Method for removing sulfamethoxazole from water by in-situ etching carbon felt modified with iron phosphide

In-situ etching of carbon felt with iron phosphide enhances the electro-Fenton process by improving H2O2 generation and activation, effectively addressing the inefficiencies of traditional methods in sulfonamide antibiotic removal and mitigating antibiotic resistance.

CN118754262BActive Publication Date: 2024-12-03SOUTH CHINA INST OF ENVIRONMENTAL SCI MEP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411249933.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-09-06
Publication Date
2024-12-03
Estimated Expiration
2044-09-06

AI Technical Summary

Technical Problem

Traditional sewage treatment methods, such as the activated sludge method, are ineffective in removing sulfonamide antibiotics like sulfamethoxazole from water, and heterogeneous electrocatalysts face challenges in efficiently generating and activating H2O2 for effective degradation in the electro-Fenton process.

Method used

A method involving in-situ etching of carbon felt with iron phosphide (FeP@ECC) using a ruthenium iridium titanium electrode as the anode and FeP@ECC as the cathode in the electro-Fenton process to enhance H2O2 generation and activation, achieving a maximum reaction rate constant of 0.28263.

Benefits of technology

The method provides efficient removal of sulfamethoxazole with improved catalytic performance, reducing antibiotic pollution and controlling resistance development, demonstrating significant academic and practical significance for environmental protection and human health.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118754262B_ABST
    Figure CN118754262B_ABST
Patent Text Reader

Abstract

The present application discloses a method for removing sulfamethoxazole from water by in-situ etched carbon felt modified with iron phosphide, which relates to the technical field of environmental pollutant treatment and aims to solve the technical problem of low removal efficiency of sulfamethoxazole in water in the prior art. The method for removing sulfamethoxazole from water by in-situ etched carbon felt modified with iron phosphide comprises the following steps: using a ruthenium iridium titanium electrode as an anode and a FeP@ECC electrode as a cathode to remove sulfamethoxazole from the target sewage, and the maximum reaction rate constant is 0.28263. Compared with the prior art, the present application provides a new type of heterogeneous electrocatalyst, and the system has efficient H2O2 electrogeneration and activation capabilities. It has important academic and practical significance for reducing antibiotic pollution and controlling the development of antibiotic resistance. The innovation and application prospects of the system are expected to provide more effective protection for environmental protection and human health.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of environmental pollutant treatment, and in particular to a method for removing sulfamethoxazole in water by using in-situ etched carbon felt modified with iron phosphide. Background Art

[0002] Nowadays, with the widespread production and use of antibiotics, they are increasingly penetrating into the water environment, and traces of antibiotics have even been found in drinking water. In addition, the continuous discharge of antibiotics leads to the development of resistance in pathogens, which may pose a serious threat to human health and ecosystems. Sulfonamide antibiotics are the most common type of antibiotics in water bodies. Due to the huge amount of wastewater generated during their production process and the complex composition, which contains a large amount of antibacterial organic matter, traditional sewage treatment methods, such as the activated sludge method, are not effective in treating sulfur-containing wastewater and often fail to meet the prescribed water quality standards.

[0003] In recent years, the electro-Fenton process (EF) has shown great application potential in the field of water treatment due to its environmental friendliness, high efficiency and no need for additional oxidants in antibiotic degradation. The EF process generates H2O2 in situ at the cathode, and then activates H2O2 with a catalyst to produce highly reactive oxygen species (ROS), thereby achieving effective degradation and thorough mineralization of antibiotic molecules. It is worth noting that compared with the homogeneous EF process, the dissolved Fe 2+ The catalyst will produce iron mud pollution and catalyst recovery difficulties. The heterogeneous EF system is more favored by researchers because of its advantages such as convenient catalyst recovery, simple operation, and fast reaction speed. However, the efficient electrogeneration of ROS in the heterogeneous EF system is still difficult because it is difficult to obtain efficient catalysis of the two reaction steps of H2O2 generation and activation at one catalytic site. Therefore, it is still a challenge to develop heterogeneous electrocatalysts that can achieve efficient generation and activation of H2O2. Summary of the invention

[0004] The present application provides a method for removing sulfamethoxazole from water by in-situ etching of carbon felt modified with iron phosphide, aiming to solve the technical problem of low removal efficiency of sulfamethoxazole in water in the prior art.

[0005] To solve the above technical problems, the embodiments of the present application provide: a method for removing sulfamethoxazole in water by in-situ etching carbon felt modified with iron phosphide, comprising the following steps: using a ruthenium iridium titanium electrode as an anode and a FeP@ECC electrode as a cathode to remove sulfamethoxazole in the target wastewater, and the maximum reaction rate constant is 0.28263.

[0006] As some optional embodiments of the present application, the FeP@ECC electrode is obtained after low-temperature phosphating and calcining treatment, and the temperature of the low-temperature phosphating and calcining treatment is ≤350°C.

[0007] As some optional embodiments of the present application, the FeP@ECC electrode is prepared by the following steps:

[0008] The carbon felt is subjected to ultrasonic treatment to remove impurities, thereby obtaining cleaned carbon felt;

[0009] The washed carbon felt was immersed in a cobalt acetate ethanol solution for 2 hours, dried and placed in a muffle furnace for calcination. After the calcination was completed, it was taken out, washed and dried to obtain ECC;

[0010] Potassium ferrocyanide and polyvinyl pyrrolidone were dispersed in a hydrochloric acid solution, magnetically stirred until clear, and then ECC was immersed in the solution for reaction. After the reaction was completed, the product was washed and dried to obtain PB@ECC.

[0011] Sodium hypophosphite and PB@ECC were placed in the upstream and downstream of a tube furnace, respectively, and calcined for 2 h under nitrogen conditions. After calcination, they were washed alternately with ethanol and deionized water to obtain a FeP@ECC electrode.

[0012] As some optional embodiments of the present application, the carbon felt is subjected to ultrasonic treatment to remove impurities to obtain cleaned carbon felt, including:

[0013] The carbon felt was placed in ethanol and deionized water for 10 min each to remove impurities and obtain clean carbon felt.

[0014] As some optional embodiments of the present application, the washed carbon felt is immersed in a cobalt acetate ethanol solution for 2 hours, dried and placed in a muffle furnace for calcination. After the calcination is completed, the carbon felt is taken out, washed and dried to obtain ECC, including:

[0015] The cleaned carbon felt was immersed in 1g / L cobalt acetate ethanol solution for 2h, dried and placed in a muffle furnace, heated to 300℃ and calcined for one hour; then heated to 400℃ and calcined for one hour; the heating rate was 5℃ / min;

[0016] After calcination, the product was taken out, cleaned and dried to obtain ECC.

[0017] As some optional embodiments of the present application, potassium ferrocyanide and polyvinyl pyrrolidone are dispersed in a hydrochloric acid solution, magnetically stirred until clear, and then ECC is immersed in the solution for reaction. After the reaction is completed, the product is washed and dried to obtain PB@ECC, including:

[0018] 0.11 g potassium ferrocyanide and 0.39 g polyvinyl pyrrolidone were dispersed in 50 mL hydrochloric acid solution with pH = 1, magnetically stirred until clear, and then ECC was immersed in it. It was then placed in a stainless steel reactor and reacted at 80°C for 24 h. After washing and drying, it was marked as PB@ECC.

[0019] As some optional embodiments of the present application, the sodium hypophosphite and PB@ECC are placed in the upstream and downstream of the tube furnace respectively, and calcined for 2 hours under nitrogen conditions; after the calcination, they are washed alternately with ethanol and deionized water to obtain a FeP@ECC electrode, including:

[0020] Sodium hypophosphite and PB@ECC were placed in the upstream and downstream of a tube furnace, respectively, and heated to 350°C at a rate of 3°C / min under nitrogen conditions and calcined for 2 h. After calcination, they were washed alternately with ethanol and deionized water to obtain a FeP@ECC electrode.

[0021] As some optional embodiments of the present application, for every 20 mg / L sulfamethoxazole, use 2×3 cm 2 Ruthenium-iridium-titanium electrode was used as the anode, using a 2×3 cm 2 FeP@ECC electrode was used as cathode.

[0022] As some optional embodiments of the present application, the ruthenium-iridium-titanium electrode is used as the anode and the FeP@ECC electrode is used as the cathode, and when sulfamethoxazole in the target wastewater is removed, the applied current is 50 mA.

[0023] As some optional embodiments of the present application, before using the ruthenium-iridium-titanium electrode as an anode and the FeP@ECC electrode as a cathode to remove sulfamethoxazole in the target sewage, the method further includes:

[0024] Obtaining target sewage;

[0025] Use 1M sulfuric acid or 0.2M sodium hydroxide to adjust the pH value of the target wastewater to ≤3.

[0026] Compared with the prior art, the present application provides a new type of heterogeneous electrocatalyst, and the system has efficient H2O2 electrogeneration and activation capabilities. It has important academic and practical significance for reducing antibiotic pollution and controlling the development of antibiotic resistance. The innovation and application prospects of this system are expected to provide more effective protection for environmental protection and human health. Specifically, the method for removing sulfamethoxazole from water by in-situ etching of carbon felt modified with iron phosphide comprises the following steps: using a ruthenium iridium titanium electrode as an anode and a FeP@ECC electrode as a cathode to remove sulfamethoxazole from the target wastewater, and the maximum reaction rate constant is 0.28263. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] In order to more clearly illustrate the specific implementation of the present application or the technical solution in the prior art, the following is a brief introduction to the drawings required for the specific implementation or the prior art description. In all drawings, similar elements or parts are generally identified by similar reference numerals. In the drawings, each element or part is not necessarily drawn according to the actual scale.

[0028] Figure 1 Schematic diagram of the preparation process of the FeP@ECC electrode involved in this application;

[0029] Figure 2 Characterization diagram of the FeP@ECC electrode involved in this application;

[0030] Figure 3 N2 adsorption-desorption isotherms of different electrodes involved in this application;

[0031] Figure 4 is the pore size distribution curve involved in this application;

[0032] Figure 5 This is the EDX element mapping image of FeP@ECC involved in this application;

[0033] Figure 6 XRD images of PB and FeP@ECC involved in this application;

[0034] Figure 7 Elemental analysis image of FeP@ECC involved in this application;

[0035] Figure 8 This is a performance comparison chart of FeP@ECC and other electrodes involved in this application;

[0036] Fig. 9 A three-dimensional EEMs image of the reaction solution involved in this application;

[0037] Fig.10 A comparison chart of the degradation performance of Fe3O4@ECC and FeP@ECC involved in this application;

[0038] Fig.11 This is a surface morphology diagram of the FeP@ECC electrode involved in this application.

[0039] The realization of the purpose, functional features and advantages of this application will be further explained in conjunction with embodiments and with reference to the accompanying drawings. DETAILED DESCRIPTION

[0040] The following will be combined with the drawings in the embodiments of the present application to clearly and completely describe the technical solutions in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.

[0041] Example 1: (1) Preparation and characterization of FeP@ECC electrode

[0042] The general process of preparation is as follows Figure 1 As shown, first, the carbon felt (CC) was placed in ethanol and deionized water for 10 min each to remove impurities. Then, the washed carbon felt was immersed in 1g / L cobalt acetate ethanol solution for 2h, dried and placed in a muffle furnace, heated to 300℃ and calcined for one hour; continued to heat to 400℃ and calcine for one hour; the heating rate was 5℃ / min, and it was marked as ECC after washing and drying. Next, 0.11 g potassium ferrocyanide and 0.39 g polyvinyl pyrrolidone were dispersed in 50 mL hydrochloric acid solution (pH = 1), magnetically stirred until clear, and then ECC was immersed, and then placed in a stainless steel reactor for reaction at 80℃ for 24 h, washed and dried, and marked as PB@ECC. Finally, 1 g of sodium hypophosphite and PB@ECC were placed in the upstream and downstream of the tube furnace, respectively, heated to 350 °C (3 °C / min) under nitrogen conditions, calcined for 2 h, and then washed alternately with ethanol and deionized water several times to obtain FeP@ECC.

[0043] (2) Characterization and experimental methods

[0044] The surface morphology and internal structure of the samples were investigated by scanning electron microscopy (SEM, Hitachi S-4800) and high-resolution transmission electron microscopy (HR-TEM, Hitachi S-3000N). TEM images were collected on a FEI Talos F200S microscope. Powder X-ray diffraction (XRD) patterns of the samples were obtained on a Bruker Advanced D8 X-ray diffractometer with Cu Kα radiation. The elemental composition and chemical state of the samples were determined by X-ray photoelectron spectroscopy (XPS) measurements using a Thermo Escalab 250xi electron spectrometer. XPS peaks were used for XPS data processing and peak fitting. Three-dimensional excitation-emission matrix fluorescence spectra (3D EEMs) were performed on a fluorescence spectrometer to further monitor the structural destruction process of the pollutants. The specific surface area of ​​the nitrogen adsorption isotherm was determined using a Micrometrics ASAP 2020 instrument.

[0045] Sulfadimethoxazole (SMZ) was selected as the target pollutant. In an air environment, 100 mL of SMZ solution (20 mg / L, 50 mM sodium sulfate) was added to a 150 mL beaker for testing. The initial pH value of the reaction solution was adjusted with 1 M sulfuric acid or 0.2 M sodium hydroxide. Ruthenium-iridium-titanium electrode (2×3 cm 2 ) and the prepared electrodes (2×3 cm 2 ) as anode and cathode respectively. Constant current was provided by a DC power supply. During the degradation experiment, 1 mL of solution was collected at intervals and filtered into a brown vial using a 0.22 µm membrane. The degradation of natural organic matter (NOM) and inorganic anions (such as Cl) were investigated by adding humic acid (HA) and sodium salts. - 、NO3 - 、H2PO4 - ) on the removal performance of SMZ. Actual water matrix tests were carried out to explore its practical application.

[0046] (3) Results and discussion

[0047] Electrode material characterization

[0048] The surface morphology and surface elements of the prepared electrode were detected using scanning electron microscopy (SEM).

[0049] The results show that the relatively smooth surface of CC ( Figure 2 Part A and Fig.11 The a part in the middle becomes rough after calcination, and the pores are increased (ECC, Figure 2 Part b and Fig.11 The specific surface area is increased. The rough surface structure is more conducive to the subsequent catalyst adhesion. After hydrothermal modification, the Prussian blue precursor particles are densely attached to the ECC surface in layers ( Figure 2 Part C, Figure 2 Part D and Fig.11 However, as the low-temperature phosphating calcination process progresses, a considerable portion of the Prussian blue particles on the surface of the PB@ECC electrode collapse, exposing more internal ECC electrodes ( Figure 2 In the e part, Figure 2 Part f, Figure 2 (g part).

[0050] Figure 3 The graph shows the N2 adsorption-desorption isotherms of different electrodes. In addition, the catalyst particles retained on the electrode surface still maintain the benign original structure and the active sites are retained. The FeP@ECC electrode obtained after low-temperature phosphating calcination treatment has a more advanced pore structure, which provides more channels for subsequent mass transfer ( Figure 4). In addition, HRTEM further confirmed the presence of PB-derived co-catalyst nanoparticles on the electrode surface ( Figure 2 h part). Figure 2 From the h part, we can see that there are two lattice fringes with spacing of 0.27 nm and 0.24 nm in FeP@ECC, corresponding to the (011) and (111) crystal planes of FeP, respectively, revealing the formation of iron phosphide. EDS element mapping of FeP@ECC electrode ( Figure 5 ) clearly shows the uniform distribution of N, P, O, Co and Fe elements on the electrode.

[0051] XRD patterns of PB and FeP@ECC are shown in Figure 2. Figure 6 As shown in the figure, the diffraction peaks of the Prussian blue precursor are consistent with potassium ferrocyanide (PDF#01-0239), indicating that it was successfully prepared. For the derivative synthesized by phosphating the Prussian blue precursor, the apparent peaks near 32.3°, 48.3°, 50.3°, 56.1° and 59.6° belong to the (011), (211), (130), (031) and (002) lattices of FeP. The broad peak around 25.1° is caused by the amorphous carbon structure in the structure.

[0052] XPS analysis shows that FeP@ECC is composed of the expected C, N, Co, Fe, and P elements ( Figure 7 Part A and Figure 7 Fourier transform infrared spectroscopy (FT-IR) showed ( Figure 7 In the sample, at 2359 cm −1 There is a sharp absorption peak at 2080 cm −1 The characteristic peak detected at is attributed to the coordinated cyano group Fe 2+ -C≡N-Fe 3+ The stretching vibration of -C≡N- in FeP@ECC is at 950 and 1080 cm −1 Two characteristic peaks appear at the , which belong to the vibration peaks of OPO and PO2 and PO3 groups respectively.

[0053] Raman spectroscopy ( Figure 7 Part (d) shows that all samples have a peak at 1340 cm -1 (D key) and 1585 cm -1There are two obvious peaks near (G bond), which are related to the existence of disordered carbon structure and graphitic carbon structure respectively. The fitting intensity values ​​of D band and G band (ID / IG) are usually used to calculate and quantify the surface defect degree of carbon materials. It can be clearly observed that ECC has the highest ID / IG intensity value of 0.9543, indicating that the addition of Co atoms enhances the degree of carbon defects, which is conducive to the generation of more active sites, promotes the transfer of outer electrons, and is conducive to the generation of hydrogen peroxide. In addition, the presence of FeP in FeP@ECC with a high degree of graphitization can accelerate the ordered π-π stacking of ECC, which is conducive to electron transfer.

[0054] (4) Evaluation of the catalytic performance of FeP@ECC and the effects of different experimental conditions

[0055] SMZ degradation performance of different cathode materials Figure 8 As shown in part a-part b. It can be seen that when CC is directly used as the cathode, the degradation rate of SMZ within 20 minutes is poor (23.94%). After in-situ etching of cobalt oxide, the degradation rate of ECC increased to 59.34%, which is due to the fact that the introduction of a small amount of metal oxides promoted the activation of H2O2. After the hydrothermal introduction of the Prussian blue precursor, the appearance of a large number of metal active sites is conducive to promoting the generation of a large amount of ROS by H2O2, further increasing the SMZ removal rate to 78.08%. As expected, after effective low-temperature phosphating and calcination treatment, the FeP@ECC electrode exhibited the best degradation performance (100%, k reached 0.28263). In addition, the degradation rate of Fe3O4@ECC obtained by direct low-temperature calcination without phosphorus doping was 76.91%, as shown Fig.10 This further illustrates that FeP@ECC has excellent catalytic performance.

[0056] from Figure 8 It can be seen from part c that with the increase of calcination temperature, the degradation of SMZ first increases and then decreases. Under the synthesis condition of 350℃, the degradation performance of FeP@ECC electrode is the best, and its reaction rate constant and degradation rate are the highest. The results show that increasing the calcination temperature is beneficial to improving the catalytic effect of the electrode. However, when the temperature reaches 450℃, the removal efficiency of SMZ decreases significantly, which may be due to the destruction of the catalyst structure and the formation of impurities caused by the increase in temperature. Therefore, the FeP@ECC electrode prepared at a calcination temperature of 350℃ was selected for the next experiment.

[0057] Figure 8Part d in the figure shows the effect of the initial pH value of the solution on the catalytic activity of the EF system. The degradation performance of FeP@ECC on SMZ was investigated in a wide pH range. It can be clearly seen that when the pH exceeds 3, the catalytic performance of FeP@ECC decreases significantly. This is because under neutral or alkaline conditions, H2O2 is extremely unstable, resulting in a decrease in its concentration, which is not conducive to the subsequent generation of ROS. Therefore, the subsequent experiments were carried out under the condition of pH=3.

[0058] Figure 8 Part (e) shows the catalytic performance of FeP@ECC under different applied currents. It can be seen that the greater the applied current, the greater the SMZ degradation rate. This is because the higher applied current promotes electron transfer during the reaction, which is beneficial to the generation of ROS and the degradation of SMZ. Based on the above results, we selected 50 mA as the most appropriate current for subsequent degradation experiments.

[0059] Depend on Figure 8 From the middle f part, we can see that the degradation effect of SMZ is the best when the initial concentration of SMZ is 20 mg / L. However, as the concentration of pollutants increases further, the degradation rate of SMZ decreases significantly. This is because SMZ and its intermediates occupy more active sites on the electrode, and free radicals cannot be produced in large quantities, resulting in a continuous decrease in degradation efficiency.

[0060] In order to study the anti-interference ability of FeP@ECC / EF system ( Figure 8 Middle g part - Figure 8 In the h part of Figure 2, the effect of adding humic acid (HA) and inorganic anions on the degradation of SMZ was studied. The effect of HA on the degradation of CAP by FeP@ECC / EF system is shown in Figure 8 It can be observed that the addition of HA has an inhibitory effect on the removal of SMZ, and the inhibitory effect becomes greater as the HA concentration increases.

[0061] The loss of catalytic activity of FeP@ECC can be explained from two key aspects:

[0062] 1) HA can compete with SMZ for the electrophilic ∙OH due to its electron-rich sites;

[0063] 2) Since HA is attached to the heterogeneous FeP@ECC surface, the interaction between H2O2 and the catalytic sites is hindered.

[0064] In addition, it can be observed that in the FeP@ECC-EF process, Cl − The presence of ∙OH can slightly inhibit the degradation of SMZ. −The oxidation generates chlorine species with lower activity than ∙OH radicals, which can also participate in the SMZ oxidative degradation process. − The degradation of SMZ was adversely affected by H2PO4 − The reaction rate with ∙OH is slow, and the formation of a weak oxidant (H2PO4∙) cannot effectively oxidize SMZ. In addition, NO3 − The presence of NO3 also led to a significant decrease in the SMZ degradation efficiency after 20 minutes of treatment, because − It will react with the more active hydroxyl radicals in the system to form less active free radicals (NO3∙).

[0065] In order to further investigate the practical application performance of the FeP@ECC / EF system, actual water samples such as deionized water, tap water (TapWater), river water (River Water) and lake water (Lake Water) were selected ( Figure 8 (i) Tap water, river water, and lake water do not contain SMZ by themselves. Therefore, appropriate amounts of SMZ were dissolved in the collected real water to prepare real water matrices (tap water, river water, and lake water) containing 20 mg / L SMZ. Deionized water was used as a control sample. After 60 min of heterogeneous EF reaction, the degradation efficiencies of SMZ were 96.9%, 80.23%, and 86.89%, respectively, which were all lower than that of ultrapure water (100%). The lower degradation efficiency and kinetics of SMZ in tap water, river water, and lake water may be due to the presence of inorganic ions and organic matter, which consume active free radicals as mentioned above. Despite the degradation differences, overall, the FeP@ECC / EF system has good SMZ removal efficiency in real water, thus establishing its potential as a promising catalyst.

[0066] Three-dimensional excitation-emission matrix fluorescence spectroscopy (3D EEMs) was used to elucidate the degradation of SMZ. The fluorescence signal of SMZ mainly comes from its conjugated heterocyclic structure. Fig. 9 As shown in the figure, there are two different fluorescence centers at Ex / Em: 250~320 / 360~480 nm and Ex / Em: 320~400 / 420~510 nm, corresponding to aromatic protein fluorophores and humic acid products, respectively. During the reaction, the fluorescence intensity at Ex / Em = 250~320 / 360~480 nm was significantly weakened, while the fluorescence intensity at Ex / Em = 320~400 / 420~510 nm was slightly increased. The above results indicate that SMZ has been deeply degraded, and the fluorescence intensity at Ex / Em = 320~400 / 420~510 nm has increased due to the accumulation of some humic acid intermediates during the degradation process.

[0067] The above are only preferred embodiments of the present application, and are not intended to limit the patent scope of the present application. Any equivalent structure or equivalent process transformation made using the contents of the present application specification and drawings, or directly or indirectly applied in other related technical fields, are also included in the patent protection scope of the present application.

Claims

1. A method for removing sulfamethoxazole from water by in-situ etching of carbon felt modified with iron phosphide, characterized in that: The following steps are involved: Obtain target sewage; use 1M sulfuric acid or 0.2M sodium hydroxide to adjust the pH value of the target sewage to ≤3; use a ruthenium-iridium-titanium electrode as an anode and a FeP@ECC electrode as a cathode to remove sulfamethoxazole in the target sewage, and the maximum reaction rate constant is 0.28263; The FeP@ECC electrode is prepared by the following steps: subjecting the carbon felt to ultrasonic treatment to remove impurities to obtain a clean carbon felt; immersing the clean carbon felt in a cobalt acetate ethanol solution for 2 hours, drying and placing it in a muffle furnace for calcination, and after the calcination is completed, taking it out, washing and drying it to obtain ECC; dispersing potassium ferrocyanide and polyvinyl pyrrolidone in a hydrochloric acid solution, stirring it magnetically until it is clear, and then immersing the ECC in it for reaction, and after the reaction is completed, washing and drying the product to obtain PB@ECC; placing sodium hypophosphite and PB@ECC in the upstream and downstream of a tubular furnace respectively, and calcining it under nitrogen for 2 hours. h; after the calcination, washing with ethanol and deionized water alternately to obtain a FeP@ECC electrode; the FeP@ECC electrode is obtained after low-temperature phosphating calcination treatment, and the temperature of the low-temperature phosphating calcination treatment is ≤350°C; the potassium ferrocyanide and polyvinyl pyrrolidone are dispersed in a hydrochloric acid solution, magnetically stirred until clear, and then ECC is immersed in the solution for reaction, and after the reaction is completed, the product is washed and dried to obtain PB@ECC, including: 0.11 g potassium ferrocyanide and 0.39 g polyvinyl pyrrolidone are dispersed in 50 mL of a hydrochloric acid solution with a pH of 1, magnetically stirred until clear, and then ECC is immersed in the solution, and then placed in a stainless steel reactor for reaction at 80°C for 24 h, and washed and dried and marked as PB@ECC; The ruthenium-iridium-titanium electrode is used as the anode and the FeP@ECC electrode is used as the cathode to remove sulfamethoxazole in the target wastewater. The applied current is 50 mA. For every 20 mg / L sulfamethoxazole, 2×3 cm 2 Ruthenium-iridium-titanium electrode was used as the anode, using a 2×3 cm 2 The FeP@ECC electrode was used as the cathode.

2. The method for removing sulfamethoxazole from water by in-situ etching of carbon felt modified with iron phosphide according to claim 1, characterized in that: The step of subjecting the carbon felt to ultrasonic treatment to remove impurities and obtain cleaned carbon felt comprises: The carbon felt was placed in ethanol and deionized water for 10 min each to remove impurities and obtain clean carbon felt.

3. The method for removing sulfamethoxazole from water by in-situ etching of carbon felt modified with iron phosphide according to claim 1, characterized in that: The washed carbon felt is immersed in a cobalt acetate ethanol solution for 2 hours, dried and placed in a muffle furnace for calcination. After the calcination is completed, the carbon felt is taken out, washed and dried to obtain ECC, comprising: The cleaned carbon felt was immersed in 1g / L cobalt acetate ethanol solution for 2h, dried and placed in a muffle furnace, heated to 300℃ and calcined for one hour; then heated to 400℃ and calcined for one hour; the heating rate was 5℃ / min; After calcination, the product was taken out, cleaned and dried to obtain ECC.

4. The method for removing sulfamethoxazole from water by in-situ etching of carbon felt modified with iron phosphide according to claim 1, characterized in that: The sodium hypophosphite and PB@ECC are placed in the upstream and downstream of the tube furnace respectively, and calcined for 2 hours under nitrogen conditions; after the calcination, they are washed alternately with ethanol and deionized water to obtain a FeP@ECC electrode, including: Sodium hypophosphite and PB@ECC were placed in the upstream and downstream of a tube furnace, respectively, and heated to 350°C at a rate of 3°C / min under nitrogen conditions and calcined for 2 h. After calcination, they were washed alternately with ethanol and deionized water to obtain a FeP@ECC electrode.