Sulfonated graphene modification-based carbon-based composite material and preparation method thereof
By using centrifugal spray drying and high-temperature carbonization processes of sulfonated graphene solution and carbon powder in carbon-based composite materials, the problems of insufficient nanoparticle dispersion and interfacial bonding force are solved, and the uniform distribution and performance of carbon-based composite materials are achieved. Improved, simplified process and suitable for mass production.
Patent Information
- Application Number
- CN202410694513.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-31
- Publication Date
- 2024-10-11
AI Technical Summary
The existing carbon-based composite materials in the pantograph slide plate have insufficient bonding force between the reinforcement phase and the matrix, resulting in poor material performance improvement, and the nanoparticles are difficult to disperse evenly, causing serious local agglomeration, and the traditional modification method is complex and difficult to Mass production can easily destroy the surface structure of nanoparticles.
The sulfonated graphene solution and carbon powder are mixed evenly and then centrifugally spray-dried to form sulfonated graphene-coated carbon powder particles, which are then kneaded and stamped with modified coal pitch, and finally carbonized at high temperature to form sulfonated graphene-based carbon powder particles. Graphene-modified carbon-based composites.
Through solution mixing and centrifugal spray drying methods, the dispersion and interfacial bonding force of graphene are improved, which avoids damage to the surface of graphene by local high energy, achieves uniform distribution and wrapped combination of nanomaterials, and improves the overall performance of the material. , simplifies the process flow and is suitable for mass production.
Smart Images

Figure CN118754667A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of composite materials, and in particular to a carbon-based composite material modified by sulfonated graphene and a preparation method thereof. Background Art
[0002] Due to its excellent mechanical and electrical properties, carbon-based composite materials have become one of the development directions of pantograph skateboard materials. However, due to the limitation of the interface bonding between the matrix and the reinforcement phase, its actual performance improvement cannot meet expectations. Ordinary physical pressing will forcibly bond the reinforcement phase to the carbon matrix, resulting in insufficient bonding force, prone to congenital microcracks and development into holes, affecting the performance of the skateboard. In response to this technical problem, some scholars have modified the surface of nanoparticles through acid treatment, electrochemical treatment, plasma treatment and other methods to improve the bonding strength between them and the matrix, but it still cannot improve the problem of nanoparticles being difficult to disperse and locally agglomerate in the carbon matrix. In addition, the process is relatively complicated and difficult to mass produce. Excessive energy will also destroy the surface structure of the nanoparticles. Summary of the invention
[0003] The purpose of the present invention is to provide a carbon-based composite material based on sulfonated graphene modification and a preparation method thereof to improve the above problems. In order to achieve the above purpose, the technical solution adopted by the present invention is as follows:
[0004] The present application provides a method for preparing a carbon-based composite material based on sulfonated graphene modification, comprising:
[0005] Adding carbon powder with an average particle size of 0.1-1 μm into the sulfonated graphene solution, and mixing them evenly to obtain a composite solution;
[0006] The composite solution is spray-dried to obtain spherical composite powder of sulfonated graphene-coated carbon powder particles;
[0007] The spherical composite powder and modified coal tar pitch are kneaded and pressed to form a green body;
[0008] The green body is carbonized at high temperature to obtain a carbon-based composite material modified by sulfonated graphene.
[0009] The present invention also provides a product, which is a carbon-based composite material based on sulfonated graphene modified and prepared by the method for preparing a carbon-based composite material based on sulfonated graphene modified.
[0010] The invention also provides the application of the product in rocket engine nozzles, aircraft brake discs and pantograph slides of electric trains.
[0011] The beneficial effects of the present invention are:
[0012] The present invention achieves the combination of the two while improving the dispersibility of graphene through the method of solution mixing and centrifugal spray drying, solves the problem of local agglomeration when nanomaterials are added to the carbon matrix, ensures the uniform distribution of graphene in the pantograph slide material, forms a wrapping combination at the particle level, improves the interface bonding force, and avoids the destruction of the graphene surface structure by local high energy of chemical modification means.
[0013] Other features and advantages of the present invention will be described in the following description, and partly become apparent from the description, or be understood by practicing the embodiments of the present invention. The purpose and other advantages of the present invention can be realized and obtained by the structures particularly pointed out in the written description, claims, and drawings. BRIEF DESCRIPTION OF THE DRAWINGS
[0014] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.
[0015] Figure 1 The present invention is a flow chart of the preparation method of carbon-based composite materials based on sulfonated graphene modification. DETAILED DESCRIPTION
[0016] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all of the embodiments. The components of the embodiments of the present invention generally described and shown in the drawings here can be arranged and designed in various different configurations. Therefore, the following detailed description of the embodiments of the present invention provided in the drawings is not intended to limit the scope of the claimed invention, but merely represents selected embodiments of the present invention. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0017] It should be noted that similar reference numerals and letters represent similar items in the following drawings, so once an item is defined in one drawing, it does not need to be further defined and explained in the subsequent drawings. At the same time, in the description of the present invention, the terms "first", "second", etc. are only used to distinguish the description and cannot be understood as indicating or implying relative importance.
[0018] The present invention provides a method for preparing a carbon-based composite material based on sulfonated graphene modification, comprising:
[0019] Adding carbon powder with an average particle size of 0.1-1 μm into the sulfonated graphene solution, and mixing them evenly to obtain a composite solution;
[0020] The composite solution is spray-dried to obtain spherical composite powder of sulfonated graphene-coated carbon powder particles;
[0021] The spherical composite powder and modified coal tar pitch are kneaded and pressed to form a green body;
[0022] The green body is carbonized at high temperature to obtain a carbon-based composite material modified by sulfonated graphene.
[0023] The carbon powder has a purity of >99.9%, a specific surface area of 27 m2 / g, a volume density of 1.35 g / cm3 and a density of 1.8 g / cm3.
[0024] The steps for preparing the sulfonated graphene solution include:
[0025] Concentrated sulfuric acid and potassium permanganate are successively added to a mixture of natural graphite sheets and sodium nitrate to obtain a mixed solution, the temperature of the mixed solution is controlled to be 25-35° C. by a warm water bath method, and mechanically stirred for 10-15 hours;
[0026] diluting the stirred mixed solution with deionized water and adding a hydrogen peroxide solution, mechanically stirring and then standing to obtain a solution after standing, filtering the solution after standing to obtain a supernatant, and washing the supernatant with concentrated hydrochloric acid and deionized water until it is neutral;
[0027] The supernatant washed to neutrality is subjected to ultrasonication and then centrifuged, and dried under vacuum conditions to obtain graphene oxide;
[0028] The graphene oxide is added to anhydrous tetrahydrofuran, and then ultrasonically dispersed to obtain an ultrasonic dispersion solution, sodium hydride is slowly added to the ultrasonic dispersion solution under a 60° C. water bath condition, and the temperature is kept for 4-6 hours, and then sulfanilic acid is added to the ultrasonic dispersion solution, and stirred at 80° C. for 20-30 hours to obtain a stirred product;
[0029] The stirred product is immersed in a hydrochloric acid solution for 12 hours, rinsed with anhydrous ethanol for 3-5 times to remove reaction residues, and dried in a vacuum oven to obtain sulfonated graphene. The sulfonated graphene is mixed with anhydrous ethanol and ultrasonically treated to obtain a sulfonated graphene solution.
[0030] The mass ratio of the sulfonated graphene to the carbon powder in the composite solution is 0.005-0.02:1.
[0031] The mixing method of adding carbon powder to the sulfonated graphene solution and then mixing the two includes mechanical stirring and ultrasonic oscillation, wherein the mechanical stirring speed is 800-1000 rpm, the stirring time is 2-4 hours, and the ultrasonic oscillation time is 1-2 hours.
[0032] The spherical composite powder and the modified coal tar pitch are mixed and kneaded in a mass ratio of 30-40:20-30.
[0033] The kneading temperature of the kneading treatment is 250-300° C., the kneading speed is 1500rpm-2000rpm and the kneading time is 1-3h. The stamping temperature of the stamping treatment is 160-180° C., the stamping pressure is 12-18MPa and the holding time is 5-10min.
[0034] The carbonization temperature change process of the high temperature carbonization includes:
[0035] First, heat up to 150-180℃ at 40-50℃ / h;
[0036] Then increase the temperature to 500-550℃ at a constant rate of 5-15℃ / h;
[0037] Then the temperature is raised to 1000-1200℃ at a rate of 50-70℃ / h;
[0038] Finally keep warm for 120-150h.
[0039] The present invention also provides a product, which is a carbon-based composite material based on sulfonated graphene modified and prepared by the method for preparing a carbon-based composite material based on sulfonated graphene modified.
[0040] The invention also provides the application of the product in rocket engine nozzles, aircraft brake discs and pantograph slides of electric trains.
[0041] The composite solution is subjected to centrifugal spray drying, comprising:
[0042] placing the composite solution in a centrifugal spray dryer;
[0043] The centrifugal spray dryer is set with a feed rate of 20-30 ml / min, a spray pressure of 0.2-0.3 MPa, an air inlet temperature of 120-130°C, and an air outlet temperature of 75-95°C;
[0044] The centrifugal spray dryer is started to spray the composite solution into the high-temperature hot air flow for drying.
[0045] like Figure 1 As shown, a flow chart of the method for preparing a carbon-based composite material based on sulfonated graphene modification of the present invention is given.
[0046] The method for preparing a carbon-based composite material based on sulfonated graphene modification of the present invention comprises the following steps:
[0047] (1) adding ultrafine carbon powder to the sulfonated graphene solution and mixing them evenly to obtain a dispersed composite solution;
[0048] (2) placing the uniformly mixed solution in step (1) in a centrifugal spray dryer, dispersing the liquid into droplets by centrifugal force, spraying in a high-temperature hot air flow for drying, and obtaining a spherical composite powder of sulfonated graphene-coated carbon powder particles;
[0049] (3) kneading and pressing the composite powder obtained in step (2) with modified coal tar into a green body;
[0050] (4) Carbonizing the green body in step (3) at high temperature to obtain a graphene-enhanced pantograph slide material.
[0051] The preparation process of sulfonated graphene solution specifically includes the following steps:
[0052] S1: Concentrated sulfuric acid and potassium permanganate are added to the mixture of natural graphite flakes and sodium nitrate, and the temperature of the mixture is controlled to 25-35°C by a warm water bath method, and mechanically stirred for 10-15h;
[0053] S2: dilute the mixture with deionized water and add hydrogen peroxide solution, stir mechanically and then let stand, filter and take the supernatant, wash with concentrated hydrochloric acid and deionized water until neutral; the concentration of hydrogen peroxide solution is 3-5wt%, the volume of hydrogen peroxide and deionized water is equal to that of concentrated sulfuric acid, the mechanical stirring time is 3-5h, and the standing time is 3-5h;
[0054] S3: After ultrasonication, the supernatant is centrifuged for 15-20 minutes, and dried under vacuum conditions to obtain graphene oxide; wherein the ultrasonication time is 1-2 hours, the centrifugal speed is 7000-8000 rpm, and the drying temperature is 75-85°C;
[0055] S4: Add graphene oxide to anhydrous tetrahydrofuran, disperse it evenly by ultrasonication, slowly add sodium hydride in a 60°C water bath, keep warm for 4-6 hours, then add sulfanilic acid to the mixture, and stir at 80°C for 20-30 hours. The volume mass ratio of graphene oxide, anhydrous tetrahydrofuran, sodium hydride and sulfanilic acid is 0.2g:250ml:1.5g:2.5g, and the ultrasonic dispersion time is 30-45min;
[0056] S5: The product is stirred and immersed in an HCl:H2O solution for 12 hours, rinsed with anhydrous ethanol for 3-5 times to remove the reaction residues, and dried in a vacuum oven for 24 hours to obtain sulfonated graphene, and finally mixed with anhydrous ethanol and ultrasonicated to obtain a sulfonated graphene solution; wherein the volume ratio of HCl to H2O is 1:1, the drying temperature is 75-85°C, the concentration of the sulfonated graphene solution is 1 mg / ml, and the ultrasonic oscillation time is 25-35 min.
[0057] In step S1, sodium nitrate and natural graphite flakes are mixed in equal proportions, the volume mass ratio of concentrated sulfuric acid, potassium permanganate and graphite flakes is 100 ml:9g:1g, and the mechanical stirring speed is 600-700rpm.
[0058] In step (1), the mass ratio of sulfonated graphene to added ultrafine carbon powder in the composite solution is 0.005-0.02:1.
[0059] In step (1), the mixing method includes mechanical stirring and ultrasonic oscillation, wherein the mechanical stirring speed is 800-1000 rpm, the stirring time is 2-4 h, and the ultrasonic oscillation time is 1-2 h.
[0060] In step (2), the feed rate of the centrifugal spray dryer is 20-30 ml / min, the spray pressure is 0.2-0.3 MPa, the inlet air temperature is 120-130°C, and the outlet air temperature is 75-95°C.
[0061] The kneading and stamping in step (3) mainly includes the following steps: kneading the spherical composite powder of sulfonated graphene-coated carbon powder particles and the modified coal tar pitch in a mass ratio of 30-40:20-30, and maintaining the obtained mixed powder under a stamping pressure of 12-18 MPa for 5-10 minutes.
[0062] The kneading temperature is 250-300°C, the rotation speed is 1500rpm-2000rpm, the kneading time is 1-3h, and the stamping temperature is 160-180°C.
[0063] The carbonization temperature is changed as follows: the temperature is increased from 40-50°C / h to 150-180°C, then the temperature is increased to 500-550°C at a constant rate of 5-15°C / h, and the temperature is increased to 1000-1200°C at a rate of 50-70°C / h, and the temperature is kept for 120-150h to obtain a pantograph slide material with uniformly dispersed graphene.
[0064] Compared with the existing method, the beneficial effects of the present invention are:
[0065] The present invention achieves a combination of the two while improving the dispersibility of graphene through the method of solution mixing and centrifugal spray drying. For liquid materials containing solid particles, the force generated by centrifugation will form a spherical surrounding structure of sulfonated graphene solution around the carbon powder particles, and then the droplets are thrown out at high speed and sprayed in a high-temperature hot air flow to achieve instant drying, thereby better maintaining the surrounding structure of carbon powder-sulfonated graphene, solving the problem of local agglomeration when nanomaterials are added to the carbon matrix, and ensuring the uniform distribution of graphene in the pantograph slide material.
[0066] The present invention utilizes centrifugal force to achieve lossless bonding of carbon powder and graphene. Compared with traditional physical pressing, the present invention forms a wrapping bond at the particle level, thereby improving the interface bonding strength and avoiding the destruction of the graphene surface structure by local high energy of chemical modification means.
[0067] The preparation method proposed in the present invention has the advantages of simple process flow, convenient operation, continuous mass production, energy saving and environmental protection, and low cost. The comprehensive performance of the prepared pantograph slide material is improved, which makes up for the shortcomings of current slide materials.
[0068] Example 1
[0069] This embodiment provides a method for preparing a carbon-based composite material based on sulfonated graphene modification, which specifically includes the following steps:
[0070] (1) 200 ml of 98% concentrated sulfuric acid and 18 g of potassium permanganate were added to a mixture of 2 g of natural graphite flakes and 2 g of sodium nitrate. The mixture was kept at a temperature of 30° C. using a warm water bath method and mechanically stirred for 10 h at a speed of 600 rpm.
[0071] (2) The mixture was diluted with 200 ml of deionized water, and then 200 ml of a 3 wt% hydrogen peroxide solution was added. The mixture was mechanically stirred for 3 h and then allowed to stand for 3 h. The supernatant was filtered and washed with concentrated hydrochloric acid and deionized water until it was neutral (pH = 7.0).
[0072] (3) The supernatant obtained in step (2) is subjected to ultrasonic treatment for 1 hour, centrifuged for 15 minutes, and dried under vacuum conditions at a temperature of 75° C. to obtain graphene oxide; wherein the centrifugal speed is 7000 rpm.
[0073] (4) 0.2 g of the graphene oxide obtained in step (3) was added to 250 ml of anhydrous tetrahydrofuran, and the mixture was evenly dispersed by ultrasonication for 30 min. 1.5 g of sodium hydride was slowly added in a 60° C. water bath and kept warm for 4 h. Subsequently, 2.5 g of sulfanilic acid was added to the mixture, and the mixture was stirred at 80° C. for 20 h.
[0074] (5) The product obtained in step (4) was immersed in a 1:1 HCl:H2O solution by volume for 12 h, rinsed with anhydrous ethanol three times to remove the reaction residue, dried in a vacuum oven at 75°C for 24 h, taken out and diluted with anhydrous ethanol to 1 mg / ml, and subjected to ultrasound for 25 min to obtain a sulfonated graphene solution.
[0075] (6) Add 100 g of ultrafine carbon powder to 500 ml of sulfonated graphene solution, stir mechanically for 2 h, and then ultrasonically vibrate for 1 h to obtain a uniformly dispersed composite solution; the mechanical stirring speed is 800 rpm.
[0076] (7) placing the solution in a centrifugal spray dryer, spraying it in a high-temperature hot air flow and drying it, to obtain a spherical composite powder of sulfonated graphene-coated carbon powder particles; wherein the centrifugal spray dryer has a feed rate of 20 ml / min, a spray pressure of 0.2 MPa, an inlet air temperature of 120°C, and an outlet air temperature of 75°C.
[0077] (8) The composite powder obtained in step (7) and the modified coal tar pitch were kneaded at a mass ratio of 30:20 at 250°C for 1 hour, and after being taken out, the mixture was kept under pressure at a stamping pressure of 12 MPa for 5 minutes; wherein the kneading machine speed was 1500 rpm and the stamping temperature was 160°C.
[0078] (9) After the green body is taken out, high-temperature carbonization is performed, the temperature is increased to 150°C at a rate of 40°C / h, then the temperature is increased to 500°C at a constant rate of 5°C / h, and the temperature is increased to 1000°C at a rate of 50°C / h. The temperature is kept at this rate for 120 hours to obtain a graphene-enhanced pantograph slide material.
[0079] Example 2
[0080] This embodiment provides a method for preparing a carbon-based composite material based on sulfonated graphene modification, which specifically includes the following steps:
[0081] (1) 200 ml of 98% concentrated sulfuric acid and 18 g of potassium permanganate were added to a mixture of 2 g of natural graphite flakes and 2 g of sodium nitrate. The mixture was kept at a temperature of 30° C. using a warm water bath method and mechanically stirred for 13 h at a speed of 650 rpm.
[0082] (2) The mixture was diluted with 200 ml of deionized water, and then 200 ml of a 4 wt% hydrogen peroxide solution was added. The mixture was mechanically stirred for 4 hours and then allowed to stand for 4 hours. The supernatant was filtered and washed with concentrated hydrochloric acid and deionized water until it was neutral (pH = 7.0).
[0083] (3) The supernatant obtained in step (2) is ultrasonicated for 1.5 hours, centrifuged for 20 minutes, and dried under vacuum conditions at a temperature of 80° C. to obtain graphene oxide; wherein the centrifugal speed is 7000 rpm.
[0084] (4) 0.2 g of the graphene oxide obtained in step (3) was added to 250 ml of anhydrous tetrahydrofuran, and the mixture was evenly dispersed by ultrasonication for 40 min. 1.5 g of sodium hydride was slowly added in a 60° C. water bath and kept warm for 5 h. Subsequently, 2.5 g of sulfanilic acid was added to the mixture, and the mixture was stirred at 80° C. for 25 h.
[0085] (5) The product obtained in step (4) was immersed in a 1:1 volume ratio HCl:H2O solution for 12 h, rinsed with anhydrous ethanol four times to remove the reaction residue, dried in a vacuum oven at 80 ° C for 24 h, taken out and diluted with anhydrous ethanol to 1 mg / ml, and ultrasonicated for 30 min to obtain a sulfonated graphene solution.
[0086] (6) Add 50 g of ultrafine carbon powder to 500 ml of sulfonated graphene solution, stir mechanically for 3 h, and then ultrasonically vibrate for 1.5 h to obtain a uniformly dispersed composite solution; the mechanical stirring speed is 900 rpm.
[0087] (7) placing the solution in a centrifugal spray dryer, spraying it in a high-temperature hot air flow and drying it, to obtain a spherical composite powder of sulfonated graphene-coated carbon powder particles; wherein the centrifugal spray dryer has a feed rate of 25 ml / min, a spray pressure of 0.25 MPa, an inlet air temperature of 125°C, and an outlet air temperature of 80°C.
[0088] (8) The composite powder obtained in step (7) and the modified coal tar pitch were kneaded at a mass ratio of 35:25 at 280° C. for 2 h, and after being taken out, the mixture was kept under pressure at a pressing pressure of 15 MPa for 8 min; wherein the kneading machine speed was 1800 rpm and the pressing temperature was 170° C.
[0089] (9) After the green body is taken out, high-temperature carbonization is performed, the temperature is increased to 160°C at a rate of 45°C / h, then the temperature is increased to 530°C at a constant rate of 10°C / h, and the temperature is increased to 1100°C at a rate of 60°C / h. The temperature is kept at this rate for 140 hours to obtain a graphene-enhanced pantograph slide material.
[0090] Example 3
[0091] This embodiment provides a method for preparing a carbon-based composite material based on sulfonated graphene modification, which specifically includes the following steps:
[0092] (1) 200 ml of 98% concentrated sulfuric acid and 18 g of potassium permanganate were added to a mixture of 2 g of natural graphite flakes and 2 g of sodium nitrate. The mixture was kept at a temperature of 30° C. using a warm water bath method and mechanically stirred for 15 h at a speed of 700 rpm.
[0093] (2) The mixture was diluted with 200 ml of deionized water, and then 200 ml of a 5 wt% hydrogen peroxide solution was added. After mechanical stirring for 5 hours, the mixture was allowed to stand for 5 hours. The supernatant was filtered and washed with concentrated hydrochloric acid and deionized water until it was neutral (pH = 7.0).
[0094] (3) The supernatant obtained in step (2) is subjected to ultrasonic treatment for 2 hours, centrifuged for 20 minutes, and dried under vacuum conditions at a temperature of 85° C. to obtain graphene oxide; wherein the centrifugal speed is 7000 rpm.
[0095] (4) 0.2 g of the graphene oxide obtained in step (3) was added to 250 ml of anhydrous tetrahydrofuran, and the mixture was evenly dispersed by ultrasonication for 45 min. 1.5 g of sodium hydride was slowly added in a 60° C. water bath and kept warm for 6 h. Subsequently, 2.5 g of sulfanilic acid was added to the mixture, and the mixture was stirred at 80° C. for 30 h.
[0096] (5) The product obtained in step (4) was immersed in a 1:1 volume ratio HCl:H2O solution for 12 h, rinsed with anhydrous ethanol 5 times to remove the reaction residue, dried in a vacuum oven at 85 ° C for 24 h, taken out and diluted with anhydrous ethanol to 1 mg / ml, and ultrasonicated for 35 min to obtain a sulfonated graphene solution.
[0097] (6) 25 g of ultrafine carbon powder was added to 500 ml of sulfonated graphene solution, mechanically stirred for 4 h, and then ultrasonically vibrated for 2 h to obtain a uniformly dispersed composite solution; the mechanical stirring speed was 1000 rpm.
[0098] (7) placing the solution in a centrifugal spray dryer, spraying it in a high-temperature hot air flow and drying it, to obtain a spherical composite powder of sulfonated graphene-coated carbon powder particles; wherein the centrifugal spray dryer has a feed rate of 30 ml / min, a spray pressure of 0.3 MPa, an inlet air temperature of 130°C, and an outlet air temperature of 95°C.
[0099] (8) The composite powder obtained in step (7) and the modified coal tar pitch are kneaded at a mass ratio of 40:30 at 300°C for 3 h, and after being taken out, the mixture is kept under pressure at a stamping pressure of 18 MPa for 10 min; wherein the kneading machine speed is 2000 rpm and the stamping temperature is 180°C.
[0100] (9) After the green body is taken out, high-temperature carbonization is performed, the temperature is increased to 180°C at a rate of 50°C / h, then the temperature is increased to 550°C at a constant rate of 15°C / h, and the temperature is increased to 1200°C at a rate of 70°C / h. The temperature is kept at this rate for 150 hours to obtain a graphene-enhanced pantograph slide material.
[0101] Comparative Example
[0102] This comparative example provides a conventional method for preparing a graphene-enhanced pantograph slide plate, comprising the following steps:
[0103] (1) 200 ml of 98% concentrated sulfuric acid and 18 g of potassium permanganate were added to a mixture of 2 g of natural graphite flakes and 2 g of sodium nitrate. The mixture was kept at a temperature of 30° C. using a warm water bath method and mechanically stirred for 13 h at a speed of 650 rpm.
[0104] (2) The mixture was diluted with 200 ml of deionized water, and then 200 ml of a 4 wt% hydrogen peroxide solution was added. The mixture was mechanically stirred for 4 hours and then allowed to stand for 4 hours. The supernatant was filtered and washed with concentrated hydrochloric acid and deionized water until it was neutral (pH = 7.0).
[0105] (3) The supernatant obtained in step (2) is ultrasonicated for 1.5 hours, centrifuged for 20 minutes, and dried under vacuum conditions at a temperature of 80° C. to obtain graphene oxide; wherein the centrifugal speed is 7000 rpm.
[0106] (4) 0.2 g of the graphene oxide obtained in step (3) was added to 250 ml of anhydrous tetrahydrofuran, and the mixture was evenly dispersed by ultrasonication for 40 min. 1.5 g of sodium hydride was slowly added in a 60° C. water bath and kept warm for 5 h. Subsequently, 2.5 g of sulfanilic acid was added to the mixture, and the mixture was stirred at 80° C. for 25 h.
[0107] (5) The product obtained in step (4) was immersed in a 1:1 volume ratio HCl:H2O solution for 12 h, rinsed with anhydrous ethanol 4 times to remove the reaction residue, and dried in a vacuum oven at 80 ° C for 24 h to obtain sulfonated graphene.
[0108] (6) Sulfonated graphene, ultrafine carbon powder, and modified coal tar pitch were kneaded at a high temperature of 300°C in a mass ratio of 4:40:30 for 3 h, and then taken out and kept under pressure for 10 min at a stamping pressure of 18 MPa; the kneading machine speed was 2000 rpm and the stamping temperature was 180°C.
[0109] (7) After the green billet is taken out, high-temperature carbonization is carried out by heating the temperature to 180°C at a rate of 50°C / h, then heating the temperature to 550°C at a constant rate of 15°C / h, and then heating the temperature to 1200°C at a rate of 70°C / h, and keeping the temperature for 150 hours.
[0110] The performance of the pantograph slide plate materials prepared in the above Examples 1-3 and the comparative example was tested. The resistivity of different slide plate materials was measured using a high-precision resistance tester, the compressive strength and flexural strength of the slide plate materials were tested using an electronic universal material testing machine, the thermal conductivity of the materials was measured using a laser thermal conductivity meter, and the average wear rate of the materials was tested using a "Z"-shaped reciprocating current-carrying friction and wear test platform. The test results are shown in Table 1:
[0111] Table 1 Performance test table of the skateboard materials prepared in the embodiments and the comparative examples
[0112]
[0113] As shown in Table 1: The present invention uses centrifugal spray drying to obtain sulfonated graphene / carbon powder coated composite powder. Compared with the method of the control example, the obtained pantograph slide material has improved flexural and compressive strength, enhanced electrical and thermal conductivity, and reduced average wear rate, which can better meet the current requirements for safe and stable current collection of pantograph slide materials under high-speed and heavy-load conditions of electrified railways. In particular, the specific spray drying conditions developed by the present invention are mainly based on the spray drying conditions developed based on the performance of the final slide material, and are not based on the spray drying conditions developed based on the performance of the spherical composite powder obtained after spray drying. This is particularly critical to the inventive concept of this application.
[0114] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
[0115] The above is only a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any person skilled in the art can easily think of changes or substitutions within the technical scope disclosed by the present invention, which should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention should be based on the protection scope of the claims.
Claims
1. A method for preparing a carbon-based composite material based on sulfonated graphene modification, characterized in that: include: Adding carbon powder with an average particle size of 0.1-1 μm into the sulfonated graphene solution, and mixing them evenly to obtain a composite solution; The composite solution is spray-dried to obtain spherical composite powder of sulfonated graphene-coated carbon powder particles; The spherical composite powder and modified coal tar pitch are kneaded and pressed to form a green body; The green body is carbonized at high temperature to obtain a carbon-based composite material modified by sulfonated graphene.
2. The method for preparing a carbon-based composite material based on sulfonated graphene modification according to claim 1, characterized in that: The purity of the carbon powder is greater than 99.9%, and the specific surface area is 27m 2 / g, volume density is 1.35g / cm 3 And the density is 1.8g / cm 3 .
3. The method for preparing a carbon-based composite material based on sulfonated graphene modification according to claim 1, characterized in that: The steps for preparing the sulfonated graphene solution include: Concentrated sulfuric acid and potassium permanganate are successively added to a mixture of natural graphite sheets and sodium nitrate to obtain a mixed solution, the temperature of the mixed solution is controlled to be 25-35° C. by a warm water bath method, and mechanically stirred for 10-15 hours; diluting the stirred mixed solution with deionized water and adding a hydrogen peroxide solution, mechanically stirring and then standing to obtain a solution after standing, filtering the solution after standing to obtain a supernatant, and washing the supernatant with concentrated hydrochloric acid and deionized water until it is neutral; The supernatant washed to neutrality is subjected to ultrasonication and then centrifuged, and dried under vacuum conditions to obtain graphene oxide; The graphene oxide is added to anhydrous tetrahydrofuran, and then ultrasonically dispersed to obtain an ultrasonic dispersion solution, sodium hydride is slowly added to the ultrasonic dispersion solution under a 60° C. water bath condition, and the temperature is kept for 4-6 hours, and then sulfanilic acid is added to the ultrasonic dispersion solution, and stirred at 80° C. for 20-30 hours to obtain a stirred product; The stirred product is immersed in a hydrochloric acid solution for 12 hours, rinsed with anhydrous ethanol for 3-5 times to remove reaction residues, and dried in a vacuum oven to obtain sulfonated graphene. The sulfonated graphene is mixed with anhydrous ethanol and ultrasonically treated to obtain a sulfonated graphene solution.
4. The method for preparing a carbon-based composite material based on sulfonated graphene modification according to claim 1, characterized in that: The mass ratio of the sulfonated graphene to the carbon powder in the composite solution is 0.005-0.02:
1.
5. The method for preparing a carbon-based composite material based on sulfonated graphene modification according to claim 1, characterized in that: The mixing method of adding carbon powder to the sulfonated graphene solution and then mixing the two includes mechanical stirring and ultrasonic oscillation, wherein the mechanical stirring speed is 800-1000 rpm, the stirring time is 2-4 hours, and the ultrasonic oscillation time is 1-2 hours.
6. The method for preparing a carbon-based composite material based on sulfonated graphene modification according to claim 1, characterized in that: The spherical composite powder and the modified coal tar pitch are mixed and kneaded in a mass ratio of 30-40:20-30.
7. The method for preparing a carbon-based composite material based on sulfonated graphene modification according to claim 1, characterized in that: The kneading temperature of the kneading treatment is 250-300° C., the kneading speed is 1500rpm-2000rpm and the kneading time is 1-3h. The stamping temperature of the stamping treatment is 160-180° C., the stamping pressure is 12-18MPa and the holding time is 5-10min.
8. The method for preparing a carbon-based composite material based on sulfonated graphene modification according to claim 1, characterized in that: The carbonization temperature change process of the high temperature carbonization includes: First, heat up to 150-180℃ at 40-50℃ / h; Then increase the temperature to 500-550℃ at a constant rate of 5-15℃ / h; Then the temperature is raised to 1000-1200℃ at a rate of 50-70℃ / h; Finally keep warm for 120-150h.
9. A product, characterized in that The product is a carbon-based composite material based on sulfonated graphene modified and prepared according to the method for preparing a carbon-based composite material based on sulfonated graphene modified according to any one of claims 1 to 9.
10. Application of the product of claim 9 in rocket engine nozzles, aircraft brake discs and pantograph slides of electric trains.
Citation Information
Patent Citations
Preparation method of silicon and carbon-coated graphene composite cathode material
CN103050666A
Carbon-coated nano silicon / graphene / cracked carbon layer composition material, preparation method, and lithium ion battery including the composition material
CN106067547A
Method for preparing pantograph carbon slide strip material from graphene oxide
CN106699181A
Graphene coated carbon composite material and preparation method thereof
CN108390024A
Preparation method of pantograph carbon sliding strip material enhanced by graphene and material