A method for preparing porous UO2 aerogel by sol-gel method

Through sol-gel method and CO2 supercritical drying technology, low-density and high-porosity uranium dioxide aerogels were prepared, which solved the problems of high density and low porosity of existing uranium oxide gels, and provided for nuclear use High-performance porous materials for fusion reaction.

CN118754203BActive Publication Date: 2024-11-26SHANDONG UNIV OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411245539.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-09-06
Publication Date
2024-11-26
Estimated Expiration
2044-09-06

AI Technical Summary

Technical Problem

The existing uranium oxide gel has high density, low porosity and uneven pore size distribution, resulting in unstable performance of nuclear fusion reactor materials.

Method used

Uranium dioxide aerogel was prepared by sol-gel method, using uranium source, complexing agent, and crosslinking agent as raw materials, and after gelation, CO2 supercritical drying and heat treatment, low-density and high porosity UO2 aerosol glue.

Benefits of technology

The preparation of UO2 aerogel with uniform pore size distribution, high porosity and low density is achieved, providing porous materials with excellent conversion effect, and improving the material performance under nuclear fusion reaction conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118754203B_ABST
    Figure CN118754203B_ABST
Patent Text Reader

Abstract

A method for preparing porous UO2 aerogel by a sol-gel method, wherein a wet gel is prepared by using a uranium source, a complexing agent, and a cross-linking agent as raw materials, and then a dry gel with low porosity, uniform pore size distribution, and low density is obtained by supercritical CO2 drying. Then, by controlling the heat treatment atmosphere and process at different stages, the components and structure of the gel are controlled, and finally a UO2 aerogel with low density, high porosity, and uniform pore size is obtained. And by controlling the components, gel, and heat treatment process, the controllable preparation of UO2 aerogel is achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The technical solution of the invention is used for preparing uranium dioxide aerogel by a sol-gel method, and belongs to the field of nuclear material preparation. Background Art

[0002] In indirect-driven inertial confinement laser fusion, the time-varying asymmetry of the drive in the black cavity is an important factor that causes the deterioration of the implosion performance, and the increase in the back reflection fraction caused by inflation is the main reason why the time-varying symmetry of the drive cannot be controlled. Therefore, the design of the black cavity tends to reduce the inflation density, but this also brings about the problem of too fast expansion of the cavity wall plasma. Preliminary research results at home and abroad show that low-density foam materials are beneficial to reducing the speed of the cavity wall plasma movement and improving the time-varying asymmetry of the black cavity drive. Therefore, the ideal foam material should be consistent with the material in the cavity and have a much lower density and uniform pore size distribution.

[0003] Aerogel is a low-density porous solid material composed of nanoparticles or polymer molecules that are aggregated with each other. It has high porosity and large internal surface area. The preparation method of aerogel is usually to first make it into a gel state through chemical reaction, and then obtain aerogel through a drying process. The sol-gel method is a conventional method for preparing uranium dioxide in the nuclear industry. However, the pores of wet gel are easily collapsed during the drying process due to the capillary force existing in the evaporation process, and the obtained is a fragmented dry gel, while supercritical drying can obtain aerogel with complete structure. Therefore, people have proposed supercritical drying of organic solvents, which can reach and maintain the supercritical state of organic solvents (250 ℃ and 300 bar) without crossing the liquid-gas phase boundary, and then reduce the pressure to ambient pressure at a constant temperature to achieve the purpose of drying. However, the process of reaching the supercritical state may destroy the cell structure of the gel through surface modification or accelerated maturation and aging. People have found that the critical conditions of CO2 (31 ℃ and 74 bar) are relatively mild compared with other organic solvents, and the structure of the gel changes very little, so CO2 supercritical drying is now a common method for preparing aerogels.

[0004] Uranium dioxide has excellent thermal stability, chemical stability, high melting point, stable performance and not easy to deform under irradiation, and is the most widely used nuclear material. Therefore, the preparation of uranium dioxide aerogel with high porosity, low density and thermal stability is of great significance to improving the conditions of nuclear fusion reactions. Summary of the invention

[0005] The technical solution of the present invention aims to provide an aerogel preparation solution to solve the problems of high density, low porosity, uneven pore size distribution, etc. of the existing uranium oxide gel, thereby solving the problem of unstable material performance in current nuclear fusion reactors.

[0006] The technical solution of the present invention adopts the sol-gel method to prepare uranium dioxide aerogel, uses a uranium source, a complexing agent, and a cross-linking agent as raw materials, gels at a certain temperature after mixing, and then obtains uranium oxide aerogel by CO2 supercritical drying of the wet gel, and then obtains UO2 aerogel by heat treatment reduction.

[0007] Compared with the prior art, the technical solution of the present invention realizes the synthesis of UO2 aerogel with low density and high porosity by selecting appropriate uranium source, complexing agent, cross-linking agent, designing raw material components, gel process, CO2 supercritical drying technology process and heat treatment conditions, solving the problems of UO2 aerogel that is difficult to prepare by the prior method, and UO2 aerogel with high density, large pore size and uneven distribution, and obtains UO2 aerogel with uniform pore size distribution, high porosity and low density. The realization of this technology provides a very potential porous material with excellent conversion effect for the black cavity lining of laser nuclear fusion target.

[0008] The present invention is a method for preparing a UO2 aerogel with high porosity, low density and thermal stability, wherein the method is carried out according to the following steps:

[0009] (1) dissolving a uranium source, a complexing agent, and a cross-linking agent in deionized water, and stirring at low temperature to form a precursor solution;

[0010] (2) placing the precursor solution in an oven to gel, and soaking the obtained wet gel in ethanol;

[0011] (3) drying the wet gel obtained in step (2) using a CO2 supercritical dryer;

[0012] (4) subjecting the dried gel to high temperature heat treatment;

[0013] (5) The gel after heat treatment in step (4) is heat treated in a reducing atmosphere to finally obtain UO2 aerogel.

[0014] Furthermore, the uranium source described in step (1) is uranyl nitrate or uranyl acetate; the complexing agent is one or more of urea, citric acid, ammonia solution, ascorbic acid, and dibutyl phthalate; and the cross-linking agent is one or more of hexamethylenetetramine, trimethylhexamethylenediamine, trimethylhexamethylenediamine, diethylamine, dipropylenetriamine, vinyltriamine, ethylenediamine, diethylenetriamine, dimethylaminopropylamine, and diethylaminopropylamine.

[0015] The uranium source, the complexing agent and the cross-linking agent are dissolved in deionized water, and the low temperature stirring temperature is 0-20°C, and the stirring time is 1-120 min. The concentration ratio of the uranium source, the complexing agent and the cross-linking agent in the raw material is 0.1-2.0: 1.0-2.0: 1.0-3.0.

[0016] Furthermore, in step (2), the temperature of the gel in the oven is 20-90°C, the gel time is 0.1-72 h, and the soaking time in ethanol is 0.1-24 h.

[0017] Furthermore, in step (3), the ethanol in the gel is replaced by liquid CO2 for 1 to 12 h, and when the CO2 supercritical state is reached, it is maintained for 0.1 to 0.5 h.

[0018] Furthermore, in step (4), the heating rate is 1-10°C / min, the heat treatment temperature is 400-600°C, and the holding time is 0.5-3 h.

[0019] Furthermore, in step (5), the reducing atmosphere is a hydrogen-argon mixture or hydrogen, the heating rate is 1-10 °C / min, the heat treatment temperature is 900-1500 °C, and the heat treatment time is 1-36 h. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 The XRD patterns of the UO2 aerogel samples prepared in Examples 1 to 11 are as follows:

[0021] Figure 2 This is a scan of the UO2 aerogel sample prepared in Example 1.

[0022] Figure 3 This is a scan of the UO2 aerogel sample prepared in Example 2.

[0023] Figure 4 This is a scan image of the UO2 aerogel sample prepared in Example 3. DETAILED DESCRIPTION

[0024] The present invention will be further described below in conjunction with the embodiments. However, the scope of the present invention is not limited to the following embodiments. It will be appreciated by those skilled in the art that various changes and modifications may be made to the present invention without departing from the spirit and scope of the present invention.

[0025] The instruments, reagents, and materials involved in the following examples, unless otherwise specified, are all conventional instruments, reagents, and materials available in the prior art and can be obtained through regular commercial channels. The experimental methods, detection methods, etc. involved in the following examples, unless otherwise specified, are all conventional experimental methods and detection methods available in the prior art.

[0026] Example:

[0027] Embodiment 1, a method for preparing porous UO2 aerogel by a sol-gel method, comprising the following steps:

[0028] (1) preparing a mixed solution of uranyl nitrate, hexamethylenetetramine and urea at a concentration ratio of 1:1.75:1.75; placing the mixed solution in an ice bath at 0°C for 5 min, and then stirring for 3 min;

[0029] (2) The mixed solution was placed in an oven at 80 °C and allowed to gel for 4 h before being immersed in ethanol for 24 h.

[0030] (3) Transfer the soaked gel to a CO2 supercritical dryer and pour 20 ml of ethanol into the chamber of the CO2 supercritical dryer to completely immerse the gel. Open the air inlet and CO2 cylinder, and open the air outlet at the same time, and use CO2 to replace the alcohol for 10 hours;

[0031] (4) After CO2 reaches the supercritical state, maintain it for 0.5 h and open the gas outlet until the pressure drops to 0;

[0032] (5) Place the supercritical dried sample in a muffle furnace, heat it to 450 °C at a rate of 5 °C / min in an air atmosphere, and keep it at that temperature for 1 h;

[0033] (6) In a tubular furnace, the temperature was raised to 450 °C at a rate of 5 °C / min in an argon atmosphere, and kept at this temperature for 5 min. Then, a mixed gas of 8% H2 and 92% Ar was introduced, and the temperature was raised to 600 °C at a rate of 5 °C / min and kept at this temperature for 1 h. Then, the temperature was raised to 1000 °C at a rate of 4 °C / min and kept at this temperature for 4 h. After cooling to room temperature, UO2 aerogel with high porosity, low density and high thermal stability was obtained.

[0034] The porosity of the uranium dioxide aerogel prepared in this example is 93.86% and the density is 0.263 g / cm 3 Its XRD spectrum is as attached Figure 1 As shown, the scanned photos are attached Figure 2 shown.

[0035] Embodiment 2, a method for preparing porous UO2 aerogel by a sol-gel method, comprising the following steps:

[0036] (1) Prepare a mixed solution of uranyl nitrate, hexamethyltetramine and citric acid at a concentration ratio of 1:1.75:1.8; place the mixed solution in an ice bath at 4°C for 5 min, and then stir for 10 min;

[0037] (2) The mixed solution was placed in an oven at 80 °C and allowed to gel for 4 h before being immersed in ethanol for 24 h.

[0038] (3) Transfer the soaked gel to a CO2 supercritical dryer and pour 20 ml of ethanol into the chamber of the CO2 supercritical dryer to completely immerse the gel. Open the air inlet and CO2 cylinder, and open the air outlet at the same time, and use CO2 to replace the alcohol for 10 hours;

[0039] (4) After CO2 reaches the supercritical state, maintain it for 0.2 h and open the gas outlet until the pressure drops to 0;

[0040] (5) Place the supercritical dried sample in a muffle furnace, heat it to 450 °C at a rate of 2 °C / min in an air atmosphere, and keep it at that temperature for 1 h;

[0041] (6) In a tubular furnace, the temperature was raised to 450 °C at a rate of 5 °C / min in an argon atmosphere, and kept at this temperature for 5 min. Then, a mixed gas of 8% H2 and 92% Ar was introduced, and the temperature was raised to 600 °C at a rate of 5 °C / min and kept at this temperature for 1 h. Then, the temperature was raised to 900 °C at a rate of 4 °C / min and kept at this temperature for 4 h. After cooling to room temperature, UO2 aerogel with high porosity, low density and high thermal stability was obtained.

[0042] The porosity of the uranium dioxide aerogel prepared in this example is 92.61% and the density is 0.352 g / cm 3 Its XRD spectrum is as attached Figure 1 As shown, the scanned photos are attached Figure 3 shown.

[0043] Embodiment 3, a method for preparing porous UO2 aerogel by sol-gel method, comprising the following steps:

[0044] (1) Prepare a mixed solution of uranyl nitrate, trimethylhexamethylenediamine and citric acid at a concentration ratio of 1.5:1.75:1.8; refrigerate the mixed solution in an ice bath at 4°C for 10 min, and then stir for 10 min;

[0045] (2) The mixed solution was placed in an oven at 60 °C and allowed to gel for 8 h before being immersed in ethanol for 12 h.

[0046] (3) Transfer the soaked gel to a CO2 supercritical dryer and pour 20 ml of ethanol into the chamber of the CO2 supercritical dryer to completely immerse the gel. Open the air inlet and CO2 cylinder, and open the air outlet at the same time, and use CO2 to replace the alcohol for 6 hours;

[0047] (4) After CO2 reaches the supercritical state, maintain it for 0.2 h and open the gas outlet until the pressure drops to 0;

[0048] (5) Place the supercritical dried sample in a muffle furnace, heat it to 450 °C at a rate of 2 °C / min in an air atmosphere, and keep it at that temperature for 1 h;

[0049] (6) In a tubular furnace, the temperature was raised to 450 °C at a rate of 10 °C / min in an argon atmosphere, and kept at this temperature for 5 min. Then, a mixed gas of 8% H2 and 92% Ar was introduced, and the temperature was raised to 600 °C at a rate of 5 °C / min and kept at this temperature for 1 h. Then, the temperature was raised to 1100 °C at a rate of 4 °C / min and kept at this temperature for 6 h. After cooling to room temperature, UO2 aerogel with high porosity, low density and high thermal stability was obtained.

[0050] The porosity of the uranium dioxide aerogel prepared in this example is 94.58% and the density is 0.248 g / cm 3 Its XRD spectrum is as attached Figure 1 As shown, the scanned photos are attached Figure 4 shown.

[0051] Embodiment 4, a method for preparing porous UO2 aerogel by a sol-gel method, comprising the following steps:

[0052] (1) Prepare a mixed solution of uranyl nitrate, trimethylhexanediamine and citric acid at a concentration ratio of 1:1.75:1.8; place the mixed solution in an ice bath at 0°C for 5 min, and then stir for 10 min;

[0053] (2) The mixed solution was placed in an oven at 70 °C and allowed to gel for 6 h before being immersed in ethanol for 24 h.

[0054] (3) Transfer the soaked gel to a CO2 supercritical dryer and pour 20 ml of ethanol into the chamber of the CO2 supercritical dryer to completely immerse the gel. Open the air inlet and CO2 cylinder, and open the air outlet at the same time, and use CO2 to replace the alcohol for 10 hours;

[0055] (4) After CO2 reaches the supercritical state, maintain it for 0.5 h and open the gas outlet until the pressure drops to 0;

[0056] (5) Place the supercritical dried sample in a muffle furnace, heat it to 450 °C at a rate of 1 °C / min in an air atmosphere, and keep it at that temperature for 1 h;

[0057] (6) In a tubular furnace, the temperature was raised to 450 °C at a rate of 5 °C / min in an argon atmosphere, and kept at this temperature for 5 min. Then, a mixed gas of 8% H2 and 92% Ar was introduced, and the temperature was raised to 600 °C at a rate of 10 °C / min, and kept at this temperature for 1 h. Then, the temperature was raised to 1200 °C at a rate of 4 °C / min, and kept at this temperature for 4 h. After cooling to room temperature, UO2 aerogel with high porosity, low density and high thermal stability was obtained.

[0058] The porosity of the uranium dioxide aerogel prepared in this example is 94.88% and the density is 0.236 g / cm 3 Its XRD spectrum is as attached Figure 1 shown.

[0059] Embodiment 5, a method for preparing porous UO2 aerogel by a sol-gel method, comprising the following steps:

[0060] (1) preparing a mixed solution of uranyl nitrate, diethylamine and ascorbic acid at a concentration ratio of 1:1.5:2.25; refrigerating the mixed solution in an ice bath at 0°C for 5 min, and then stirring for 30 min;

[0061] (2) The mixed solution was placed in an oven at 50 °C and allowed to gel for 10 h before being immersed in ethanol for 24 h.

[0062] (3) Transfer the soaked gel to a CO2 supercritical dryer and pour 20 ml of ethanol into the chamber of the CO2 supercritical dryer to completely immerse the gel. Open the air inlet and CO2 cylinder, and open the air outlet at the same time, and use CO2 to replace the alcohol for 10 hours;

[0063] (4) After CO2 reaches the supercritical state, maintain it for 0.1 h and open the gas outlet until the pressure drops to 0;

[0064] (5) Place the supercritical dried sample in a muffle furnace, heat it to 500 °C at a rate of 2 °C / min in an air atmosphere, and keep it at this temperature for 2 h;

[0065] (6) In a tubular furnace, in an argon atmosphere, the temperature was raised to 500 °C at a rate of 10 °C / min, and kept at this temperature for 10 min. Then, a mixed gas of 8% H2 and 92% Ar was introduced, and the temperature was raised to 600 °C at a rate of 2 °C / min, and kept at this temperature for 1 h; then, the temperature was raised to 1000 °C at a rate of 2 °C / min, and kept at this temperature for 4 h. After cooling to room temperature, UO2 aerogel with high porosity, low density and high thermal stability was obtained.

[0066] The porosity of the uranium dioxide aerogel prepared in this example is 95.35% and the density is 0.227 g / cm 3 Its XRD spectrum is as attached Figure 1 shown.

[0067] Embodiment 6, a method for preparing porous UO2 aerogel by a sol-gel method, comprising the following steps:

[0068] (1) Prepare a mixed solution of uranyl acetate, dibutyl phthalate and dipropylene triamine at a concentration ratio of 1:1.5:2.5; refrigerate the mixed solution in an ice bath at 0°C for 5 min, and then stir for 30 min;

[0069] (2) The mixed solution was placed in an oven at 30 °C and allowed to gel for 36 h before being immersed in ethanol for 24 h.

[0070] (3) Transfer the soaked gel to a CO2 supercritical dryer and pour 20 ml of ethanol into the chamber of the CO2 supercritical dryer to completely immerse the gel. Open the air inlet and CO2 cylinder, and open the air outlet at the same time, and use CO2 to replace the alcohol for 10 hours;

[0071] (4) After CO2 reaches the supercritical state, maintain it for 0.1 h and open the gas outlet until the pressure drops to 0;

[0072] (5) Place the supercritical dried sample in a muffle furnace, heat it to 500 °C at a rate of 2 °C / min in an air atmosphere, and keep it at this temperature for 2 h;

[0073] (6) In a tubular furnace, in an argon atmosphere, the temperature was raised to 500 °C at a rate of 10 °C / min, and kept at this temperature for 10 min. Then, a mixed gas of 8% H2 and 92% Ar was introduced, and the temperature was raised to 600 °C at a rate of 2 °C / min, and kept at this temperature for 1 h; then, the temperature was raised to 1200 °C at a rate of 2 °C / min, and kept at this temperature for 4 h. After cooling to room temperature, UO2 aerogel with high porosity, low density and high thermal stability was obtained.

[0074] The porosity of the uranium dioxide aerogel prepared in this example is 95.22% and the density is 0.23 g / cm 3 Its XRD spectrum is as attached Figure 1 shown.

[0075] Embodiment 7, a method for preparing porous UO2 aerogel by a sol-gel method, comprising the following steps:

[0076] (1) preparing a mixed solution of uranyl acetate, dibutyl phthalate and ethylenetriamine at a concentration ratio of 1:1.5:2; refrigerating the mixed solution in an ice bath at 10°C for 30 min, and then stirring for 15 min;

[0077] (2) The mixed solution was placed in an oven at 30 °C and allowed to gel for 36 h before being immersed in ethanol for 24 h.

[0078] (3) Transfer the soaked gel to a CO2 supercritical dryer and pour 20 ml of ethanol into the chamber of the CO2 supercritical dryer to completely immerse the gel. Open the air inlet and CO2 cylinder, and open the air outlet at the same time, and use CO2 to replace the alcohol for 10 hours;

[0079] (4) After CO2 reaches the supercritical state, maintain it for 0.1 h and open the gas outlet until the pressure drops to 0;

[0080] (5) Place the supercritical dried sample in a muffle furnace, heat it to 500 °C at a rate of 2 °C / min in an air atmosphere, and keep it at this temperature for 2 h;

[0081] (6) In a tubular furnace, in an argon atmosphere, the temperature was raised to 500 °C at a rate of 10 °C / min, and kept at this temperature for 10 min. Then, a mixed gas of 8% H2 and 92% Ar was introduced, and the temperature was raised to 600 °C at a rate of 2 °C / min, and kept at this temperature for 1 h; then, the temperature was raised to 1300 °C at a rate of 2 °C / min, and kept at this temperature for 8 h. After cooling to room temperature, UO2 aerogel with high porosity, low density and high thermal stability was obtained.

[0082] The porosity of the uranium dioxide aerogel prepared in this example is 90.81% and the density is 0.336 g / cm 3 Its XRD spectrum is as attached Figure 1 shown.

[0083] Embodiment 8, a method for preparing porous UO2 aerogel by a sol-gel method, comprising the following steps:

[0084] (1) preparing a mixed solution of uranyl acetate, ammonia solution and ethylenediamine at a concentration ratio of 1:1:1.5; refrigerating the mixed solution in an ice bath at 0°C for 5 min, and then stirring for 30 min;

[0085] (2) The mixed solution was placed in an oven at 60 °C and allowed to gel for 10 h before being immersed in ethanol for 24 h.

[0086] (3) Transfer the soaked gel to a CO2 supercritical dryer and pour 20 ml of ethanol into the chamber of the CO2 supercritical dryer to completely immerse the gel. Open the air inlet and CO2 cylinder, and open the air outlet at the same time, and use CO2 to replace the alcohol for 10 hours;

[0087] (4) After CO2 reaches the supercritical state, maintain it for 0.1 h and open the gas outlet until the pressure drops to 0;

[0088] (5) Place the supercritical dried sample in a muffle furnace, heat it to 550 °C at a rate of 5 °C / min in an air atmosphere, and keep it at this temperature for 3 h;

[0089] (6) In a tubular furnace, in an argon atmosphere, the temperature was raised to 500 °C at a rate of 10 °C / min, and kept at this temperature for 10 min. Then, a mixed gas of 8% H2 and 92% Ar was introduced, and the temperature was raised to 600 °C at a rate of 2 °C / min, and kept at this temperature for 2 h; then, the temperature was raised to 1400 °C at a rate of 2 °C / min, and kept at this temperature for 5 h. After cooling to room temperature, UO2 aerogel with high porosity, low density and high thermal stability was obtained.

[0090] The porosity of the uranium dioxide aerogel prepared in this example is 94.82% and the density is 0.24 g / cm 3 Its XRD spectrum is as attached Figure 1 shown.

[0091] Embodiment 9, a method for preparing porous UO2 aerogel by a sol-gel method, comprising the following steps:

[0092] (1) preparing a mixed solution of uranyl acetate, ascorbic acid and diethylenetriamine at a concentration ratio of 1:1.5:1.5; refrigerating the mixed solution in an 8°C ice bath for 10 min, and then stirring for 15 min;

[0093] (2) The mixed solution was placed in an oven at 80 °C and allowed to gel for 4 h before being immersed in ethanol for 12 h.

[0094] (3) Transfer the soaked gel to a CO2 supercritical dryer and pour 20 ml of ethanol into the chamber of the CO2 supercritical dryer to completely immerse the gel. Open the air inlet and CO2 cylinder, and open the air outlet at the same time, and use CO2 to replace the alcohol for 10 hours;

[0095] (4) After CO2 reaches the supercritical state, maintain it for 0.1 h and open the gas outlet until the pressure drops to 0;

[0096] (5) Place the supercritical dried sample in a muffle furnace, heat it to 500 °C at a rate of 2 °C / min in an air atmosphere, and keep it at this temperature for 2 h;

[0097] (6) In a tubular furnace, in an argon atmosphere, the temperature was raised to 500 °C at a rate of 10 °C / min, and kept at this temperature for 10 min. Then, a mixed gas of 8% H2 and 92% Ar was introduced, and the temperature was raised to 700 °C at a rate of 2 °C / min, and kept at this temperature for 2 h; then, the temperature was raised to 1400 °C at a rate of 2 °C / min, and kept at this temperature for 3 h. After cooling to room temperature, UO2 aerogel with high porosity, low density and high thermal stability was obtained.

[0098] The porosity of the uranium dioxide aerogel prepared in this example is 93.62% and the density is 0.276 g / cm 3 Its XRD spectrum is as attached Figure 1 shown.

[0099] Embodiment 10, a method for preparing porous UO2 aerogel by a sol-gel method, comprising the following steps:

[0100] (1) preparing a mixed solution of uranyl acetate, urea and dimethylaminopropylamine at a concentration ratio of 1:1.75:1.75; refrigerating the mixed solution in an ice bath at 0°C for 10 min, and then stirring for 30 min;

[0101] (2) The mixed solution was placed in an oven at 90 °C and allowed to gel for 2 h before being immersed in ethanol for 24 h.

[0102] (3) Transfer the soaked gel to a CO2 supercritical dryer and pour 20 ml of ethanol into the chamber of the CO2 supercritical dryer to completely immerse the gel. Open the air inlet and CO2 cylinder, and open the air outlet at the same time, and use CO2 to replace the alcohol for 5 hours;

[0103] (4) After CO2 reaches the supercritical state, maintain it for 0.1 h and open the gas outlet until the pressure drops to 0;

[0104] (5) Place the supercritical dried sample in a muffle furnace, heat it to 500 °C at a rate of 2 °C / min in an air atmosphere, and keep it at this temperature for 2 h;

[0105] (6) In a tubular furnace, in an argon atmosphere, the temperature was raised to 500 °C at a rate of 10 °C / min, and kept at this temperature for 10 min. Then, a mixed gas of 8% H2 and 92% Ar was introduced, and the temperature was raised to 700 °C at a rate of 2 °C / min, and kept at this temperature for 1 h; then, the temperature was raised to 1500 °C at a rate of 2 °C / min, and kept at this temperature for 3 h. After cooling to room temperature, UO2 aerogel with high porosity, low density and high thermal stability was obtained.

[0106] The porosity of the uranium dioxide aerogel prepared in this example is 95.82% and the density is 0.193 g / cm 3 Its XRD spectrum is as attached Figure 1 shown.

[0107] Embodiment 11, a method for preparing porous UO2 aerogel by a sol-gel method, comprising the following steps:

[0108] (1) preparing a mixed solution of uranyl acetate, citric acid and diethylaminopropylamine at a concentration ratio of 1:1.75:1.75; placing the mixed solution in an ice bath at 0°C for 10 min, and then stirring for 30 min;

[0109] (2) The mixed solution was placed in an oven at 90 °C and allowed to gel for 2 h before being immersed in ethanol for 24 h.

[0110] (3) Transfer the soaked gel to a CO2 supercritical dryer and pour 20 ml of ethanol into the chamber of the CO2 supercritical dryer to completely immerse the gel. Open the air inlet and CO2 cylinder, and open the air outlet at the same time, and use CO2 to replace the alcohol for 5 hours;

[0111] (4) After CO2 reaches the supercritical state, maintain it for 0.1 h and open the gas outlet until the pressure drops to 0;

[0112] (5) Place the supercritical dried sample in a muffle furnace, heat it to 500 °C at a rate of 2 °C / min in an air atmosphere, and keep it at this temperature for 2 h;

[0113] (6) In a tubular furnace, the temperature was raised to 500 °C at a rate of 5 °C / min in an argon atmosphere, and kept at this temperature for 10 min. Then, a mixed gas of 8% H2 and 92% Ar was introduced, and the temperature was raised to 700 °C at a rate of 2 °C / min, and kept at this temperature for 1 h. Then, the temperature was raised to 1000 °C at a rate of 2 °C / min, and kept at this temperature for 6 h. After cooling to room temperature, UO2 aerogel with high porosity, low density and high thermal stability was obtained.

[0114] The porosity of the uranium dioxide aerogel prepared in this example is 95.5% and the density is 0.21 g / cm 3 Its XRD spectrum is as attached Figure 1 shown.

[0115] The density and porosity of each example are shown in Table 1 below.

[0116] Table 1 Density and porosity of specific examples

[0117] sample Embodiment 1 Embodiment 2 Embodiment 3 Embodiment 4 Embodiment 5 Embodiment 6 Embodiment 7 Embodiment 8 Embodiment 9 Embodiment 10 Embodiment 11 <![CDATA[Density (g / cm 3 )]]> 0.263 0.352 0.248 0.236 0.227 0.23 0.336 0.24 0.276 0.193 0.21 Porosity(%) 93.86 92.61 94.58 94.88 95.35 95.22 90.81 94.82 93.62 95.82 95.5

[0118] Comparative Example 1:

[0119] The difference from Example 1 is that in step (6), the temperature is raised to 450°C at a rate of 15°C / min in an argon atmosphere in a tubular furnace, kept warm for 5 min, and then a mixed gas of 8% H2 and 92% Ar is introduced, and then the temperature is raised to 1000°C at a rate of 15°C / min and kept warm for 4 h; the other experimental conditions are the same. The porosity of the product prepared in this comparative example is 75.2% and the density is 0.56 g / cm3 .

[0120] Comparative Example 2:

[0121] The difference from Example 1 is that the drying method selected is freeze drying instead of supercritical drying. The other experimental conditions are the same. The porosity of the product prepared in this comparative example is 62.6% and the density is 0.62 g / cm 3 .

[0122] By the attached Figure 1 It can be seen that the products prepared in Examples 1 to 11 all have diffraction peaks at 28.3°, 32.7°, 47°, 55.7°, 58.4°, 68.5°, 75.7°, 78.1°, and 87.3°. It can be seen that the UO2 aerogel prepared by the present invention has the same properties, and compared with the UO2 standard PDF card (PDF#41-1422), the diffraction peaks of the XRD spectrum are completely consistent and there are no extra impurity peaks.

[0123] The microscopic morphologies of the UO2 aerogels prepared in Examples 1 to 11 are basically similar, all showing the shape of "micron flowers" with a single particle size of 2-5 μm. It is this special morphology that makes the UO2 aerogel have the characteristics of high porosity and low density. This low-density and high-porosity foam material can reduce the movement speed of the cavity wall plasma and improve the time-varying asymmetry of the black cavity drive.

[0124] There are no public reports on the preparation of UO2 aerogels, so this method provides a new and feasible solution for the preparation and structural control of UO2 aerogels.

Claims

1. A method for preparing porous UO2 aerogel by a sol-gel process, characterized in that: The preparation process includes the following steps: (1) Dissolve the uranium source, complexing agent, and cross-linking agent in deionized water and stir evenly at low temperature to form a precursor solution; (2) placing the precursor solution in an oven to gel, and soaking the resulting wet gel in ethanol; (3) drying the wet gel obtained in step (2) using a CO2 supercritical dryer; (4) subjecting the dried gel to high temperature heat treatment; (5) The gel heat-treated in step (4) is heat-treated in a reducing atmosphere to finally obtain UO2 aerogel.

2. The method for preparing porous UO2 aerogel by a sol-gel method as claimed in claim 1, characterized in that: The uranium source described in step (1) is uranyl nitrate or uranyl acetate; the complexing agent is one or more of urea, citric acid, ammonia solution, ascorbic acid, and dibutyl phthalate; and the cross-linking agent is one or more of hexamethylenetetramine, trimethylhexamethylenediamine, trimethylhexamethylenediamine, diethylamine, dipropylenetriamine, vinyltriamine, ethylenediamine, diethylenetriamine, dimethylaminopropylamine, and diethylaminopropylamine.

3. A method for preparing porous UO2 aerogel by a sol-gel method as described in claim 1, wherein the uranium source, the complexing agent, and the cross-linking agent are dissolved in deionized water, the low-temperature stirring temperature is 0-20°C, and the stirring time is 1-120 min; the concentration ratio of the uranium source, the complexing agent, and the cross-linking agent in the raw material is 0.1-2.0: 1.0-2.0: 1.0-3.

0.

4. The method for preparing porous UO2 aerogel by a sol-gel method as claimed in claim 1, characterized in that: In step (2), the temperature of the gel in the oven is 20-90° C., the gel time is 0.1-72 h, and the soaking time in ethanol is 0.1-72 h.

5. The method for preparing porous UO2 aerogel by a sol-gel method as claimed in claim 1, characterized in that: In step (3), the ethanol in the gel is replaced by liquid CO2 for 1 to 12 h, and the supercritical state of CO2 is maintained for 0.1 to 24 h.

6. The method for preparing porous UO2 aerogel by a sol-gel method as claimed in claim 1, characterized in that: In step (4), the heating rate is 1-10 °C / min, the heat treatment temperature is 400-600 °C, and the holding time is 0.1-12 h.

7. The method for preparing porous UO2 aerogel by a sol-gel method as claimed in claim 1, characterized in that: In step (5), the reducing atmosphere is a hydrogen-argon mixture or hydrogen, the heating rate is 1-10 °C / min, the heat treatment temperature is 900-1500 °C, and the heat treatment time is 0.1-36 h.