Curing agent for embankment soft rock as well as preparation method and application of curing agent
Through the use of industrial waste residue geopolymer, bio-glue and other combined curing agents, the problem of poor strength and easy disintegration of embankment soft rock has been solved, the mechanical properties and water stability have been significantly improved, a dense structure has been formed, and the risk of geological disasters has been reduced. economic losses.
Patent Information
- Application Number
- CN202410784737.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-18
- Publication Date
- 2024-10-11
AI Technical Summary
Embankment soft rock has poor strength and is easy to disintegrate, leading to geological disasters such as landslides and collapses. Existing curing agents have problems such as poor hydrophobicity and durability, high cost, and long construction period. The components are not properly formulated and cannot be effectively improved. Mechanical properties and compactness.
Using a combination of industrial waste residue geopolymer, bio-glue, accelerator, early strength agent and thickener, the curing agent is prepared through stirring and compaction processes to form a living gel to fill the pores of soft rock and enhance the cohesion and cohesion between particles. The denseness of the structure hinders the flow of moisture.
It significantly improves the compactness and unconfined compressive strength of embankment soft rock, reduces the permeability coefficient, enhances water stability, reduces economic losses, and provides good application potential and technical advantages.
Smart Images

Figure CN118754516A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of engineering materials, and in particular relates to a curing agent for soft rock of embankment, a preparation method and application thereof. Background Art
[0002] Because the soft rock of the embankment contains a large amount of highly hydrophilic minerals such as kaolinite, montmorillonite, and illite, it shows poor strength, strong hydrophilicity, and easy disintegration and softening under freeze-thaw cycles, dry-wet cycles, pH changes, and complex environments, which can easily cause geological disasters such as landslides and collapses. The soft rock of the embankment is prone to disintegration under natural conditions, resulting in a significant decrease in its mechanical properties. It is mainly distributed in the southwest of my country. The climate in this region is characterized by heavy rainfall, frequent rainstorms, and large fluctuations in temperature and humidity, which causes the soft rock to humidify and deform, soften and disintegrate, and absorb water and expand, posing serious safety hazards to the stability of projects such as embankments and building bases. Therefore, it is necessary to improve the soft rock of the embankment through a curing agent.
[0003] Traditional soft rock curing agents are cementitious materials and alkaline activated materials. They are widely used in the reinforcement of soft rocks because of their wide sources of preparation materials, simple methods of use and low costs. However, they have poor hydrophobicity and durability, and cannot show good mechanical properties and anti-seepage performance in the later stage. They are prone to shrinkage cracks and other shortcomings, causing large deformation and even collapse of soft rocks in embankments, resulting in huge economic losses. At present, high-efficiency modifiers are used to reinforce soft rocks, but they are expensive, have a long construction period, high construction costs, slow reaction rates, poor modification effects, and limited applicability, which are not conducive to being used as curing agents for improving soft rocks in embankments; in addition, the existing curing agent components for soft rocks are not reasonably allocated, and the effect of improving the mechanical properties and density of soft rocks is not ideal. Summary of the invention
[0004] The purpose of the embodiment of the present invention is to provide a curing agent for soft rock of embankment, so as to improve the mechanical properties of soft rock by enhancing the density of soft rock and the interaction force between particles;
[0005] The second purpose of the embodiment of the present invention is to provide a method for preparing a curing agent for soft rock of embankment;
[0006] The third purpose of the embodiment of the present invention is to provide an application of a curing agent for soft rock in embankments.
[0007] In order to solve the above technical problems, the technical solution adopted by the present invention is a curing agent for soft rock of embankment, comprising the following components: 10 to 15 parts of industrial waste geopolymer, 1 to 5 parts of bio-glue, 1 to 3 parts of accelerator, 0.5 to 1 part of early strength agent, 3 to 5 parts of thickener, and 10 to 15 parts of deionized water.
[0008] Furthermore, the industrial waste slag geopolymer specifically includes the following components: 30wt% of nano silicon dioxide, 10wt% of blast furnace slag, 20wt% of steel slag powder, 30wt% of plant ash, and 10wt% of alkali activator.
[0009] Furthermore, the bio-gum is one or more combinations of xanthan gum, carrageenan, gellan gum, and gum arabic.
[0010] Furthermore, the accelerator is a composition in which maltodextrin, calcium lignin sulfonate, montmorillonite powder and hydroxymethyl cellulose are mixed in a mass fraction ratio of (2-5): (1-3): (0.5-1): (1-2).
[0011] Furthermore, the early strength agent is a composition of calcium chloride, sodium sulfate and triethanolamine in a mass fraction ratio of (3-5): (1-3): (2-5).
[0012] Furthermore, the thickener is a composition in which maltodextrin, calcium lignin sulfonate, montmorillonite powder and hydroxymethyl cellulose are mixed in a ratio of (2-5): (1-3): (0.5-1): (1-2) by mass fraction.
[0013] The above-mentioned method for preparing the curing agent for soft rock of embankment comprises the following steps:
[0014] S1. Weigh the following parts by weight: 10-15 parts of industrial waste geopolymer, 1-5 parts of bio-glue, 1-3 parts of accelerator, 0.5-1 parts of early strength agent, 3-5 parts of thickener, and 10-15 parts of deionized water;
[0015] S2. At room temperature, the industrial waste geopolymer and bio-glue weighed in step S1 are placed in a container filled with 70% deionized water, and stirred at 200-300 r / min for 1-2 hours while maintaining the stirring temperature at 30-50° C. to obtain a viscous slurry;
[0016] S3, adding the early strength agent and accelerator washed with anhydrous ethanol to the viscous slurry of step S2 at room temperature, adjusting the speed to 500-700 r / min, adjusting the stirring temperature to 70-80° C., and stirring for 4-5 hours to obtain a curing agent mixture;
[0017] S4, adding a thickener to the curing agent mixture in step S3, and adding the remaining 30% of deionized water, adjusting the stirring temperature to 25-30° C., stirring at a stirring speed of 300-500 r / min, and continuously stirring for 1-2 hours to obtain the embankment soft rock curing agent.
[0018] The application of a curing agent for soft rock of an embankment in the construction of an embankment containing soft rock comprises the following steps:
[0019] Step 1, mechanically stir the embankment soft rock and the embankment soft rock curing agent in a mass ratio of 80: (3-5), stirring time 0.5-1h, stirring speed 100-200r / min, and stirring evenly;
[0020] Step 2, the mixture obtained in step 1 is sealed with a plastic film for 12 to 14 hours, and the curing agent of the soft rock of the embankment is added thereto again, and the mixture is mixed in a ratio of (5 to 10): 100, with a stirring time of 0.5 to 1 hour and a stirring speed of 100 to 200 r / min;
[0021] Step 3: Fill the mixed material obtained in step 2 into the area that needs to be solidified, and then compact it until the compaction degree reaches more than 95%, thereby completing the reinforcement of the soft rock of the embankment.
[0022] The beneficial effects of the present invention are
[0023] The present invention aims at the reinforcement problem of soft rock in embankments, and realizes significant improvement of the internal structure of soft rock through reasonable design of curing agent components. After the curing agent system reacts with the soft rock, an active gel phase is generated to fill the pore structure of the soft rock. This process is accompanied by a coating effect on the surface of the soil particles, which significantly enhances the cohesion between the particles. Therefore, under the action of external load stress, the relative displacement between the particles is restricted, which is manifested as an increase in the density of the soil body and an improvement in the unconfined compressive strength. At the same time, the formation of gel material constructs a relatively dense and low-permeability new structure, which effectively hinders the mobility of free water inside the soft rock, resulting in a decrease in the permeability coefficient, reducing the expansion, dissolution and other diseases caused by water, and enhancing the water stability of the structure.
[0024] The curing agent provided by the present invention strengthens the connection between soft rock particles through chemical action, reduces the pore size and connectivity, and promotes the formation of a more compact and waterproof structure. Among them, the interaction between specific functional groups (such as hydroxyl and carboxyl) in the cured product and the surface ions of soil particles further suppresses the discrete tendency of particles, enhances the bridge effect and overall bonding strength between particles, and is suitable for engineering practices such as embankment soft rock reinforcement and slope protection, showing good application potential and technical advantages. This method does not require complex construction technology, and in view of its high curing efficiency and excellent durability, it provides a practical solution to the stability problem of soft rock on embankments in complex geological and harsh climatic environments, effectively alleviating safety hazards and reducing possible economic losses. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0026] Figure 1 This is the SEM morphology of the soft rock of the embankment without the addition of curing agent;
[0027] Figure 2 This is the scanning electron microscope morphology of the soft rock of the embankment with 3% curing agent added in Example 6;
[0028] Figure 3 is a graph showing the conductivity change of soft rock in the embankment at different dosages of the curing agent in Example 6;
[0029] Figure 4 is the total amount of dissolved solids in the soft rock of the embankment at different dosages of the curing agent in Example 6;
[0030] Figure 5 is the pH of the soft rock of the embankment at different dosages of the curing agent in Example 6;
[0031] Figure 6 is the splitting tensile strength of the soft rock of the embankment at different dosages of the curing agent in Example 6;
[0032] Figure 7 is the unconfined compressive strength of the soft rock of the embankment at different dosages of the curing agent in Example 6;
[0033] Figure 8 is the permeability coefficient of the soft rock of the embankment at different dosages of the curing agent in Example 6. DETAILED DESCRIPTION
[0034] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0035] The curing agent for the soft rock of the embankment provided in this embodiment is proportioned according to the following weight parts: 10-15 parts of industrial waste slag geopolymer, 1-5 parts of biological glue, 1-3 parts of accelerator, 0.5-1 parts of early strength agent, 3-5 parts of thickener, and 10-15 parts of deionized water; in some possible embodiments, the industrial waste slag geopolymer specifically includes the following components: 30wt% nano-silicon dioxide, 10wt% blast furnace slag, 20wt% steel slag powder, 30wt% plant ash, and 10wt% alkali activator. This embodiment utilizes the hydroxyl and carboxyl groups in the biological glue to hydrogen bond and bridge with the cations on the soft rock particles, change the charged properties between the particles, and increase the degree of polymerization between the soil particles; the aluminosilicate contained in the industrial waste slag geopolymer undergoes a condensation reaction and a hydration reaction with the silicon oxide contained in the soft rock to generate an aluminum silica gel with a three-dimensional grid structure. This part of the proportion is determined by theoretical calculation and field tests, and is verified by combining specific engineering application cases. The proper amount of each component added plays an important role in improving the cementing material. When the amount of alkali activator added is too much or too little, the strength and degree of crystallization of the silicate gel material formed will decrease.
[0036] In some specific embodiments, the bio-gum is at least one of xanthan gum, carrageenan, gellan gum, and gum arabic;
[0037] In some possible implementations, the accelerator is specifically composed of maltodextrin, calcium lignin sulfonate, montmorillonite powder, and hydroxymethyl cellulose in a mass fraction ratio of (2-5): (1-3): (0.5-1): (1-2). The hydrophilic groups contained in the components of the accelerator of this implementation change the activity of the interface on which it acts, thereby changing the bonding ability of the molecular chain, and the curing performance shows an increasing trend.
[0038] In some possible implementations, the early strength agent is specifically composed of calcium chloride, sodium sulfate, and triethanolamine in a mass fraction ratio of (3-5): (1-3): (2-5). Calcium chloride and sodium sulfate react with soft rock to generate a water-insoluble hydrated aluminate, which changes the relative concentration of ions, inhibits the diffusion of double electric layers between particles, accelerates the improvement of the strength of the cementing material and promotes its early hardening.
[0039] In some possible embodiments, the thickener includes maltodextrin, calcium lignin sulfonate, montmorillonite powder, and hydroxymethyl cellulose in a ratio of (2-5): (1-3): (0.5-1): (1-2) by mass fraction. A large number of carboxyl groups and hydrophobic molecular groups inside the components of the thickener of this embodiment increase the interaction of polar groups inside the structure, hinder the mutual movement between particles, and thus improve the bonding degree of the reaction substances.
[0040] Example 1
[0041] A method for preparing a soft rock curing agent for embankment, which is specifically carried out according to the following steps:
[0042] S1. Weigh the following parts by weight: 12.5 parts of industrial waste geopolymer, 2.5 parts of bio-glue, 2 parts of accelerator, 0.75 parts of early strength agent, 4 parts of thickener, and 12.5 parts of deionized water;
[0043] S2. At room temperature, the weighed industrial waste geopolymer and bio-glue were put into a container filled with 70% deionized water, stirred at 250 r / min, and the stirring temperature was kept at 40° C. The stirring was continued for 1.5 h to obtain a viscous slurry;
[0044] S3. At room temperature, add the early strength agent and accelerator washed with anhydrous ethanol to the viscous slurry obtained in step S2, and adjust the speed to 600 r / min, the stirring temperature to 75° C., and the stirring time to 4.5 h to obtain a curing agent mixture;
[0045] S4. Add a thickener to the curing agent mixture in step S3, and add the remaining 30% of deionized water, adjust the stirring temperature to 27.5° C., and continue stirring for 1 hour at a stirring speed of 400 r / min to obtain the embankment soft rock curing agent.
[0046] A method for using a curing agent for soft rock of embankment, specifically according to the following steps:
[0047] S5. Mechanically stir the embankment soft rock and curing agent in a ratio of 80:4, with a stirring time of 0.75 h and a stirring speed of 150 r / min, and stir evenly;
[0048] S6, sealing the mixture obtained in S5 with a plastic film for 13 hours, adding a curing agent thereto again, and mixing at a ratio of 7.5:100, with a stirring time of 0.75 hours and a stirring speed of 150 r / min;
[0049] S7, filling the mixed material obtained in S6 into the area to be solidified, and then compacting it. When the compaction degree reaches more than 95%, the reinforcement of the soft rock of the embankment is completed.
[0050] Example 2
[0051] S1. Weigh the following weight fractions: 10 parts of industrial waste geopolymer, 1 part of bio-glue, 1 part of accelerator, 0.5 parts of early strength agent, 3 parts of thickener, and 10 parts of deionized water;
[0052] S2. At room temperature, the weighed industrial waste geopolymer and bio-glue were put into a container filled with 70% deionized water, stirred at 200 r / min, and the stirring temperature was kept at 30° C. The stirring was continued for 1 hour to obtain a viscous slurry;
[0053] S3. At room temperature, add the early strength agent and accelerator washed with anhydrous ethanol to the viscous slurry obtained in step S2, and adjust the speed to 500 r / min, the stirring temperature to 70° C., and the stirring time to 4 h to obtain a curing agent mixture;
[0054] S4, adding a thickener to the curing agent mixture in step S3, and adding the remaining 30% of deionized water, adjusting the stirring temperature to 25° C., stirring at a stirring speed of 300 r / min, and continuously stirring for 1 hour to obtain the embankment soft rock curing agent;
[0055] S5. Mechanically stir the embankment soft rock and the curing agent in a mass ratio of 80:3, with a stirring time of 0.5 h and a stirring speed of 100 r / min, and stir evenly;
[0056] S6, sealing the mixture obtained in S5 with a plastic film for 12 hours, adding a curing agent thereto again, and mixing at a ratio of 5:100, with a stirring time of 0.5 hours and a stirring speed of 100 r / min;
[0057] S7, filling the mixed material obtained in S6 into the area to be solidified, and then compacting it, and the compaction degree reaches more than 95%, thus completing the reinforcement of the soft rock of the embankment.
[0058] Example 3
[0059] S1. Weigh the following parts by weight: 15 parts of industrial waste geopolymer, 5 parts of bio-glue, 3 parts of accelerator, 1 part of early strength agent, 5 parts of thickener, and 15 parts of deionized water;
[0060] S2. At room temperature, the weighed industrial waste geopolymer and bio-glue were put into a container filled with 70% deionized water, stirred at 300 r / min, and the stirring temperature was kept at 50° C. The stirring was continued for 2 h to obtain a viscous slurry;
[0061] S3. At room temperature, add the early strength agent and accelerator washed with anhydrous ethanol to the viscous slurry obtained in step S2, and adjust the speed to 700 r / min, the stirring temperature to 80° C., and the stirring time to 5 h to obtain a curing agent mixture;
[0062] S4, adding a thickener to the curing agent mixture in step S3, and adding the remaining 30% of deionized water, adjusting the stirring temperature to 30° C., stirring at a stirring speed of 500 r / min, and continuously stirring for 2 hours to obtain the embankment soft rock curing agent;
[0063] S5. Mechanically stir the embankment soft rock and the curing agent in a mass ratio of 80:5 for 1 hour at a stirring speed of 200 r / min until they are evenly stirred;
[0064] S6, sealing the mixture obtained in S5 with a plastic film for 14 hours, adding a curing agent thereto again, and mixing at a ratio of 10:100, stirring for 1 hour at a stirring speed of 200 r / min;
[0065] S7, filling the mixed material obtained in S6 into the area to be solidified, and then compacting it, and the compaction degree reaches more than 95%, thus completing the reinforcement of the soft rock of the embankment.
[0066] Example 4
[0067] The following weight fractions are weighed in S1: 14 parts of industrial waste geopolymer, 2 parts of bio-glue, 2 parts of accelerator, 1 part of early strength agent, 3 parts of thickener, and 11 parts of deionized water; the rest are the same as in Example 1.
[0068] Example 5
[0069] The following weight fractions are weighed in S1: 13 parts of industrial waste geopolymer, 3 parts of bio-glue, 1 part of accelerator, 0.5 parts of early strength agent, 4 parts of thickener, and 12 parts of deionized water; the rest are the same as in Example 1.
[0070] Example 6
[0071] The following weight fractions are weighed in S1: 13 parts of industrial waste geopolymer, 4 parts of bio-glue, 2 parts of accelerator, 1 part of early strength agent, 4 parts of thickener, and 13 parts of deionized water; the rest are the same as in Example 1.
[0072] Embodiment 7,
[0073] The following weight fractions are weighed in S1: 12 parts of industrial waste geopolymer, 5 parts of bio-glue, 2 parts of accelerator, 0.5 parts of early strength agent, 4 parts of thickener, and 14 parts of deionized water; the rest are the same as in Example 1.
[0074] Embodiment 8,
[0075] The following weight fractions are weighed in S1: 11 parts of industrial waste geopolymer, 2 parts of bio-glue, 1 part of accelerator, 0.5 parts of early strength agent, 5 parts of thickener, and 15 parts of deionized water; the rest are the same as in Example 1.
[0076] Embodiment 9,
[0077] The following weight fractions are weighed in S1: 11 parts of industrial waste geopolymer, 3 parts of bio-glue, 1 part of accelerator, 0.5 parts of early strength agent, 5 parts of thickener, and 15 parts of deionized water; the rest are the same as in Example 1.
[0078] Embodiment 10,
[0079] The following weight fractions are weighed in S1: 14 parts of industrial waste geopolymer, 1 part of bio-glue, 1 part of accelerator, 0.5 parts of early strength agent, 3 parts of thickener, and 15 parts of deionized water; the rest are the same as in Example 1.
[0080] Embodiment 11,
[0081] The following weight fractions are weighed in S1: 14 parts of industrial waste geopolymer, 2 parts of bio-glue, 1 part of accelerator, 0.5 parts of early strength agent, 3 parts of thickener, and 14 parts of deionized water; the rest are the same as in Example 1.
[0082] Embodiment 12,
[0083] The following weight fractions are weighed in S1: 13 parts of industrial waste geopolymer, 1 part of bio-glue, 3 parts of accelerator, 0.5 parts of early strength agent, 4 parts of thickener, and 15 parts of deionized water; the rest are the same as in Example 1.
[0084] Embodiment 13,
[0085] The following weight fractions are weighed in S1: 13 parts of industrial waste geopolymer, 1 part of bio-glue, 2 parts of accelerator, 0.5 parts of early strength agent, 4 parts of thickener, and 10 parts of deionized water; the rest are the same as in Example 1.
[0086] Embodiment 14,
[0087] The following weight fractions are weighed in S1: 11 parts of industrial waste geopolymer, 3 parts of bio-glue, 1 part of accelerator, 1 part of early strength agent, 4 parts of thickener, and 12.5 parts of deionized water; the rest are the same as in Example 1.
[0088] Embodiment 15,
[0089] The following weight fractions are weighed in S1: 12.5 parts of industrial waste geopolymer, 1 part of bio-glue, 1 part of accelerator, 0.5 parts of early strength agent, 5 parts of thickener, and 14 parts of deionized water; the rest are the same as in Example 1.
[0090] Embodiment 16,
[0091] The following weight fractions are weighed in S1: 15 parts of industrial waste geopolymer, 4 parts of bio-glue, 1 part of accelerator, 0.5 parts of early strength agent, 3 parts of thickener, and 12.5 parts of deionized water; the rest are the same as in Example 1.
[0092] Embodiment 17,
[0093] The following weight fractions are weighed in S1: 15 parts of industrial waste geopolymer, 2 parts of bio-glue, 3 parts of accelerator, 0.75 parts of early strength agent, 5 parts of thickener, and 15 parts of deionized water; the rest are the same as in Example 1.
[0094] Embodiment 18,
[0095] The following weight fractions are weighed in S1: 10 parts of industrial waste geopolymer, 1 part of bio-glue, 1 part of accelerator, 0.75 parts of early strength agent, 3 parts of thickener, and 10 parts of deionized water; the rest are the same as in Example 1.
[0096] Embodiment 19,
[0097] The following weight fractions are weighed in S1: 15 parts of industrial waste geopolymer, 1 part of bio-glue, 2 parts of accelerator, 1 part of early strength agent, 5 parts of thickener, and 10 parts of deionized water; the rest are the same as in Example 1.
[0098] Embodiment 20,
[0099] The following weight fractions are weighed in S1: 12.5 parts of industrial waste geopolymer, 3 parts of bio-glue, 1 part of accelerator, 1 part of early strength agent, 5 parts of thickener, and 12.5 parts of deionized water; the rest are the same as in Example 1.
[0100] Comparative Example 1
[0101] No curing agent is used to solidify the soft rock of the embankment.
[0102] Comparative Example 2
[0103] No bio-glue was added to S1, and the rest was the same as in Example 9.
[0104] Comparative Example 3
[0105] No early strength agent was added to S1, and the rest was the same as in Example 9.
[0106] Comparative Example 4
[0107] No thickener was added to S1, and the rest was the same as in Example 9.
[0108] Comparative Example 5
[0109] Commonly used soft rock curing agents on the market1.
[0110] Comparative Example 6
[0111] Commonly used soft rock curing agents on the market 2.
[0112] Mechanical properties tests and permeability tests were performed on Examples 1-20 and Comparative Examples 1-4, and the test results are shown in Table 1.
[0113] Table 1 Performance test table of soft rock reinforced embankment with curing agent
[0114]
[0115] The data in Table 1 are as follows: the splitting tensile strength of Example 4 is 1065 kPa, the unconfined compressive strength is 2011 kPa, and the permeability coefficient is 4.35×10 -7 m / s, compared with the comparative example 1 without adding the curing agent, the splitting tensile strength is increased by 157%, the unconfined compressive strength is increased by 293%, and the permeability coefficient is reduced by 83%; it can be seen that after adding the curing agent of this embodiment, the mechanical properties of the soft rock of the embankment are significantly improved, and the permeability coefficient is greatly reduced.
[0116] It can be found from the data of Examples 1-20 and Comparative Examples 1-6 in Table 1 that the use of the curing agent in the present invention can effectively improve the mechanical properties and hydrophobic properties of the soft rock of the embankment. Figure 1 , Figure 2 , the terrestrial soft rock components to which the curing agent of this embodiment is added are more likely to be cemented, the microstructure is denser, the pore filling degree is higher, the cohesive body inside the structure is more uniform and dense, and it exhibits higher mechanical properties and better hydrophobic properties on a macro scale. The contact between particles is mostly face-to-face contact, which has a certain resistance to external rainwater infiltration; while a large number of pores appear on the surface of the sample without adding the curing agent, and the contact between particles is mostly point contact, which provides a channel for external rainwater infiltration. When the amount of early strength agent added is too much, the degree and speed of the combination of the cementitious material and the soft rock particles are hindered, and the strength and hydrophobic performance are not significantly improved. Adding too much thickener slows down the curing of soft rock cracks because it contains a large number of hydroxyl groups and polar molecules, hinders the overlap between particles, and reduces the pore filling rate of particles.
[0117] Figures 3 to 8 The effects of different curing agent dosages on the performance of soft rock in embankment are demonstrated. Figure 3 It is revealed that the introduction of curing agent leads to a decreasing trend of the conductivity of soft rock. This phenomenon can be attributed to the gel generated by the curing agent reaction, which effectively blocks the ion transmission channel, thereby inhibiting the movement of ions and reducing the conductivity. Figure 4 The data in show that as the amount of curing agent added increases, the total amount of dissolved solids in soft rock decreases. This effect comes from the stronger connection between particles promoted by the curing agent. This process reduces the pore volume and number, forms a denser structure, and indirectly reduces the content of soluble matter. Regarding pH changes, Figure 5It shows that the pH value of soft rock and soil decreases with the increase of curing agent dosage. The fundamental reason is that the gel material generated by the curing reaction strengthens the connection between particles, reduces the dispersion of the soil, and causes the pH value to shift to a lower value. In terms of mechanical properties, Figure 6 and Figure 7 The splitting tensile strength and unconfined compressive strength show a trend of increasing with the increase of curing agent dosage. Specifically, the curing agent directly improves the tensile strength of soft rock by enhancing the bonding force between particles and effectively inhibiting the deformation and displacement of particles; at the same time, the filling and compaction of the gel body causes large pores to transform into small pores or even close, significantly improving the unconfined compressive strength. Figure 8 This shows that the permeability coefficient decreases with the increase of the curing agent dosage, which is consistent with the above results, that is, the increase of gel effectively blocks the internal water flow path, reduces the possibility of water migration, and thus reduces the permeability coefficient. In summary, the reasonable addition of the curing agent in this embodiment can not only improve the microstructure of soft rock through physical and chemical effects, reduce ion migration and soluble solid content, but also significantly enhance its mechanical stability and reduce permeability, providing a powerful performance improvement method for the engineering application of soft rock materials.
[0118] Each embodiment in this specification is described in a related manner, and the same or similar parts between the embodiments can be referred to each other, and each embodiment focuses on the differences from other embodiments. In particular, for the system embodiment, since it is basically similar to the method embodiment, the description is relatively simple, and the relevant parts can be referred to the partial description of the method embodiment.
[0119] The above description is only a preferred embodiment of the present invention and is not intended to limit the protection scope of the present invention. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention are included in the protection scope of the present invention.
Claims
1. A curing agent for soft rock of embankment, characterized in that: The invention comprises the following components: 10-15 parts of industrial waste residue geopolymer, 1-5 parts of biological glue, 1-3 parts of accelerator, 0.5-1 parts of early strength agent, 3-5 parts of thickener and 10-15 parts of deionized water.
2. A curing agent for soft rock of embankment according to claim 1, characterized in that: The industrial waste slag geopolymer specifically comprises the following components: 30 wt% of nano silicon dioxide, 10 wt% of blast furnace slag, 20 wt% of steel slag powder, 30 wt% of plant ash, and 10 wt% of alkali activator.
3. The curing agent for soft rock of embankment according to claim 1, characterized in that: The biological gum is one or more combinations of xanthan gum, carrageenan, gellan gum and gum arabic.
4. The curing agent for soft rock of embankment according to claim 1, characterized in that: The accelerator is a composition in which maltodextrin, calcium lignin sulfonate, montmorillonite powder and hydroxymethyl cellulose are mixed in a mass fraction ratio of (2-5): (1-3): (0.5-1): (1-2).
5. The curing agent for soft rock of embankment according to claim 1, characterized in that: The early strength agent is a composition prepared by mixing calcium chloride, sodium sulfate and triethanolamine in a mass fraction ratio of (3-5): (1-3): (2-5).
6. The curing agent for soft rock of embankment according to claim 1, characterized in that: The thickener is a composition in which maltodextrin, calcium lignin sulfonate, montmorillonite powder and hydroxymethyl cellulose are mixed in a mass fraction ratio of (2-5): (1-3): (0.5-1): (1-2).
7. A method for preparing a curing agent for soft rock of embankment according to any one of claims 1 to 6, characterized in that: The following steps are involved: S1. Weigh the following parts by weight: 10-15 parts of industrial waste geopolymer, 1-5 parts of bio-glue, 1-3 parts of accelerator, 0.5-1 parts of early strength agent, 3-5 parts of thickener, and 10-15 parts of deionized water; S2. At room temperature, the industrial waste geopolymer and bio-glue weighed in step S1 are placed in a container filled with 70% deionized water, and stirred at 200-300 r / min for 1-2 hours while maintaining the stirring temperature at 30-50° C. to obtain a viscous slurry; S3, adding the early strength agent and accelerator washed with anhydrous ethanol to the viscous slurry of step S2 at room temperature, adjusting the speed to 500-700 r / min, adjusting the stirring temperature to 70-80° C., and stirring for 4-5 hours to obtain a curing agent mixture; S4, adding a thickener to the curing agent mixture in step S3, and adding the remaining 30% of deionized water, adjusting the stirring temperature to 25-30° C., stirring at a stirring speed of 300-500 r / min, and continuously stirring for 1-2 hours to obtain the embankment soft rock curing agent.
8. Use of a curing agent for soft rock of embankment as claimed in any one of claims 1 to 6 in the construction of embankment containing soft rock, characterized in that: The following steps are involved: Step 1, mechanically stir the embankment soft rock and the embankment soft rock curing agent in a mass ratio of 80: (3-5), stirring time 0.5-1h, stirring speed 100-200r / min, and stirring evenly; Step 2, the mixture obtained in step 1 is sealed with a plastic film for 12 to 14 hours, and the curing agent of the soft rock of the embankment is added thereto again, and the mixture is mixed in a ratio of (5 to 10): 100, with a stirring time of 0.5 to 1 hour and a stirring speed of 100 to 200 r / min; Step 3: Fill the mixed material obtained in step 2 into the area that needs to be solidified, and then compact it until the compaction degree reaches more than 95%, thereby completing the reinforcement of the soft rock of the embankment.
Citation Information
Patent Citations
Nano-fiber curing agent for disintegrating carbonaceous mudstone as well as preparation and use methods thereof
CN112250390A
Soft rock disintegrating soil modifier, preparation method thereof and soft rock disintegrating soil improvement method