid separation to obtain oxidized molybdenum disulfide; The molybdenum disulfide oxide, water and tannic acid are mixed and subjected to ultrasonic stripping to obtain a tannic acid-modified molybdenum disulfide oxide dispersion; The tannic acid-modified molybdenum disulfide oxide dispersion is subjected to solid-liquid separation and solid drying to obtain tannic acid-modified molybdenum disulfide oxide.

2. The preparation method according to claim 1, characterized in that: The oxidation reaction comprises: a first oxidation reaction and a second oxidation reaction are performed in sequence; the temperature of the first oxidation reaction is 0 to 3° C., and the time is 0.2 to 1 h; the temperature of the second oxidation reaction is 33 to 37° C., and the time is 2.8 to 3.2 h.

3. The preparation method according to claim 1, characterized in that: The mass ratio of molybdenum disulfide oxide to tannic acid is (11-13):(3-20); the power of the ultrasonic stripping is 300-600W, and the time is 2-48h.

4. Tannic acid-modified oxidized molybdenum disulfide prepared by the preparation method according to any one of claims 1 to 3.

5. The tannic acid modified oxidized molybdenum disulfide according to claim 4, characterized in that: The particle size of the tannic acid modified oxidized molybdenum disulfide is 50 to 2000 nm.

6. A tannic acid modified oxidized molybdenum disulfide composite membrane prepared from the following raw materials in percentage by mass: High molecular weight polymer 10-30%; Polar organic solvent 47~89.99%; 0.01-3% of the tannic acid-modified oxidized molybdenum disulfide according to claim 4 or 5; Porogen 0.01~20%.

7. The tannic acid modified oxidized molybdenum disulfide composite film according to claim 6, characterized in that: The tannic acid modified oxidized molybdenum disulfide composite membrane has a thickness of 0.010-0.035 mm, an average pore size of 3.5-5 nm, a porosity of 45-75%, and a membrane surface water contact angle of 40°-65°.

8. The tannic acid modified oxidized molybdenum disulfide composite film according to claim 6 or 7, characterized in that: The high molecular polymer is one or more of polyethersulfone, polysulfone and polyimide; The porogen is one or more of polyethylene glycol, polyvinyl pyrrolidone, sodium lauryl sulfate, lithium chloride and water; The polar organic solvent is one or more of N,N-dimethylformamide, N,N-dimethylacetamide and N-methylpyrrolidone.

9. The method for preparing the tannic acid modified oxidized molybdenum disulfide composite film according to any one of claims 6 to 8, comprising the following steps: Mixing the prepared raw materials to obtain a film casting solution; The casting solution is coated to form a film, and is placed in an air bath and a coagulation bath in sequence to obtain the tannic acid modified molybdenum disulfide oxide composite film.

10. The preparation method according to claim 9, characterized in that: The temperature of the coagulation bath is 0-90° C., the time of the coagulation bath is 30-120 seconds; the coagulation bath is water or an organic solvent-water mixed solution.

Citation Information

Cited By

  • Molybdenum oxide-molybdenum disulfide poly-tannic acid electrode material and preparation method and application thereof

    CN121075823A

  • Molybdenum oxide-molybdenum disulfide@polytannic acid electrode materials, their preparation methods and applications

    CN121075823B