Preparation method of metal organic framework nanorod cluster / rGO composite material

The MOF material is converted into a nanorod cluster structure through microwave irradiation, and is in close contact with rGO, which solves the interface problem when the metal-organic framework is combined with graphene, significantly improves the catalytic performance and thermal stability, and achieves efficient photonics. catalytic effect.

CN118755104AActive Publication Date: 2024-10-11UNIV OF SHANGHAI FOR SCI & TECH

Patent Information

Application Number
CN202411079453.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-07
Publication Date
2024-10-11
Estimated Expiration
2044-08-07

AI Technical Summary

Technical Problem

When metal organic framework materials are combined with graphene, it is difficult to achieve precise placement and interface enhancement, resulting in a reduction in catalytic active sites and poor thermal stability, which limits its application in the field of catalysis.

Method used

The microwave irradiation method is used to convert the MOF material into a nanorod cluster structure, which is in close contact with rGO. It builds an in-situ hot spot through the microwave popcorn effect, increases the specific surface area and active sites of the material, and forms an efficient composite interface.

Benefits of technology

It significantly improves the specific surface area and photocatalytic performance of MOF and rGO composite materials, improves the conversion rate and selectivity of NO oxidation and CO2 reduction, and enhances the thermal stability of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118755104A_ABST
    Figure CN118755104A_ABST
Patent Text Reader

Abstract

The invention relates to a preparation method of a metal organic framework (MOF) nanorod cluster / rGO composite material, which comprises the following steps: placing an MOF / rGO composite material with a one-dimensional structure in a closed reactor, and carrying out microwave irradiation in a certain atmosphere to obtain the composite material formed by nanorod cluster-shaped MOF and rGO. Compared with the prior art, based on the microwave popcorn effect, the structure of the composite material is changed, the specific surface area and active sites of the material are greatly improved, and the application potential is huge.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of nanomaterials, and in particular to a method for preparing a metal organic framework nanorod cluster / rGO composite material based on microwave popcorn effect. Background Art

[0002] Metal organic frameworks (MOFs) are organic-inorganic hybrid materials with intramolecular pores formed by self-assembly of organic ligands and metal ions or clusters through coordination bonds. MOF materials have an ordered porous structure, a large specific surface area, and adjustable organic ligands or metal ions, and have broad application prospects. However, due to the poor conductivity of MOFs, their practical application is limited. Graphene is a sp 2 Two-dimensional materials composed of hybrid carbon atoms have extremely high electron mobility (250,000cm 2 ·V -1 ·s -1 ) and large specific surface area (2630m 2 ·g -1 ). If MOF materials can be effectively composited with graphene materials (GO / rGO, etc.), the conductivity of MOF materials can be effectively improved, and more adsorption and catalytic sites can be provided, thus expanding their applications in various fields. However, most MOFs are large-sized crystal structures, which cannot effectively expose active sites and cannot form the maximum interface contact with rGO. Therefore, it is necessary to develop a method to achieve a composite interface with good compatibility, electron transport and stability between MOFs of specific morphology and rGO.

[0003] Patent application 202310704536.0 discloses a metal-organic framework-graphene composite material, which is composed of a metal-organic framework and functionalized graphene composited together through supramolecular interactions; the organic ligand molecule of the metal-organic framework is tetracarboxyphenylporphyrin iron, and the coordinated metal ion is at least one of cobalt, nickel, copper, and zinc; the functionalized graphene is graphene modified with organic small molecules, and the organic small molecules include at least one of 5-amino-1-naphthalenesulfonic acid, sodium anthraquinone-2-sulfonate, and naphthalene-1-sulfonic acid. The metal organic framework host of the invention and the functionalized graphene guest form a heterogeneous structure through supramolecular interaction, which is beneficial to the electronic conduction of the composite material, greatly improving the gas sensing performance, and has the characteristics of strong selectivity, high sensitivity, low power consumption, and high stability. However, it is difficult for MOF to achieve precise placement on the graphene sheet. MOF is easy to self-assemble and crystallize, and it is easy to agglomerate, resulting in a reduction in catalytic active sites, which hinders the formation of an effective interface between MOF and graphene; and MOF materials have poor thermal stability, and the traditional calcination method for enhancing the interface is prone to cause the collapse of the pore structure and the conversion of MOF materials into metal elements or metal carbides, which lose their semiconductor properties and become completely inactivated. Therefore, how to develop a new catalyst synthesis method to achieve precise placement and interface enhancement of MOF materials on the graphene surface is particularly important for improving the photocatalytic performance of MOF-rGO composite materials. Summary of the invention

[0004] The purpose of the present invention is to overcome the defects of the above-mentioned prior art and provide a method for preparing a metal organic framework nanorod cluster / rGO composite material which can greatly improve the specific surface area and active sites of the material and significantly strengthen the composite interface between MOF and rGO.

[0005] The objective of the present invention can be achieved by the following technical scheme: a method for preparing a metal organic framework nanorod cluster / rGO composite material, wherein a MOF / rGO composite material having a one-dimensional structure is placed in a closed reactor and subjected to microwave irradiation in a certain atmosphere to obtain a composite material formed by nanorod cluster MOF and rGO.

[0006] Furthermore, the MOF material uses metal ions as the metal center and tetrakis(4-carboxyphenyl)porphine (TCPP), terephthalic acid (PTA), 2-aminoterephthalic acid (H2ATA) or trimesic acid (H3BTC) as the ligand.

[0007] Furthermore, the metal ions include Zr 4+ , Fe 3+ 、V 4+ 、Bi 3+ 、Ti 4+ 、Zn 2+ 、Co 3+ , Cu2+ .

[0008] Furthermore, the MOF and rGO composite material is prepared by the following method:

[0009] The ligand is dissolved in a solvent, and metal salt and graphene powder are added, and the mixture is stirred and ultrasonicated for 0.5 to 1 hour to form a suspension. The suspension is transferred to a microwave reactor, heated to 90-180°C, reacted for 0.5-2 hours, cooled to room temperature, centrifuged, washed to obtain a solid product, and dried at 70 to 90°C to obtain a MOF / rGO composite material with a one-dimensional structure.

[0010] Furthermore, the mass ratio of the ligand to the graphene powder is 100:5-40.

[0011] Furthermore, the solvent is N,N-dimethylformamide.

[0012] Furthermore, during the microwave irradiation process, the microwave power is 50 to 1200 W and the microwave frequency is 1 to 15 GHz.

[0013] Furthermore, the certain atmosphere is air, argon, nitrogen, carbon dioxide or vacuum. Preferably, vacuum or nitrogen,

[0014] Furthermore, the microwave irradiation time is 2-600s, and the number of irradiation cycles is 1-10 times.

[0015] Compared with the prior art, the present invention has the following beneficial effects:

[0016] The principle of microwave popcorn is to use microwave radiation energy to induce the steam of water inside the popcorn to produce thermal expansion and contraction effect, so that the popcorn expands rapidly and forms a fluffy structure. The present invention uses the wave absorbing and heat releasing properties of reduced graphene oxide to construct an in-situ hot spot, so that the nano-bundle MOF material located on reduced graphene oxide (rGO) can also "pop" like popcorn under the action of solid-phase microwaves. The original one-dimensional structure of MOF expands into a nanorod cluster structure and is in close contact with rGO. This structural change greatly increases the specific surface area and active sites of the material and significantly strengthens the composite interface between MOF and rGO.

[0017] The present invention adopts a microwave modification method, which has the advantages of being simple, environmentally friendly, and highly efficient. At the same time, the solid-phase microwave method is used to construct an in-situ hot spot, produce a microwave popcorn effect, and realize controllable adjustment of the selected MOF morphology, significantly strengthening the composite interface between the MOF material and rGO, and further improving the material performance: for example, the metal organic framework nanorod cluster / rGO composite material obtained after solid-phase microwave treatment of the present invention has a high conversion rate and high selectivity for NO oxidation; the photocatalytic performance of the material is improved, etc. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 These are the SEM images of the stone metal organic framework nanorod clusters / rGO composite material prepared in Example 1 and the sample before microwave.

[0019] Figure 2 XRD patterns of the metal organic framework nanorod cluster / rGO composite material and the sample before microwave prepared in Example 2;

[0020] Figure 3 N2 adsorption-desorption isotherms of the metal organic framework nanorod cluster / rGO composite material and the sample before microwave prepared in Example 3;

[0021] Figure 4 Comparison of NO oxidation performance of the metal organic framework nanorod cluster / rGO composite materials prepared in Examples 1 to 5 and the pre-microwave sample of Example 3 under LED simulated sunlight;

[0022] Figure 5 Comparison of NO oxidation performance of the metal organic framework nanorod cluster / rGO composite material prepared in Example 6 with that of Comparative Examples 1 and 2 under LED simulated sunlight;

[0023] Figure 6 A comparison chart of the photocatalytic CO2 reduction performance of the metal organic framework nanorod cluster / rGO composite material prepared in Example 8 and Example 9 and the sample before microwave under the same conditions;

[0024] Figure 7 This is a comparison chart of the photocatalytic CO2 reduction performance of the metal organic framework nanorod cluster / rGO composite material prepared in Example 10 and Example 11 and the sample before microwave under the same conditions;

[0025] Figure 8 This is a comparison chart of the photocatalytic CO2 reduction performance of the metal organic framework nanorod clusters / rGO composite materials prepared in Example 12 and Example 13 and the pre-microwave samples under the same conditions. DETAILED DESCRIPTION

[0026] The present invention is described in detail below with reference to the accompanying drawings and specific embodiments.

[0027] The composite catalytic material of the present invention mainly uses the microwave method to compound MOF and rGO. Microwave is an electromagnetic wave with a wavelength between infrared and radio waves, usually defined as a wavelength range between 1 mm and 1 m. Microwave is a low-energy electromagnetic radiation that can propagate in transparent media such as air, glass, and plastic, and has some special physical and chemical properties. Microwave technology is widely used in the fields of communication and wireless technology, medical diagnosis and treatment, astronomical observation, and material synthesis and processing. Especially in the field of material synthesis and processing, the microwave method is a synthesis method that acts on the inside of the material and achieves an efficient and uniform thermal effect from the inside out by affecting the dipole vibration of the molecules. In solid-phase heating, based on the ultra-high wave absorption and heat release performance of carbon-based materials, rapid chemical reactions can be achieved within seconds.

[0028] The metal organic framework nanorod cluster / rGO composite material of the present invention is prepared by the following method:

[0029] S1: Preparation of MOF material: dissolve the ligand in a solvent, add metal salt and graphene powder (GO), stir and ultrasonicate for 0.5-1h to form a suspension, and transfer the suspension to a polytetrafluoroethylene microwave reactor, heat to 90-180°C, react for 0.5-2h, cool to room temperature, centrifuge and wash the solid product with DMF and methanol, and dry at 70-90°C to obtain a MOF / rGO composite material;

[0030] Among them, MOF materials use metal ions such as Zr, Fe, V, Bi, Ti, Zn, Co, and Cu as metal centers, and four organic molecules such as tetrakis (4-carboxyphenyl) porphine (TCPP), terephthalic acid (PTA), 2-aminoterephthalic acid (H2ATA), and trimesic acid (H3BTC) as ligands. The solvent is N,N-dimethylformamide (DMF), and the GO source is commercially available from Shenzhen Suiheng, model SH-GO-1208.

[0031] S2: irradiation using solid phase microwaves;

[0032] The MOF / rGO composite material obtained in step S1 is placed in a quartz sealed container and irradiated with solid-phase microwave to obtain a product; during the microwave irradiation process, the reaction conditions are set to a microwave power of 50 to 1200 W, a microwave frequency of 1 to 15 GHz, and a reaction atmosphere of air, argon, nitrogen, carbon dioxide or vacuum.

[0033] The following embodiments are implemented based on the above technical solution of the present invention, and provide detailed implementation methods and specific operation processes, but the protection scope of the present invention is not limited to the following embodiments.

[0034] Embodiment 1:

[0035] Metal organic framework nanorod clusters / rGO composite materials are prepared by the following method:

[0036] S1: Add 100 mg TCPP to 50 mL DMF solution and stir to form a transparent purple solution. Add 150 mg zirconium tetrachloride (ZrCl4) and 48 mg GO powder to the brown solution. After that, stir and ultrasonicate the mixture for 30 minutes to form a suspension. Transfer the suspension to a polytetrafluoroethylene microwave reactor and heat it to 100°C within 15 minutes using a programmed microwave digestion system. After the microwave reactor was kept at 90°C for 30 minutes, it was cooled to room temperature. The solid product was centrifuged and washed with DMF and methanol to obtain the solid product. Dry at 80°C to form a dark red powder, and obtain a Zr-TCPP / rGO composite material sample (morphology as shown Figure 1 (shown in a).

[0037] S2: The sample was evenly placed at the bottom of a quartz sealed container, the reaction atmosphere was air, and then the microwave frequency was 2.45 GHz, the microwave power was 300 W, and the reaction was performed for 5 seconds to obtain a dark red powder (morphology as Figure 1 (as shown in b).

[0038] The microstructure and structure of the composite material sample prepared in Example 1 were characterized by transmission electron microscopy (SEM, FEIQuanta FEG). Figure 1 (ab), where a is the morphology of the MOF nanorod cluster / rGO composite material prepared in Example 1 before microwave reaction, and b is the morphology after microwave reaction. It can be found that after solid-phase microwave thermal shock, the MOF nanorods combined with rGO exploded from the center to form a nanorod cluster assembled flower ball structure, which greatly increased the specific surface area and the interface coupling with rGO.

[0039] Embodiment 2:

[0040] The preparation method is different from that in Example 1 in that the amount of GO added is 12 mg and the reaction temperature is 120° C. The sample is evenly placed at the bottom of a quartz sealed container, the reaction atmosphere is Ar, and then the microwave frequency is 2.45 GHz, the microwave power is 500 W, and the reaction is performed for 15 seconds to obtain a deep red powder.

[0041] The crystal structure of the sample was characterized by X-ray diffraction (XRD, Bruker D8 ADVANCE). The XRD patterns of the metal organic framework nanorod cluster / rGO composite material prepared in Example 2 and the sample before microwave were as follows: Figure 2 As shown, XRD confirmed that the crystallinity was significantly improved after microwave irradiation.

[0042] Embodiment 3:

[0043] The preparation method is different from that in Example 1 in that the amount of GO added is 24 mg and the reaction temperature is 150° C. The sample is evenly placed at the bottom of a quartz sealed container, the reaction atmosphere is vacuum, and then the microwave frequency is 2.45 GHz, the microwave power is 700 W, and the reaction is performed for 5 seconds to obtain a deep red powder.

[0044] Figure 3 The N2 adsorption-desorption isotherms of the metal organic framework nanorod cluster / rGO composite material and the sample before microwave prepared in Example 3; Figure 3 It can be seen that the adsorption capacity of the sample before microwave is 239.4m 2 / g, and the adsorption capacity of the sample obtained after microwave was 586.1m 2 / g, it can be seen that the specific surface area is increased due to the change in the solid phase morphology after microwave treatment of the present invention, thereby greatly improving the adsorption capacity of the material.

[0045] Embodiment 4:

[0046] The preparation method of Zr-TCPP / rGO composite material samples is the same as that in Example 1. The samples are evenly placed at the bottom of a quartz sealed container. The reaction atmosphere is CO2. Then, at a microwave frequency of 5.45 GHz and a microwave power of 900 W, the reaction is carried out for 30 seconds to obtain a deep red powder.

[0047] Embodiment 5:

[0048] The preparation method of Zr-TCPP / rGO composite material samples is the same as that in Example 2. The samples are evenly placed at the bottom of a quartz sealed container, the reaction atmosphere is N2, and then at a microwave frequency of 7.45 GHz, a microwave power of 1200 W, a reaction time of 120 s, and irradiation cycles of 2 times to obtain a black-red powder.

[0049] Figure 4 The NO oxidation performance of the metal organic framework nanorod cluster / rGO composite materials prepared in Examples 1 to 5 and the sample before microwave in Example 3 under LED simulated sunlight is compared; it can be seen from the figure that the NO removal rate of MOF / rGO after microwave irradiation is significantly improved compared with that before microwave, among which Example 3 has the highest NO removal rate, reaching 68.5%.

[0050] Embodiment 6:

[0051] The preparation method of Zr-TCPP / rGO composite material samples is the same as that in Example 3. The samples are evenly placed at the bottom of a quartz sealed container, the reaction atmosphere is N2, and then at a microwave frequency of 10.45 GHz, a microwave power of 1200 W, a reaction time of 240 s, and 4 irradiation cycles, a black-red powder is obtained.

[0052] Embodiment 7:

[0053] The preparation method is different from that in Example 1 in that the amount of GO added is 6 mg and the reaction temperature is 150° C. The sample is evenly placed at the bottom of a quartz sealed container, the reaction atmosphere is vacuum, and then at a microwave frequency of 2.45 GHz, a microwave power of 700 W, a reaction time of 600 s, and 10 irradiation cycles, a black-red powder is obtained.

[0054] Embodiment 8:

[0055] The preparation method is different from that of Example 1 in that the ligand is PTA and the metal source is vanadyl sulfate (VOSO4). The sample is evenly placed at the bottom of a quartz sealed container, the reaction atmosphere is air, and then the microwave frequency is 2.45 GHz, the microwave power is 300 W, and the reaction is performed for 30 seconds to obtain a gray-green powder.

[0056] Embodiment 9:

[0057] The preparation method is different from that of Example 8 in that the amount of GO added is 30 mg. The sample is evenly placed at the bottom of a quartz sealed container, the reaction atmosphere is vacuum, and then the microwave frequency is 2.45 GHz, the microwave power is 700 W, and the reaction is performed for 30 seconds to obtain a gray-green powder.

[0058] Embodiment 10:

[0059] The preparation method is different from that of Example 1 in that the ligand is H3BTC, the metal source is bismuth oxynitrate pentahydrate (Bi(NO3)3·5H2O), the amount of GO added is 24 mg, the reaction temperature is 150°C, and the temperature is kept for 1 hour. The sample is evenly placed at the bottom of a quartz sealed container, the reaction atmosphere is CO2, and then at a microwave frequency of 5.45 GHz, the microwave power is 1200 W, the reaction is 120 seconds, and the number of irradiation cycles is 2 times to obtain a light gray powder.

[0060] Embodiment 11:

[0061] The preparation method is different from that of Example 10 in that the amount of GO added is 48 mg. The sample is evenly placed at the bottom of a quartz sealed container, the reaction atmosphere is N2, and then at a microwave frequency of 5.45 GHz, a microwave power of 1200 W, a reaction time of 60 s, and an irradiation cycle of 1 time, a light gray powder is obtained.

[0062] Embodiment 12:

[0063] The preparation method is different from that of Example 1 in that the ligand is H2ATA, the metal source is ferric chloride hexahydrate (FeCl3·6H2O), the solvent is ultrapure water, the reaction temperature is 120°C, and the temperature is kept for 1 hour. The sample is evenly placed at the bottom of a quartz sealed container, the reaction atmosphere is Ar, and then the microwave frequency is 2.45 GHz, the microwave power is 300 W, and the reaction is carried out for 30 seconds to obtain a brown powder.

[0064] Embodiment 13:

[0065] The difference between the preparation method and Example 1 is that the amount of GO added is 24 mg. The sample is evenly placed at the bottom of a quartz sealed container, the reaction atmosphere is Ar, and then at a microwave frequency of 7.45 GHz and a microwave power of 500 W, the reaction is performed for 45 seconds to obtain a brown powder.

[0066] Comparative Example 1

[0067] The MOF of Example 1 without rGO was directly placed at the bottom of a quartz sealed container in an air-atmosphere reaction atmosphere, and then reacted for 5 seconds at a microwave frequency of 2.45 GHz and a microwave power of 300 W to obtain a powder.

[0068] Comparative Example 2

[0069] The MOF and rGO of Example 1 were used, mixed and then ultrasonically dispersed.

[0070] The performance tests of the materials obtained in the above examples and comparative examples are as follows:

[0071] 1. The method for testing the NO oxidation performance of the samples prepared in the above embodiments and comparative examples during the photocatalytic process comprises the following steps:

[0072] (1) In a continuous flow reactor, the reactor surface is sealed with quartz glass;

[0073] (2) In each experiment, simulated exhaust gas containing 500 ppb NO was passed at a rate of 2.0 L / min through a reactor containing 0.10 g of the composite material sample prepared in step S1 of each embodiment and comparative example (i.e. before microwave) and the composite material sample prepared in step S2 (i.e. after microwave).

[0074] (3) After 30 min of dark adsorption, when the photocatalyst is in an adsorption-desorption equilibrium state, turn on the LED light (JS-LT225-32W, 420nm~750nm) to simulate sunlight for photocatalytic reaction.

[0075] (4) Using NO-NO2-NO X A dynamic analyzer (Thermo Scientific 42i-TL) was used to monitor the concentration changes of NO and NO2 online.

[0076] The results are as follows:

[0077] NO removal rate before microwave (%) NO removal rate after microwave treatment (%) Example 1 17.6 32.5 Example 2 19.5 36.1 Example 3 20.4 68.5 Example 4 17.6 54.7 Example 5 19.5 45.1 Example 6 20.4 49.5 Example 7 15.7 53.9 Example 8 23.4 59.5 Example 9 21.5 57.1 Example 10 15.3 47.5 Embodiment 11 15.7 36.1 Example 12 27.5 74.3 Embodiment 13 25.4 66.9 Comparative Example 1 13.7 13.7 Comparative Example 2 13.5 13.5

[0078] As shown in the table above, the NO oxidation performance of the metal organic framework nanorod C cluster / rGO composite materials prepared in Examples 1-13 and Comparative Examples 1-2 before and after microwaves under the irradiation of LED simulated sunlight; Figure 5 The NO oxidation performance of the metal organic framework nanorod cluster / rGO composite material prepared in Example 6 before and after microwaves is compared with that of Comparative Examples 1 and 2 under LED simulated sunlight;

[0079] From the above table and Figure 5 It was further confirmed that the metal organic framework nanorod clusters / rGO composite material obtained after solid phase microwave had high conversion rate and high selectivity for NO oxidation, among which Example 3 had the highest NO removal rate, reaching 68.5%, and NO 3 -The selectivity reached 98.7%.

[0080] 2. The performance test method of using the samples prepared in each embodiment and comparative example as catalytic materials in the photocatalytic CO2 reduction reaction includes the following steps:

[0081] Gas-solid phase photocatalytic CO2 reduction occurs in a closed quartz glass reactor at room temperature without the addition of any sacrificial agents or co-catalysts.

[0082] (1) Add 20 mg of photocatalyst (i.e., the sample prepared in each embodiment and comparative example) and 20 mL of deionized water to the bottom of a quartz reactor for ultrasonic dispersion.

[0083] (2) The reactor was transferred to a vacuum oven and dried at 60° C. After the water was completely evaporated, the catalyst powder remained at the bottom of the reactor, forming a uniform photocatalytic layer.

[0084] (3) Take 0.084 g of sodium bicarbonate (NaHCO3) powder and add it into the reactor tank. The reactor is purged with N2 for 30 minutes.

[0085] (4) 30 μL of sulfuric acid (H2SO4) (2 M) was injected into the reaction tank, and the CO2 and H2O vapor required for the photocatalytic reduction of CO2 were obtained through the reaction of H2SO4 and NaHCO3.

[0086] (5) The quartz reactor was placed under a 300W Xe lamp light source (MC-X301, Beijing Meiruichen Technology Co., Ltd.). A filter (AM1.5 G) was used, and the photocatalytic layer obtained in step (2) was 10 cm away from the light source. After 4 hours of illumination, the reactor was assembled on a gas chromatograph to analyze its composition and content.

[0087] The results are as follows:

[0088]

[0089] Figure 6 A comparison chart of the photocatalytic CO2 reduction performance of the metal organic framework nanorod cluster / rGO composite material prepared in Example 8 and Example 9 and the sample before microwave under the same conditions; Figure 7 This is a comparison chart of the photocatalytic CO2 reduction performance of the metal organic framework nanorod cluster / rGO composite material prepared in Example 10 and Example 11 and the sample before microwave under the same conditions; Figure 8 This is a comparison chart of the photocatalytic CO2 reduction performance of the metal organic framework nanorod clusters / rGO composite materials prepared in Example 12 and Example 13 and the pre-microwave samples under the same conditions.

[0090] Combining the above table with Figure 6-8 It can be seen that the photocatalytic CO2 reduction performance of the metal organic framework nanorod cluster / rGO composite material obtained after solid phase microwave treatment is significantly improved, among which Example 12 has the highest CO yield of 23.11 μmol g -1 h -1 The original one-dimensional structure of MOF expanded into a nanorod cluster structure and was in close contact with rGO. The structural change caused by solid-phase microwave greatly increased the specific surface area and active sites of the material, further improving the photocatalytic performance of the material.

[0091] 3. The metal organic framework nanorod cluster / rGO composite materials and pre-microwave samples prepared in each embodiment and comparative example were analyzed using N2 adsorption-desorption isotherms (Micromeritics ASAP2020), and the adsorption-desorption isotherms of N2 for the samples at 77K were measured. Before the test, about 0.10g of the test sample was placed and vacuum pretreated at 80°C for 6h. The corresponding specific surface area of ​​the test sample was calculated according to the Brunauer-Emmet-Tell (BET) equation. The results are as follows:

[0092]

[0093] Among them, Figure 3The specific surface area of ​​the metal organic framework nanorod cluster / rGO composite material prepared in Example 3 and the sample before microwave treatment is 586.1 m 2 / g, almost before microwave (239.4m 2 / g) is 2.5 times. Combining the above table and Figure 3 It is confirmed that the structural changes caused by microwave irradiation of the sample greatly increase the specific surface area of ​​the material. And the specific surface area of ​​the example sample is greater than that of the comparative example.

[0094] The above description of the embodiments is to facilitate the understanding and use of the invention by those skilled in the art. It is obvious that those skilled in the art can easily make various modifications to these embodiments and apply the general principles described herein to other embodiments without creative work. Therefore, the present invention is not limited to the above embodiments, and improvements and modifications made by those skilled in the art based on the disclosure of the present invention without departing from the scope of the present invention should be within the scope of protection of the present invention.

Claims

1. A method for preparing a metal organic framework nanorod cluster / rGO composite material, characterized in that: A MOF / rGO composite material with a one-dimensional structure is placed in a closed reactor and subjected to microwave irradiation in a certain atmosphere to obtain a composite material formed by nanorod cluster MOF and rGO.

2. The method for preparing a metal organic framework nanorod cluster / rGO composite material according to claim 1, characterized in that: MOF materials use metal ions as metal centers and tetrakis(4-carboxyphenyl)porphine (TCPP), terephthalic acid (PTA), 2-aminoterephthalic acid (H2ATA) or trimesic acid (H3BTC) as ligands.

3. The method for preparing a metal organic framework nanorod cluster / rGO composite material according to claim 2, characterized in that: The metal ions include Zr 4+ , Fe 3+ 、V 4+ 、Bi 3+ 、Ti 4+ 、Zn 2+ 、Co 3+ , Cu 2+ .

4. A method for preparing a metal organic framework nanorod cluster / rGO composite material according to any one of claims 1 to 3, characterized in that: The MOF and rGO composite material is prepared by the following method: The ligand is dissolved in a solvent, and metal salt and graphene powder are added, and the mixture is stirred and ultrasonicated for 0.5 to 1 hour to form a suspension. The suspension is transferred to a microwave reactor, heated to 90-180°C, reacted for 0.5-2 hours, cooled to room temperature, centrifuged, washed to obtain a solid product, and dried at 70 to 90°C to obtain a MOF / rGO composite material with a one-dimensional structure.

5. The method for preparing a metal organic framework nanorod cluster / rGO composite material according to claim 4, characterized in that: The mass ratio of the ligand to the graphene powder is 100:5-40.

6. The method for preparing a metal organic framework nanorod cluster / rGO composite material according to claim 4, characterized in that: The solvent is N,N-dimethylformamide.

7. The method for preparing a metal organic framework nanorod cluster / rGO composite material according to claim 1, characterized in that: In the microwave irradiation process, the microwave power is 50-1200W and the microwave frequency is 1-15GHz.

8. The method for preparing a metal organic framework nanorod cluster / rGO composite material according to claim 1, characterized in that: The certain atmosphere is air, argon, nitrogen, carbon dioxide or vacuum.

9. The method for preparing a metal organic framework nanorod cluster / rGO composite material according to claim 1, characterized in that: The microwave irradiation time is 2-600s, and the irradiation cycle times are 1-10 times.

Citation Information

Patent Citations

  • Supported bifunctional catalytic composite material and preparation method thereof

    CN110721728A

  • Preparation method and application of popcorn-based porous carbon material electrode

    CN113582302A

  • Magnetic graphene oxide-metal organic framework nano composite material as well as preparation method and application thereof

    CN114797782A

  • Method for preparing carbon-metal organic frameworks composite using microwave

    KR1020180108221A

Cited By

  • Preparation method of composite additive for lead-carbon battery

    CN122117919A