Preparation method of chalcogenide glass substrate 1064nm and 7.7-10.5 [mu] m antireflection film system
By evaporating Y2O3, YbF3 and ZnSe film layers layer by layer on the chalcogenide glass substrate, the problem of insufficient transmittance of the dual-band anti-reflection coating system on the chalcogenide glass substrate in the existing technology is solved, and efficient optical performance improvement is achieved. Achieving transmittances of 98.2% and 98.8%.
Patent Information
- Application Number
- CN202410921388.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-10
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2044-07-10
AI Technical Summary
The transmittance of the dual-band antireflection coating system coated on the existing chalcogenide glass substrate in the 1064nm and 7.7-10.5μm bands has not yet reached the optimal effect and needs to be further improved.
A preparation method is adopted to evaporate Y2O3, YbF3 and ZnSe film layers layer by layer on a chalcogenide glass substrate. The specific steps include cleaning treatment, evaporation process in a vacuum coating machine, and controlling the thickness and deposition rate of each layer of film. Repeat plating on both sides to improve transmittance.
The transmittance of 98.2% in the 1064nm band and 98.8% in the 7.7-10.5 μm band is achieved, which exceeds the dual-band transmittance in the background technology and significantly improves the optical performance of the chalcogenide glass substrate.
Smart Images

Figure CN118754457A_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to the infrared field, and more specifically to a method for preparing a 1064nm and 7.7-10.5μm antireflection film system on a chalcogenide glass substrate. Background Art
[0002] In the field of infrared optical coatings, chalcogenide glass has unique advantages as an infrared lens material. The transmittance characteristics of chalcogenide glass make it an ideal choice for infrared lens materials, especially in applications that require high transmittance.
[0003] Chinese patent document CN117567044A discloses a dual-band (i.e., near-infrared and far-infrared) antireflection film system coated on a chalcogenide glass substrate, wherein the transmittance in the 1064nm band is 97.42%, and the transmittance in the 8-12μm band is 95.58%. However, there is still a need to further improve the transmittance of the dual-band antireflection film system coated on the chalcogenide glass substrate. Summary of the invention
[0004] In view of the problems existing in the background technology, an object of the present disclosure is to provide a method for preparing a 1064nm and 7.7-10.5μm antireflection film system on a chalcogenide glass substrate, which can improve the transmittance in the dual bands of 1064nm and 7.7-10.5μm.
[0005] Thus, a method for preparing a 1064 nm and 7.7-10.5 μm antireflection film system on a chalcogenide glass substrate comprises the following steps:
[0006] S1, cleaning the surface of the accompanying plating sheet and the product of the chalcogenide glass substrate as the lens, the chalcogenide glass substrate is an IG06 substrate, and the thickness of the accompanying plating sheet is 0.9-1.5 mm;
[0007] S2, put the cleaned lens into the fixture, and hang the fixture with the lens into the cavity of the vacuum coating machine, and set the temperature of the cavity to 120-130℃;
[0008] S3, vacuum coating machine starts to evacuate, and the vacuum degree reaches 1.5×10 -3 Pa, turn on the auxiliary coating ion source of the vacuum coating machine for cleaning, the cleaning time is 6 minutes, the anode voltage of the ion source is 220V, the anode current is 1.0-2.5A, and the emitter current is 1.3-1.5A;
[0009] S4, maintaining the aforementioned vacuum degree, evaporating a first Y2O3 film layer on the first surface of the lens, the deposition rate of the first Y2O3 film layer is 0.3nm / s, the film thickness of the first Y2O3 film layer is controlled to be 15nm±1nm, and ion source assisted evaporation is not used;
[0010] S5, evaporating a first YbF3 film layer on the plated first Y2O3 film layer, the deposition rate of the first YbF3 film layer is 0.6nm / s, the film thickness of the first YbF3 film layer is controlled to be 66.2nm±3nm, and ion source assisted evaporation is not used;
[0011] S6, evaporating a first ZnSe film layer on the plated first YbF3 film layer, the deposition rate of the first ZnSe film layer is 0.8nm / s, the film thickness of the first ZnSe film layer is controlled to be 48.3nm±2nm, and ion source assisted evaporation is not used;
[0012] S7, evaporating a second YbF3 film layer on the plated first ZnSe film layer, the deposition rate of the second YbF3 film layer is 0.6nm / s, the film thickness of the second YbF3 film layer is controlled to be 80.2nm±3nm, and ion source assisted evaporation is not used;
[0013] S8, evaporating a second ZnSe film layer on the plated second YbF3 film layer, the deposition rate of the second ZnSe film layer is 0.8 nm / s, the film thickness of the second ZnSe film layer is controlled to be 608.3 nm±5 nm, and ion source assisted evaporation is not used;
[0014] S9, evaporating a third YbF3 film layer on the plated second ZnSe film layer, the deposition rate of the third YbF3 film layer is 0.6 nm / s, the film thickness of the third YbF3 film layer is controlled to be 800 nm±5 nm, and ion source assisted evaporation is not used;
[0015] S10, evaporating a second Y2O3 film layer on the plated third YbF3 film layer, the deposition rate of the second Y2O3 film layer is 0.3nm / s, the film thickness of the second Y2O3 film layer is controlled to be 15nm±1nm, and ion source assisted evaporation is not used;
[0016] S11, evaporating a fourth YbF3 film layer on the plated second Y2O3 film layer, the deposition rate of the fourth YbF3 film layer is 0.6nm / s, the film thickness of the fourth YbF3 film layer is controlled to be 421.5nm±5nm, and ion source assisted evaporation is not used;
[0017] S12, evaporating a third ZnSe film layer on the plated fourth YbF3 film layer, the deposition rate of the third ZnSe film layer is 0.8 nm / s, the film thickness of the third ZnSe film layer is controlled to be 32 nm±2 nm, and ion source assisted evaporation is not used;
[0018] S13, vapor-depositing a fifth YbF3 film layer on the plated third ZnSe film layer, the deposition rate of the fifth YbF3 film layer is 0.6 nm / s, the film thickness of the fifth YbF3 film layer is controlled to be 156.8 nm±5 nm, and ion source assisted vapor deposition is not used;
[0019] S14, vapor-depositing a fourth ZnSe film layer on the plated fifth YbF3 film layer, the deposition rate of the fourth ZnSe film layer is 0.8 nm / s, the film thickness of the fourth ZnSe film layer is controlled to be 26 nm±1 nm, and ion source assisted vapor deposition is not used;
[0020] S15, after the fourth ZnSe film layer is deposited, the vacuum chamber is cooled to below 60°C and the fixture, the accompanying deposition sheet and the product are taken out;
[0021] S16, repeat steps S1 to S15, and sequentially evaporate the first Y2O3 film layer, the first YbF3 film layer, the first ZnSe film layer, the second YbF3 film layer, the second ZnSe film layer, the third YbF3 film layer, the second Y2O3 film layer, the fourth YbF3 film layer, the third ZnSe film layer, the fifth YbF3 film layer, and the fourth ZnSe film layer on the second opposite side of the lens.
[0022] The beneficial effects of the present disclosure are as follows: In the method for preparing the 1064 nm and 7.7-10.5 μm antireflection film system of the chalcogenide glass substrate according to the present disclosure, a first Y2O3 film layer with a film thickness of 15 nm±1 nm, a first YbF3 film layer with a film thickness of 66.2 nm±3 nm, a first ZnSe film layer with a film thickness of 48.3 nm±2 nm, a second YbF3 film layer with a film thickness of 80.2 nm±3 nm, a second ZnSe film layer with a film thickness of 608.3 nm±5 nm, a third YbF3 film layer with a film thickness of 800 nm±5 nm, a second YbF3 film layer with a film thickness of 15 nm±1 nm are plated on both sides of the accompanying plate and the product of the chalcogenide glass substrate as the lens. The Y2O3 film layer, the fourth YbF3 film layer with a thickness of 421.5nm±5nm, the third ZnSe film layer with a thickness of 32nm±2nm, the fifth YbF3 film layer with a thickness of 156.8nm±5nm, and the fourth ZnSe film layer with a thickness of 26nm±1nm, based on the tests of 1064nm band (near infrared band) and 7.7-10.5μm (far infrared band) of the accompanying coating film, have a transmittance of 98.2% in the 1064nm band and an average transmittance of 98.8% in the 7.7-10.5μm band, that is, the transmittances in both bands exceed 98%, which exceed the transmittances in both bands of the patent literature mentioned in the background technology. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 It is a structural schematic diagram of coating 1064nm and 7.7-10.5um antireflection film systems on both sides of a co-plating sheet and a product including a chalcogenide glass substrate according to the preparation method of the 1064nm and 7.7-10.5um antireflection film system on a chalcogenide glass substrate disclosed in the present invention.
[0024] Figure 2It is a curve diagram of the transmittance of the accompanying coating sheet of Example 1 coated with 1064nm and 7.7-10.5μm antireflection films on both sides in the 1064nm band.
[0025] Figure 3 It is a curve diagram of the transmittance of the accompanying coating sheet of Example 1 coated with 1064nm and 7.7-10.5μm antireflection films on both sides in the 7.7-10.5μm band. DETAILED DESCRIPTION
[0026] It will be understood that the disclosed embodiments are merely examples of the present disclosure, which may be implemented in various forms, and therefore, the specific details disclosed herein should not be interpreted as limiting, but merely as a basis for the claims and as a representative basis for teaching one of ordinary skill in the art to implement the present disclosure in various ways.
[0027] [Method for preparing 1064nm and 7.7-10.5μm antireflection film system on chalcogenide glass substrate]
[0028] The method for preparing the 1064 nm and 7.7-10.5 μm antireflection film system of the chalcogenide glass substrate disclosed in the present invention comprises the following steps:
[0029] S1, cleaning the surface of the accompanying plating sheet and the product of the chalcogenide glass substrate as the lens, the chalcogenide glass substrate is an IG06 substrate, and the thickness of the accompanying plating sheet is 0.9-1.5 mm;
[0030] S2, put the cleaned lens into the fixture, and hang the fixture with the lens into the cavity of the vacuum coating machine, and set the temperature of the cavity to 120-130℃;
[0031] S3, vacuum coating machine starts to evacuate, and the vacuum degree reaches 1.5×10 -3 Pa, turn on the auxiliary coating ion source of the vacuum coating machine for cleaning, the cleaning time is 6 minutes, the anode voltage of the ion source is 220V, the anode current is 1.0-2.5A, and the emitter current is 1.3-1.5A;
[0032] S4, maintaining the aforementioned vacuum degree, evaporating a first Y2O3 film layer on the first surface of the lens, the deposition rate of the first Y2O3 film layer is 0.3nm / s, the film thickness of the first Y2O3 film layer is controlled to be 15nm±1nm, and ion source assisted evaporation is not used;
[0033] S5, evaporating a first YbF3 film layer on the plated first Y2O3 film layer, the deposition rate of the first YbF3 film layer is 0.6nm / s, the film thickness of the first YbF3 film layer is controlled to be 66.2nm±3nm, and ion source assisted evaporation is not used;
[0034] S6, evaporating a first ZnSe film layer on the plated first YbF3 film layer, the deposition rate of the first ZnSe film layer is 0.8nm / s, the film thickness of the first ZnSe film layer is controlled to be 48.3nm±2nm, and ion source assisted evaporation is not used;
[0035] S7, evaporating a second YbF3 film layer on the plated first ZnSe film layer, the deposition rate of the second YbF3 film layer is 0.6nm / s, the film thickness of the second YbF3 film layer is controlled to be 80.2nm±3nm, and ion source assisted evaporation is not used;
[0036] S8, evaporating a second ZnSe film layer on the plated second YbF3 film layer, the deposition rate of the second ZnSe film layer is 0.8 nm / s, the film thickness of the second ZnSe film layer is controlled to be 608.3 nm±5 nm, and ion source assisted evaporation is not used;
[0037] S9, evaporating a third YbF3 film layer on the plated second ZnSe film layer, the deposition rate of the third YbF3 film layer is 0.6 nm / s, the film thickness of the third YbF3 film layer is controlled to be 800 nm±5 nm, and ion source assisted evaporation is not used;
[0038] S10, evaporating a second Y2O3 film layer on the plated third YbF3 film layer, the deposition rate of the second Y2O3 film layer is 0.3nm / s, the film thickness of the second Y2O3 film layer is controlled to be 15nm±1nm, and ion source assisted evaporation is not used;
[0039] S11, evaporating a fourth YbF3 film layer on the plated second Y2O3 film layer, the deposition rate of the fourth YbF3 film layer is 0.6nm / s, the film thickness of the fourth YbF3 film layer is controlled to be 421.5nm±5nm, and ion source assisted evaporation is not used;
[0040] S12, evaporating a third ZnSe film layer on the plated fourth YbF3 film layer, the deposition rate of the third ZnSe film layer is 0.8 nm / s, the film thickness of the third ZnSe film layer is controlled to be 32 nm±2 nm, and ion source assisted evaporation is not used;
[0041] S13, vapor-depositing a fifth YbF3 film layer on the plated third ZnSe film layer, the deposition rate of the fifth YbF3 film layer is 0.6 nm / s, the film thickness of the fifth YbF3 film layer is controlled to be 156.8 nm±5 nm, and ion source assisted vapor deposition is not used;
[0042] S14, vapor-depositing a fourth ZnSe film layer on the plated fifth YbF3 film layer, the deposition rate of the fourth ZnSe film layer is 0.8 nm / s, the film thickness of the fourth ZnSe film layer is controlled to be 26 nm±1 nm, and ion source assisted vapor deposition is not used;
[0043] S15, after the fourth ZnSe film layer is deposited, the vacuum chamber is cooled to below 60°C and the fixture, the accompanying deposition sheet and the product are taken out;
[0044] S16, repeat steps S1 to S15, and sequentially evaporate the first Y2O3 film layer, the first YbF3 film layer, the first ZnSe film layer, the second YbF3 film layer, the second ZnSe film layer, the third YbF3 film layer, the second Y2O3 film layer, the fourth YbF3 film layer, the third ZnSe film layer, the fifth YbF3 film layer, and the fourth ZnSe film layer on the second opposite side of the lens.
[0045] In the preparation method of the 1064nm and 7.7-10.5μm antireflection film system of the chalcogenide glass substrate according to the present disclosure, a first Y2O3 film layer with a film thickness of 15nm±1nm, a first YbF3 film layer with a film thickness of 66.2nm±3nm, a first ZnSe film layer with a film thickness of 48.3nm±2nm, a second YbF3 film layer with a film thickness of 80.2nm±3nm, a second ZnSe film layer with a film thickness of 608.3nm±5nm, a third YbF3 film layer with a film thickness of 800nm±5nm, and a second Y2O3 film layer with a film thickness of 15nm±1nm are plated on both sides of the accompanying plate and the product of the chalcogenide glass substrate as the lens. The fourth YbF3 film layer with a thickness of 421.5nm±5nm, the third ZnSe film layer with a thickness of 32nm±2nm, the fifth YbF3 film layer with a thickness of 156.8nm±5nm, and the fourth ZnSe film layer with a thickness of 26nm±1nm, based on the tests of 1064nm band (near infrared band) and 7.7-10.5μm (far infrared band) of the accompanying plating film, the transmittance in the 1064nm band is 98.2%, and the average transmittance in the 7.7-10.5μm band is 98.8%, that is, the transmittance in both bands exceeds 98%, which exceeds the transmittance in both bands of the patent literature mentioned in the background technology.
[0046] In the 1064nm and 7.7-10.5μm anti-reflection film systems coated on the chalcogenide glass substrate of the present invention, the total thickness of the eleven film layers (constituting the anti-reflection film system on each surface) coated on each of the first and second opposite surfaces of the co-plating sheet and the product of the chalcogenide glass substrate serving as a lens is 2269.3nm±33nm.
[0047] The eleven film layers coated on each surface are composed of two Y2O3 film layers, five YbF3 film layers and four ZnSe film layers. Among them, the film thickness of the two Y2O3 film layers is consistent, the film thickness of the five YbF3 film layers is larger in the middle and smaller at both ends in the anti-reflection film system, and the film thickness of the four ZnSe film layers is larger in the middle and smaller at both ends in the anti-reflection film system. This thickness distribution is conducive to the buffering release of film layer stress and is conducive to the overall reduction of the thickness of the film layers on each surface of the chalcogenide glass substrate. In the anti-reflection film system on each surface, the first Y2O3 film layer is located on the chalcogenide glass substrate, the YbF3 film layer / ZnSe film layer is composed of two pairs of adjacent first Y2O3 film layers, and the YbF3 film layer / ZnSe film layer is composed of another two pairs located on the outermost surface of the anti-reflection film system, and the third YbF3 film layer and the second Y2O3 film layer are between the two pairs of YbF3 film layers / ZnSe film layers and the other two pairs of YbF3 film layers / ZnSe film layers.
[0048] The surface cleaning in step S1 is beneficial to improving the surface conditions of the first and second surfaces of the accompanying plating sheet and the product, and helps to improve the bonding performance of the anti-reflection film system on each surface with the corresponding surfaces of the accompanying plating sheet and the product.
[0049] The temperature of the chamber in step S2 helps to eliminate the stress on each surface of the accompanying plating sheet and the product (ie, each of the first surface and the second surface) and the first Y2O3 film layer, and also helps the growth of the film layer on each surface of the accompanying plating sheet and the product.
[0050] In step S3, an ion source is used for cleaning. The bombardment and sputtering of argon ions ionized by a working gas such as argon gas will cause the impurities, oil molecules, and oxides adsorbed on the surface of each surface of the accompanying coating sheet and the product to be separated from the substrate surface, thereby greatly improving the interface state, which is helpful to improve the bonding performance between the first Y2O3 film layer and the chalcogenide glass substrate. At the same time, through the bombardment of argon ions on each surface of the chalcogenide glass substrate, the various surfaces of the chalcogenide glass substrate can be heated, which is helpful for the growth of the first Y2O3 film layer and reduces the growth stress of the first Y2O3 film layer.
[0051] In one example, in step S1 , the thickness of the accompanying plating sheet is 1.0 mm.
[0052] In one example, in step S1, the surface of the lens is cleaned by ultrasonic wave or hand wiping.
[0053] In one example, in step S2, the temperature of the chamber is set to 130°C.
[0054] In one example, in step S3, the anode current is 1.2A and the emitter current is 1.5A.
[0055] In one example, in step S3, the ion source is a Hall ion source, and argon gas is used as the working gas.
[0056] In one example, in step S4, the thickness of the first Y2O3 film layer is controlled to be 15 nm; in step S5, the thickness of the first YbF3 film layer is controlled to be 66.2 nm; in step S6, the thickness of the first ZnSe film layer is controlled to be 48.3 nm; in step S7, the thickness of the second YbF3 film layer is controlled to be 80.2 nm; in step S8, the thickness of the second ZnSe film layer is controlled to be 608.3 nm; in step S9, the thickness of the third YbF3 film layer is controlled to be 800 nm; in step S10, the thickness of the second Y2O3 film layer is controlled to be 15 nm; in step S11, the thickness of the fourth YbF3 film layer is controlled to be 421.5 nm; in step S12, the thickness of the third ZnSe film layer is controlled to be 32 nm; in step S13, the thickness of the fifth YbF3 film layer is controlled to be 156.8 nm; in step S14, the thickness of the fourth ZnSe film layer is controlled to be 26 nm.
[0057] In one example, in steps S5 to S9 and steps S11 to S14, the evaporation is carried out by resistance heating evaporation, that is, the YbF3 film layer and the ZnSe film layer are evaporated by resistance heating; in steps S4 and 10, the evaporation is carried out by electron beam evaporation, that is, the Y2O3 film layer is evaporated by electron beam.
[0058] [test]
[0059] Example 1
[0060] Example 1 adopts the following steps:
[0061] S1, using ultrasonic cleaning to clean the surface of the accompanying plating sheet and the product of the chalcogenide glass substrate as the lens, the chalcogenide glass substrate is an IG06 substrate, and the thickness of the accompanying plating sheet is 1.0 mm;
[0062] S2, placing the cleaned lens into a fixture, and hanging the fixture with the lens into the cavity of a vacuum coating machine, the temperature of the cavity is set to 130°C, the vacuum coating machine is a vacuum coating machine with a Hall ion source equipped with a neutralizer manufactured and sold by Chengdu Siwork Vacuum Technology Co., Ltd., the Hall ion source equipped with a neutralizer is purchased from Boton Optoelectronics Technology Co., Ltd., and argon is used as the working gas;
[0063] S3, vacuum coating machine starts to evacuate, and the vacuum degree reaches 1.5×10 -3 Pa, turn on the auxiliary coating ion source of the vacuum coating machine for cleaning, the cleaning time is 6 minutes, the anode voltage of the ion source is 220V, the anode current is 1.2A, and the emitter current is 1.5A;
[0064] S4, maintaining the aforementioned vacuum degree, evaporating a first Y2O3 film layer on the first surface of the lens, the deposition rate of the first Y2O3 film layer is 0.3nm / s, the film thickness of the first Y2O3 film layer is controlled to be 15nm, and ion source assisted evaporation is not used, and electron beam evaporation is used for evaporation;
[0065] S5, vapor-depositing a first YbF3 film layer on the plated first Y2O3 film layer, the deposition rate of the first YbF3 film layer is 0.6 nm / s, the film thickness of the first YbF3 film layer is controlled to be 66.2 nm, and the evaporation is performed by resistance heating evaporation without using ion source assisted evaporation;
[0066] S6, evaporating a first ZnSe film layer on the plated first YbF3 film layer, the deposition rate of the first ZnSe film layer is 0.8nm / s, the film thickness of the first ZnSe film layer is controlled to be 48.3nm, and the evaporation is carried out by resistance heating evaporation without using ion source assisted evaporation;
[0067] S7, vapor-depositing a second YbF3 film layer on the plated first ZnSe film layer, the deposition rate of the second YbF3 film layer is 0.6 nm / s, the film thickness of the second YbF3 film layer is controlled to be 80.2 nm, and the evaporation is carried out by resistance heating evaporation without using ion source assisted evaporation;
[0068] S8, evaporating a second ZnSe film layer on the plated second YbF3 film layer, the deposition rate of the second ZnSe film layer is 0.8 nm / s, the film thickness of the second ZnSe film layer is controlled to be 608.3 nm, and the evaporation is carried out by resistance heating evaporation without using ion source assisted evaporation;
[0069] S9, vapor-depositing a third YbF3 film layer on the plated second ZnSe film layer, the deposition rate of the third YbF3 film layer is 0.6 nm / s, the film thickness of the third YbF3 film layer is controlled to be 800 nm, and the evaporation is performed by resistance heating evaporation without using ion source assisted evaporation;
[0070] S10, evaporating a second Y2O3 film layer on the plated third YbF3 film layer, the deposition rate of the second Y2O3 film layer is 0.3nm / s, the film thickness of the second Y2O3 film layer is controlled to be 15nm, and ion source assisted evaporation is not used, and electron beam evaporation is used for evaporation;
[0071] S11, vapor-depositing a fourth YbF3 film layer on the plated second Y2O3 film layer, the deposition rate of the fourth YbF3 film layer is 0.6 nm / s, the film thickness of the fourth YbF3 film layer is controlled to be 421.5 nm, and the evaporation is performed by resistance heating evaporation without using ion source assisted evaporation;
[0072] S12, vapor-depositing a third ZnSe film layer on the plated fourth YbF3 film layer, the deposition rate of the third ZnSe film layer is 0.8 nm / s, the film thickness of the third ZnSe film layer is controlled to be 32 nm, ion source assisted vapor deposition is not used, and the vapor deposition is carried out by resistance heating evaporation;
[0073] S13, vapor-depositing a fifth YbF3 film layer on the plated third ZnSe film layer, the deposition rate of the fifth YbF3 film layer is 0.6 nm / s, the film thickness of the fifth YbF3 film layer is controlled to be 156.8 nm, and the evaporation is performed by resistance heating evaporation without using ion source assisted evaporation;
[0074] S14, vapor-depositing a fourth ZnSe film layer on the plated fifth YbF3 film layer, the deposition rate of the fourth ZnSe film layer is 0.8 nm / s, the film thickness of the fourth ZnSe film layer is controlled to be 26 nm, ion source assisted vapor deposition is not used, and the vapor deposition is carried out by resistance heating evaporation;
[0075] S15, after the fourth ZnSe film layer is deposited, the vacuum chamber is cooled to below 60°C and the fixture, the accompanying deposition sheet and the product are taken out;
[0076] S16, repeat steps S1 to S15, and sequentially evaporate the first Y2O3 film layer, the first YbF3 film layer, the first ZnSe film layer, the second YbF3 film layer, the second ZnSe film layer, the third YbF3 film layer, the second Y2O3 film layer, the fourth YbF3 film layer, the third ZnSe film layer, the fifth YbF3 film layer, and the fourth ZnSe film layer on the second opposite side of the lens.
[0077] Figure 2 It is a curve diagram of the transmittance of the accompanying coating sheet of Example 1 coated with 1064nm and 7.7-10.5μm antireflection films on both sides in the 1064nm band. Figure 3 It is a curve diagram of the transmittance of the accompanying coating sheet of Example 1 coated with 1064nm and 7.7-10.5μm antireflection films on both sides in the 7.7-10.5μm band.
[0078] from Figure 2 It can be seen that the transmittance in the 1064nm band (near infrared band) is 98.2%; Figure 3 It can be seen that the average transmittance in the 7.7-10.5 μm band (far infrared band) is 98.8%, that is, the transmittance in both bands exceeds 98%, both exceeding the transmittance in both bands of the patent literature mentioned in the background technology.
[0079] The above detailed description is used to describe multiple exemplary embodiments, but this document is not intended to be limited to the explicitly disclosed combinations. Therefore, unless otherwise stated, the various features disclosed herein can be combined together to form multiple additional combinations that are not shown for the sake of simplicity.
Claims
1. A method for preparing a 1064nm and 7.7-10.5μm antireflection film system on a chalcogenide glass substrate, characterized in that: Includes steps: S1, cleaning the surface of the accompanying plating sheet and the product of the chalcogenide glass substrate as the lens, the chalcogenide glass substrate is an IG06 substrate, and the thickness of the accompanying plating sheet is 0.9-1.5 mm; S2, put the cleaned lens into the fixture, and hang the fixture with the lens into the cavity of the vacuum coating machine, and set the temperature of the cavity to 120-130℃; S3, vacuum coating machine starts to evacuate, and the vacuum degree reaches 1.5×10 -3 Pa, turn on the auxiliary coating ion source of the vacuum coating machine for cleaning, the cleaning time is 6 minutes, the anode voltage of the ion source is 220V, the anode current is 1.0-2.5A, and the emitter current is 1.3-1.5A; S4, maintaining the aforementioned vacuum degree, evaporating a first Y2O3 film layer on the first surface of the lens, the deposition rate of the first Y2O3 film layer is 0.3nm / s, the film thickness of the first Y2O3 film layer is controlled to be 15nm±1nm, and ion source assisted evaporation is not used; S5, evaporating a first YbF3 film layer on the plated first Y2O3 film layer, the deposition rate of the first YbF3 film layer is 0.6nm / s, the film thickness of the first YbF3 film layer is controlled to be 66.2nm±3nm, and ion source assisted evaporation is not used; S6, evaporating a first ZnSe film layer on the plated first YbF3 film layer, the deposition rate of the first ZnSe film layer is 0.8nm / s, the film thickness of the first ZnSe film layer is controlled to be 48.3nm±2nm, and ion source assisted evaporation is not used; S7, evaporating a second YbF3 film layer on the plated first ZnSe film layer, the deposition rate of the second YbF3 film layer is 0.6nm / s, the film thickness of the second YbF3 film layer is controlled to be 80.2nm±3nm, and ion source assisted evaporation is not used; S8, evaporating a second ZnSe film layer on the plated second YbF3 film layer, the deposition rate of the second ZnSe film layer is 0.8 nm / s, the film thickness of the second ZnSe film layer is controlled to be 608.3 nm±5 nm, and ion source assisted evaporation is not used; S9, evaporating a third YbF3 film layer on the plated second ZnSe film layer, the deposition rate of the third YbF3 film layer is 0.6 nm / s, the film thickness of the third YbF3 film layer is controlled to be 800 nm±5 nm, and ion source assisted evaporation is not used; S10, evaporating a second Y2O3 film layer on the plated third YbF3 film layer, the deposition rate of the second Y2O3 film layer is 0.3nm / s, the film thickness of the second Y2O3 film layer is controlled to be 15nm±1nm, and ion source assisted evaporation is not used; S11, evaporating a fourth YbF3 film layer on the plated second Y2O3 film layer, the deposition rate of the fourth YbF3 film layer is 0.6nm / s, the film thickness of the fourth YbF3 film layer is controlled to be 421.5nm±5nm, and ion source assisted evaporation is not used; S12, evaporating a third ZnSe film layer on the plated fourth YbF3 film layer, the deposition rate of the third ZnSe film layer is 0.8 nm / s, the film thickness of the third ZnSe film layer is controlled to be 32 nm±2 nm, and ion source assisted evaporation is not used; S13, vapor-depositing a fifth YbF3 film layer on the plated third ZnSe film layer, the deposition rate of the fifth YbF3 film layer is 0.6 nm / s, the film thickness of the fifth YbF3 film layer is controlled to be 156.8 nm±5 nm, and ion source assisted vapor deposition is not used; S14, vapor-depositing a fourth ZnSe film layer on the plated fifth YbF3 film layer, the deposition rate of the fourth ZnSe film layer is 0.8 nm / s, the film thickness of the fourth ZnSe film layer is controlled to be 26 nm±1 nm, and ion source assisted vapor deposition is not used; S15, after the fourth ZnSe film layer is deposited, the vacuum chamber is cooled to below 60°C and the fixture, the accompanying deposition sheet and the product are taken out; S16, repeat steps S1 to S15, and sequentially evaporate the first Y2O3 film layer, the first YbF3 film layer, the first ZnSe film layer, the second YbF3 film layer, the second ZnSe film layer, the third YbF3 film layer, the second Y2O3 film layer, the fourth YbF3 film layer, the third ZnSe film layer, the fifth YbF3 film layer, and the fourth ZnSe film layer on the second opposite side of the lens.
2. The method for preparing a 1064 nm and 7.7-10.5 μm antireflection film system on a chalcogenide glass substrate according to claim 1, characterized in that: In step S1, the thickness of the accompanying plating sheet is 1.0 mm.
3. The method for preparing a 1064 nm and 7.7-10.5 μm antireflection film system on a chalcogenide glass substrate according to claim 1, characterized in that: In step S1, the surface of the lens is cleaned by ultrasonic wave or hand wiping.
4. The method for preparing a 1064 nm and 7.7-10.5 μm antireflection film system on a chalcogenide glass substrate according to claim 1, characterized in that: In step S2, the temperature of the chamber is set to 130°C.
5. The method for preparing a 1064 nm and 7.7-10.5 μm antireflection film system on a chalcogenide glass substrate according to claim 1, characterized in that: In step S3, the anode current is 1.2A and the emitter current is 1.5A.
6. The method for preparing a 1064 nm and 7.7-10.5 μm antireflection film system on a chalcogenide glass substrate according to claim 1, characterized in that: In step S3, the ion source is a Hall ion source, and argon gas is used as the working gas.
7. The method for preparing a 1064 nm and 7.7-10.5 μm antireflection film system on a chalcogenide glass substrate according to claim 1, characterized in that: In step S4, the film thickness of the first Y2O3 film is controlled to be 15 nm; In step S5, the film thickness of the first YbF3 film is controlled to be 66.2 nm; In step S6, the film thickness of the first ZnSe film layer is controlled to be 48.3 nm; In step S7, the film thickness of the second YbF3 film is controlled to be 80.2 nm; In step S8, the film thickness of the second ZnSe film layer is controlled to be 608.3 nm; In step S9, the thickness of the third YbF3 film layer is controlled to be 800 nm; In step S10, the film thickness of the second Y2O3 film is controlled to be 15 nm; In step S11, the thickness of the fourth YbF3 film layer is controlled to be 421.5 nm; In step S12, the film thickness of the third ZnSe film layer is controlled to be 32n nm; In step S13, the thickness of the fifth YbF3 film is controlled to be 156.8 nm; In step S14, the film thickness of the fourth ZnSe film is controlled to be 26 nm.
8. The method for preparing a 1064 nm and 7.7-10.5 μm antireflection film system on a chalcogenide glass substrate according to claim 1, characterized in that: In steps S5 to S9 and steps S11 to S14, the evaporation is carried out by resistance heating evaporation; In step S4 and step S10, electron beam evaporation is used for evaporation.
Citation Information
Patent Citations
Preparation method for plating dual-band antireflection film system on chalcogenide glass substrate
CN117567044A
3.7-4.8 [mu]m and 7.7-9.5 [mu]m dual-band antireflection film with BaF2 substrate and preparation method thereof
CN113866852A
Visible infrared ultra-wide spectrum color separation film based on all-dielectric film
CN118210093A
Preparation method for plating two-waveband film system on calcium fluoride substrate
CN118291920A
Anti-reflective coatings for ir-transmitting substrates
US20230193452A1