Sludge drying method with interface evaporation driven by solar energy

Through solar-driven interfacial evaporation technology and photothermal interfacial evaporation of modified balsa wood blocks, combined with moisture sensors and ultrasonic removal, the problems of high energy consumption and high carbon emissions in sludge drying technology are solved, achieving high efficiency and low cost. , low-carbon emission sludge drying and heavy metal removal.

CN118754389AActive Publication Date: 2024-10-11QUZHOU RES INST OF ZHEJIANG UNIV +1
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202410888003.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-04
Publication Date
2024-10-11
Estimated Expiration
2044-07-04

AI Technical Summary

Technical Problem

Existing sludge drying technology has high energy consumption, high carbon emissions, high costs, and the inability to effectively reduce heavy metals in sludge. It is difficult to achieve an efficient drying method with low cost, low energy consumption, and low carbon emissions.

Method used

Solar-driven interfacial evaporation technology is used to conduct photothermal interfacial evaporation through modified balsa wood blocks (delignified balsa wood blocks), combined with real-time monitoring of moisture sensors and ultrasonic removal of heavy metals, to achieve low-carbon drying of sludge and removal of heavy metals. .

Benefits of technology

It achieves efficient drying of sludge and removal of heavy metals, reducing carbon emissions by more than 95%. It is simple to operate, low in cost, and the materials can be recycled. It is suitable for sludge drying with various moisture contents and achieves sludge drying. Real-time monitoring of processes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118754389A_ABST
    Figure CN118754389A_ABST
Patent Text Reader

Abstract

The invention relates to a solid waste treatment technology, and aims to provide a sludge drying method for solar-driven interface evaporation. The method comprises the following steps: cutting balsa wood into long columns, dipping the long columns in a lignin-removing solution, and performing vacuum freeze-drying treatment; then sequentially dropwise adding an ammonium persulfate solution and a pyrrole dispersion liquid on the upper surface of the lignin-removed light wood block, and enabling ammonium persulfate as an oxidizing agent to be subjected to oxidative polymerization reaction with pyrrole to form a polypyrrole layer; vertically inserting the light wood block into the water-containing sludge, and respectively arranging moisture sensors on the polypyrrole layer and the intersection interface of the light wood block and the sludge; a photo-thermal interface evaporation effect is formed on the polypyrrole layer by utilizing sunlight irradiation, the moisture content change condition is known by monitoring the difference of voltage values through a moisture sensor based on a hydroelectric effect caused by evaporation, and the sludge drying progress is confirmed. According to the method disclosed by the invention, the sludge is dried by utilizing sunlight, so that the dependence on traditional fossil energy is reduced; operation is easy and convenient, cost is low, operation is safe, and evaporation materials can be recycled.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to solid waste treatment technology, and in particular to sludge drying treatment. The photothermal interface evaporation technology is used to perform low-carbon drying on water-containing sludge and remove heavy metals, while achieving real-time monitoring of the sludge moisture content. Background Art

[0002] Sludge is a waste generated during sewage treatment. It is mainly composed of suspended matter removed from sewage and contains a large amount of organic and inorganic substances (such as heavy metals). Proper treatment of sludge is a key link to ensure environmental protection and prevent secondary pollution. Traditional sludge treatment technology mainly includes steps such as concentration, conditioning, dehydration, stabilization, drying or incineration. The water content in sludge is usually greater than 90%, so sludge drying is a key step in the sludge treatment process. Especially before the sludge needs to be incinerated or other forms of resource utilization, its water content must be greatly reduced to ensure the calorific value.

[0003] Traditional sludge drying technologies mainly include: mechanical dehydration, thermal drying and solar drying. Mechanical dehydration includes centrifugal dehydration, belt filter press and screw press, etc. These methods can reduce the moisture content of sludge from more than 90% to about 70% to 80%. Although mechanical dehydration can effectively reduce the volume of sludge, it consumes a lot of energy and usually cannot reduce the moisture content to a level suitable for incineration. Therefore, mechanical dehydration can only be used as a pre-dehydration treatment, and more in-depth drying treatment is still required later. Thermal drying technology is currently a widely used sludge drying method. By directly or indirectly heating the water in the sludge to evaporate, the moisture content of the sludge can be reduced to less than 50%, or even lower. This method is highly efficient, but the energy consumption, carbon emissions and operating costs are all high. In order to reduce the energy consumption of sludge drying, the invention patent "A high-temperature heat pump superheated steam drying system" (CN117700068 A) provides a technology that combines a high-temperature heat pump with superheated steam drying, and uses a steam circulation device to extract the water vapor generated by drying for circulation, which effectively improves energy efficiency, but the system still requires a lot of electric energy to drive. In order to further reduce energy consumption and reduce carbon emissions, the invention patent "Controllable temperature sludge drying system and temperature control method" (CN117945621 A) provides a method of converting solar energy into electrical energy and powering the sludge drying system, but this method requires complex optoelectronic and control systems, which increases equipment costs. In addition, there is also an invention patent "Solar thermal coupling sludge drying system" (CN 108409095 A) that uses a trough solar thermal collection and storage system as a heat source for a disc indirect sludge drying system. This method is simpler and has lower energy consumption than the above two invention patents, but it does not remove heavy metals from the sludge.

[0004] Therefore, finding a low-cost, low-energy, low-carbon emission, clean, environmentally friendly and efficient sludge drying method is an urgent problem that needs to be solved. Summary of the invention

[0005] The technical problem to be solved by the present invention is to overcome the deficiencies of the prior art and provide a sludge drying method by solar-driven interface evaporation.

[0006] In order to solve the technical problem, the solution of the present invention is:

[0007] A sludge drying method using solar-driven interfacial evaporation is provided, comprising the following steps:

[0008] (1) dissolving sodium hypochlorite and glacial acetic acid in water and mixing them evenly to prepare a delignification solution;

[0009] (2) cutting balsa wood into long cylinders, completely immersing them in a delignified solution, and heating them at 100° C. for 12 to 16 hours; taking them out, rinsing them with water until the pH value of the rinsing solution is neutral, and performing vacuum freeze drying to obtain delignified balsa wood blocks;

[0010] (3) dripping an ammonium persulfate solution and a pyrrole dispersion onto the upper surface of the delignified balsa wood block in sequence, so that the ammonium persulfate as an oxidant reacts with the pyrrole for an oxidative polymerization reaction; after reacting for 10 to 20 minutes, washing the residual liquid on the surface with water; and then performing a vacuum freeze-drying treatment to obtain a delignified balsa wood block having a polypyrrole layer on the upper surface;

[0011] (4) taking a number of delignified balsa wood blocks with polypyrrole layers, inserting them vertically into the water-containing sludge, ensuring that 80% to 90% of their height is exposed outside the sludge; respectively setting moisture sensors on the polypyrrole layer of the balsa wood block and on the interface with the sludge, and each sensor is connected to a detection recorder through a signal line;

[0012] The sunlight is irradiated on the surface of the sludge and the balsa wood block, and a photothermal interface evaporation effect is formed on the polypyrrole layer. Based on the hydroelectric effect caused by evaporation, the difference in the voltage value of the moisture sensor monitoring is formed at different positions, and the voltage difference is used to monitor the change of moisture content at different positions. When the moisture content monitoring data meets the expected value, the balsa wood block is taken out, and the sludge has been dried at this time.

[0013] (5) The balsa wood block is immersed in an acid solution and subjected to a heavy metal removal operation under ultrasonic conditions; after being taken out, the residual acid and heavy metals are removed by rinsing with clean water until the pH value of the rinsing solution is between 6 and 7; the balsa wood block is then dried to obtain a reusable balsa wood block.

[0014] As a preferred embodiment of the present invention, in the step (1), when preparing the delignification solution, 4 to 6 g of sodium hypochlorite and 1 to 2 mL of glacial acetic acid are added to every 100 mL of water.

[0015] As a preferred embodiment of the present invention, in step (2), the material of the balsa wood block is fir, paulownia or pine; the long column is a cylinder or a square column, with a height of 10 to 20 cm and a radial dimension or lateral width of 2 to 5 cm.

[0016] As a preferred embodiment of the present invention, in step (2) or step (3), the freeze-drying treatment is carried out in a freeze dryer, the drying temperature is set to -40°C, the drying time is 12 to 24 hours, and the vacuum degree is lower than 10Pa; after drying, the temperature is slowly raised to room temperature at a rate of 0.4 to 0.6°C / min to avoid damage to the internal structure of the wood.

[0017] As a preferred embodiment of the present invention, in the step (3), 2 to 3 g of ammonium persulfate is added to 100 mL of water, and the mixture is mixed to obtain an ammonium persulfate solution; 0.5 to 1 mL of pyrrole is added to 100 mL of water, and the mixture is mixed to obtain a pyrrole dispersion; and the ammonium persulfate solution and the pyrrole dispersion are added dropwise in equal volumes, and the amount of the added dropwise amount is controlled so that the thickness of the polypyrrole layer is 50 to 100 microns.

[0018] As a preferred embodiment of the present invention, in step (4), the moisture content of the sludge is between 90% and 98%, the total volume of the balsa wood blocks used accounts for 5% to 10% of the total volume of the sludge, and the balsa wood blocks are evenly arranged in the sludge in an array.

[0019] As a preferred embodiment of the present invention, in step (4), the moisture sensor has a copper electrode; when it is monitored that the voltage difference between the two electrodes is continuously and stably lower than 0.02 to 0.05 V, the drying process is terminated, and the moisture content of the sludge is between 30% and 40%.

[0020] As a preferred embodiment of the present invention, in the step (5), the cleaning time under ultrasonic conditions is 10 to 30 minutes; the ultrasonic frequency is set to 28 kHz, and the ultrasonic power is set to 500 to 1000 W.

[0021] As a preferred embodiment of the present invention, in step (5), the acidic solution is 0.1 mol / L hydrochloric acid or 0.1 mol / L nitric acid solution; and the heavy metals removed by ultrasound include at least copper, lead, zinc and cadmium.

[0022] Description of the invention principle:

[0023] The present invention proposes to use modified balsa wood as a photothermal evaporation medium to improve the sludge drying efficiency while strengthening the removal effect of the evaporator on heavy metals in the sludge, thereby achieving the goal of reducing pollution and carbon emissions. The relevant technical principles are as follows:

[0024] (1) Material selection and preparation:

[0025] Balsa wood (fir, paulownia, pine) was chosen as the substrate mainly because of its low density and high porosity. These balsa woods grow fast in nature, are easy to process, and have relatively low cost. However, the water transport capacity of the original wood is poor. The lignin in the balsa wood is removed through specific chemical treatment, the cellulose-rich structure is retained, the original pore structure of the balsa wood is not destroyed, and the porosity of the material is further increased. It has super hydrophilicity and provides an ideal water transport medium for water evaporation. Ammonium persulfate solution and pyrrole dispersion are sequentially dripped on the upper surface of the delignified balsa wood block. Ammonium persulfate acts as an oxidant to react with pyrrole for oxidative polymerization to generate polypyrrole. Since the upper surface of the balsa wood block has an extremely high specific surface area and porosity, the generated fine polypyrrole is quickly adsorbed on the fiber surface and is difficult to desorb. This modification not only does not affect the pore structure of the balsa wood block, but also improves its ability to absorb and convert light and heat energy. During the freeze-drying process, the temperature is slowly raised to room temperature at a rate of 0.4-0.6°C / min to avoid damage to the wood structure, which would affect the subsequent evaporation and heavy metal adsorption and removal effects.

[0026] (2) Photothermal interface evaporation:

[0027] The polypyrrole layer significantly improves the photothermal efficiency of the material, enabling it to quickly absorb sunlight and convert it into heat energy. This efficient photothermal conversion promotes the rapid evaporation of water in the sludge. The high specific surface area and pore structure of the polypyrrole delignified balsa wood block enable it to quickly transfer heat energy while in contact with the sludge, accelerate water evaporation, and efficiently and quickly reduce the moisture content of the sludge. In addition, by connecting electrodes on the upper surface of the polypyrrole delignified balsa wood block and the sludge interface, the electrode material is a corrosion-resistant copper electrode. The hydroelectric effect caused by evaporation causes the voltage between the electrodes to change, realizing real-time monitoring of the sludge moisture. This self-detection technology can not only determine the end time of drying, but also adjust the processing parameters according to the sludge drying state and optimize the drying process.

[0028] (3) High efficiency adsorption of heavy metals:

[0029] In addition to the drying effect, the polypyrrole delignified balsa wood block also has the function of adsorbing heavy metals. After delignification, the lignin in the cell wall of the wood is removed, leaving more gaps, that is, increased porosity. These pores serve as channels for water and pollutants, not only promoting the transmission and evaporation of water, but also providing more surface area for the adsorption of heavy metals (such as copper, lead, cadmium, zinc, etc.) and organic pollutants in the sludge. During the drying process, as the water evaporates, the heavy metal ions in the sludge will increase their contact opportunities on the surface of the polypyrrole delignified balsa wood block due to the concentration effect, thereby improving the adsorption efficiency. In addition, the heat generated during the evaporation process also helps to open more pores and active sites, enhancing the adsorption of pollutants such as heavy metals. After drying, the balsa wood blocks are taken out and ultrasonically cleaned with acid to remove heavy metals and impurities adsorbed from the sludge. Due to the extremely strong adsorption ability of polypyrrole on the fiber surface, no obvious desorption occurs and the pore structure is not affected. The polypyrrole delignified balsa wood blocks show extremely strong physical and chemical stability and can be repeatedly recycled to reduce the cost of material use.

[0030] Based on the above principle, modified balsa wood blocks (polypyrrole delignified balsa wood blocks) are used to achieve efficient evaporation of water in sludge and efficient removal of heavy metals by combining interface evaporation and chemical adsorption processes, as well as an ingenious moisture self-detection method. The moisture content is detected in real time to determine the end time of drying.

[0031] Compared with the prior art, the present invention has the following advantages:

[0032] 1. The present invention uses sunlight to dry sludge, reducing dependence on traditional fossil energy and reducing carbon emissions by more than 95% compared to traditional drying methods;

[0033] 2. The present invention is simple and convenient to operate, low in cost, safe in operation, and the evaporation material can be recycled;

[0034] 3. The specifications of the cork blocks used in the present invention are adjustable, and are suitable for drying sludge with various moisture contents, and have high evaporation efficiency;

[0035] 4. The present invention not only plays the role of efficient evaporation, but also plays the role of efficient removal of heavy metals in sludge, with a removal rate of more than 70%;

[0036] 5. A moisture sensor is installed on the cork block to realize real-time monitoring of the sludge drying process and to adjust the evaporation conditions. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] Figure 1 It is a flow chart of the present invention. DETAILED DESCRIPTION

[0038] The present invention is further described in detail below in conjunction with the accompanying drawings and specific embodiments.

[0039] Part I Implementation of the Invention

[0040] The sludge drying method of solar-driven interfacial evaporation of the present invention comprises the following steps:

[0041] (1) Add 4-6 g of sodium hypochlorite and 1-2 mL of glacial acetic acid to every 100 mL of water and mix well to prepare a delignification solution;

[0042] (2) cutting balsa wood into long cylinders, completely immersing them in a delignified solution, and heating them at 100° C. for 12 to 16 hours; taking them out, rinsing them with water until the pH value of the rinsing solution is neutral, and performing vacuum freeze drying to obtain delignified balsa wood blocks;

[0043] The material of the balsa wood block can be balsa fir, paulownia or pine; the shape of the long column can be cylindrical or square, with a height of 10 to 20 cm and a radial dimension or lateral width of 2 to 5 cm. The freeze-drying process is carried out in a freeze dryer, with a drying temperature set at -40°C, a drying time of 12 to 24 hours, and a vacuum degree set below 10 Pa; after drying, the temperature is slowly raised to room temperature at a rate of 0.4 to 0.6°C / minute to avoid damage to the internal structure of the wood.

[0044] (3) Add 2-3 g of ammonium persulfate to every 100 mL of water, mix well to obtain an ammonium persulfate solution; add 0.5-1 mL of pyrrole to every 100 mL of water, mix well to obtain a pyrrole dispersion; drip the ammonium persulfate solution and the pyrrole dispersion onto the upper surface of the delignified balsa wood block in equal volumes, so that the ammonium persulfate acts as an oxidant and reacts with the pyrrole for oxidative polymerization; control the dripping amount so that the thickness of the polypyrrole layer is 50-100 microns. After reacting for 10-20 minutes, rinse the residual liquid on the surface with water; then perform vacuum freeze drying to obtain a delignified balsa wood block with a polypyrrole layer on the upper surface;

[0045] The freeze drying process is carried out in a freeze dryer, with the drying temperature set at -40°C, the drying time set at 12 to 24 hours, and the vacuum degree set below 10Pa; after drying, the temperature is slowly raised to room temperature at a rate of 0.4 to 0.6°C / minute to avoid damage to the internal structure of the wood.

[0046] (4) Take a number of delignified balsa wood blocks with polypyrrole layers, insert them vertically into the water-containing sludge, and ensure that 80% to 90% of their height is exposed outside the sludge; respectively set moisture sensors on the polypyrrole layer of the balsa wood block and the interface with the sludge, and each sensor is connected to a detection recorder through a signal line; allow sunlight to irradiate the surface of the sludge and the balsa wood block, and form a photothermal interface evaporation effect on the polypyrrole layer; based on the hydroelectric effect caused by evaporation, a difference in the voltage value of the moisture sensor monitoring is formed at different positions, and the voltage difference is used to monitor the change of moisture content at different positions; when the moisture content monitoring data meets the expected value, remove the balsa wood block, and the sludge has also been dried;

[0047] As an optional solution, the moisture content of the sludge is between 90% and 98%, the total volume of the balsa wood blocks used accounts for 5% to 10% of the total volume of the sludge, and the balsa wood blocks are evenly arranged in the sludge in an array; the moisture sensor has copper electrodes; when it is monitored that the voltage difference between the two electrodes is continuously and stably lower than 0.02 to 0.05V, the drying process is terminated, and the moisture content of the sludge is between 30% and 40%.

[0048] (5) The balsa wood block is immersed in an acid solution and subjected to a heavy metal removal operation under ultrasonic conditions; after being taken out, the residual acid and heavy metals are removed by rinsing with clean water until the pH value of the rinsing solution is between 6 and 7; the balsa wood block is then dried to obtain a reusable balsa wood block.

[0049] As an optional solution, the cleaning time under ultrasonic conditions is 10 to 30 minutes; the ultrasonic frequency is set to 28 kHz, and the ultrasonic power is 500 to 1000 W; the acidic solution is 0.1 mol / L hydrochloric acid or 0.1 mol / L nitric acid solution; the heavy metals removed by ultrasound include at least copper, lead, zinc, and cadmium.

[0050] Part II Specific Examples and Comparative Examples Specific embodiment 1

[0052] (1) To every 100 mL of clean water, 4 g of sodium hypochlorite and 1 mL of glacial acetic acid were added in sequence and mixed evenly to prepare a delignified solution.

[0053] (2) Cut balsa wood into long cylinders, where balsa wood is selected, and the size of the long cylinder is set to be 10 cm in height and 2 cm in bottom diameter; and completely immerse it in a delignification solution and heat it at 100°C for 12 hours. After the heating is completed, rinse the balsa wood block with clean water and detect the pH of the rinse solution until the pH of the rinse solution reaches neutral, thereby obtaining a treated balsa wood block.

[0054] (3) The treated balsa wood blocks were placed in a freeze dryer for drying, with the drying temperature set at -40°C, the drying time set at 12 hours, and the vacuum degree set at less than 10 Pa. After the drying time was over, the temperature was slowly raised to room temperature at a rate of 0.4°C / min to obtain delignified balsa wood blocks.

[0055] (4) Add 2 g of ammonium persulfate to every 100 mL of clean water and mix well to obtain an ammonium persulfate solution; add 0.5 mL of pyrrole to every 100 mL of water and mix well to obtain a pyrrole dispersion; prepare for the subsequent polypyrrole layer.

[0056] (5) The ammonium persulfate solution and the pyrrole dispersion were sequentially dripped onto the upper surface of the delignified balsa wood block, and the dripping amount was controlled so that the thickness of the polypyrrole layer was 50 μm. After reacting for 10 minutes, the liquid residue on the surface was rinsed with clean water, and then the wood block was placed in a freeze dryer for drying, and the drying temperature was set to minus 40 degrees Celsius, the drying time was 12 hours, and the vacuum degree was less than 10 Pa. After the drying time was over, the temperature was slowly raised to room temperature at a rate of 0.4°C / min to obtain a delignified balsa wood block with a polypyrrole layer on the upper surface.

[0057] (6) Prepare several polypyrrole delignified wood blocks according to the above steps (1-5), and place them in the sludge. The selected sludge has a moisture content of 90%, and the volume of the polypyrrole delignified wood blocks accounts for 5% of the sludge volume; and the sludge polypyrrole delignified wood blocks are evenly placed on the sludge in an array, ensuring that 10% of the height of the wood blocks is immersed in the sludge and 90% of the height is exposed to the sludge, and the sludge is placed under sunlight. A moisture sensor is set at the interface between the polypyrrole delignified wood block and the sludge. The sensor can detect and record the change in moisture. The moisture sensor measures the voltage change generated by the hydroelectric effect caused by evaporation through two copper electrodes installed on the upper surface of the polypyrrole delignified wood block and the sludge, and determines the moisture content in the sludge by real-time monitoring of the voltage. When the monitored voltage is lower than the set threshold of 0.02V and remains stable, the wood block is removed to end the drying, and the final sludge moisture content is 40%.

[0058] (7) After the sludge is dried, the polypyrrole delignified light wood block is taken out, and the heavy metal removal rate of the sludge is 74%. The wood block is subjected to heavy metal removal operation, and the heavy metals mainly include harmful metals such as copper, lead, zinc, and cadmium. The wood block is soaked in 0.1mol / L hydrochloric acid, and ultrasonic cleaning is used as an auxiliary. The ultrasonic cleaning time is set to 10 minutes, the ultrasonic frequency is set to 28kHZ, and the ultrasonic power is set to 500W. After the cleaning is completed, rinse with clean water to remove residual hydrochloric acid solution and heavy metals. When the pH of the rinse liquid is detected to be between 6, the rinsing is stopped, and the rinsed wood block is dried to finally obtain a reusable polypyrrole delignified light wood block. Specific embodiment 2

[0060] (1) To every 100 mL of clean water, 5 g of sodium hypochlorite and 1.5 mL of glacial acetic acid were added in sequence and mixed evenly to prepare a delignification solution.

[0061] (2) Cutting balsa wood into rectangular cylinders, wherein paulownia wood is selected as the balsa wood, and the size of the rectangular cylinder is set to 15 cm in height and 3.5 cm in bottom width; and completely immersing the rectangular cylinder in a delignification solution, and heating the rectangular cylinder at 100°C for 14 hours. After the heating is completed, the balsa wood block is rinsed with clean water, and the pH of the rinse liquid is detected until the pH of the rinse liquid reaches neutral, thereby obtaining a treated balsa wood block.

[0062] (3) The treated balsa wood blocks were placed in a freeze dryer for drying, with the drying temperature set at -40°C, the drying time set at 18 hours, and the vacuum degree set at less than 10 Pa. After the drying time was over, the temperature was slowly raised to room temperature at a rate of 0.5°C / min to obtain delignified balsa wood blocks.

[0063] (4) Add 2.5 g of ammonium persulfate to every 100 mL of clean water and mix well to obtain an ammonium persulfate solution; add 0.75 mL of pyrrole to every 100 mL of water and mix well to obtain a pyrrole dispersion; prepare for the subsequent polypyrrole layer.

[0064] (5) The ammonium persulfate solution and the pyrrole dispersion were sequentially dripped onto the upper surface of the delignified balsa wood block, and the dripping amount was controlled so that the thickness of the polypyrrole layer was 75 μm. After 15 minutes of reaction, the liquid residue on the surface was rinsed with clean water, and then the wood block was placed in a freeze dryer for drying, and the drying temperature was set to minus 40 degrees Celsius, the drying time was 18 hours, and the vacuum degree was less than 10 Pa. After the drying time was over, the temperature was slowly raised to room temperature at a rate of 0.5°C / min to obtain a delignified balsa wood block with a polypyrrole layer on the upper surface.

[0065] (6) Prepare several polypyrrole delignified wood blocks according to the above steps (1-5), and place them in the sludge. The selected sludge has a moisture content of 94%, and the volume of the polypyrrole delignified wood blocks accounts for 7.5% of the sludge volume; and the sludge polypyrrole delignified wood blocks are evenly placed on the sludge in an array, ensuring that 15% of the height of the wood blocks is immersed in the sludge and 85% of the height is exposed to the sludge, and the sludge is placed under sunlight. A moisture sensor is set at the interface between the polypyrrole delignified wood block and the sludge. The sensor can detect and record the change in moisture. The moisture sensor measures the voltage change generated by the hydroelectric effect caused by evaporation through two copper electrodes installed on the upper surface of the polypyrrole delignified wood block and the sludge, and determines the moisture content in the sludge by real-time monitoring of the voltage. When the monitored voltage is lower than the set threshold value of 0.035V and remains stable, the wood block is removed to end the drying, and the final sludge moisture content is 34%.

[0066] (7) After the sludge is dried, the polypyrrole delignified light wood block is taken out, and the heavy metal removal rate of the sludge is 78%. The wood block is subjected to heavy metal removal operation, and the heavy metals mainly include harmful metals such as copper, lead, zinc, and cadmium. The wood block is soaked in 0.1mol / L nitric acid solution, and ultrasonic cleaning is used as an auxiliary. The ultrasonic cleaning time is set to 20 minutes, the ultrasonic frequency is set to 28kHZ, and the ultrasonic power is set to 750W. After the cleaning is completed, rinse with clean water to remove residual nitric acid solution and heavy metals. When the pH of the rinse solution is detected to be between 6.5, the rinsing is stopped, and the rinsed wood block is dried to finally obtain a reusable polypyrrole delignified light wood block.

[0067] Specific embodiment example 3

[0068] (1) To every 100 mL of clean water, 6 g of sodium hypochlorite and 2 mL of glacial acetic acid were added in sequence and mixed evenly to prepare a delignified solution.

[0069] (2) Cut balsa wood into long cylinders. The balsa wood is pine wood. The size of the long cylinder is set to 20 cm in height and 5 cm in bottom diameter. The long cylinder is completely immersed in the delignification solution and heated at 100°C for 16 hours. After the heating is completed, the balsa wood block is rinsed with clean water and the pH of the rinse liquid is tested until the pH of the rinse liquid reaches neutral, thereby obtaining a treated balsa wood block.

[0070] (3) The treated balsa wood blocks were placed in a freeze dryer for drying, the drying temperature was set to -40°C, the drying time was 24 hours, the vacuum degree was less than 10 Pa, and after the drying time was over, the temperature was slowly raised to room temperature at a rate of 0.6°C / min to obtain delignified balsa wood blocks.

[0071] (4) Add 3 g of ammonium persulfate to every 100 mL of clean water and mix well to obtain an ammonium persulfate solution; add 1 mL of pyrrole to every 100 mL of water and mix well to obtain a pyrrole dispersion; prepare for the subsequent polypyrrole layer.

[0072] (5) The ammonium persulfate solution and the pyrrole dispersion were sequentially dripped onto the upper surface of the delignified balsa wood block, and the dripping amount was controlled so that the thickness of the polypyrrole layer was 100 μm. After reacting for 20 minutes, the liquid residue on the surface was rinsed with clean water, and then the wood block was placed in a freeze dryer for drying, and the drying temperature was set to minus 40 degrees Celsius, the drying time was 24 hours, and the vacuum degree was less than 10 Pa. After the drying time was over, the temperature was slowly raised to room temperature at a rate of 0.6°C / min to obtain a delignified balsa wood block with a polypyrrole layer on the upper surface.

[0073] (6) Prepare several polypyrrole delignified wood blocks according to the above steps (1-5), and place them in the sludge. The selected sludge has a moisture content of 98%, and the volume of the polypyrrole delignified wood blocks accounts for 10% of the sludge volume; and the sludge polypyrrole delignified wood blocks are evenly placed on the sludge in an array, ensuring that 20% of the height of the wood blocks is immersed in the sludge and 80% of the height is exposed outside the sludge, and the sludge is placed under sunlight. A moisture sensor is set at the interface between the polypyrrole delignified wood block and the sludge. The sensor can detect and record the change in moisture. The moisture sensor measures the voltage change generated by the hydroelectric effect caused by evaporation through two copper electrodes installed on the upper surface of the polypyrrole delignified wood block and the sludge, and determines the moisture content in the sludge by real-time monitoring of the voltage. When the monitored voltage is lower than the set threshold of 0.05V and remains stable, the wood block is removed to end the drying, and the final sludge moisture content is 30%.

[0074] (7) After the sludge is dried, take out the polypyrrole delignified light wood block, and the heavy metal removal rate of the sludge is 80%. The wood block is subjected to heavy metal removal operation, and the heavy metals mainly include harmful metals such as copper, lead, zinc, and cadmium. The wood block is soaked in a 0.1mol / L hydrochloric acid solution, and ultrasonic cleaning is used as an auxiliary. The ultrasonic cleaning time is set to 30 minutes, the ultrasonic frequency is set to 28kHZ, and the ultrasonic power is set to 1000W. After the cleaning is completed, rinse with clean water to remove residual hydrochloric acid solution and heavy metals. When the pH of the rinse liquid is detected to be between 7, the rinsing is stopped, and the rinsed wood block is dried to finally obtain a reusable polypyrrole delignified light wood block.

[0075] Comparative Example 1

[0076] The steps of Example 1 are referred to, except that the delignification heating and impregnation treatment is not performed; that is, the interior of the balsa wood block used for sludge drying still retains the original lignin component, and its upper surface is also provided with a polypyrrole layer.

[0077] After the same drying steps and treatment time, the final sludge moisture content is 72%, and the heavy metal removal rate of the sludge is 20%.

[0078] Comparative Example 2

[0079] The steps of Example 1 were followed, except that the operation of dropping the ammonium persulfate solution and the pyrrole dispersion was not performed; that is, the upper surface of the balsa wood block used for sludge drying was not provided with a polypyrrole layer.

[0080] After the same drying steps and treatment time, the final sludge moisture content is 89%, and the heavy metal removal rate of the sludge is 15%.

[0081] Comparative Example 3

[0082] Refer to the steps of Example 1, except that the balsa wood block is replaced by the absorbent cotton strip used in the conventional technology; that is, a common absorbent material is used, and its upper surface is also provided with a polypyrrole layer.

[0083] After the same drying steps and treatment time, the final sludge moisture content is 75%, and the heavy metal removal rate of the sludge is 25%.

[0084] Comparative Example 4

[0085] The water-absorbing material is prepared with reference to the contents described in "A Salt Lake Brine Concentration Device" (CN202222429630.3); that is, other water-absorbing materials are used to replace the balsa wood blocks of the present invention and placed in the water-containing sludge.

[0086] After the same drying steps and treatment time, the final sludge moisture content was 45%, and the heavy metal removal rate of the sludge was 32%.

[0087] Comparative Example 5

[0088] Commercially available water-absorbing sponges were purchased as the water-absorbing material; that is, ordinary commercial water-absorbing materials were used instead of the balsa wood blocks of the present invention and placed in the aqueous sludge.

[0089] After the same drying steps and treatment time, the final sludge moisture content is 50%, and the heavy metal removal rate of the sludge is 30%.

[0090] Comparative Example 6

[0091] A hydrophilic modified commercial hydrophobic polyurethane sponge was prepared as a water-absorbing material with reference to the contents recorded in the journal article "Preparation and Performance of Modified PU Sponge Three-Dimensional Porous Interface Evaporator"; that is, a specific modified water-absorbing material was used to replace the balsa wood block of the present invention and placed in the aqueous sludge.

[0092] After the same drying steps and treatment time, the final sludge moisture content was 42%, and the heavy metal removal rate of the sludge was 35%.

[0093] Data Analysis and Conclusions:

[0094] From the above specific embodiments of the present invention, as well as the changes in the parameters and elements in the comparative examples, the final moisture content and heavy metal removal rate data changes after the replacement can be concluded as follows:

[0095] Compared with traditional water-absorbing materials or unmodified balsa wood blocks, the specific embodiments of the present invention have significant advantages in reducing the moisture content of sludge and improving the heavy metal removal rate. This is mainly due to the following points: (1) Material preparation and modification: The modified balsa wood block (Py-H-wood) is treated with a polypyrrole coating, which not only improves the photothermal conversion efficiency, but also increases the adsorption sites on the surface, effectively adsorbing heavy metals. (2) Improved utilization of the photothermal effect: The addition of the polypyrrole layer enables the wood block to more effectively convert light energy into heat energy under sunlight, accelerates the evaporation process of water, and thus reduces the moisture content of the sludge. (3) Improved heavy metal adsorption effect: Compared with traditional water-absorbing materials, Py-H-wood shows better performance in removing heavy metals, which is attributed to the special treatment of its surface, which increases its adsorption capacity for heavy metals.

[0096] In addition, for the specific drying object of sludge, the modified balsa wood block photothermal interface evaporation material prepared by the present invention shows better adaptability and matching, thus showing higher drying efficiency and heavy metal removal efficiency. The drying principle for sludge characteristics is as follows:

[0097] (1) By removing lignin, the pore structure inside the balsa wood block is significantly improved, while retaining the original water migration path inside the wood, the porosity is increased, so that the ability of water to migrate and diffuse inside the wood is further enhanced. Sludge contains a large number of macromolecular impurities (organic matter, pathogens, etc.). This structural optimization not only improves the water absorption and water transfer rate of the balsa wood block, but also ensures the rapid rise and evaporation of water, reducing the possibility of blockage in the internal channels. In comparison, although traditional water-absorbing materials (such as polyurethane sponges) or other synthetic materials also have a high porosity, the pore structure inside these materials is usually a disordered and interlaced three-dimensional structure, which is relatively closed and cannot form a smooth migration channel. In long-term use in high-impurity application scenarios, blockage is likely to occur and performance degradation.

[0098] (2) As the water evaporates, the fluidity of the sludge deteriorates and the viscosity increases. The present invention uses delignified balsa wood blocks as water-absorbing materials, which have high mechanical properties. Good structural stability can be maintained in both low-moisture and high-moisture sludge, while other water-absorbing materials (such as hydrophilic sponges) easily change their structure with changes in moisture, thereby affecting water transmission performance and further affecting drying efficiency.

[0099] (3) The modified balsa wood blocks provide a large number of specific heavy metal active adsorption sites, which can capture more heavy metals, thereby improving the removal efficiency of heavy metals. However, traditional absorbent materials are weak in the removal of heavy metals and mainly rely on physical adsorption, which is less efficient.

[0100] (4) Based on the above principles, the photothermal interface evaporation material of the present invention has good recycling performance and uses natural light wood blocks as raw materials. Compared with traditional organic materials, it reduces the disposal cost and the impact on the environment while treating sludge, which meets the requirements of sustainable development.

[0101] In summary, the modified balsa wood block of the present invention not only fully adapts to the unique properties of sludge, but also improves the efficiency and environmental safety of sludge treatment through the optimization of structure and function. Specifically, the sludge drying method of solar-driven interfacial evaporation provided by the present invention selects low-cost, low-density, high-porosity balsa wood as raw material, removes lignin therein to increase porosity, and improves the photothermal conversion efficiency and water evaporation rate with a polypyrrole coating, so that the system can quickly and efficiently reduce the water content in the sludge. At the same time, the heavy metals in the sludge are efficiently removed by enhanced adsorption, reducing the potential risk of environmental pollution. In addition, the integrated moisture sensor realizes real-time monitoring and adjustment of the drying process. Therefore, the method has the effect of efficient evaporation and efficient removal of heavy metals, and the method is simple to operate, low maintenance cost, non-toxic and harmless materials, stable physical and chemical properties, and recyclable. It is a sludge drying and disposal technology with great commercial application prospects, high efficiency, low cost, low energy consumption, low carbon, and environmental protection.

[0102] Obviously, those skilled in the art may make various subsequent applications, supplements, modifications and variations to the present invention without departing from the spirit and scope of the present invention. If various applications, supplements, modifications and variations based on the present invention fall within the scope of the claims of the present invention and their equivalents, the present invention is also intended to include such applications, supplements, modifications and variations.

Claims

1. A sludge drying method using solar-driven interfacial evaporation, characterized in that: The following steps are involved: (1) dissolving sodium hypochlorite and glacial acetic acid in water and mixing them evenly to prepare a delignification solution; (2) cutting balsa wood into long cylinders, completely immersing them in a delignified solution, and heating them at 100° C. for 12 to 16 hours; taking them out, rinsing them with water until the pH value of the rinsing solution is neutral, and performing vacuum freeze drying to obtain delignified balsa wood blocks; (3) dripping an ammonium persulfate solution and a pyrrole dispersion onto the upper surface of the delignified balsa wood block in sequence, so that the ammonium persulfate as an oxidant reacts with the pyrrole for an oxidative polymerization reaction; after reacting for 10 to 20 minutes, washing the residual liquid on the surface with water; and then performing a vacuum freeze-drying treatment to obtain a delignified balsa wood block having a polypyrrole layer on the upper surface; (4) taking a number of delignified balsa wood blocks with polypyrrole layers, inserting them vertically into the water-containing sludge, ensuring that 80% to 90% of their height is exposed outside the sludge; respectively setting moisture sensors on the polypyrrole layer of the balsa wood block and on the interface with the sludge, and each sensor is connected to a detection recorder through a signal line; The sunlight is irradiated on the surface of the sludge and the balsa wood block, and a photothermal interface evaporation effect is formed on the polypyrrole layer. Based on the hydroelectric effect caused by evaporation, the difference in the voltage value of the moisture sensor monitoring is formed at different positions, and the voltage difference is used to monitor the change of moisture content at different positions. When the moisture content monitoring data meets the expected value, the balsa wood block is taken out, and the sludge has been dried at this time. (5) The balsa wood block is immersed in an acid solution and subjected to a heavy metal removal operation under ultrasonic conditions; after being taken out, the residual acid and heavy metals are removed by rinsing with clean water until the pH value of the rinsing solution is between 6 and 7; the balsa wood block is then dried to obtain a reusable balsa wood block.

2. The method according to claim 1, characterized in that In the step (1), when preparing the delignification solution, 4 to 6 g of sodium hypochlorite and 1 to 2 mL of glacial acetic acid are added to every 100 mL of water.

3. The method according to claim 1, characterized in that: In the step (2), the material of the balsa wood block is fir, paulownia or pine; the long column is a cylinder or a square column, with a height of 10 to 20 cm and a radial dimension or lateral width of 2 to 5 cm.

4. The method according to claim 1, characterized in that: In step (2) or step (3), the freeze drying treatment is carried out in a freeze dryer, the drying temperature is set to -40°C, the drying time is set to 12 to 24 hours, and the vacuum degree is lower than 10Pa; after the drying is completed, the temperature is slowly raised to room temperature at a rate of 0.4 to 0.6°C / min to avoid damage to the internal structure of the wood.

5. The method according to claim 1, characterized in that In the step (3), 2-3 g of ammonium persulfate is added to 100 mL of water, and the mixture is mixed to obtain an ammonium persulfate solution; 0.5-1 mL of pyrrole is added to 100 mL of water, and the mixture is mixed to obtain a pyrrole dispersion; and the ammonium persulfate solution and the pyrrole dispersion are added dropwise in equal volumes, and the amount of the added drops is controlled so that the thickness of the polypyrrole layer is 50-100 μm.

6. As a preferred embodiment of the present invention, in step (4), the moisture content of the sludge is between 90% and 98%, the total volume of the balsa wood blocks used accounts for 5% to 10% of the total volume of the sludge, and the balsa wood blocks are evenly arranged in the sludge in an array.

7. According to the method of claim 1, in the step (4), the moisture sensor has a copper electrode; when it is monitored that the voltage difference between the two electrodes is continuously and stably lower than 0.02-0.05V, the drying process is terminated, and the moisture content of the sludge is between 30% and 40%.

8. The method according to claim 1, wherein in step (5), the cleaning time under ultrasonic conditions is 10 to 30 minutes; the ultrasonic frequency is set to 28 kHz, and the ultrasonic power is set to 500 to 1000 W.

9. The method according to claim 1, wherein in step (5), the acidic solution is 0.1 mol / L hydrochloric acid or 0.1 mol / L nitric acid solution; and the heavy metals removed by ultrasound include at least copper, lead, zinc, and cadmium.

Citation Information

Patent Citations

  • Preparation method of material with solar water evaporation and efficient metal ion adsorption functions

    CN111675275A

  • Method for in-situ preparation of three-dimensional multifunctional adsorption material from corn pith and application of three-dimensional multifunctional adsorption material

    CN113198428A

  • Preparation method of isotropic conductive paper

    CN114030046A

  • Preparation method of graded porous wood aerogel-based electrode material

    CN114864296A

  • Preparation method of photo-thermal coating composite material for solar interface evaporation

    CN115975499A