Modified magnesium hydroxide flame retardant and preparation method thereof

Through the preparation method of modified magnesium hydroxide flame retardant, the combination of wet grinding and organic amine modifiers is used to improve the flame retardant efficiency and dispersion of magnesium hydroxide and solve its flame retardancy in polymer materials. The problems of low efficiency and reduced mechanical properties have been achieved, and better composite material properties have been achieved.

CN118755152APending Publication Date: 2024-10-11JIANGXI GUANGYUAN CHEM +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411036159.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

The flame retardant efficiency of magnesium hydroxide flame retardant in polymer materials is low and the addition amount is large, which leads to a reduction in the mechanical properties of the material, and uneven mixing with transition metal compounds affects the flame retardant effect.

Method used

A transition metal-coated magnesium hydroxide slurry is formed by wet grinding magnesium hydroxide with a surface modifier and a transition metal salt solution, and mixed with an organic amine modifier to form a modified magnesium hydroxide flame retardant , to improve its catalytic carbon-forming ability and dispersion.

Benefits of technology

It significantly improves the flame retardant efficiency and dispersion of magnesium hydroxide, enhances the comprehensive performance of composite materials, reduces the impact on the mechanical properties of polymer materials, and expands the application fields of magnesium hydroxide.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004971121920000051
    Figure BDA0004971121920000051
  • Figure BDA0004971121920000061
    Figure BDA0004971121920000061
  • Figure BDA0004971121920000071
    Figure BDA0004971121920000071
Patent Text Reader

Abstract

The invention provides a modified magnesium hydroxide flame retardant and a preparation method thereof, and relates to the technical field of inorganic flame retardants. The preparation method comprises the following steps: mixing and grinding a magnesium hydroxide coarse material and a surface modifier to obtain magnesium hydroxide particles, and performing wet grinding on the magnesium hydroxide particles and a transition metal salt solution to obtain transition metal coated magnesium hydroxide slurry; and adding an organic amine modifier into the slurry, and grinding to obtain the modified magnesium hydroxide flame retardant. According to the preparation method disclosed by the invention, magnesium hydroxide is modified by utilizing the catalytic char formation performance of transition metal ions and the pH regulation function, coordination function and hydrophobicity of an organic amine long carbon chain; the obtained modified magnesium hydroxide flame retardant has good fluidity, dispersibility, catalytic char formation capability and smoke suppression effect, the addition amount of magnesium hydroxide in the use process is reduced, and the influence of magnesium hydroxide on the mechanical property of a composite material is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of inorganic flame retardants, and in particular to a modified magnesium hydroxide flame retardant and a preparation method thereof. Background Art

[0002] Polymer materials are widely used, but they are flammable and release toxic and harmful gases during combustion, which pollute the environment and cause secondary harm to people. Therefore, in order to reduce the probability of fire and the amount of toxic smoke released, it is necessary to modify the polymer materials to make them flame retardant. Adding flame retardants to polymer materials is one of the common methods, which is economical, simple and easy.

[0003] Magnesium hydroxide is a classic filling flame retardant. It releases bound water when the material is heated and decomposed during combustion, absorbing a large amount of latent heat to reduce the surface temperature of the synthetic material it fills in the flame. It has the effect of inhibiting the decomposition of polymers and cooling the generated combustible gases. The decomposed magnesium oxide is also a good refractory material. Covering the surface of the burning material, it can also help improve the fire resistance of the synthetic material. At the same time, the water vapor it releases can also be used as a smoke suppressant. Therefore, magnesium hydroxide is recognized as an excellent flame retardant with the triple functions of flame retardancy, smoke suppression and filling in the rubber and plastic industry. It is widely used in rubber, chemicals, building materials, plastics and electronics, unsaturated polyesters, paints, coatings and other polymer materials. However, as an inorganic flame retardant, magnesium hydroxide needs to be added to the material in large quantities during use to exert certain flame retardant properties, and the flame retardant efficiency is low. After adding a large amount of magnesium hydroxide, the mechanical properties of polymer materials will also be reduced, limiting its scope of application.

[0004] Transition metals have a catalytic carbonization effect and can promote the cross-linking of carbon layers, thereby forming a denser carbon layer. Studies have found that by adding 1-2% of transition metal compounds to the PP / APP / PER system, the limiting oxygen index value of the composite material can be increased from 29.0% to 31.0%, and the UL-94 test is increased from V-1 to V-0, with obvious effects. However, the transition metal compound and magnesium hydroxide are not mixed evenly, which will affect the flame retardant effect, and the large amount of magnesium hydroxide added is easy to agglomerate in the polymer material, making it difficult to obtain a composite material with excellent performance.

[0005] Therefore, how to improve the flame retardant properties of magnesium hydroxide flame retardant and its dispersion performance in polymer materials, thereby reducing its influence on the mechanical properties of polymer materials is a problem that needs to be solved urgently by those skilled in the art. Summary of the invention

[0006] The object of the present invention is to provide a modified magnesium hydroxide flame retardant and a preparation method thereof, so as to solve the problem that the magnesium hydroxide flame retardant has low flame retardant efficiency, large addition amount and is not easy to disperse, resulting in reduced mechanical properties of polymer materials.

[0007] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0008] The present invention provides a method for preparing a modified magnesium hydroxide flame retardant, comprising the following steps:

[0009] 1) mixing and grinding a magnesium hydroxide coarse material with a surface modifier to obtain magnesium hydroxide particles, and wet-grinding the magnesium hydroxide particles and a transition metal salt solution to obtain a transition metal-coated magnesium hydroxide slurry;

[0010] 2) Mixing the transition metal ion-coated magnesium hydroxide slurry with an organic amine modifier and grinding the mixture to obtain a modified magnesium hydroxide flame retardant.

[0011] Preferably, the surface modifier in step 1) comprises one or more of acrylate, polyacrylic acid, methyl methacrylate oligomer, monolauryl phosphate, potassium monododecyl phosphate, potassium lauryl ether phosphate, and ammonium sulfate of fatty alcohol polyoxyethylene ether;

[0012] The mass ratio of the surface modifier to magnesium hydroxide is 1:50-1000.

[0013] Preferably, the transition metal ion in the transition metal salt solution in step 1) is Ce 4+ ,La 3+ and Ni 3+ One or more of the following;

[0014] The mass ratio of the transition metal ion to the magnesium hydroxide is 1:100-1000.

[0015] Preferably, the particle size of the magnesium hydroxide coarse material in step 1) is 0.1 to 50 μm.

[0016] Preferably, the grinding temperature in step 1) is 55-90° C., and the particle size of the magnesium hydroxide particles is 0.1-10 μm.

[0017] Preferably, the wet grinding time in step 1) is 1 to 3 hours.

[0018] Preferably, the general formula of the organic amine modifier in step 2) is Wherein R1 is an alkane group, R2 and R3 are independently H or an alkane group;

[0019] The mass ratio of the organic amine modifier to the magnesium hydroxide crude material is 1:50-200.

[0020] Preferably, the grinding time in step 2) is 1 to 3 hours.

[0021] The present invention also provides a modified magnesium hydroxide flame retardant prepared by the above preparation method.

[0022] The present invention has at least the following beneficial effects:

[0023] The catalytic carbonization function of transition metals is utilized to improve the catalytic carbonization ability of magnesium hydroxide, thereby improving the flame retardant efficiency of magnesium hydroxide; through the pH adjustment function and coordination function of organic amines, transition metals and magnesium ions are coordinated to form a stable modified coating layer, which can reduce the agglomeration and overlap of particles, enhance the powder fluidity and hydrophobicity of particles, and improve the dispersibility of particles in a polymer matrix, which is of great significance to improving the comprehensive performance of composite materials and expanding the application field of magnesium hydroxide. The present invention has the advantages of scientific and reasonable design, simple operation process, low production cost and easy large-scale production. DETAILED DESCRIPTION

[0024] The present invention provides a method for preparing a modified magnesium hydroxide flame retardant, comprising the following steps:

[0025] 1) mixing and grinding a magnesium hydroxide coarse material with a surface modifier to obtain magnesium hydroxide particles, and wet-grinding the magnesium hydroxide particles and a transition metal salt solution to obtain a transition metal-coated magnesium hydroxide slurry;

[0026] 2) Mixing the transition metal ion-coated magnesium hydroxide slurry with an organic amine modifier and grinding the mixture to obtain a modified magnesium hydroxide flame retardant.

[0027] In the present invention, the surface modifier in step 1) comprises one or more of acrylate, polyacrylic acid, methyl methacrylate oligomer, monolauryl phosphate, potassium monododecyl phosphate, potassium lauryl ether phosphate, and ammonium fatty alcohol polyoxyethylene ether sulfate.

[0028] In the present invention, the mass ratio of the surface modifier to magnesium hydroxide is 1:50-1000, preferably 1:200-800, more preferably 1:300-700, more preferably 1:400-600, and even more preferably 1:450-550.

[0029] In the present invention, the transition metal ion in the transition metal salt solution in step 1) is Ce 4+ ,La 3+ and Ni 3+ One or more of the .

[0030] In the present invention, the mass ratio of the transition metal ion to magnesium hydroxide is 1:100-1000, preferably 1:200-800, more preferably 1:300-700, more preferably 1:400-600, and even more preferably 1:450-550.

[0031] In the present invention, before the magnesium hydroxide particles are mixed with the transition metal salt solution in step 1), the magnesium hydroxide particles are preferably mixed with water to form a slurry with a solid content of 50-80%, and the solid content is preferably 55-75%, more preferably 60-70%, and more preferably 65%.

[0032] In the present invention, the particle size of the magnesium hydroxide coarse material in step 1) is 0.1 to 50 μm, preferably 10 to 45 μm, more preferably 20 to 40 μm, and more preferably 30 to 40 μm.

[0033] In the present invention, the grinding temperature in step 1) is 55-90°C, preferably 60-85°C, more preferably 65-80°C, and more preferably 70-75°C.

[0034] In the present invention, the particle size of the magnesium hydroxide particles is 0.1 to 10 μm, preferably 1 to 9 μm, more preferably 2 to 8 μm, more preferably 3 to 7 μm, and even more preferably 4 to 6 μm.

[0035] In the present invention, the wet grinding time in step 1) is 1 to 3 hours, preferably 1.5 to 2.5 hours, more preferably 1.8 to 2.3 hours, and more preferably 2 hours.

[0036] In the present invention, the general formula of the organic amine modifier in step 2) is wherein R1 is an alkane group, preferably a straight-chain alkane group, more preferably an alkane group with 1 to 18 carbon atoms, and more preferably an alkane group with 2 to 10 carbon atoms; R2 and R3 are independently H or an alkane group, preferably a straight-chain alkane group, more preferably an alkane group with 1 to 18 carbon atoms, and more preferably an alkane group with 2 to 10 carbon atoms;

[0037] The mass ratio of the organic amine modifier to the magnesium hydroxide crude material is 1:50-200, preferably 1:70-180, further preferably 1:90-160, more preferably 1:110-140, and even more preferably 1:120-130.

[0038] In the present invention, the grinding time in step 2) is 1 to 3 hours, preferably 1.5 to 2.5 hours, more preferably 1.8 to 2.3 hours, and more preferably 2 hours.

[0039] In the present invention, after the grinding in step 2) is completed, the modified magnesium hydroxide flame retardant needs to be washed, centrifugally dehydrated and dried in sequence; the water content after drying is ≤0.4%, preferably 0.1-0.4%, and more preferably 0.2-0.3%.

[0040] The technical solutions provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the protection scope of the present invention.

[0041] Example 1

[0042] 1 kg of magnesium hydroxide coarse material with a diameter of 40 to 50 μm and 100 mL of a 2 wt% polyacrylic acid solution are added to a grinder, and ground at 75°C until the particle size of the magnesium hydroxide particles is 3.0 to 3.5 μm. Water is added to prepare a slurry with a solid content of 70%, and 150 mL of a 20 g / mL cerium nitrate (Ce(NO3)4) solution is added. Wet grinding is performed for 2 hours to obtain a transition metal Ce-coated magnesium hydroxide slurry.

[0043] 250 mL of 2 wt% n-butylamine solution was added to the above slurry, and the mixture was stirred and ground for 1 hour to obtain a mixed slurry containing a modified magnesium hydroxide flame retardant. The slurry was washed with water, centrifuged and dried to a water content of less than 0.4% to obtain a modified magnesium hydroxide flame retardant product 1.

[0044] The above steps were repeated twice to obtain product 2 and product 3.

[0045] The performance of products 1 to 3 and unmodified magnesium hydroxide particles were tested. 50 wt % of the above four magnesium hydroxide particles were added to polypropylene material and the limiting oxygen index thereof was tested. The test results are shown in Table 1.

[0046] Table 1 Performance test results of unmodified magnesium hydroxide particles and modified magnesium hydroxide flame retardant products 1 to 3

[0047]

[0048] The difference between the preparation method of the unmodified magnesium hydroxide particles and the preparation method of the modified magnesium hydroxide particles described in this embodiment is that no transition metal salt and n-butylamine are added.

[0049] It can be seen from Table 1 that after modification, the whiteness, moisture, particle size and other indicators of the product are not greatly affected, the oil absorption and oxygen index are significantly improved, and the contact angle is increased from 0 to 94.9°, which significantly improves the compatibility of magnesium hydroxide and resin and improves the flame retardant performance.

[0050] Example 2

[0051] 1 kg of magnesium hydroxide coarse material with a diameter of 30 to 40 μm and 100 mL of 1.0 wt% surface modifier monolauryl phosphate are added to a grinder and ground at 85°C until the particle size of the magnesium hydroxide particles is 2.5 to 3.0 μm. Water is added to prepare a slurry with a solid content of 65%, and 100 mL of lanthanum nitrate (La(NO3)3) solution with a concentration of 5 g / mL is added. Wet grinding is performed for 1.5 hours to obtain a magnesium hydroxide slurry coated with transition metal La.

[0052] Add 500 mL of 1.5 wt% N-methyloctadecylamine solution to the above slurry, stir and grind for 1 hour to obtain a mixed slurry containing modified magnesium hydroxide flame retardant, wash the slurry with water, centrifuge and dry it to a water content of less than 0.4% to obtain modified magnesium hydroxide flame retardant product 4.

[0053] The above steps were repeated twice to obtain product 5 and product 6.

[0054] The performance of products 1 to 3 and unmodified magnesium hydroxide particles were tested. 60 wt % of the above four magnesium hydroxide particles were added to polypropylene material and the limiting oxygen index thereof was tested. The test results are shown in Table 1.

[0055] Table 2 Performance test results of unmodified magnesium hydroxide particles and modified magnesium hydroxide flame retardant products 4 to 6

[0056]

[0057] The difference between the preparation method of the unmodified magnesium hydroxide particles and the preparation method of the modified magnesium hydroxide particles described in this embodiment is that no transition metal salt and N-methyloctadecylamine are added.

[0058] It can be seen from Table 2 that after modification, the whiteness, moisture, particle size and other indicators of the product are not greatly affected, the oil absorption and oxygen index are significantly improved, and the contact angle is increased from 0 to 99.1°, which significantly improves the compatibility of magnesium hydroxide with the resin and improves the flame retardant properties.

[0059] Example 3

[0060] 1 kg of magnesium hydroxide coarse material with a diameter of 30 to 50 μm and 100 mL of 0.7 wt% of the surface modifier fatty alcohol polyoxyethylene ether ammonium sulfate are added into a grinder, and ground at 65°C until the particle size of the magnesium hydroxide particles is 2.2 to 3.0 μm. Water is added to prepare a slurry with a solid content of 65%, and 100 mL of a nickel nitrate (Ni(NO3)3) solution with a concentration of 4 g / mL is added. Wet grinding is performed for 3 hours to obtain a transition metal Ni-coated magnesium hydroxide slurry.

[0061] 800 mL of 2.0 wt% triethanolamine solution was added to the above slurry, and the mixture was stirred and ground for 1 h to obtain a mixed slurry containing a modified magnesium hydroxide flame retardant. The slurry was washed with water, centrifuged and dried to a water content of less than 0.4% to obtain a modified magnesium hydroxide flame retardant product 7.

[0062] The above steps were repeated twice to obtain product 8 and product 9.

[0063] The performance of products 1 to 3 and unmodified magnesium hydroxide particles were tested. 60 wt % of the above four magnesium hydroxide particles were added to polypropylene material and the limiting oxygen index thereof was tested. The test results are shown in Table 1.

[0064] Table 3 Performance test results of unmodified magnesium hydroxide particles and modified magnesium hydroxide flame retardant products 7 to 9

[0065]

[0066] The difference between the preparation method of the unmodified magnesium hydroxide particles and the preparation method of the modified magnesium hydroxide particles described in this embodiment is that no transition metal salt and triethanolamine are added.

[0067] It can be seen from Table 3 that after modification, the whiteness, moisture, particle size and other indicators of the product are not greatly affected, the oil absorption and oxygen index are significantly improved, and the contact angle is increased from 0 to 103.1 0 , which significantly improved the compatibility of magnesium hydroxide with resin and improved the flame retardant properties.

[0068] The methods and standards for the performance tests in the above embodiments are as follows:

[0069] Whiteness: tested according to GB / T5950-2008 standard;

[0070] Oil absorption: tested in accordance with DB / T5211.15-2014 standard; Oxygen index test: tested in accordance with GB / T2406.2-2009 standard;

[0071] Particle size distribution: Laser particle distribution measuring instrument measures particle distribution;

[0072] Specific surface area: using BET multi-point tester;

[0073] Loss on ignition: tested according to GB / T 33385-2016; Moisture content: tested according to GB / T 6284;

[0074] Surface contact angle: The Mg(OH)2 sample was pressed into a cake shape using the infrared pressing method, and the water contact angle of Mg(OH)2 before and after modification was measured.

[0075] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for preparing a modified magnesium hydroxide flame retardant, characterized in that: The following steps are involved: 1) mixing and grinding a magnesium hydroxide coarse material with a surface modifier to obtain magnesium hydroxide particles, and wet-grinding the magnesium hydroxide particles and a transition metal salt solution to obtain a transition metal-coated magnesium hydroxide slurry; 2) Mixing the transition metal ion-coated magnesium hydroxide slurry with an organic amine modifier and grinding the mixture to obtain a modified magnesium hydroxide flame retardant.

2. The method for preparing a modified magnesium hydroxide flame retardant according to claim 1, characterized in that: In the step 1), the surface modifier comprises one or more of acrylate, polyacrylic acid, methyl methacrylate oligomer, monolauryl phosphate, potassium monododecyl phosphate, potassium lauryl ether phosphate, and ammonium sulfate of fatty alcohol polyoxyethylene ether; The mass ratio of the surface modifier to magnesium hydroxide is 1:50-1000.

3. A method for preparing a modified magnesium hydroxide flame retardant according to claim 2, characterized in that, The transition metal ion in the transition metal salt solution in step 1) is Ce 4+ ,La 3+ and Ni 3+ One or more of the following; The mass ratio of the transition metal ion to the magnesium hydroxide is 1:100-1000.

4. A method for preparing a modified magnesium hydroxide flame retardant according to claim 2 or 3, characterized in that: The particle size of the magnesium hydroxide coarse material in step 1) is 0.1 to 50 μm.

5. The method for preparing a modified magnesium hydroxide flame retardant according to claim 4, characterized in that: The grinding temperature in step 1) is 55-90° C., and the particle size of the magnesium hydroxide particles is 0.1-10 μm.

6. The method for preparing a modified magnesium hydroxide flame retardant according to claim 5, characterized in that: The wet grinding time in step 1) is 1 to 3 hours.

7. The method for preparing a modified magnesium hydroxide flame retardant according to claim 6, characterized in that: The general formula of the organic amine modifier in step 2) is Wherein R1 is an alkane group, R2 and R3 are independently H or an alkane group; The mass ratio of the organic amine modifier to the magnesium hydroxide crude material is 1:50-200.

8. A method for preparing a modified magnesium hydroxide flame retardant according to claim 6 or 7, characterized in that: The grinding time in step 2) is 1 to 3 hours.

9. The modified magnesium hydroxide flame retardant prepared by the preparation method of any one of claims 1 to 8.