Metallurgical slag-based inorganic cementing material as well as preparation method and application thereof

By using steel slag powder, blast furnace slag powder, fly ash and gypsum excitation materials in metallurgical slag, adjusting the proportion of excitation materials and stirring process, the problems of low utilization rate and expansion cracking of metallurgical slag in concrete are solved, and high strength is achieved , Preparation and application of low-cost metallurgical slag-based inorganic cementitious materials.

CN118754583AInactive Publication Date: 2024-10-11WUHAN CHONGDE ENVIRONMENTAL PROTECTION ENG CO LTD
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
CN202410748265.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-11
Publication Date
2024-10-11
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The utilization rate of existing metallurgical slag in concrete is low, and the activated cementitious material will expand and crack due to shrinkage and deformation, with low strength. It is difficult to coordinate the properties of fly ash, slag and steel slag to achieve stable condensation and high strength.

Method used

Steel slag powder, blast furnace slag powder, fly ash and gypsum are used as excitation materials. By adjusting the type and proportion of excitation materials and combining with stirring treatment, metallurgical slag-based inorganic cementitious materials with stable performance are prepared. The proportion of excitation materials is ≤25%. Gypsum excitation materials account for at least 20%, with a ratio of 3:1-1:5, including desulfurized limestone, phosphogypsum, titanium gypsum, etc.

Benefits of technology

It realizes the maximum utilization of metallurgical slag-based inorganic cementitious materials, reduces costs, improves compressive strength and flexural strength, overcomes the problems of expansion and uneven performance in traditional cementitious systems, and obtains stable volume properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118754583A_ABST
    Figure CN118754583A_ABST
Patent Text Reader

Abstract

The invention relates to a metallurgical slag-based inorganic cementing material which comprises steel slag powder, blast furnace slag powder, fly ash, a first excitation material and a second excitation material. The ratio of the excitation material in the cementing material is less than or equal to 25%, so that the maximum utilization of solid wastes can be realized, and the overall cost is low. The gelling system provided by the invention is relatively good in volume stability. The problems that in a traditional gelling system, the utilization rate of steel slag is low, free calcium oxide and magnesium oxide expand and are uneven in distribution, and consequently the gelling system is concentrated in stress and uneven in material performance are solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of materials, and in particular relates to a metallurgical slag-based inorganic gelling material. Background Art

[0002] In recent years, my country's infrastructure has developed rapidly, and the industrialization of steel smelting has also developed rapidly, which has brought about the treatment of solid waste. The main solid wastes are mainly fly ash, slag and steel slag. Among them, fly ash and slag are widely used as admixtures in the cement concrete industry, but the utilization rate of steel slag is extremely low.

[0003] Slag is a molten product with calcium aluminosilicate as the main component obtained when iron plants smelt pig iron in blast furnaces. It is an industrial solid waste residue obtained after water quenching and granulation. Most of it is glassy and has potential hydraulic gelling properties.

[0004] Steel slag is formed at high temperatures during steelmaking. The C2S and C3S minerals in the steel slag discharged from steelmaking are relatively complete in crystallization and have large crystal grain sizes, resulting in a dense overall structure of the steel slag. Steel slag can be added to concrete as an admixture to reduce water demand and greatly improve the fluidity of the fresh slurry. Steel slag also has a volcanic ash effect. When added to concrete as an admixture in a certain ratio, it will react with cement to form industrial-grade slaked lime powder for secondary hydration. The hydration products fill the voids in the concrete structure, thereby improving the internal density of the concrete and enhancing the later strength of the concrete. At the same time, the addition of steel slag effectively slows down the thermal rate of cement hydration, greatly offsetting the cracking phenomenon caused by temperature in large-volume concrete. Although steel slag has potential gelling activity, it requires certain stimulation measures to be fully utilized. Simply using industrial chemical reagents to stimulate steel slag powder is costly and not conducive to industrial application. More importantly, the stimulated cementitious material will expand and crack due to shrinkage and deformation, and has low strength.

[0005] Fly ash is the fine ash collected from the flue gas after coal combustion. The main oxide components of fly ash are: SiO2, Al2O3, FeO, Fe2O3, CaO, TiO2, etc. It is one of the industrial waste slags with the largest discharge volume in my country. There are many studies on fly ash cementitious materials at present, and the basic formula is also similar. The later strength of fly ash cementitious materials is relatively high. Although fly ash itself has certain activity, its early excitation effect is limited, resulting in low early strength.

[0006] From the above, it can be seen that since fly ash, slag and steel slag have different properties and different gelling properties, it is an urgent problem to be solved in this field to coordinate and stimulate the properties of the three to achieve a reasonable setting time and stable performance of the final material, and to meet the compressive strength and flexural strength standards. Summary of the invention

[0007] To achieve the above objectives, the inventors conducted experiments on metallurgical slag-based inorganic gelling materials. After multiple experiments, the inventors adjusted the types and proportions of the exciting materials and finally obtained a metallurgical slag-based inorganic gelling material with stable performance.

[0008] Specifically provided is a metallurgical slag-based inorganic gelling material, including steel slag powder, blast furnace slag powder, fly ash, a first excitation material and a second excitation material.

[0009] Furthermore, the first excitation material and the second excitation material are different, and at least one of the first excitation material and the second excitation material is a gypsum-based excitation material.

[0010] Furthermore, the total proportion of the first excitation material and the second excitation material is ≤25%.

[0011] The further gypsum-based energizing material comprises at least 20% of the total of the first energizing material and the second energizing material.

[0012] Furthermore, the ratio of the first excitation material to the second excitation material is 3:1-1:5.

[0013] Further gypsum-based stimulating materials are one or more of desulfurized gypsum, phosphogypsum, titanium gypsum and fluorinated gypsum.

[0014] Further non-gypsum stimulating materials are one or more of desulfurization slag, electrolytic manganese slag, sodium carbonate, and magnesium smelting slag.

[0015] Furthermore, the first excitation material and the second excitation material are both gypsum-based excitation materials.

[0016] Further inorganic gelling material specific surface area ≥ 450m 2 / kg.

[0017] Furthermore, the present invention also provides a method for preparing an inorganic gelling material, which comprises the following steps: respectively ball-milling steel slag powder, blast furnace slag powder, fly ash, a first excitation material and a second excitation material, weighing and mixing them uniformly in proportion, transferring the obtained mixture to a mixer, stirring uniformly to obtain a pure slurry and curing.

[0018] Specifically, the mixing time is 5-60min; the stirring speed is 200-800r / min, and the stirring time is 5-60min.

[0019] Furthermore, the present invention also provides an application of an inorganic gelling material, and the inorganic gelling material can be used alone or mixed with clinker.

[0020] Specifically, the inorganic gelling material and the clinker are mixed and used, and the clinker accounts for 0-25%.

[0021] The beneficial effects of the present invention include:

[0022] The present invention provides a metallurgical slag-based inorganic gelling material, in which the proportion of an excitation material in the gelling material is ≤25%, thereby achieving maximum utilization of solid waste and having low overall cost.

[0023] In another aspect of the present invention, the performance and proportion of the exciting material are studied, and two different exciting material systems are selected, preferably gypsum exciting materials. The two different material proportions in the exciting material system are studied to achieve the best setting performance and obtain a material with low final cost and high compressive strength and flexural strength.

[0024] In another aspect of the present invention, the gelling system of the present invention has good volume stability, thus overcoming the problems of low utilization rate and uneven distribution of steel slag in the traditional gelling system, which leads to stress concentration in the gelling system, expansion, and uneven material properties.

[0025] In another aspect of the present invention, the exciting material is preferably gypsum, which has low cost, is easy to use and has excellent performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 . Solidification time of different types of excitation material combinations

[0027] Figure 2 .Compression strength of different types of exciting materials combination

[0028] Figure 3 .Flexural strength of different types of excitation material combinations

[0029] Figure 4 . Solidification time of different proportions of gypsum-based stimulating materials

[0030] Figure 5 .Compressive strength of different proportions of gypsum-based materials

[0031] Figure 6 .Flexural strength of gypsum-based materials with different ratios DETAILED DESCRIPTION

[0032] Unless otherwise defined, all scientific and technical terms used in the present invention have the same meanings as commonly understood by one of ordinary skill in the art to which the present invention relates.

[0033] In order to further verify the efficacy of the excitation material of the present invention, a comparison of different excitation material combinations is provided in certain embodiments.

[0034] In order to further verify the efficacy of the excitation material of the present invention, in certain embodiments, a comparison of combinations of excitation materials with different ratios is provided.

[0035] In order to further verify the efficacy of the exciting material of the present invention, different proportions of steel slag powder, blast furnace slag powder and fly ash are provided for comparison in certain embodiments.

[0036] In order to further verify the efficacy of the stimulating material of the present invention, the metallurgical slag-based inorganic gelling material of the present invention and the clinker ratio are provided in certain embodiments to further verify its efficacy.

[0037] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0038] Example 1. Comparison of different excitation material combinations

[0039] Using 30 parts of steel slag powder, 40 parts of blast furnace slag powder, and 10 parts of fly ash as the benchmark, adjust the excitation materials and verify different combinations of excitation materials.

[0040] The combination of excitation materials is shown in Table 1

[0041] Table 1. Excitation material combination ratio

[0042]

[0043]

[0044] Statistical Group 1-5 Setting time and compressive strength of metallurgical slag-based inorganic cementitious materials

[0045] Table 2. Test results of the combination of exciting materials

[0046]

[0047] As shown in the statistical results in the table above, group 1 has the longest solidification time and poor performance; groups 4 and 5 have the shortest solidification time and the highest compressive strength and flexural strength.

[0048] Example 2. Comparison of different excitation material ratios

[0049] Using 30 parts of steel slag powder, 40 parts of blast furnace slag powder and 10 parts of fly ash as the benchmark, adjust the excitation materials and verify the combination of different excitation material ratios.

[0050] The combination of excitation materials is shown in Table 3

[0051] Table 3. Combination ratio of gypsum-based excitation materials

[0052]

[0053] Statistical Group 1-5 Setting time and compressive strength of metallurgical slag-based inorganic cementitious materials

[0054] Table 4. Performance test of gypsum-based excitation material ratio combination

[0055]

[0056] As shown in the above table, group 3-7 has the shortest coagulation time and the best performance. Group 1-2 and group 8-10 have a longer coagulation time and relatively poor performance.

[0057] Example 3. Combinations of different gypsum-based stimulating materials

[0058] Using 30 parts of steel slag powder, 40 parts of blast furnace slag powder and 10 parts of fly ash as the benchmark, adjust the excitation materials and verify the combination of different excitation material ratios.

[0059] The combination of excitation materials is shown in Table 5

[0060] Table 5. Gypsum-based excitation material combinations

[0061]

[0062] Statistical Group 1-18 Solidification Time and Compressive Strength of Metallurgical Slag-Based Inorganic Cementitious Materials

[0063] Table 6. Gypsum-based excitation material combination performance test

[0064]

[0065] As shown in the statistical results in the above table, groups 1-18 all have short coagulation times and the best performance.

Claims

1. A metallurgical slag-based inorganic gelling material, characterized in that: The invention comprises steel slag powder, blast furnace slag powder, fly ash, a first excitation material and a second excitation material. The sum of the first excitation material and the second excitation material is ≤25%. The first excitation material and the second excitation material are different, and at least one of the first excitation material and the second excitation material is a gypsum excitation material.

2. The inorganic gelling material according to any one of claims 1, characterized in that: The gypsum-based excitation material accounts for at least 20% of the total of the first excitation-based material and the second excitation-based material.

3. The inorganic gelling material according to claim 1 or 2, characterized in that: The ratio of the first excitation material to the second excitation material is 3:1-1:

5.

4. The inorganic gelling material according to any one of claims 1 to 3, characterized in that: The gypsum-based activating material is one or more of desulfurized gypsum, phosphogypsum, titanium gypsum and fluorinated gypsum.

5. The inorganic gelling material according to any one of claims 1 to 4, characterized in that: The non-gypsum stimulating material is one or more of desulfurization slag, electrolytic manganese slag, sodium carbonate, low modulus liquid water glass, and a modifier.

6. The inorganic gelling material according to any one of claims 1 to 4, characterized in that: The first excitation material and the second excitation material are both gypsum-based excitation materials.

7. The inorganic gelling material according to any one of claims 1 to 6, characterized in that: The specific surface area of ​​the inorganic gelling material is ≥450m 2 / kg.

8. The method for preparing an inorganic gelling material according to any one of claims 1 to 7, characterized in that: The preparation method comprises the following steps: steel slag powder, blast furnace slag powder, fly ash, the first excitation material and the second excitation material are respectively ball-milled, weighed in proportion and mixed evenly, the obtained mixture is transferred to a mixer, stirred evenly to obtain a pure slurry and cured.

9. The use of the inorganic gelling material according to any one of claims 1 to 6, characterized in that: The inorganic gelling material is used alone or mixed with clinker.

10. Use of the inorganic gelling material according to any one of claims 9, characterized in that The inorganic gelling material and the clinker are mixed for use, and the clinker accounts for 0-25%.

Citation Information

Patent Citations

  • Low-temperature ceramic curing agent of red mud from Bayer process

    CN101624267A

  • Composite gel material and preparation method thereof

    CN102633461A

  • Cementing material, precast concrete and preparation method of precast concrete

    CN109608068A

  • All-solid-waste cementing material containing refining slag and preparation method of all-solid-waste cementing material

    CN110304851A

  • Cementing material taking mineral slag-steel slag-gypsum as raw materials and preparation method thereof

    CN110683774A