Cement activity enhancer and preparation method thereof
Through compound technologies such as slag powder, nano-calcium carbonate and modified nano-silica, the problems of complex composition and poor adaptability of existing cement enhancers have been solved, and the flexural compressive strength and comprehensive performance of cement have been significantly improved, achieving Cost reduction and stability improvement.
Patent Information
- Application Number
- CN202410954892.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-17
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2044-07-17
AI Technical Summary
Existing cement reinforcements have complex components, poor adaptability, and poor strength enhancement effects, which affect the stability and safety of concrete.
Using the compound technology of slag powder, nano-calcium carbonate and modified nano-silica, activator and dispersant, a cement active enhancer with high specific surface area and good dispersion is prepared through ball milling and ultrasonic methods to promote cement water Chemicalization process to improve flexural strength.
It significantly improves the flexural and compressive strength of cement specimens, reduces cement production costs, and improves the comprehensive performance of concrete. It has good adaptability and is suitable for different application scenarios.
Smart Images

Figure CN118754485A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of cement admixtures, and in particular relates to a cement activity enhancer and a preparation method thereof. Background Art
[0002] Concrete, with its advantages of wide material supply, low cost and simple construction, is widely used in infrastructure projects such as houses, roads and bridges, ports, dams, etc. It is one of the most commonly used building materials in the civil engineering industry and is also the second largest consumable in the world. In recent years, my country has made large-scale investments in infrastructure such as transportation systems (highways, high-speed railways), urban supporting facilities (housing construction, subways), water conservancy (water storage and water diversion projects) and electricity (power generation and transmission projects). A large number of public and civil facilities have been built and are planned to be built, and the demand for concrete materials is also increasing. Although concrete has a series of advantages such as low price, abundant raw materials, easy use, high compressive strength and wide application range. However, due to the design defects of concrete itself and the influence of environmental factors, some concrete will suffer from corrosion, alkali-aggregate reaction, freeze-thaw damage, and even cracks, which seriously affect the stability and safety of the structure. Sulphoaluminate cement has excellent properties such as high early strength, high impermeability, high frost resistance and strong corrosion resistance. It is currently a widely used cement.
[0003] Cement active enhancers can fully stimulate cement mixed materials, thereby reducing the amount of cement clinker, saving a lot of mineral resources and energy, and greatly reducing the cost of cement production. At present, there are many cement enhancers on the market, which also have certain cement enhancement effects. However, they all have the problems of complex ingredients, poor adaptability to cement admixtures, poor strength enhancement effect, and poor comprehensive performance. Therefore, in order to solve these shortcomings of common cement enhancers, a new type of cement active enhancer with small dosage, good enhancement effect, small impact on the water consumption of cement standard consistency, and no adverse effect on the adaptability of concrete admixtures is needed. Summary of the invention
[0004] The invention provides a cement activity enhancer. The cement activity enhancer is compounded with a plurality of raw materials to achieve remarkable synergistic effect. The multi-directional joint action promotes the cement hydration process, improves the flexural and compressive strengths of cement specimens, and reduces the cement production cost.
[0005] In order to achieve the above technical objectives, the technical solution adopted by the present invention is: A cement active enhancer is prepared from the following raw materials in parts by weight: 60-80 parts of slag powder, 5-8 parts of enhancer, 0.5-1 part of activator, 1-3 parts of inorganic salt and 3-5 parts of dispersant.
[0006] Preferably, the slag powder is a mixture of diatomaceous earth, phosphorus slag and graphene oxide in a mass ratio of 1:1:(0.05-0.08).
[0007] Preferably, the slag powder is prepared by the following method: diatomaceous earth, phosphorus slag and graphene oxide are mixed according to a mass ratio and added into a ball mill, the speed of the ball mill is set to 200-300 r / min, and the powder is ball milled for 30 minutes.
[0008] Preferably, the reinforcing agent is composed of nano calcium carbonate and modified nano silicon dioxide in a mass ratio of 2:1, wherein the particle size of the nano calcium carbonate is 100 nm.
[0009] Preferably, the modified nano-silicon dioxide is prepared by the following method: Step 1, weighing silica nanoparticles, adding an appropriate amount of deionized water thereto, ultrasonicating at room temperature for 20 min, then heating to 45° C. and keeping the temperature constant for 15 min to obtain a silica nanodispersion liquid; the nano silica particle size is 20-60 nm; Step 2: add 0.5 g of perfluorooctyltriethoxysilane and 10 ml of 5% acetic acid solution to the silica nano-dispersion, stir and heat to 80°C, react for 30 minutes, and then dry the suspension at 80°C for 8 hours to constant weight to obtain modified nano-silica.
[0010] Preferably, the usage ratio of the nano-silicon dioxide to deionized water is 20g:100ml.
[0011] Preferably, the activator is CaO and Na 2 SO 4 The composition is based on a mass ratio of 1:(0.5-0.8).
[0012] Preferably, the inorganic salt is NaCl or CaCl 2 .
[0013] Preferably, the dispersant is one of calcium lignin sulfonate, sodium lignin sulfonate, and sulfonated melamine formaldehyde resin.
[0014] A method for preparing the above-mentioned cement active enhancer comprises the following steps: (1) Preparation of slag powder; (2) preparing modified nano-silicon dioxide, and uniformly mixing nano-calcium carbonate and modified nano-silicon dioxide according to a mass ratio to obtain a reinforcing agent; (3) Weigh the remaining raw materials by weight and mix them evenly with the slag powder and reinforcing agent.
[0015] The dosage of the cement activity enhancer prepared by the invention is 4-6‰ of the mass of cement.
[0016] Phosphorus slag is a product obtained by using phosphate ore, silica and coke as raw materials to form a melt at a high temperature of 1400-1600℃ when producing yellow phosphorus by electric furnace method, and then quenching it with water. The main minerals of the slag are wollastonite, lanceolite, and calcite, and the main chemical components are CaO and SiO 2 , also contains a small amount of Al 2 O 3 , Fe 2 O 3 ,MgO,P 2 O 5 etc., with high potential activity. However, directly using phosphorus slag as a cement concrete admixture usually has the adverse effects of long setting time and low early strength. The present invention uses phosphorus slag, diatomaceous earth and graphene oxide in combination, and on the one hand, reduces the particle size of slag micropowder by ball milling, and has a suitable specific surface area. On the other hand, the interaction between the components of ball milling is more sufficient. As the friction between substances and other effects are enhanced, the particles are gradually refined, the structure of some crystals is destroyed, and more active sites are exposed, so that the amorphous gel participating in the hydration reaction process is increased, which can better improve the activity of cement.
[0017] The reinforcing agent of the present invention is made of nano calcium carbonate and modified nano silicon dioxide in a specific ratio. Although nano calcium carbonate also has the advantages of nano materials with high specific surface area, its activity is relatively low; while the modified nano silicon dioxide of the present invention bonds groups such as silanol and fluorosilane to the surface of silicon dioxide nano particles, which improves the dispersibility of nano particles and the surface activity of the groups. After being used in combination with nano calcium carbonate, the two can produce a synergistic effect, and the surface group activity and nano particle dispersibility are further enhanced. The two work together to promote the formation of CSH active groups in the cement hydration process, and significantly improve the compressive strength of cement.
[0018] After the activator used in the present invention is mixed with the mineral powder, under suitable conditions, the crystal structure in the mineral powder particles is disintegrated to release more active SiO 2 、Al 2 O 3 and with SO 4 2- , Ca(OH) 2 The products such as AFt and calcium silicate hydrate gel (CSH) are generated through joint reactions, which better ensure the strength of the cement system.
[0019] The beneficial effect of the present invention is that under the joint action of the activator, enhancer and mineral powder of the present invention, the mineral powder releases a large amount of active SiO2 and Al2O3, and a hydration reaction occurs between SiO2 and Al2O3 and Ca(OH)2 produced by cement hydration to generate a large amount of hydration products such as CSH, C2ASH8 and C4AH13, which promotes the cement hydration process. At the same time, its hydration products and nanoparticles also fill the gaps after the cement slurry is solidified, reduce the porosity of the cement slurry after solidification, improve the flexural and compressive strengths of the specimens, reduce the amount of cement clinker used, and improve the comprehensive performance of cement, which has good application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 TEM images of the nano-silicon dioxide in the reinforcing agent of the present invention before and after modification; a) is before modification, and b) is after modification. DETAILED DESCRIPTION
[0021] The technical solution of the present invention is further described below in conjunction with specific embodiments, but is not limited thereto.
[0022] Unless otherwise specified, the raw materials used in the present invention are commercially available. Nano-silicon dioxide was purchased from Nanjing Hongde Nanomaterials Co., Ltd. with an average particle size of 20 nm. Phosphorus slag was purchased from a yellow phosphorus manufacturer in Jining City, Shandong Province, with a density of 2.89 g / cm 3 , with a specific surface area of 430m 2 / kg, its specific composition is shown in Table 1 below: Table 1 Main chemical composition of phosphorus slag
[0023] Example 1 A cement active enhancer is prepared from the following raw materials in parts by weight: 60 parts of slag powder, 5 parts of enhancer, 0.5 parts of activator, 1 part of inorganic salt and 3 parts of dispersant.
[0024] The slag powder is a mixture of diatomaceous earth, phosphorus slag and graphene oxide in a mass ratio of 1:1:0.05.
[0025] The slag micropowder is prepared by the following method: diatomaceous earth, phosphorus slag and graphene oxide are mixed according to a mass ratio and added into a ball mill, the speed of the ball mill is set to 200-300 r / min, and the slag micropowder is obtained by ball milling for 30 minutes.
[0026] The reinforcing agent is composed of nano calcium carbonate and modified nano silicon dioxide in a mass ratio of 2:1, wherein the particle size of the nano calcium carbonate is 100 nm.
[0027] The modified nano silicon dioxide is prepared by the following method: Step 1, weigh silica nanoparticles, add appropriate amount of deionized water thereto, ultrasonicate at room temperature for 20 min, then heat to 45°C and keep constant temperature for 15 min to obtain silica nanodispersion; the dosage ratio of the nanosilica to deionized water is 20g:100ml.
[0028] Step 2: add 0.5 g of perfluorooctyltriethoxysilane and 10 ml of 5% acetic acid solution to the silica nano-dispersion, stir and heat to 80°C, react for 30 minutes, and then dry the suspension at 80°C for 8 hours to constant weight to obtain modified nano-silica.
[0029] The activator is CaO and Na 2 SO 4 According to the mass ratio of 1:0.5.
[0030] The inorganic salt is NaCl.
[0031] The dispersant is one of calcium lignin sulfonate, sodium lignin sulfonate and sulfonated melamine formaldehyde resin.
[0032] A method for preparing the above-mentioned cement active enhancer comprises the following steps: (1) Preparation of slag powder; (2) preparing modified nano-silicon dioxide, and uniformly mixing nano-calcium carbonate and modified nano-silicon dioxide according to a mass ratio to obtain a reinforcing agent; (3) Weigh the remaining raw materials by weight and mix them evenly with the slag powder and reinforcing agent.
[0033] Example 2 A cement active enhancer is prepared from the following raw materials in parts by weight: 70 parts of slag powder, 7 parts of enhancer, 0.8 parts of activator, 2 parts of inorganic salt and 4 parts of dispersant.
[0034] The slag powder is a mixture of diatomaceous earth, phosphorus slag and graphene oxide in a mass ratio of 1:1:0.06.
[0035] The slag micropowder is prepared by the following method: diatomaceous earth, phosphorus slag and graphene oxide are mixed according to a mass ratio and added into a ball mill, the speed of the ball mill is set to 200-300 r / min, and the slag micropowder is obtained by ball milling for 30 minutes.
[0036] The reinforcing agent is composed of nano calcium carbonate and modified nano silicon dioxide in a mass ratio of 2:1, wherein the particle size of the nano calcium carbonate is 100 nm.
[0037] The modified nano silicon dioxide is prepared by the following method: Step 1, weigh silica nanoparticles, add appropriate amount of deionized water thereto, ultrasonicate at room temperature for 20 min, then heat to 45°C and keep constant temperature for 15 min to obtain silica nanodispersion; the dosage ratio of the nanosilica to deionized water is 20g:100ml.
[0038] Step 2: add 0.5 g of perfluorooctyltriethoxysilane and 10 ml of 5% acetic acid solution to the silica nano-dispersion, stir and heat to 80°C, react for 30 minutes, and then dry the suspension at 80°C for 8 hours to constant weight to obtain modified nano-silica.
[0039] The activator is CaO and Na 2 SO 4 It is composed in a mass ratio of 1:0.7.
[0040] The inorganic salt is CaCl 2 .
[0041] The dispersant is one of calcium lignin sulfonate, sodium lignin sulfonate and sulfonated melamine formaldehyde resin.
[0042] A method for preparing the above-mentioned cement active enhancer comprises the following steps: (1) Preparation of slag powder; (2) preparing modified nano-silicon dioxide, and uniformly mixing nano-calcium carbonate and modified nano-silicon dioxide according to a mass ratio to obtain a reinforcing agent; (3) Weigh the remaining raw materials by weight and mix them evenly with the slag powder and reinforcing agent.
[0043] Example 3 A cement active enhancer is prepared from the following raw materials in parts by weight: 80 parts of slag powder, 8 parts of enhancer, 1 part of activator, 3 parts of inorganic salt and 5 parts of dispersant.
[0044] The slag powder is a mixture of diatomaceous earth, phosphorus slag and graphene oxide in a mass ratio of 1:1:0.08.
[0045] The slag micropowder is prepared by the following method: diatomaceous earth, phosphorus slag and graphene oxide are mixed according to a mass ratio and added into a ball mill, the speed of the ball mill is set to 200-300 r / min, and the slag micropowder is obtained by ball milling for 30 minutes.
[0046] The reinforcing agent is composed of nano calcium carbonate and modified nano silicon dioxide in a mass ratio of 2:1, wherein the particle size of the nano calcium carbonate is 100 nm.
[0047] The modified nano silicon dioxide is prepared by the following method: Step 1, weigh silica nanoparticles, add appropriate amount of deionized water thereto, ultrasonicate at room temperature for 20 min, then heat to 45°C and keep constant temperature for 15 min to obtain silica nanodispersion; the dosage ratio of the nanosilica to deionized water is 20g:100ml.
[0048] Step 2: add 0.5 g of perfluorooctyltriethoxysilane and 10 ml of 5% acetic acid solution to the silica nano-dispersion, stir and heat to 80°C, react for 30 minutes, and then dry the suspension at 80°C for 8 hours to constant weight to obtain modified nano-silica.
[0049] The activator is CaO and Na 2 SO 4 It is composed in a mass ratio of 1:0.8.
[0050] The inorganic salt is CaCl 2 .
[0051] The dispersant is one of calcium lignin sulfonate, sodium lignin sulfonate and sulfonated melamine formaldehyde resin.
[0052] A method for preparing the above-mentioned cement active enhancer comprises the following steps: (1) Preparation of slag powder; (2) preparing modified nano-silicon dioxide, and uniformly mixing nano-calcium carbonate and modified nano-silicon dioxide according to a mass ratio to obtain a reinforcing agent; (3) Weigh the remaining raw materials by weight and mix them evenly with the slag powder and reinforcing agent.
[0053] Example 4 A cement active enhancer is prepared from the following raw materials in parts by weight: 65 parts of slag powder, 7 parts of enhancer, 0.6 parts of activator, 2 parts of inorganic salt and 3 parts of dispersant.
[0054] The slag powder is a mixture of diatomaceous earth, phosphorus slag and graphene oxide in a mass ratio of 1:1:0.05.
[0055] The slag micropowder is prepared by the following method: diatomaceous earth, phosphorus slag and graphene oxide are mixed according to a mass ratio and added into a ball mill, the speed of the ball mill is set to 200-300 r / min, and the slag micropowder is obtained by ball milling for 30 minutes.
[0056] The reinforcing agent is composed of nano calcium carbonate and modified nano silicon dioxide in a mass ratio of 2:1, wherein the particle size of the nano calcium carbonate is 100 nm.
[0057] The modified nano silicon dioxide is prepared by the following method: Step 1, weigh silica nanoparticles, add an appropriate amount of deionized water thereto, ultrasonicate at room temperature for 20 min, then heat to 45°C and keep the temperature constant for 15 min to obtain a silica nanodispersion liquid; the dosage ratio of the nanosilica to deionized water is 20g:100ml.
[0058] Step 2: add 0.5 g of perfluorooctyltriethoxysilane and 10 ml of 5% acetic acid solution to the silica nano-dispersion, stir and heat to 80°C, react for 30 minutes, and then dry the suspension at 80°C for 8 hours to constant weight to obtain modified nano-silica.
[0059] The activator is CaO and Na 2 SO 4 It is composed in a mass ratio of 1:0.8.
[0060] The inorganic salt is CaCl 2 .
[0061] The dispersant is one of calcium lignin sulfonate, sodium lignin sulfonate and sulfonated melamine formaldehyde resin.
[0062] A method for preparing the above-mentioned cement active enhancer comprises the following steps: (1) Preparation of slag powder; (2) preparing modified nano-silicon dioxide, and uniformly mixing nano-calcium carbonate and modified nano-silicon dioxide according to a mass ratio to obtain a reinforcing agent; (3) Weigh the remaining raw materials by weight and mix them evenly with the slag powder and reinforcing agent.
[0063] Comparative Example 1 A cement active enhancer, whose principle and composition are basically the same as those of Example 4, except that the enhancer is nano calcium carbonate.
[0064] Comparative Example 2 A cement active enhancer, whose principle and composition are basically the same as those of Example 4, except that the enhancer is modified nano-silicon dioxide.
[0065] Comparative Example 3 A cement active enhancer, whose principle and composition are basically the same as those in Example 4, except that the enhancer is composed of nano calcium carbonate and unmodified nano silicon dioxide in a mass ratio of 2:1.
[0066] Comparative Example 4 A cement active enhancer, whose principle and composition are basically the same as those of Example 4, except that the slag powder is diatomaceous earth.
[0067] Comparative Example 5 A cement active enhancer, whose principle and composition are basically the same as those of Example 4, except that the slag powder is phosphorus slag.
[0068] Comparative Example 6 A cement active enhancer, whose principle and composition are basically the same as those of Example 4, except that the slag powder is graphene oxide.
[0069] Comparative Example 7 A cement active enhancer, whose principle and composition are basically the same as those of Example 4, except that the activator is CaO.
[0070] Comparative Example 8 A cement active enhancer, the principle and composition of which are basically the same as those of Example 4, except that the activator is Na 2 SO 4 .
[0071] Application Example 1 A cement is composed of a cement base material and a cement activation enhancer prepared in Example 1; the cement activation enhancer is used in an amount of 5‰ of the weight of the cement base material; the mass percentage of the cement base material is: 72% cement clinker, 23% fly ash, and 5% limestone. The above materials are mixed and ground in a cement test mill to obtain cement.
[0072] Application Example 2 A cement is composed of a cement base material and a cement activation enhancer prepared in Example 1; the cement activation enhancer is used in an amount of 5‰ of the weight of the cement base material; the mass percentage of the cement base material is: 75% cement clinker, 20% fly ash, and 5% limestone. The above materials are mixed and ground in a cement test mill to obtain cement.
[0073] Application Example 3 A cement is composed of a cement base material and a cement activation enhancer prepared in Example 1; the cement activation enhancer is used in an amount of 5‰ of the weight of the cement base material; the mass percentage of the cement base material is: 70% cement clinker, 25% fly ash, and 5% limestone. The above materials are mixed and ground in a cement test mill to obtain cement.
[0074] Application Example 4 A cement is composed of a cement base material and a cement activation enhancer prepared in Example 2; the cement activation enhancer is used in an amount of 5‰ of the weight of the cement base material; the mass percentage of the cement base material is: 72% cement clinker, 23% fly ash, and 5% limestone. The above materials are mixed and ground in a cement test mill to obtain cement.
[0075] Application Example 5 A cement is composed of a cement base material and a cement activation enhancer prepared in Example 2; the cement activation enhancer is used in an amount of 5‰ of the weight of the cement base material; the mass percentage of the cement base material is: 75% cement clinker, 20% fly ash, and 5% limestone. The above materials are mixed and ground in a cement test mill to obtain cement.
[0076] Application Example 6 A cement is composed of a cement base material and a cement activation enhancer prepared in Example 1; the cement activation enhancer is used in an amount of 5‰ of the weight of the cement base material; the mass percentage of the cement base material is: 70% cement clinker, 25% fly ash, and 5% limestone. The above materials are mixed and ground in a cement test mill to obtain cement.
[0077] Application Example 7 A cement is composed of a cement base material and a cement activation enhancer prepared in Example 3; the cement activation enhancer is used in an amount of 5‰ of the weight of the cement base material; the mass percentage of the cement base material is: 72% cement clinker, 23% fly ash, and 5% limestone. The above materials are mixed and ground in a cement test mill to obtain cement.
[0078] Application Example 8 A cement is composed of a cement base material and the cement activation enhancer prepared in Example 3; the cement activation enhancer is used in an amount of 5‰ of the weight of the cement base material; the mass percentage of the cement base material is: 75% cement clinker, 20% fly ash, and 5% limestone. The above materials are mixed and ground in a cement test mill to obtain cement.
[0079] Application Example 9 A cement is composed of a cement base material and a cement activation enhancer prepared in Example 3; the cement activation enhancer is used in an amount of 5‰ of the weight of the cement base material; the mass percentage of the cement base material is: 70% cement clinker, 25% fly ash, and 5% limestone. The above materials are mixed and ground in a cement test mill to obtain cement.
[0080] Application Example 10 A cement is composed of a cement base material and a cement activation enhancer prepared in Example 3; the cement activation enhancer is used in an amount of 5‰ of the weight of the cement base material; the mass percentage of the cement base material is: 72% cement clinker, 23% fly ash, and 5% limestone. The above materials are mixed and ground in a cement test mill to obtain cement.
[0081] Application Example 11 A cement is composed of a cement base material and a cement activation enhancer prepared in Example 4; the cement activation enhancer is used in an amount of 5‰ of the weight of the cement base material; the mass percentage of the cement base material is: 75% cement clinker, 20% fly ash, and 5% limestone. The above materials are mixed and ground in a cement test mill to obtain cement.
[0082] Application Example 12 A cement is composed of a cement base material and a cement activation enhancer prepared in Example 4; the cement activation enhancer is used in an amount of 5‰ of the weight of the cement base material; the mass percentage of the cement base material is: 70% cement clinker, 25% fly ash, and 5% limestone. The above materials are mixed and ground in a cement test mill to obtain cement.
[0083] Application Comparative Example 1 A cement is composed of cement base materials; the mass percentage of the cement base materials is: 80% cement clinker, 15% fly ash, and 5% limestone. The above materials are mixed and ground in a cement test mill to obtain cement.
[0084] Application effect test In order to further illustrate the use effect of the present invention, the performance tests were performed on the cement prepared by application examples 1-12 and comparative example 1 using the cement active enhancers prepared by embodiments 1-4 of the present invention to prepare cement; cement standard consistency water consumption, setting time, and stability test method (GB / T 1346-2005); cement mortar fluidity test standard (GB / T 2419-2005); cement mortar strength test method (GB / T 17671-1999), and the results are shown in Table 2.
[0085] Table 2 Performance test results
[0086] It can be seen from Table 1 that, compared with the comparative example 1, the 3d and 28d strengths of cements prepared by using the cement active enhancers of Examples 1-4 of the present invention are equivalent to or slightly higher than those of the comparative example 1, which indicates that after using the cement active enhancer of the present invention, the amount of cement clinker is reduced by about 10%, and a comparable use effect can still be achieved, thereby achieving the purpose of reducing the cost of cement.
[0087] The cement active enhancers prepared in Examples 1-4 and Comparative Examples 1-8 were added to cement base materials at a dosage of 5‰ to prepare cement, and the mass percentage of the cement base materials was: 70% cement clinker, 25% fly ash, and 5% limestone; wherein the blank control was a cement base material without any cement active agent. The prepared cement was subjected to performance tests; cement standard consistency water consumption, setting time, and stability test methods (GB / T 1346-2005); cement mortar fluidity test standard (GB / T 2419-2005); cement mortar strength test method (GB / T 17671-1999), and the results are shown in Table 3.
[0088] Table 3 Performance test results
[0089] It can be seen from the data in Table 2 that compared with the blank comparative example, the 3d and 28d compressive strength and flexural strength of the cement in comparative examples 1-3 are improved, but the overall strength improvement effect is lower than that of the cement prepared in examples 1-4. This is mainly due to the synergistic effect of the nano-calcium carbonate and modified nano-silicon dioxide in the present invention using a reasonable ratio. 2 The surface hydroxyl groups are replaced by perfluorooctyltriethoxysilane, which reduces the surface energy and the tendency of agglomeration (e.g. Figure 1 As shown), it has good dispersibility, and groups such as silanol and fluorosilane are bonded to the surface of silica nanoparticles, which improves the surface activity of the nanoparticle groups. The two nanoparticles work together to promote the formation of CSH active groups in the cement hydration process, significantly improving the compressive strength of cement. Compared with the blank comparative example, the compressive strength and flexural strength of the cement 3d and 28d in Examples 4-6 are improved, but the overall strength improvement effect is lower than that of the cement prepared in Examples 1-4. This is mainly because the present invention uses phosphorus slag, diatomaceous earth, and graphene oxide in a suitable proportion, and interacts with other reinforcing agents and stimulants, so that more active raw materials participate in the hydration reaction and promote the increase of amorphous gel in the process, which can better improve the strength of cement. Compared with the blank comparative example, the cement strength improvement effect of Examples 7-8 is weaker overall, which shows that the single stimulant has a weak stimulating effect on the cement of the present invention. Only when the two stimulants are in a suitable proportion, the two work synergistically, and after being blended with the mineral micropowder, the crystal structure in the mineral micropowder particles is promoted to disintegrate, and more active SiO 2 、Al 2 O 3 and with SO 4 2- , Ca(OH) 2The products such as AFt and calcium silicate hydrate gel (CSH) are generated by the common reaction, which better guarantees the strength of the cement system. Changing any one of the raw material composition and dosage cannot achieve the effect described in the present invention.
[0090] It should be noted that the above embodiments are only some embodiments of the preferred methods of implementing the present invention, rather than all embodiments. Obviously, based on the above embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.
Claims
1. A cement activity enhancer, It is characterized in that The invention is prepared from the following raw materials in parts by weight: 60-80 parts of slag micropowder, 5-8 parts of reinforcing agent, 0.5-1 part of activator, 1-3 parts of inorganic salt and 3-5 parts of dispersant.
2. The cement active enhancer according to claim 1, It is characterized in that The slag powder is a mixture of diatomite, phosphorus slag and graphene oxide in a mass ratio of 1:1:(0.05-0.08).
3. The cement active enhancer according to claim 2, It is characterized in that The slag micropowder is prepared by the following method: diatomaceous earth, phosphorus slag and graphene oxide are mixed according to a mass ratio and added into a ball mill, the speed of the ball mill is set to 200-300 r / min, and the slag micropowder is obtained by ball milling for 30 minutes.
4. The cement activity enhancer according to claim 1, It is characterized in that The reinforcing agent is composed of nano calcium carbonate and modified nano silicon dioxide in a mass ratio of 2:1, wherein the particle size of the nano calcium carbonate is 100 nm.
5. The cement activity enhancer according to claim 1, It is characterized in that The modified nano silicon dioxide is prepared by the following method: Step 1, weighing silica nanoparticles, adding an appropriate amount of deionized water thereto, ultrasonicating at room temperature for 20 min, then heating to 45° C. and keeping the temperature constant for 15 min to obtain a silica nanodispersion liquid; Step 2: add 0.5 g of perfluorooctyltriethoxysilane and 10 ml of 5% acetic acid solution to the silica nano-dispersion, stir and heat to 80°C, react for 30 minutes, and then dry the suspension at 80°C for 8 hours to constant weight to obtain modified nano-silica.
6. The cement activity enhancer according to claim 5, It is characterized in that The dosage ratio of the nano silicon dioxide to deionized water is 20g:100ml.
7. The cement activity enhancer according to claim 1, It is characterized in that The activator is CaO and Na 2 SO 4 The composition is based on a mass ratio of 1:(0.5-0.8).
8. The cement activity enhancer according to claim 1, It is characterized in that The inorganic salt is NaCl or CaCl 2 .
9. The cement activity enhancer according to claim 1, It is characterized in that The dispersant is one of calcium lignin sulfonate, sodium lignin sulfonate and sulfonated melamine formaldehyde resin.
10. A method for preparing the cement active enhancer according to any one of claims 1 to 9, It is characterized in that It includes the following steps: (1) Preparation of slag powder; (2) preparing modified nano-silicon dioxide, and uniformly mixing nano-calcium carbonate and modified nano-silicon dioxide according to a mass ratio to obtain a reinforcing agent; (3) Weigh the remaining raw materials by weight and mix them evenly with the slag powder and reinforcing agent.
Citation Information
Patent Citations
Inorganic cement reinforcer
CN1033789A
Slag micro-powder for baking-free brick enhancing water-proof performance and preparation method thereof
CN107663037A
Method of producing exothermic mold powder in form of sprayed granules
US20190210097A1
Metal smelting waste residue-derived material, preparation method therefor and application thereof
WO2024109477A1