Low-gas-content large-flow-state durable concrete and preparation method thereof

By optimizing the composition of concrete materials and water-reducing agent formulas, we designed durable concrete with low air content and high fluidity, which solved the problem of high air content affecting mechanical properties and appearance, and improved the appearance quality of concrete without sacrificing durability. Meet demanding engineering application requirements.

CN118754564APending Publication Date: 2024-10-11CCCC SECOND HARBOR ENGINEERING CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410968330.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-18
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

When improving the durability of existing concrete, it is easy to cause high air content, which affects the mechanical properties and appearance quality. Especially in precast concrete products, it is difficult to improve the appearance problem without sacrificing durability.

Method used

By optimizing the composition of concrete materials and water-reducing agent formulas, we design durable concrete with low air content and high fluidity, combine it with retarded polycarboxylic acid high-efficiency water-reducing agent, air-entraining agent and defoaming agent, and adjust the amount of materials and slurry. Ensure the durability and appearance quality of concrete.

Benefits of technology

It can improve the appearance quality and mechanical properties of concrete without reducing durability, meet more stringent engineering application requirements, and have good impermeability, frost resistance and aesthetics.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118754564A_ABST
    Figure CN118754564A_ABST
Patent Text Reader

Abstract

The invention discloses low-gas-content large-flow-state durable concrete and a preparation method thereof, and belongs to the technical field of concrete. The low-gas-content large-flow-state durable concrete is mainly prepared from the following raw materials in parts by mass: 450 to 473 parts of P.O52.5 cement, 677 to 720 parts of II-zone medium sand, 1127 to 1157 parts of gravel, 152 to 156 parts of water and 5.850 to 6.419 parts of a retarding type polycarboxylic acid high-efficiency water reducing agent. According to the invention, concrete composition materials are optimized, and on the premise of ensuring good aesthetics and fluidity, defoaming and air entraining components in a water reducer formula are adjusted, so that when the air content is not greater than 2%, the impermeability reaches P10 or more, the relative dynamic elastic modulus of freezing resistance F300 reaches 60% or more, the freezing resistance mass loss is not greater than 5%, and the anti-freezing property is excellent. The chloride ion diffusion coefficient is less than 7 * 10 <-12 > m < 2 > / s, and the 56d electric flux is not more than 1000C.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of concrete, and in particular to low-air-containing, high-fluidity, durable concrete and a preparation method thereof. Background Art

[0002] As a building material widely used in buildings and engineering structures, concrete must meet a variety of performance requirements, among which durability is the key factor in determining its service life and maintaining structural integrity. Durability includes the permeability of concrete to environmental factors such as water, salt, and chemicals, as well as its resistance to freeze-thaw cycles. In order to ensure that concrete has good durability when the environmental category and action level are Ⅱ-C, a certain amount of air content is usually introduced into concrete to improve its impermeability and frost resistance.

[0003] In the traditional concrete preparation process, in order to improve durability, air is often introduced by adding air-entraining agents to form small and dispersed pores, which can provide space to release freezing pressure and avoid internal damage caused by freeze-thaw cycles. When concrete with a high air content is subjected to freeze-thaw cycles, the bubbles formed inside can serve as a refuge for unfrozen water, reducing material expansion and damage caused by ice crystal formation. At the same time, these pores can also block the penetration channels of water and harmful chemicals to a certain extent, thereby improving the concrete's impermeability and chemical corrosion resistance.

[0004] However, when the air content in concrete exceeds 3.0%, it will not only have a negative impact on its mechanical properties, but also form a large number of bubbles on the surface and inside of the concrete, and even cause honeycomb phenomenon, which seriously damages the appearance quality of the concrete. Especially in the production of precast concrete products such as precast beams, the smoothness and consistency of the appearance are one of the important criteria for evaluating product quality. The bubbles and pitting caused by high air content not only reduce the aesthetics, but also may become a potential weakness, affecting the bearing capacity and durability of the structure.

[0005] To solve these problems, the industry has made a variety of attempts. For example, some methods suggest the use of chemical additives, such as defoamers, to reduce unwanted bubbles. However, this approach often requires fine dosage control and may affect the workability of the concrete. In addition, some high-performance concretes reduce the required water and air content by optimizing particle grading and using high-performance cement, but the cost is relatively high and has higher requirements for the selection of raw materials and construction technology.

[0006] Therefore, although there are many methods to improve the durability of concrete in the prior art, they often ignore the appearance quality of concrete. Especially for precast concrete components, how to improve the appearance of concrete without sacrificing durability is still a challenge faced by technical personnel in this field. Summary of the invention

[0007] In order to solve the problem of concrete appearance without reducing the durability of concrete (durability is reflected by conventional indicators such as impermeability, chloride ion content, electrical flux, and frost resistance), the present invention provides a low-air-content, high-fluidity durable concrete and a preparation method thereof, which not only meets various technical indicators of durability, but also ensures good appearance quality to meet more stringent engineering application requirements.

[0008] The low-air-containing, high-fluidity durable concrete is mainly composed of the following raw materials, calculated by weight: 450-473 parts of P·O52.5 cement, 677-720 parts of zone II medium sand, 1127-1157 parts of crushed stone, 152-156 parts of water, and 5.850-6.419 parts of slow-setting polycarboxylic acid high-efficiency water-reducing agent.

[0009] Preferably, the low-air-content, high-fluidity, durable concrete is mainly composed of the following raw materials, calculated by weight: 456-470 parts of P·O52.5 cement, 679-720 parts of zone II medium sand, 1127-1157 parts of crushed stone, 155 parts of groundwater, and 5.928-6.110 parts of slow-setting polycarboxylic acid high-efficiency water reducer.

[0010] Preferably, the low-air-content, high-fluidity, durable concrete is mainly composed of the following raw materials, calculated by weight: 456-470 parts of P·O52.5 cement, 679-720 parts of zone II medium sand, 282-289 parts of 5-10 mm crushed stone, 845-868 parts of 10-20 mm crushed stone, 155 parts of groundwater, and 5.928-6.110 parts of slow-setting polycarboxylic acid high-efficiency water reducer.

[0011] Preferably, the alkali content in the P·O52.5 cement is ≤0.6%, the C3A content in the clinker is ≤8.0%, and the other technical requirements comply with the provisions of GB 175.

[0012] Preferably, the sand in zone II is hard and clean natural river sand.

[0013] Preferably, the fineness of the sand in zone II is 2.6-3.0, the mud content is 1.5%-2.5%, the mud content is ≤0.5%, and the other technical requirements comply with the provisions of JTG / T 3650.

[0014] Preferably, the porosity of the crushed stone is less than 40%, the crushing index is less than 20%, the ratio of the compressive strength of the parent rock to the design strength of the concrete is ≥1.5, the mud content is ≤1.0%, the mud block content is ≤0.5%, the needle-like particle content is less than 10%, and the other technical requirements are in accordance with the provisions of JTG / T 3650.

[0015] Preferably, the particle size of the crushed stone is 5 to 20 mm.

[0016] More preferably, the crushed stone is composed of crushed stone with a particle size of 5 to 10 mm and crushed stone with a particle size of 10 to 20 mm mixed in a mass ratio of 0.30 to 0.35:1.

[0017] More preferably, the crushed stone is composed of a mixture of crushed stone with a particle size of 5 to 10 mm and crushed stone with a particle size of 10 to 20 mm in a mass ratio of 0.32 to 0.34:1.

[0018] Preferably, the water is groundwater, and its performance indicators comply with the provisions of JGJ 63.

[0019] Preferably, the performance indexes of the slow-setting polycarboxylic acid high-efficiency water reducer meet the requirements of GB 8076.

[0020] Preferably, the low-air-content, high-fluidity, durable concrete further comprises an air-entraining agent and a defoaming agent.

[0021] More preferably, the amount of the defoamer added is 0.025% to 0.05% wt of the amount of the slow-setting polycarboxylic acid high-efficiency water-reducing agent added, and the amount of the air-entraining agent added is 0.05% to 0.075% wt of the amount of the slow-setting polycarboxylic acid high-efficiency water-reducing agent added.

[0022] More preferably, the amount of the defoamer added is 0.05%wt of the amount of the slow-setting polycarboxylic acid high-efficiency water-reducing agent added, and the amount of the air-entraining agent added is 0.05%wt of the amount of the slow-setting polycarboxylic acid high-efficiency water-reducing agent added.

[0023] More preferably, the air entraining agent is a TSC560 ether-based air entraining agent, and the defoaming agent is a TSC1200 polyether-based defoaming agent.

[0024] Preferably, the pore size of the bubbles in the air-containing high-flow durable concrete is 20 to 300 μm.

[0025] More preferably, the pore size of the bubbles in the air-containing high-flow durable concrete is 50-100 μm.

[0026] Preferably, the air content of the low-air-content, high-fluidity, durable concrete is 1.0% to 2.0%.

[0027] More preferably, the air content of the low-air-content, high-fluidity, durable concrete is 1.3% to 1.8%.

[0028] The method for preparing the low-air-containing, high-fluidity, durable concrete comprises the following steps:

[0029] The crushed stone, the medium sand in zone II and the P·O52.5 cement are uniformly mixed according to the designed mass fraction to obtain a solid mixture; the slow-setting polycarboxylic acid high-efficiency water-reducing agent and water are uniformly mixed according to the designed mass fraction and then added to the solid mixture, and the mixture is uniformly mixed; and the low-air-containing, high-fluidity durable concrete is obtained through construction pouring, curing and curing.

[0030] Compared with the prior art, the beneficial effects of the present invention are:

[0031] 1. The present invention adopts the idea of ​​concrete mix design volume method to design low-air-containing, high-fluidity durable concrete mix to solve two technical problems: the first is the selection of sandstone materials and cement and other solid materials; the second is the adjustment of water reducer formula and dosage change. Under the premise of meeting various working properties and physical appearance quality of concrete, its durability is ensured not to be affected.

[0032] 2. The low-air-containing, high-flowability, durable concrete provided by the present invention has good working performance, good mechanical properties, good volume stability, good durability, and more importantly, good appearance performance. By optimizing concrete materials, using the cement concrete volume method mix ratio design idea, adjusting the water-reducing agent formula, and verifying its durability through hardening concrete, the test results meet the requirements.

[0033] 3. The present invention optimizes the concrete composition materials and adjusts the defoaming and air entraining components in the water reducing agent formula to achieve an air content of no more than 2%, an impermeability of more than P10, a relative dynamic elastic modulus of frost resistance F300 of more than 60%, a frost resistance mass loss of no more than 5%, and a chloride ion diffusion coefficient of less than 7×10 -12 m 2 / s, 56d electric flux is not greater than 1000C. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1 This is a diagram of bucket specimens prepared in Examples 1 to 6 of the present invention.

[0035] Figure 2 Diagram of a prefabricated T-beam prepared with low-air-content, high-fluidity, durable concrete in Example 6 of the present invention. DETAILED DESCRIPTION

[0036] The technical scheme of the present invention is further described below by way of examples. The raw materials used in the examples can be purchased from the market or prepared by conventional methods.

[0037] The various performance indicators of the materials used are as follows:

[0038] P·O52.5 cement: ordinary silicate cement or silicate cement with stable quality, alkali content not more than 0.6%, C3A content in clinker not more than 8.0%, density 3120kg / m 3 , and the rest of the technical requirements shall comply with the provisions of GB 175-2023 "General Portland Cement".

[0039] Medium sand in zone II: As fine aggregate, hard and clean natural river sand is used, with a fineness of 2.6-3.0, a mud content of 2.3%, a mud content of no more than 0.5%, and an apparent density of 2676kg / m 3 , and the other technical requirements comply with the provisions of JTG / T 3650-2020 "Technical Specifications for Highway Bridge and Culvert Construction".

[0040] Crushed stone: As coarse aggregate, hard and durable crushed stone is used, with a porosity of less than 40%, a crushing index of less than 20%, a ratio of the compressive strength of the coarse aggregate parent rock to the design strength of concrete of not less than 1.5, a mud content of not more than 1.0%, a mud block content of not more than 0.5%, a needle-like particle content of less than 10%, a particle size of 5-20mm continuous grading, composed of 5-10mm single particle grade and 10-20mm single particle grade two grades of materials in a ratio of 25%:75%, and an apparent density of 2718kg / m 3 , and the rest of the technical requirements are in compliance with the provisions of JTG / T 3650-2020 "Technical Specifications for Highway Bridge and Culvert Construction".

[0041] Water: Groundwater. After testing for pH value, insoluble matter, soluble matter, chloride, sulfate, alkali content and other indicators, the results are in compliance with the requirements of JGJ 63-2006 "Standard for Water for Concrete".

[0042] Slow-setting polycarboxylic acid high-efficiency water reducer: It has good compatibility with cementitious materials, and its performance indicators meet the requirements of GB 8076-2008 "Concrete Admixtures".

[0043] When the volume method in JGJ 55-2011 "Ordinary Concrete Mix Design Code" is used to design the mix proportion of low-air-containing, high-flowing, durable concrete, the following formula is used for calculation:

[0044]

[0045] In the formula, m c0 To calculate the amount of cement per cubic meter of concrete (kg / m 3 );

[0046] m f0 To calculate the amount of mineral admixture per cubic meter of concrete (kg / m 3 );

[0047] mg0 To calculate the amount of coarse aggregate per cubic meter of concrete (kg / m 3 );

[0048] m s0 To calculate the amount of fine aggregate per cubic meter of concrete (kg / m 3 );

[0049] m w0 To calculate the water consumption per cubic meter of concrete (kg / m 3 );

[0050] ρ c is the cement density (kg / m 3 );

[0051] ρ f is the density of mineral admixture (kg / m 3 );

[0052] ρ g is the apparent density of coarse aggregate (kg / m 3 );

[0053] ρ s is the apparent density of fine aggregate (kg / m 3 );

[0054] ρ w is the density of water (kg / m 3 ).

[0055] When α=1.5, the amounts of various materials used in the mix ratios of Examples 1 to 6 of the present invention are calculated.

[0056] Example 1

[0057] A low-gas, high-flow, durable concrete, which is composed of the following raw materials according to the amount of raw materials per cubic meter of concrete: P·O52.5 cement 456kg / m 3 ; Medium sand in zone II: 702kg / m 3 ; 5-10mm crushed stone 286kg / m 3 ; 10~20mm crushed stone 860kg / m 3 , water 155kg / m 3 ; Slow-setting polycarboxylic acid high-efficiency water reducer 5.928kg / m 3 .

[0058] The method for preparing the low-air-containing, high-fluidity, durable concrete comprises the following steps:

[0059] Crushed stone, medium sand in zone II and P·O52.5 cement are weighed according to the designed mass, put into a mixing pot and stirred evenly to obtain a solid mixture; slow-setting polycarboxylic acid high-efficiency water reducer and water are weighed according to the designed mass, mixed evenly and added to the solid mixture, stirred for 120 seconds, stirred evenly, and the low-air-containing, high-flowability durable concrete is obtained through construction pouring, curing and maintenance.

[0060] Example 2

[0061] A low-gas-containing, high-flowability, durable concrete, which is composed of the following raw materials according to the amount of raw materials used per cubic meter of concrete: P·O52.5 cement 461kg / m 3 ; Medium sand in zone II: 704kg / m 3 ; 5-10mm crushed stone 287kg / m 3 ; 10~20mm crushed stone 861kg / m 3 , water 152kg / m 3 ; Slow-setting polycarboxylic acid high-efficiency water reducer 5.993kg / m 3 .

[0062] The method for preparing the low-air-containing, high-fluidity, durable concrete comprises the following steps:

[0063] Crushed stone, zone II medium sand and P·O52.5 cement are weighed according to the designed mass, put into a mixing pot and stirred evenly to obtain a solid mixture; slow-setting polycarboxylic acid high-efficiency water reducer and water are weighed according to the designed mass, mixed evenly and added to the solid mixture, stirred for 120 seconds, stirred evenly, and the low-air-containing, high-flowability durable concrete is obtained through construction pouring, curing and maintenance.

[0064] Example 3

[0065] A low-gas, high-flow, durable concrete, which consists of the following raw materials, according to the amount of raw materials per cubic meter of concrete: P·O52.5 cement 473kg / m 3 ; Medium sand in zone II: 677kg / m 3 ; 5-10mm crushed stone 288kg / m 3 ; 10~20mm crushed stone 865kg / m 3 , water 156kg / m 3 ; Slow-setting polycarboxylic acid high-efficiency water reducer 6.419kg / m 3 .

[0066] The method for preparing the low-air-containing, high-fluidity, durable concrete comprises the following steps:

[0067] Crushed stone, medium sand in zone II and P·O52.5 cement are weighed according to the designed mass, put into a mixing pot and stirred evenly to obtain a solid mixture; slow-setting polycarboxylic acid high-efficiency water reducer and water are weighed according to the designed mass, mixed evenly and added to the solid mixture, stirred for 120 seconds, and the low-air-containing, high-flowability durable concrete is obtained through construction pouring, curing and maintenance.

[0068] Example 4

[0069] A low-gas-containing, high-flowability, durable concrete, which is composed of the following raw materials according to the amount of raw materials per cubic meter of concrete: P·O52.5 cement 450kg / m 3 ; Medium sand in zone II: 706kg / m 3 ; 5-10mm crushed stone 288kg / m 3 ; 10~20mm crushed stone 864kg / m 3 , water 153kg / m 3 ; Slow-setting polycarboxylic acid high-efficiency water reducer 5.850kg / m 3 ;

[0070] Wherein, defoamer and air entraining agent are added to the slow-setting polycarboxylic acid high-efficiency water reducer, the defoamer added in an amount of 0.05%wt of the slow-setting polycarboxylic acid high-efficiency water reducer, and the air entraining agent added in an amount of 0.05%wt of the slow-setting polycarboxylic acid high-efficiency water reducer.

[0071] The method for preparing the low-air-containing, high-fluidity, durable concrete comprises the following steps:

[0072] Crushed stone, medium sand in zone II and P·O52.5 cement are weighed according to the designed mass, put into a mixing pot and stirred evenly to obtain a solid mixture; defoaming agent, air entraining agent, slow-setting polycarboxylic acid high-efficiency water reducer and water are weighed according to the designed mass, mixed evenly and added to the solid mixture, stirred for 120 seconds, and the low-air-containing, high-flowability durable concrete is obtained through construction pouring, curing and maintenance.

[0073] Example 5

[0074] A low-gas-containing, high-flowability, durable concrete, which is composed of the following raw materials according to the amount of raw materials per cubic meter of concrete: P·O52.5 cement 470kg / m 3 ; Medium sand in zone II: 679kg / m 3 ; 5-10mm crushed stone 289kg / m 3 ; 10~20mm crushed stone 868kg / m 3 , water 155kg / m 3 ; Slow-setting polycarboxylic acid high-efficiency water reducer 6.110kg / m 3 ;

[0075] Wherein, defoamer and air entraining agent are added to the slow-setting polycarboxylic acid high-efficiency water reducer, the defoamer added in an amount of 0.05%wt of the slow-setting polycarboxylic acid high-efficiency water reducer, and the air entraining agent added in an amount of 0.05%wt of the slow-setting polycarboxylic acid high-efficiency water reducer.

[0076] The method for preparing the low-air-containing, high-fluidity, durable concrete comprises the following steps:

[0077] Crushed stone, medium sand in zone II and P·O52.5 cement are weighed according to the designed mass, put into a mixing pot and stirred evenly to obtain a solid mixture; defoaming agent, air entraining agent, slow-setting polycarboxylic acid high-efficiency water reducer and water are weighed according to the designed mass, mixed evenly and added to the solid mixture, stirred for 120 seconds, and the low-air-containing, high-flowability durable concrete is obtained through construction pouring, curing and maintenance.

[0078] Example 6

[0079] A low-gas, high-flow, durable concrete, which is composed of the following raw materials according to the amount of raw materials per cubic meter of concrete: P·O52.5 cement 456kg / m 3 ; Medium sand in zone II: 720kg / m 3 ; 5-10mm crushed stone 282kg / m 3 ; 10~20mm crushed stone 845kg / m 3 , water 155kg / m 3 ; Slow-setting polycarboxylic acid high-efficiency water reducer 5.928kg / m 3 ;

[0080] Wherein, defoamer and air entraining agent are added to the slow-setting polycarboxylic acid high-efficiency water reducer, the defoamer added in an amount of 0.05%wt of the slow-setting polycarboxylic acid high-efficiency water reducer, and the air entraining agent added in an amount of 0.05%wt of the slow-setting polycarboxylic acid high-efficiency water reducer.

[0081] The method for preparing the low-air-containing, high-fluidity, durable concrete comprises the following steps:

[0082] Crushed stone, medium sand in zone II and P·O52.5 cement are weighed according to the designed mass, put into a mixing pot and stirred evenly to obtain a solid mixture; defoaming agent, air entraining agent, slow-setting polycarboxylic acid high-efficiency water reducer and water are weighed according to the designed mass, mixed evenly and added to the solid mixture, stirred for 120 seconds, and the low-air-containing, high-flowability durable concrete is obtained through construction pouring, curing and maintenance.

[0083] Tests and Results

[0084] According to the test method standard JTG 3420-2020 "Test Procedure for Cement and Cement Concrete for Highway Engineering", the slump, slump expansion, air content, workability, 7d and 28d compressive strength of the low-gas-containing, high-flowability durable concrete prepared in Examples 1 to 6 were determined, and a water bucket specimen was retained to observe the appearance quality; a 1000x microscope was used to measure the bubble pore diameter of the low-gas-containing, high-flowability durable concrete prepared in Examples 1 to 6, and the statistical results were bubble pore diameters of not less than 90% of the number; the results are shown in Table 1.

[0085] Table 1 Test data of low-air-containing, high-fluidity, durable concrete prepared in Examples 1 to 6

[0086]

[0087] The low-air-content, high-flowing, durable concrete described in Example 2 is based on Example 1, with the water-cement ratio lowered and the water consumption appropriately reduced. The low-air-content, high-flowing, durable concrete described in Example 3 is based on Examples 1 and 2, with the slurry volume increased and the sand ratio reduced. The low-air-content, high-flowing, durable concrete described in Example 4 is based on Examples 1 to 3, with the slurry volume adjusted and the defoamer and air-entraining agent components in the slow-setting polycarboxylic acid high-efficiency water-reducing agent newly added. The low-air-content, high-flowing, durable concrete described in Example 5 is based on Example 4, with the slurry volume and sand ratio adjusted. The low-air-content, high-flowing, durable concrete described in Example 6 is based on Examples 1 to 5, with the slurry volume and sand ratio adjusted.

[0088] It can be seen from Table 1 that the low-air-content, high-fluidity, durable concrete provided by the present invention has good fluidity and workability, and is easy to cast and form; the air content is relatively low, the appearance has a small amount of bubbles and is even smooth, and the appearance is good.

[0089] Referring to the 45-3 prefabricated T-beam of the left span of the North Beach Approach Bridge of the Yellow River Bridge, the low-gas-containing high-flow durable concrete prepared in Examples 1 to 6 in Examples 1 to 6 was used to prepare the prefabricated T-beam. According to the test method standard of JTG 3420-2020 "Test Procedure for Cement and Cement Concrete for Highway Engineering", the durability tests such as impermeability, chloride ion diffusion, electric flux (56d) and frost resistance of the low-gas-containing high-flow durable concrete were measured, and the results are shown in Table 2.

[0090] Table 2 Durability test data of low-air-containing, high-fluidity durable concrete prepared in Examples 1 to 6

[0091]

[0092] It can be seen from Table 2 that the low-gas-containing, high-flow durable concrete provided by the present invention can meet the technical requirements of durability while meeting the appearance requirements. On the basis of determining the materials, by adjusting the material dosage and the water-reducing component in the water-reducing agent, a more excellent low-gas-containing, high-flow durable concrete can be obtained. Combining the data in Tables 1 and 2, it can be seen that Example 6 presents the best ratio effect.

[0093] It should be understood that the above embodiments are only used to illustrate the content of the present invention and are not used to limit the protection scope of the present invention. In addition, it should be understood that the mix ratio adjustment described in the present invention mainly refers to the slurry dosage (slurry collection ratio), sand ratio, and the combination change of the defoamer and air entraining agent in the water reducer component. It is believed that the fluctuation in the impact on the test results is not too obvious within the scope indicated by the example. In specific implementation, the combination of the above three can be obtained by trial mixing to obtain the best match. The above examples are preferred examples referred to in the present invention and shall not be used as data examples to limit the present invention. In this field, the data adjustment ratio can be appropriately changed and modified, and the adjusted data is also regarded as the spirit and principle of the present invention. Any modification, adjustment, replacement, and improvement made within this spirit and principle should be included in the protection scope of the present invention.

Claims

1. A low-air-containing, high-fluidity, durable concrete, characterized in that: Calculated by weight, it is mainly composed of the following raw materials: 450-473 parts of P·O52.5 cement, 677-720 parts of medium sand in zone II, 1127-1157 parts of crushed stone, 152-156 parts of water, and 5.850-6.419 parts of slow-setting polycarboxylic acid high-efficiency water-reducing agent.

2. The low-air-containing, high-fluidity, durable concrete according to claim 1, characterized in that: Calculated by weight, it is mainly composed of the following raw materials: 456-470 parts of P·O52.5 cement, 679-720 parts of medium sand in Zone II, 1127-1157 parts of crushed stone, 155 parts of groundwater, and 5.928-6.110 parts of slow-setting polycarboxylic acid high-efficiency water-reducing agent.

3. The low-air-containing, high-fluidity, durable concrete according to claim 1, characterized in that: The alkali content in the P·O52.5 cement is ≤0.6%, and the C3A content in the clinker is ≤8.0%; The fineness of the sand in zone II is 2.6-3.0, the mud content is 1.5%-2.5%, and the mud content is ≤0.5%; The porosity of the crushed stone is less than 40%, the crushing index is less than 20%, the ratio of the compressive strength of the parent rock to the design strength of the concrete is ≥1.5, the mud content is ≤1.0%, the mud block content is ≤0.5%, and the needle-like particle content is less than 10%; The water is groundwater.

4. The low-air-containing, high-fluidity, durable concrete according to claim 1, characterized in that: The particle size of the crushed stone is 5 to 20 mm.

5. The low-air-containing, high-fluidity, durable concrete according to claim 1 or 4, characterized in that: The crushed stone is composed of crushed stone with a particle size of 5 to 10 mm and crushed stone with a particle size of 10 to 20 mm, which are mixed in a mass ratio of 0.30 to 0.35:

1.

6. The low-air-containing, high-fluidity, durable concrete according to claim 5, characterized in that: The crushed stone is composed of crushed stone with a particle size of 5 to 10 mm and crushed stone with a particle size of 10 to 20 mm mixed in a mass ratio of 0.32 to 0.34:

1.

7. The low-air-containing, high-fluidity, durable concrete according to claim 1, characterized in that: The low-air-content, high-fluidity, durable concrete also contains a defoamer and an air-entraining agent.

8. The low-air-containing, high-fluidity, durable concrete according to claim 7, characterized in that: The addition amount of the defoamer is 0.025% to 0.05% wt of the addition amount of the slow-setting polycarboxylic acid high-efficiency water-reducing agent, and the addition amount of the air-entraining agent is 0.05% to 0.075% wt of the addition amount of the slow-setting polycarboxylic acid high-efficiency water-reducing agent.

9. The low-air-containing, high-fluidity, durable concrete according to claim 7, characterized in that: The air entraining agent is a TSC560 ether air entraining agent, and the defoaming agent is a TSC1200 polyether defoaming agent.

10. A method for preparing the low-air-containing, high-fluidity, durable concrete according to any one of claims 1 to 9, comprising the following steps: The crushed stone, the medium sand in zone II and the P·O52.5 cement are uniformly mixed according to the designed mass fraction to obtain a solid mixture; the slow-setting polycarboxylic acid high-efficiency water-reducing agent and water are uniformly mixed according to the designed mass fraction and then added to the solid mixture, and the mixture is uniformly mixed; and the low-air-containing, high-fluidity durable concrete is obtained through construction pouring, curing and curing.

Citation Information

Patent Citations

  • Control method of pores in surface of fair-faced concrete

    CN110240447A

  • High-water-retention anti-segregation high-durability precast beam artificial-vibration-free concrete and preparation method thereof

    CN114890755A