Ternary positive electrode material and preparation method thereof
Through wet mixing and spray-drying granulation of amorphous ternary precursors and lithium sources, the problem of difficulty and high cost in the preparation process of ternary cathode materials is solved, the consistency and stability of the materials are improved, and the electrochemistry is improved. performance.
Patent Information
- Application Number
- CN202410737019.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-07
- Publication Date
- 2024-10-11
AI Technical Summary
The existing ternary cathode material preparation process is difficult to implement, the cost is high, and the consistency and stability of the resulting materials are poor.
An amorphous ternary precursor is generated by reacting an aqueous solution of mixed salt with an alkali, and is configured with a lithium source as a slurry for spray drying and granulation, followed by sintering, avoiding the need for precise control of product properties using complexing agents and achieving Uniform mixing and optimization of particle size distribution at the molecular level.
The preparation process is simplified, the cost is reduced, the consistency and stability of the ternary cathode material is improved, and the electrochemical performance is improved.
Smart Images

Figure CN118754207A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of ternary positive electrode materials, and in particular relates to a ternary positive electrode material and a preparation method thereof. Background Art
[0002] The positive electrode of the ternary lithium battery includes a ternary positive electrode material.
[0003] In some related technologies, the preparation process of ternary positive electrode materials is difficult to implement and has high cost, and the consistency and stability of the obtained ternary positive electrode materials are poor. Summary of the invention
[0004] The present invention at least partially solves the problems that the existing ternary positive electrode material preparation process is difficult to implement, the cost is high, and the consistency and stability of the obtained ternary positive electrode material are poor, and provides a ternary positive electrode material and a preparation method thereof.
[0005] In a first aspect, an embodiment of the present invention provides a method for preparing a ternary positive electrode material, which comprises:
[0006] The aqueous solution of the mixed salt is reacted with a base to generate an amorphous ternary precursor; the mixed salt comprises a nickel salt, a cobalt salt, and a manganese salt;
[0007] Preparing a slurry; the slurry includes a lithium source and the ternary precursor;
[0008] The slurry is spray-dried and granulated to obtain a dry material;
[0009] The dried material is sintered to obtain a ternary positive electrode material.
[0010] Optionally, the molar ratio of nickel, cobalt and manganese in the mixed salt is x:y:z;
[0011] Where x+y+z=1,0 <x≤0.6,0.1<y≤0.4。
[0012] Optionally, the nickel salt includes at least one of the following: nickel sulfate, nickel nitrate, nickel chloride, nickel acetate, and nickel bromide;
[0013] The cobalt salt includes at least one of the following: cobalt sulfate, cobalt nitrate, cobalt chloride, cobalt acetate, and cobalt bromide;
[0014] The manganese salt includes at least one of the following: manganese sulfate, manganese nitrate, manganese chloride, manganese acetate, and manganese bromide;
[0015] The alkali includes at least one of the following: sodium hydroxide and potassium hydroxide.
[0016] Optionally, the ratio of the total amount of nickel, cobalt and manganese in the mixed salt to the amount of hydroxide ion in the base is 1:(1.95-2.05).
[0017] Optionally, the step of reacting the mixed salt aqueous solution with a base to generate an amorphous ternary precursor comprises:
[0018] The mixed salt aqueous solution and the alkali aqueous solution are added to the reaction container in parallel to react and generate an amorphous ternary precursor.
[0019] Optionally, the total molar concentration of nickel, cobalt and manganese in the aqueous solution of the mixed salt is between 1.0 mol / L and 4.0 mol / L;
[0020] The molar concentration of hydroxide ions in the aqueous solution of the alkali is between 2.0 mol / L and 8.0 mol / L.
[0021] Optionally, the temperature in the reaction vessel is between 50°C and 55°C;
[0022] The reaction time of the aqueous solution of the mixed salt and the aqueous solution of the alkali in the reaction container is 3 hours to 7 hours.
[0023] Optionally, the ratio of the amount of lithium in the slurry to the total amount of nickel, cobalt and manganese is (1-1.13):1;
[0024] The solid content of the slurry is 20wt% to 40wt%;
[0025] The slurry further comprises a metal oxide additive, and the content of the metal oxide additive in the solid component of the slurry is in the range of 0.05 wt % to 0.25 wt %.
[0026] Optionally, the preparing the slurry comprises: preparing the slurry by sand milling and mixing;
[0027] The D50 particle size of the solid component of the slurry is between 500nm and 1000nm.
[0028] Optionally, the atomization pressure of the spray drying is 0.9 MPa to 1.0 MPa, the air inlet temperature is 200° C. to 250° C., and the air outlet temperature is 70° C. to 100° C.
[0029] Optionally, the D50 particle size of the dried material is between 3 μm and 6 μm.
[0030] Optionally, sintering the dried material includes:
[0031] The dried material is kept at 700° C. to 750° C. for 5 h to 8 h, and then kept at 800° C. to 850° C. for 8 h to 12 h.
[0032] In a second aspect, an embodiment of the present invention provides a ternary positive electrode material, which is prepared according to any one of the methods for preparing a ternary positive electrode material according to the embodiments of the present invention.
[0033] In the embodiment of the present invention, the ternary precursor is amorphous, so there is no need to use a complexing agent (such as ammonia water) to accurately control the properties of the product during its preparation, so that it is easy to implement, low-cost, and pollution-free (because there is no ammonia water); and in the embodiment of the present invention, the ternary precursor and the lithium source are configured as a slurry, that is, the two are wet mixed, so that uniform mixing at the molecular level can be achieved, and the consistency and stability of the ternary positive electrode material can be improved; and by spray drying for granulation, the amorphous ternary precursor can be used to obtain a material with the desired particle size distribution, structure, and micromorphology, thereby reducing the risk of hard agglomeration during sintering and improving the electrochemical properties of the ternary positive electrode material. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] Figure 1 A flow chart of a method for preparing a ternary positive electrode material according to an embodiment of the present invention;
[0035] Figure 2 A flow chart of another method for preparing a ternary positive electrode material according to an embodiment of the present invention;
[0036] Figure 3 This is a scanning electron microscope image (magnification 8000 times) of a dry material obtained in a method for preparing a ternary positive electrode material according to an embodiment of the present invention;
[0037] Figure 4 This is a scanning electron microscope image (magnification 2000 times) of a ternary positive electrode material obtained in a method for preparing a ternary positive electrode material in an embodiment of the present invention. DETAILED DESCRIPTION
[0038] In order to enable those skilled in the art to better understand the technical solution of the present invention, the present invention is further described in detail below in conjunction with the accompanying drawings and specific implementation methods.
[0039] It should be understood that the specific embodiments and drawings described herein are only used to explain the present invention rather than to limit the present invention.
[0040] It can be understood that, in the absence of conflict, the various embodiments of the present invention and the various features therein can be combined with each other.
[0041] It can be understood that, for the convenience of description, the drawings of the present invention only show the parts related to the embodiments of the present invention, while the parts unrelated to the embodiments of the present invention are not shown in the drawings.
[0042] It can be understood that, in the absence of conflict, the functions and steps marked in the flowcharts and block diagrams of the embodiments of the present invention may occur in an order different from that marked in the drawings.
[0043] Lithium batteries (lithium secondary batteries) have the advantages of high energy density, high operating voltage, long cycle life, low self-discharge, and no memory effect. Therefore, they have been widely used in new energy vehicles (such as power batteries), power generation and energy storage (such as photovoltaic storage) and other fields.
[0044] Lithium batteries can be divided into ternary lithium batteries and lithium iron phosphate batteries according to the different positive electrode materials. Among them, ternary lithium batteries have the advantages of high capacity and good safety. For example, their energy density can reach 200Wh / kg~300Wh / kg, while the energy density of lithium iron phosphate batteries is usually below 200Wh / kg.
[0045] The main active ingredient of the positive electrode of the ternary lithium battery is the ternary positive electrode material, and the preparation process of the ternary positive electrode material has a great influence on its particle size distribution, structure, micromorphology, etc., which in turn affects its electrochemical performance.
[0046] In some related technologies, ternary positive electrode materials can be prepared by the method of co-precipitation-high-temperature solid-phase sintering, that is, a ternary metal mixed salt solution is used as a raw material, reacted under the action of liquid alkali and a chelating agent, and a co-precipitation product is obtained through nucleation and growth, and then a ternary precursor is obtained through filtration, washing, and drying. Thereafter, the ternary precursor and a lithium salt are solid-phase mixed by ball milling, and the ternary positive electrode material is obtained after calcination.
[0047] According to the above method, ammonia water, lactose and other complexing agents are used in the preparation of the ternary precursor to control the particle size distribution, structure, microscopic morphology, etc. of the ternary precursor. Since the properties of the product need to be precisely controlled, it is difficult to achieve and the cost is high. In particular, when ammonia water is used as a complexing agent, the working environment is harmful to the human body, and free ammonia may be generated due to poor sealing, resulting in secondary pollution. Moreover, this method will also produce a large amount of ammonia-containing wastewater, which needs to be further treated (such as stripping) before it can be discharged, so it is more difficult to achieve and the cost is higher.
[0048] At the same time, due to the limited uniformity of ball milling mixing (solid phase mixing), the resulting ternary positive electrode material has poor consistency and stability.
[0049] In a first aspect, an embodiment of the present invention provides a method for preparing a ternary positive electrode material.
[0050] The embodiment of the present invention is used to prepare a ternary positive electrode material, specifically a ternary positive electrode material used as an active material of the positive electrode of a lithium battery (ternary lithium battery).
[0051] It should be understood that the ternary positive electrode material prepared in the embodiment of the present invention may also be suitable for other applications.
[0052] Reference Figure 1 The method for preparing the ternary positive electrode material of the embodiment of the present invention includes:
[0053] S101. reacting an aqueous solution of a mixed salt with a base to generate an amorphous ternary precursor.
[0054] Among them, the mixed salt includes nickel salt, cobalt salt and manganese salt.
[0055] In the embodiment of the present invention, soluble salts (mixed salts) of ternary metals (M), namely nickel salt, cobalt salt and manganese salt, are dissolved in water to obtain an aqueous solution of the mixed salt, and then the aqueous solution of the mixed salt is reacted with an alkali to generate a ternary precursor, namely, nickel cobalt manganese hydroxide (Ni x Co y Mn z (OH)2) precipitation.
[0056] Among them, the ternary precursor is "amorphous", that is, no complexing agent such as ammonia water is used in its preparation to control the properties of the product. It only needs the ternary metal ions of nickel, cobalt and manganese to react with hydroxide ions to produce precipitation.
[0057] It should be understood that the precipitate produced above can be further subjected to separation, drying and other operations to obtain a ternary precursor.
[0058] For example, the aqueous solution after the reaction can be centrifuged and washed to separate the precipitate of nickel, cobalt and manganese hydroxide, and then dried at 60° C. to 70° C. to obtain an amorphous ternary precursor.
[0059] S102, preparing slurry.
[0060] Among them, the slurry includes a lithium source and a ternary precursor.
[0061] The ternary precursor obtained above is mixed with a lithium source, water, etc. (wet mixing) to obtain a uniform slurry (solid-liquid mixture).
[0062] Among them, lithium source refers to substances containing lithium elements, such as lithium hydroxide, lithium carbonate, lithium nitrate, lithium acetate, lithium phosphate, etc.
[0063] S103, spray drying and granulating the slurry to obtain a dry material.
[0064] The slurry obtained above is granulated by spray drying to obtain solid particles (dried material) in which the lithium source and nickel, cobalt and manganese hydroxides are uniformly mixed.
[0065] S104, sintering the dried material to obtain a ternary positive electrode material.
[0066] The dried material obtained above is sintered to obtain a polycrystalline ternary positive electrode material product.
[0067] It should be understood that the sintered product can also be subjected to screening and other operations to obtain a ternary positive electrode material.
[0068] It should be understood that the ternary positive electrode material obtained above is the active material of the positive electrode of the ternary lithium battery, and it also needs to be mixed with a binder, etc., and dried, die-cut, etc. to obtain a positive electrode sheet product.
[0069] It should be understood that the ternary lithium battery may also include other structures such as a negative electrode sheet, a separator, an electrolyte, a casing, etc., which will not be described in detail here.
[0070] In the embodiment of the present invention, the ternary precursor is amorphous, so there is no need to use a complexing agent (such as ammonia water) to accurately control the properties of the product during its preparation, so that it is easy to implement, low-cost, and pollution-free (because there is no ammonia water); and in the embodiment of the present invention, the ternary precursor and the lithium source are configured as a slurry, that is, the two are wet mixed, so that uniform mixing at the molecular level can be achieved, and the consistency and stability of the ternary positive electrode material can be improved; and by spray drying for granulation, the amorphous ternary precursor can be used to obtain a material with the desired particle size distribution, structure, and micromorphology, thereby reducing the risk of hard agglomeration during sintering and improving the electrochemical properties of the ternary positive electrode material.
[0071] Optionally, the molar ratio of nickel, cobalt and manganese in the mixed salt is x:y:z; wherein x+y+z=1, 0 <x≤0.6,0.1<y≤0.4。
[0072] As one embodiment of the present invention, when the total amount of the ternary metal (M) in the mixed salt is 1, the amount of nickel (x) may be less than 0.6, further less than 0.5, and the amount of cobalt (y) may be between 0.1 and 0.4, further between 0.2 and 0.35, and the amount of manganese (z) is the remainder.
[0073] For example, as one embodiment of the present invention, x=y=z=0.33.
[0074] Optionally, the nickel salt includes at least one of the following: nickel sulfate, nickel nitrate, nickel chloride, nickel acetate, and nickel bromide; the cobalt salt includes at least one of the following: cobalt sulfate, cobalt nitrate, cobalt chloride, cobalt acetate, and cobalt bromide; the manganese salt includes at least one of the following: manganese sulfate, manganese nitrate, manganese chloride, manganese acetate, and manganese bromide; the alkali includes at least one of the following: sodium hydroxide and potassium hydroxide.
[0075] As one embodiment of the present invention, the mixed salt can be in the form of sulfate (NiSO4, CoSO4, MnSO4), nitrate (Ni(NO3)2, Co(NO3)2, Mn(NO3)2), chloride (NiCl2, CoCl2, MnCl2), acetate (Ni(CH3COO)2, Co(CH3COO)2, Mn(CH3COO)2), bromide (NiBr2, CoBr2, MnBr2), etc.
[0076] As one embodiment of the present invention, the base that reacts with the mixed salt may be in the form of NaOH, KOH, etc.
[0077] Optionally, the ratio of the total amount of nickel, cobalt and manganese in the mixed salt to the amount of hydroxide ion in the base is 1:(1.95-2.05).
[0078] As one embodiment of the present invention, the ratio of the total amount of the ternary metal (M) in the mixed salt to the amount of the hydroxide ion in the base may be 1:(1.95-2.05), and may further be 1:2.
[0079] Optional, see Figure 2 , reacting the mixed salt aqueous solution with a base to generate an amorphous ternary precursor (S101) includes:
[0080] S1011. Adding a mixed salt aqueous solution and an alkali aqueous solution into a reaction container in parallel to react and generate an amorphous ternary precursor.
[0081] As one embodiment of the present invention, the mixed salt aqueous solution and the alkali aqueous solution may be added to a reaction container (such as a reactor) in parallel, and the reaction is continued in the reaction container to generate a ternary precursor precipitate.
[0082] Optionally, the total molar concentration of nickel, cobalt and manganese in the aqueous solution of the mixed salt is between 1.0 mol / L and 4.0 mol / L; the molar concentration of hydroxide ions in the aqueous solution of the alkali is between 2.0 mol / L and 8.0 mol / L.
[0083] As one embodiment of the present invention, the total molar concentration of the ternary metal (M) in the aqueous solution of the mixed salt can be 1.0 mol / L to 4.0 mol / L, and further can be 1.5 mol / L to 3.5 mol / L; correspondingly, the molar concentration of the hydroxide ion in the aqueous solution of the alkali can be 2.0 mol / L to 8.0 mol / , and further can be 3.0 mol / L to 7.0 mol / L.
[0084] Optionally, the temperature in the reaction container is 50° C. to 55° C.; and the reaction time of the aqueous solution of the mixed salt and the aqueous solution of the alkali in the reaction container is 3 h to 7 h.
[0085] As one embodiment of the present invention, the reaction temperature for producing the ternary precursor can be 50°C to 55°C, and can be further 55°C; and the reaction time can be 3h to 7h, and can be further 5h. After this time, the grains have completed the nucleation and initial growth process, and discharge can begin.
[0086] It should be understood that during the reaction, a protective atmosphere may be introduced into the reaction vessel, such as nitrogen gas being introduced into the bottom of the reactor at a flow rate of 0.08 L / min to 0.12 L / min.
[0087] Optionally, the ratio of the amount of lithium in the slurry to the total amount of nickel, cobalt and manganese is (1 to 1.13):1; the solid content of the slurry is 20wt% to 40wt%; the slurry also includes a metal oxide additive, and the content of the metal oxide additive in the solid component of the slurry is 0.05wt% to 0.25wt%.
[0088] As one embodiment of the present invention, in the slurry, the ratio of the amount of lithium in the lithium source to the total amount of the ternary metal (M) (Li / M ratio) can be (1-1.13):1, and further can be 1.08:1.
[0089] As one embodiment of the present invention, the slurry may further contain metal oxide additives, such as one or more of zirconium oxide, tungsten oxide, magnesium oxide, aluminum oxide, zinc oxide, lanthanum oxide, yttrium oxide, and strontium oxide. The mass percentage of the metal oxide additive in all solid components of the slurry is 0.05wt% to 0.25wt%, and further 0.1wt% to 0.2wt%.
[0090] As one embodiment of the present invention, in the slurry, the mass percentage of all solid components (solid content) is 20wt% to 40wt%, and can further be 25wt% to 35wt%.
[0091] Optional, see Figure 2 , preparing the slurry (S102) includes:
[0092] S1021. Prepare slurry by sand grinding and mixing.
[0093] The D50 particle size of the solid component of the slurry is between 500nm and 1000nm.
[0094] As one method of an embodiment of the present invention, the solid components of the slurry may be preliminarily mixed with water, and then sand-milled with a sand mill to obtain a slurry.
[0095] As one embodiment of the present invention, the sand grinding time should be such that the D50 particle size (median particle size) of the solid component in the resulting slurry is between 500nm and 1000nm, and can further be between 500nm and 700nm, such as 500nm; this particle size range can make the primary grains smaller during sintering, which is beneficial to improving the rate performance of the product.
[0096] Optionally, the atomization pressure of the spray drying is 0.9MPa-1.0MPa, the air inlet temperature is 200℃-250℃, and the air outlet temperature is 70℃-100℃.
[0097] As one embodiment of the present invention, when the slurry is spray-dried and granulated, the atomization pressure can be 0.9MPa-1.0MPa, and further can be 0.92MPa-0.98MPa; the inlet air temperature can be 200℃-250℃, and further can be 200℃-230℃; and the outlet air temperature can be 70℃-100℃, and further can be 80℃-90℃; the above atomization parameters can ensure that the dry material of the desired structure is obtained.
[0098] Optionally, the D50 particle size of the dried material is between 3 μm and 6 μm.
[0099] As one embodiment of the present invention, the D50 particle size (median particle size) of the dry material obtained by granulation through spray drying can be 3 μm to 6 μm, and can further be 4 μm.
[0100] Optional, see Figure 2 , sintering the dried material (S104) includes:
[0101] S1041. Keep the dried material at 700°C to 750°C for 5h to 8h, and then keep it at 800°C to 850°C for 8h to 12h.
[0102] As a method of an embodiment of the present invention, the sintering of the dried material can be carried out in two stages. First, the dried material is heated to 700°C~750°C and kept warm for 5h~8h, and can be further kept warm at 700°C for 5h; then the dried material is continued to be heated to 800°C~850°C and kept warm for 8h~12h, and can be further kept warm at 800°C for 12h.
[0103] In a second aspect, an embodiment of the present invention provides a ternary positive electrode material, which is prepared according to any one of the methods for preparing a ternary positive electrode material according to the embodiments of the present invention.
[0104] The ternary positive electrode material of the embodiment of the present invention is prepared by the above method for preparing the ternary positive electrode material, so that its properties (such as particle size distribution, structure, micromorphology, etc.) conform to the characteristics of the product prepared by the above method.
[0105] Embodiment 1:
[0106] Embodiment 1 A ternary positive electrode material is prepared by the method of the embodiment of the present invention, and a lithium battery including the ternary positive electrode material is prepared, which includes the following steps:
[0107] (1) Preparation of positive electrode
[0108] A1. NiSO4 (nickel salt), CoSO4 (cobalt salt), and MnSO4 (manganese salt) are prepared into a mixed salt aqueous solution according to the molar ratio of x:y:z, wherein x=y=z=0.33.
[0109] Nitrogen gas (protective atmosphere) was passed into the bottom of the reactor at a flow rate of 0.10 L / min, the temperature of the reactor was raised to 50° C., and the above mixed salt aqueous solution and NaOH (alkali) aqueous solution were added into the reactor in parallel.
[0110] Among them, the total molar concentration of ternary metals (M) Ni, Co, and Mn in the aqueous solution of the mixed salt is 2.0 mol / L, and the molar concentration of NaOH is 4.0 mol / L; and the flow rates of the aqueous solution of the mixed salt and the aqueous solution of NaOH are controlled to ensure that the molar ratio of the ternary metals to the molar ratio of NaOH is 1:2.
[0111] After 5 h of reaction, the material was discharged continuously, washed with water by centrifugation and dried at 65 °C to obtain an amorphous ternary precursor, namely Ni 0.33 Co 0.33 Mn 0.33 (OH)2.
[0112] A2. The ternary precursor, lithium hydroxide (lithium source), and zirconium oxide (metal oxide) are mixed to obtain a solid component, wherein the Li / M ratio is controlled at 1.08, and zirconium oxide accounts for 0.02wt% of the total solid component.
[0113] Water was added to the solid component until the solid content was 20 wt %. After stirring, the mixture was added to a sand mill for sand grinding to obtain a uniform slurry with a D50 of 500 nm.
[0114] A3. The slurry is spray dried and granulated to obtain a dry material with a D50 of 4 um.
[0115] Among them, the atomization pressure of spray drying is 0.92MPa, the inlet air temperature is 200℃, and the outlet air temperature is 80℃.
[0116] The SEM images of the dried material were taken as reference. Figure 3 It can be seen that the particles of the product obtained by spray drying granulation have regular morphology, excellent sphericity, little difference in particle size, and uniform distribution.
[0117] A4. Place the dried material in a sintering furnace and sinter in an air atmosphere. The sintering process includes: heating to 700°C and keeping it warm for 7 hours, then heating to 800°C and keeping it warm for 8 hours.
[0118] After sintering, the material is sieved to obtain a ternary positive electrode material.
[0119] The scanning electron microscope (SEM) photos of the obtained ternary cathode material are shown in Figure 2. Figure 4 It can be seen that the particles of the ternary positive electrode material obtained by the method of the embodiment of the present invention have regular morphology, excellent sphericity, little difference in particle size, and uniform distribution.
[0120] A5. Using the ternary positive electrode material as the active material, the ternary positive electrode material, the conductive agent SP (carbon black), the binder PVDF (polytetrafluoroethylene), and the dispersant polyetherimide were mixed in NMP (N-methylpyrrolidone) in a mass ratio of 96.8:1:2:0.2 to obtain a positive electrode slurry. The positive electrode slurry was heated to 400 g / m 2 The surface density is evenly coated on the aluminum foil and then divided into strips, and the surface density is 3.4g / cm 3 The compaction density is rolled to obtain a positive electrode sheet.
[0121] (2) Preparation of negative electrode sheet
[0122] Artificial graphite, SP, CMC (carboxymethyl cellulose), and SBR (styrene-butadiene rubber) were mixed uniformly in deionized water at a mass ratio of 95.8:1:1.2:2 to obtain a negative electrode slurry. The negative electrode slurry was heated at 200 g / m 2 The surface density is evenly coated on the copper foil and then divided into strips, and the surface density is 1.65g / cm 3 The compaction density is rolled to obtain a negative electrode sheet.
[0123] (3) Preparation of electrolyte
[0124] The solvent is prepared with EC (ethylene carbonate) and EMC (ethyl methyl carbonate) in a mass ratio of 3:7, lithium hexafluorophosphate (LiPF6) is used as the lithium salt, the electrolyte concentration is prepared at 1.15 mol / L, and 1wt% of FEC (fluoroethylene carbonate), 2wt% of MMDS (methylene methanedisulfonate), 1wt% of TMSP (trimethylsilyl phosphate), and 1wt% of TPP (triphenyl phosphate) are added as film-forming additives.
[0125] (4) Preparation of diaphragm
[0126] A 9 μm thick polyethylene porous membrane was used as the substrate, and a 3 μm thick ceramic and a 2 μm thick PVDF (polyvinylidene fluoride) glue were coated on the surface to obtain a 9PE+3CCS+2PCS separator.
[0127] (5) Preparation of soft-pack lithium batteries
[0128] The above positive electrode sheet, negative electrode sheet, electrolyte and separator were used to assemble a 2Ah soft-pack lithium battery, which was formed and degassing, then charged to 4.35V at 0.3C and stopped at 0.05C.
[0129] The discharge DC internal resistance (DCR) and capacity retention rate after 500 cycles of charge and discharge of the soft-pack lithium battery were tested, and the results are shown in Table 1.
[0130] Embodiment 2:
[0131] Example 2 is similar to Example 1, except that the preparation process of the ternary positive electrode material includes:
[0132] B1. NiSO4 (nickel salt), CoSO4 (cobalt salt), and MnSO4 (manganese salt) are prepared into a mixed salt aqueous solution according to the molar ratio of x:y:z, where x=0.5, y=0.2, and z=0.3.
[0133] Nitrogen gas (protective atmosphere) was passed into the bottom of the reactor at a flow rate of 0.12 L / min, the temperature of the reactor was raised to 53° C., and the above mixed salt aqueous solution and NaOH (alkali) aqueous solution were added into the reactor in parallel.
[0134] Among them, the total molar concentration of ternary metals (M) Ni, Co, and Mn in the aqueous solution of the mixed salt is 3.0 mol / L, and the molar concentration of NaOH is 4.0 mol / L; and the flow rates of the aqueous solution of the mixed salt and the aqueous solution of NaOH are controlled to ensure that the molar ratio of the ternary metals to the molar ratio of NaOH is 1:2.
[0135] After 7 hours of reaction, the material was discharged continuously, washed with water by centrifugation and dried at 65 °C to obtain an amorphous ternary precursor, namely Ni 0.5 Co 0.2 Mn 0.3 (OH)2.
[0136] B2. The ternary precursor, lithium hydroxide (lithium source), and zirconium oxide (metal oxide) are mixed to obtain a solid component, wherein the Li / M ratio is controlled at 1.06, and zirconium oxide accounts for 0.15wt% of the total solid component.
[0137] Water was added to the solid component until the solid content was 35 wt %. After stirring, the mixture was added to a sand mill for sand grinding to obtain a uniform slurry with a D50 of 800 nm.
[0138] B3. The slurry is spray dried and granulated to obtain a dry material with a D50 of 4 um.
[0139] Among them, the atomization pressure of spray drying is 0.98MPa, the inlet air temperature is 250℃, and the outlet air temperature is 100℃.
[0140] B4. Place the dried material in a sintering furnace and sinter in an air atmosphere. The sintering process includes: heating to 725°C and keeping it warm for 6 hours, then heating to 830°C and keeping it warm for 9 hours.
[0141] After sintering, the material is sieved to obtain a ternary positive electrode material.
[0142] Embodiment 3:
[0143] Example 3 is similar to Example 1, except that the preparation process of the ternary positive electrode material includes:
[0144] C1. NiSO4 (nickel salt), CoSO4 (cobalt salt), and MnSO4 (manganese salt) are prepared into a mixed salt aqueous solution according to the molar ratio of x:y:z, wherein x=0.6, y=0.2, and z=0.2.
[0145] Nitrogen gas (protective atmosphere) was passed into the bottom of the reactor at a flow rate of 0.1 L / min, the temperature of the reactor was raised to 53° C., and the above mixed salt aqueous solution and NaOH (alkali) aqueous solution were added into the reactor in parallel.
[0146] Among them, the total molar concentration of ternary metals (M) Ni, Co, and Mn in the aqueous solution of the mixed salt is 4.0 mol / L, and the molar concentration of NaOH is 8.0 mol / L; and the flow rates of the aqueous solution of the mixed salt and the aqueous solution of NaOH are controlled to ensure that the molar ratio of the ternary metals to the molar ratio of NaOH is 1:2.
[0147] After 7 hours of reaction, the material was discharged continuously, washed with water by centrifugation and dried at 65 °C to obtain an amorphous ternary precursor, namely Ni 0.6 Co 0.2 Mn 0.2 (OH)2.
[0148] C2, the ternary precursor, lithium carbonate (lithium source), and magnesium oxide (metal oxide) are mixed to obtain a solid component, wherein the Li / M ratio is controlled at 1.02, and zirconium oxide accounts for 0.15wt% of the total solid component.
[0149] Water was added to the solid component until the solid content was 35 wt %. After stirring, the mixture was added to a sand mill for sand grinding to obtain a uniform slurry with a D50 of 800 nm.
[0150] C3. The slurry is spray dried and granulated to obtain a dry material with a D50 of 4 um.
[0151] Among them, the atomization pressure of spray drying is 1.0MPa, the inlet air temperature is 230℃, and the outlet air temperature is 90℃.
[0152] C4. Place the dried material in a sintering furnace and sinter in an air atmosphere. The sintering process includes: heating to 725°C and keeping it warm for 6 hours, then heating to 830°C and keeping it warm for 9 hours.
[0153] After sintering, the material is sieved to obtain a ternary positive electrode material.
[0154] Embodiment 4:
[0155] Example 4 is similar to Example 1, except that the preparation process of the ternary positive electrode material includes:
[0156] D1. NiSO4 (nickel salt), CoSO4 (cobalt salt), and MnSO4 (manganese salt) are prepared into a mixed salt aqueous solution according to the molar ratio of x:y:z, wherein x=0.6, y=0.2, and z=0.2.
[0157] Nitrogen gas (protective atmosphere) was passed into the bottom of the reactor at a flow rate of 0.12 L / min, the temperature of the reactor was raised to 52° C., and the above mixed salt aqueous solution and NaOH (alkali) aqueous solution were added into the reactor in parallel.
[0158] Among them, the total molar concentration of ternary metals (M) Ni, Co, and Mn in the aqueous solution of the mixed salt is 2.5 mol / L, and the molar concentration of NaOH is 3.5 mol / L; and the flow rates of the aqueous solution of the mixed salt and the aqueous solution of NaOH are controlled to ensure that the molar ratio of the ternary metals to the molar ratio of NaOH is 1:2.
[0159] After 6 hours of reaction, the material was discharged continuously, washed with water by centrifugation and dried at 70 °C to obtain an amorphous ternary precursor, namely Ni 0.6 Co 0.2 Mn 0.2 (OH)2.
[0160] D2. The ternary precursor, lithium nitrate (lithium source), and magnesium oxide (metal oxide) are mixed to obtain a solid component, wherein the Li / M ratio is controlled at 1.11, and zirconium oxide accounts for 0.2 wt% of the total solid component.
[0161] Water was added to the solid component until the solid content was 40 wt %. After stirring, the mixture was added to a sand mill for sand grinding to obtain a uniform slurry with a D50 of 700 nm.
[0162] D3. The slurry is spray dried and granulated to obtain a dry material with a D50 of 5 um.
[0163] Among them, the atomization pressure of spray drying is 1.0MPa, the inlet air temperature is 250℃, and the outlet air temperature is 80℃.
[0164] D4. Place the dried material in a sintering furnace and sinter in an air atmosphere. The sintering process includes: heating to 730°C and keeping it warm for 7 hours, then heating to 820°C and keeping it warm for 10 hours.
[0165] After sintering, the material is sieved to obtain a ternary positive electrode material.
[0166] Comparative Example 1:
[0167] In Comparative Example 1, a commercially available NCM523 type ternary positive electrode material is used (ammonia water is used as a complexing agent in the preparation of its ternary precursor), and other contents are the same as those in Example 1.
[0168] Table 1. Performance of soft-pack lithium batteries in Examples and Comparative Examples
[0169]
[0170]
[0171] Referring to Table 1, the discharge DCR of each embodiment does not exceed 5.5mΩ, and the 500-cycle capacity retention rate is at least 90.8%. The kinetics and cycle performance are better than those of the comparative example. This is because wet mixing and spray drying granulation are used in the embodiments of the present invention, thereby obtaining small primary grains and high product consistency.
[0172] Moreover, in the embodiment of the present invention, no complexing agent such as ammonia water is used in the preparation process of the ternary precursor, so it is easy to implement, low in cost, and does not cause pollution problems.
[0173] It is to be understood that the above embodiments are merely exemplary embodiments used to illustrate the principles of the present invention, but the present invention is not limited thereto. For those of ordinary skill in the art, various modifications and improvements can be made without departing from the spirit and essence of the present invention, and these modifications and improvements are also considered to be within the scope of protection of the present invention.
Claims
1. A method for preparing a ternary positive electrode material, It is characterized in that include: The aqueous solution of the mixed salt is reacted with a base to generate an amorphous ternary precursor; the mixed salt comprises a nickel salt, a cobalt salt, and a manganese salt; Prepare slurry; The slurry includes a lithium source and the ternary precursor; The slurry is spray-dried and granulated to obtain a dry material; The dried material is sintered to obtain a ternary positive electrode material.
2. The method according to claim 1, It is characterized in that The molar ratio of nickel, cobalt and manganese in the mixed salt is x:y:z; Where x+y+z=1,0 <x≤0.6,0.1<y≤0.4。 3. The method according to claim 1, It is characterized in that The nickel salt includes at least one of the following: nickel sulfate, nickel nitrate, nickel chloride, nickel acetate, and nickel bromide; The cobalt salt includes at least one of the following: cobalt sulfate, cobalt nitrate, cobalt chloride, cobalt acetate, and cobalt bromide; The manganese salt includes at least one of the following: manganese sulfate, manganese nitrate, manganese chloride, manganese acetate, and manganese bromide; The alkali includes at least one of the following: sodium hydroxide and potassium hydroxide.
4. The method according to claim 1, It is characterized in that The ratio of the total amount of nickel, cobalt and manganese in the mixed salt to the amount of hydroxide ions in the base is 1:(1.95-2.05).
5. The method according to claim 1, It is characterized in that The step of reacting the mixed salt aqueous solution with a base to generate an amorphous ternary precursor comprises: The mixed salt aqueous solution and the alkali aqueous solution are added to the reaction container in parallel to react and generate an amorphous ternary precursor.
6. The method according to claim 5, It is characterized in that The total molar concentration of nickel, cobalt and manganese in the aqueous solution of the mixed salt is 1.0 mol / L to 4.0 mol / L; The molar concentration of hydroxide ions in the aqueous solution of the alkali is between 2.0 mol / L and 8.0 mol / L.
7. The method according to claim 5, It is characterized in that The temperature in the reaction vessel is 50°C to 55°C; The reaction time of the aqueous solution of the mixed salt and the aqueous solution of the alkali in the reaction container is 3 hours to 7 hours.
8. The method according to claim 1, It is characterized in that The ratio of the amount of lithium in the slurry to the total amount of nickel, cobalt and manganese is (1-1.13):1; The solid content of the slurry is 20wt% to 40wt%; The slurry further comprises a metal oxide additive, and the content of the metal oxide additive in the solid component of the slurry is in the range of 0.05 wt % to 0.25 wt %.
9. The method according to claim 1, It is characterized in that The slurry preparation includes: preparing the slurry by sand milling and mixing; The D50 particle size of the solid component of the slurry is between 500nm and 1000nm.
10. The method according to claim 1, It is characterized in that The atomization pressure of the spray drying is 0.9MPa-1.0MPa, the air inlet temperature is 200°C-250°C, and the air outlet temperature is 70°C-100°C.
11. The method according to claim 1, It is characterized in that The D50 particle size of the dried material is between 3 μm and 6 μm.
12. The method according to claim 1, It is characterized in that The sintering of the dried material comprises: The dried material is kept at 700° C. to 750° C. for 5 h to 8 h, and then kept at 800° C. to 850° C. for 8 h to 12 h.
13. A ternary cathode material, It is characterized in that The ternary positive electrode material is prepared according to the method for preparing a ternary positive electrode material according to any one of claims 1 to 12.
Citation Information
Cited By
Preparation method of single crystal lithium ion positive electrode material, positive electrode material and battery
CN120736574A
Lithium-containing precursor and preparation method thereof, positive electrode material and battery
CN120736575A
Lithium-containing composite precursor and preparation method thereof, positive electrode material and battery
CN120757161A
Lithium-containing composite precursor, preparation method thereof, positive electrode material and battery
CN120757161B