Preparation method of super-amphiphobic radiation refrigeration material
By preparing superamphiphobic radiation refrigeration materials and using porous structure and fluorosilane modification technology, the problems of low reflectivity and poor self-cleaning performance of radiation refrigeration materials in complex environments have been solved, and efficient refrigeration performance and weather resistance have been achieved.
Patent Information
- Application Number
- CN202410874868.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-02
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2044-07-02
AI Technical Summary
Existing radiation refrigeration materials are easily contaminated by low surface energy pollutants in complex environments, resulting in reduced reflectivity and poor self-cleaning performance, and cannot effectively maintain refrigeration performance.
Using the preparation method of super amphiphobic radiation refrigeration materials, polyvinylidene fluoride-hexafluoropropylene is mixed with alumina dispersion, and ingredients such as isopropyl alcohol, water and tetraethyl silicate are added to form a spray liquid, which is then scraped and coated The porous structure material is prepared by spraying process and modified by vapor deposition fluorosilane to achieve high reflectivity and high emissivity while also having excellent self-cleaning performance.
It achieves 99% solar reflectivity and 97% infrared emissivity in complex environments, can reduce the ambient temperature at high temperatures, has good weather resistance and self-cleaning performance, and is suitable for ground objects such as buildings and vehicles.
Smart Images

Figure CN118755321A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the fields of radiation refrigeration materials and super-amphiphobic materials, and in particular to a method for preparing a super-amphiphobic radiation refrigeration material. Background Art
[0002] In recent years, global warming has led to a continuous rise in the earth's temperature and an intensification of the urban heat island effect. Especially in the hot summer, strong solar radiation causes the ground temperature to rise sharply, which has increased human dependence on power systems such as air conditioning, greatly increased energy consumption and generated a large amount of greenhouse gas emissions, exacerbating climate change and global warming. Therefore, the development of more environmentally friendly and energy-saving refrigeration technology is of great significance to alleviating the energy crisis and climate change.
[0003] Zero-energy, zero-pollution passive daytime radiative cooling (PDRC) is considered to be one of the most feasible solutions to replace traditional electric cooling. According to the second law of thermodynamics, heat will always spontaneously transfer from the surface of a high-temperature object to the surface of a low-temperature object. This process is irreversible. There are three forms of heat transfer in nature, including heat conduction, heat convection, and thermal radiation. Thermal radiation is fundamentally generated by the energy level transition of matter. For any object with a temperature greater than 0K, the thermal radiation process can be achieved by emitting electromagnetic waves. Radiative cooling materials can efficiently reflect sunlight with a wavelength of 0.3-2.5μm, and can emit their own heat in the form of electromagnetic waves through the 8-13μm "atmospheric transparent window" to the cold outer space (3K), thereby achieving a zero-energy cooling method.
[0004] However, due to the surface wettability of these radiation cooling materials, dust and pollutant particles can easily adhere to the surface, resulting in low solar spectrum reflectivity and reduced thermal emissivity, which seriously affects their radiation cooling performance. Radiative cooling materials that only have superhydrophobic self-cleaning properties are still easily contaminated by low surface energy pollutants in the actual environment, such as oil stains, bird droppings, etc., and low surface energy pollutants even cause the temperature to rise due to their high solar spectrum absorption rate, causing the radiation cooling materials to lose their cooling performance. In order to make the radiation cooling material superhydrophobic to most low surface energy pollutants in a complex environment, it is urgent to design a good daytime radiation cooling material with superamphiphobic properties and excellent weather resistance in a complex environment. Summary of the invention
[0005] In order to overcome the problems existing in the prior art, the present invention proposes a method for preparing a super-amphiphobic radiation refrigeration material. The method is simple, efficient, low-cost, good in performance, and can be mass-produced. The prepared material has both high reflectivity and high emissivity, and has excellent self-cleaning liquid-repellent properties and good weather resistance in complex environments. At the same time, it solves the problems of low reflectivity and poor self-cleaning performance of the radiation refrigeration material.
[0006] In order to achieve the above object, the technical solution adopted by the present invention is:
[0007] A first aspect of the present invention provides a method for preparing a super-amphiphobic radiation refrigeration material, comprising the following steps:
[0008] (1) dissolving polyvinylidene fluoride-hexafluoropropylene in acetone and then adding alumina dispersion to prepare a radiation refrigeration material base liquid;
[0009] (2) mixing isopropyl alcohol, water and silicon dioxide to prepare liquid A, and mixing tetraethyl silicate, hydrochloric acid and ethanol to prepare liquid B. Liquid A and liquid B are mixed to prepare a super-amphiphobic spray liquid;
[0010] (3) After the radiation cooling material base liquid is obtained by a doctor blade method, the super-amphiphobic spray liquid is sprayed onto the radiation cooling substrate by a spraying method to obtain the super-amphiphobic radiation cooling material.
[0011] Preferably, the mass fraction of aluminum oxide in the aluminum oxide dispersion is 4-6wt%, and the dispersion medium is ethanol and ultrapure water in a mass ratio of 1:(0.5-1.5); further preferably, the mass fraction of aluminum oxide in the aluminum oxide dispersion is 5wt%, and the dispersion medium is ethanol and ultrapure water in a mass ratio of 1:1.
[0012] Preferably, the mass ratio of the dispersion medium of the polyvinylidene fluoride-hexafluoropropylene, acetone and alumina dispersion is 2:7:(3-5); further preferably, the mass ratio of the dispersion medium of the polyvinylidene fluoride-hexafluoropropylene, acetone and alumina dispersion is 2:7:4.
[0013] Preferably, the particle size of the alumina particles in the alumina dispersion is 250-350 nm; the particle size of the silicon dioxide is 25-35 nm; further preferably, the particle size of the alumina particles in the alumina dispersion is 280-320 nm; the particle size of the silicon dioxide is 28-32 nm.
[0014] Preferably, the content of silicon dioxide in the liquid A is 1-10wt%, the content of tetraethyl silicate in the liquid B is 50-60wt%, and the mass ratio of the liquid A to the liquid B is 1:(0.3-0.7).
[0015] Preferably, in step (3), the scraping parameters of the scraping method are 30 cm / min and the scraping distance is 20 cm.
[0016] Preferably, in step (3), the spraying method is: placing the super-amphiphobic spray liquid under a pressure of 0.3-0.5 MPa, first placing the radiation refrigeration substrate on a hot table at 65°C and heating it for 5 minutes, then adjusting the spray brush to a distance of 15 cm from the surface of the radiation refrigeration substrate, the spray brush angle is 60° to the surface of the radiation refrigeration substrate, and spraying the solution on the surface of the substrate.
[0017] Preferably, in step (3), the spraying amount of the super-amphiphobic spraying liquid on each square centimeter of the radiation cooling substrate is 0.1-0.2 g.
[0018] Preferably, after the super-amphiphobic radiation refrigeration material is prepared in step (3), the surface is modified with fluorosilane by vapor deposition, and finally washed and dried.
[0019] Further preferably, the fluorosilane material used for the surface fluorosilane modification includes 1H,1H,2H,2H-perfluorodecyltrichlorosilane.
[0020] After vapor deposition fluorination, long-chain fluorosilane is grafted to achieve a super-amphiphobic effect. The large pores of the substrate will make the performance better. Secondly, 30nm silicon oxide nanoparticles and hydrolyzed tetraethyl silicate will increase the reflectivity of the base film and the overall sunlight and infrared emissivity. The macroporous structure of the base film makes the super-amphiphobic structure more stable and effective in the long term. The two functional layers complement each other.
[0021] Further preferably, the surface fluorosilane modification is as follows: firstly, the sprayed super-amphiphobic radiation refrigeration material and an open container are placed in a sealed environment, and then 1H, 1H, 2H, 2H-perfluorodecyltrichlorosilane is dripped into the container, and vacuum is drawn to allow the super-amphiphobic radiation refrigeration material to stand at room temperature in a vacuum-sealed environment for 10-20 minutes.
[0022] A second aspect of the present invention provides a super-amphiphobic radiation refrigeration material, which is prepared by the preparation method of the super-amphiphobic radiation refrigeration material.
[0023] Compared with the prior art, the present invention has the following beneficial effects:
[0024] The ratio of non-solvent water, ethanol, and alumina and the selection of alumina particle size are the key to the high performance of this radiant refrigeration material. Such a process will enable the casting liquid to form a uniformly dispersed porous structure.
[0025] The porous structure of the substrate film of the present invention mainly plays a role of high reflectivity (radiative cooling function); the super-amphiphobic mechanism of the present invention is that the hydrolyzed tetraethyl silicate will form a protruding multi-porous structure with silicon oxide nanoparticles, and long-chain fluorosilane is grafted after vapor deposition fluorination to achieve a super-amphiphobic effect. The most critical process is the amount of liquid B (tetraethyl silicate, isopropyl alcohol, ethanol, hydrochloric acid), and liquid B controls the morphology of the entire super-amphiphobic process, including the final super-amphiphobic performance and mechanical properties.
[0026] The super-amphiphobic radiation cooling material prepared by the present invention has a reflectivity of 99% in the sunlight band and an emissivity of 97% in the atmospheric window. It can cause a sub-ambient temperature drop of 5°C in hot weather (≈35°C). While having high reflectivity and high emissivity, it has excellent self-cleaning and liquid-repellent properties, which makes it have good weather resistance in complex environments. This super-amphiphobic radiation cooling material that combines radiation cooling with super-amphiphobic self-cleaning properties is expected to achieve expanded production and can be used in buildings, vehicles and other ground objects, which is of great significance to alleviating the energy crisis and climate change. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 Schematic diagram of modeling of super-amphiphobic radiation cooling materials;
[0028] Figure 2 This is a physical picture of the super-amphiphobic radiation cooling material;
[0029] Figure 3 This is the SEM image of the super-amphiphobic radiation cooling material;
[0030] Figure 4 This is a SEM image of a glass substrate sprayed with super-amphiphobic spray liquid alone;
[0031] Figure 5 The solar spectrum reflectivity and infrared emissivity diagram of the super-amphiphobic radiation cooling material;
[0032] Figure 6 This is the contact angle data diagram of super-amphiphobic radiation cooling material;
[0033] Figure 7 This is the pore size distribution diagram of super-amphiphobic radiation cooling material;
[0034] Figure 8 This is a set of pictures for outdoor temperature testing;
[0035] Fig. 9 The effect of different amounts of liquid B added on CA and SA;
[0036] Fig.10 The effect of different amounts of B liquid added on mechanical properties;
[0037] Fig.11The effect of different silica solid contents on CA and SA. DETAILED DESCRIPTION
[0038] The specific embodiments of the present invention are further described below. It should be noted that the description of these embodiments is used to help understand the present invention, but does not constitute a limitation of the present invention. In addition, the technical features involved in each embodiment of the present invention described below can be combined with each other as long as they do not conflict with each other.
[0039] The experimental methods in the following examples are conventional methods unless otherwise specified, and the experimental materials used in the following examples are commercially available unless otherwise specified.
[0040] The test methods in the following embodiments are as follows:
[0041] 1) Take photos of real objects: Use the front camera of your phone to take photos.
[0042] 2) Reflectivity and emissivity test: The UV spectrophotometer model is Hitachi UH5700, which tests the reflectivity in the 200-3000nm band. The infrared emission model is INVENIO R, with a resolution of 4cm-1, 32scans, and a scanning band range of 2.5μm-25μm, which tests the infrared emissivity of the material.
[0043] 3) Surface morphology analysis: The surface morphology of the layer was photographed using a Thermo Fisher Axia scanning electron microscope, and the pore size of the material surface microstructure was counted using ImageJ.
[0044] 4) Wettability: The static contact angle was measured 3-5 times at different positions of each sample using a Data Physics OC20 goniometer, and the rolling angle was measured using an adjustable tilt stage.
[0045] 5) Outdoor cooling effect test: The test device is an independent car model. Three groups of comparative tests are conducted using super-amphiphobic radiation cooling materials of the same thickness, commercial cloth wrapping, and no wrapping. Thermocouples are placed in the grooves covered by the samples, and the multi-channel temperature tester AT4208 is used to record the cooling temperature and air temperature of the samples. The power meter TES-1333R is used to synchronously test the solar power. The humidity thermometer TP500 is used to record the temperature and humidity changes of the environment in real time.
[0046] 6) Gravel impact test: Place the sample on a 45° inclined table and impact the sample with gravel of a certain mass at a certain height. After the impact, use a DataPhysicsOC20 goniometer to perform 3-5 measurements at different positions of each sample. Use an adjustable angle inclined table to measure the rolling angle. The mechanical properties of the material are determined by the contact angle and rolling angle.
[0047] Example 1
[0048] This example explores the effect of the B liquid content on the super-amphiphobic performance.
[0049] The preparation of super-amphiphobic radiation cooling material includes the following steps:
[0050] (1) Add 2 g of vinylidene fluoride-hexafluoropropylene to 7 g of acetone, stir evenly, and then ultrasonicate for 30 min to form a uniform dispersion.
[0051] (2) Add a non-solvent containing 5 wt% of 300 nm aluminum oxide dispersion to the above dispersion, the non-solvent consists of 50% ethanol and 50% ultrapure water, and the mass ratio of vinylidene fluoride-hexafluoropropylene: acetone: non-solvent is 2:7:4. After stirring evenly, ultrasonic dispersion is performed for 1 hour to obtain a stable white dispersion, i.e., the base liquid of the radiation refrigeration material.
[0052] (3) Take 2 g of isopropyl alcohol, 5 g of ultrapure water, and 0.3 g of silicon dioxide, stir evenly, and then ultrasonicate for 1 h to form a uniform dispersion liquid A. Take 3 g of tetraethyl silicate, 1 g of 0.1 mol / L dilute hydrochloric acid, and 1.5 g of ethanol, stir evenly, and then ultrasonicate for 1 h to obtain a stably dispersed liquid B. By adding different masses of liquid B to liquid A, super-amphiphobic spray liquids with different super-amphiphobic properties and mechanical properties can be obtained.
[0053] (4) using a scraping method to obtain a radiative cooling substrate using a radiative cooling base liquid, the scraping parameters of the scraping machine are set to 30 cm / min, and the scraping distance is 20 cm; spraying the super-amphiphobic spray liquid onto the radiative cooling base film by a spraying method to obtain a super-amphiphobic radiative cooling material, wherein the spraying is as follows: placing the super-amphiphobic spray liquid under a pressure of 0.3-0.5 MPa, first placing the radiative cooling substrate on a hot plate at 65°C and heating it for 5 minutes, then adjusting the spray brush to a distance of 15 cm from the surface of the radiative cooling substrate, the spray brush angle is 60° with the surface of the radiative cooling substrate, and spraying the solution on the surface of the substrate.
[0054] (5) Surface fluorosilane modification by vapor deposition: first, the sprayed super-amphiphobic radiation cooling material and an open container are placed in a sealed environment, and then a drop of 1H,1H,2H,2H-perfluorodecyltrichlorosilane is dripped into the container, and the super-amphiphobic radiation cooling material is allowed to stand at room temperature in a vacuum-sealed environment for 15 minutes, and finally washed and dried to obtain the super-amphiphobic radiation cooling material.
[0055] According to the above preparation process, super-amphiphobic spray liquids with B liquid addition amounts of 0g, 1g, 2g, 3g, 4g, 5g, and 6g were used for spraying respectively; the super-amphiphobic performance liquids with 7 B liquid addition amounts have different mechanical properties, and the ethylene glycol contact angle rolling angle and the maximum anti-gravel quality corresponding to different B liquid addition amounts are shown in Table 1 below:
[0056] Table 1
[0057] Amount of liquid B added (g) Contact angle (°) Roll angle (°) Gravel mass (g) 0 177 1 12 1 168 1 45 2 170 1 55 3 169 1 58 4 167 2 54 5 161 2 36 6 162 4 20
[0058] It can be seen from the above table that with the increase in the amount of B liquid added, the performance of the superamphiphobic material only decreases slightly, but its mechanical properties are greatly improved, reaching the optimal value at 3g, so the optimal addition amount is 3g of B liquid.
[0059] Figure 2 This is a physical picture of the super-amphiphobic radiation cooling material prepared when the addition amount of liquid B is 3g; Figure 3 The SEM image of the super-amphiphobic radiation cooling material prepared when the addition amount of liquid B is 3g. Figure 3 It can be seen that the material has a multi-level porous micro-nano structure, and the multi-level pore structure makes the membrane material have an ultra-high solar reflectivity.
[0060] Figure 4 This is the SEM image of the super-amphiphobic spray liquid sprayed on the glass substrate when the addition amount of liquid B is 3g. Figure 4 It can be seen that the silicon oxide particles on the surface introduce relatively rough micron protrusions to the membrane surface, which not only enhances the overall scattering degree, but also makes the surface have super-amphiphobic properties with high contact angle and low rolling angle for low surface tension solvents. Figure 5 The solar spectrum reflectivity and infrared emissivity of the super-amphiphobic radiation cooling material prepared when the addition amount of liquid B is 3g are shown in the figure. Figure 5 It can be seen that the prepared super-amphiphobic radiation cooling material has a reflectivity of up to 99% in the solar light band and an emissivity of 97% in the 8-13μm atmospheric window.
[0061] Figure 6 The contact angle data of the super-amphiphobic radiation cooling material prepared when the addition amount of liquid B is 3g is shown in FIG. Figure 6 It can be seen that the liquid-repellent property of the super-amphiphobic layer is very excellent, with contact angles of more than 150° and rolling angles less than 5° for water and various oil droplets.
[0062] Figure 7 The pore size distribution diagram of the super-amphiphobic radiation cooling material prepared when the addition amount of liquid B is 3g, Figure 7 It can be seen that the pore size distribution of the super-amphiphobic radiative cooling film is 6±5μm.
[0063] Figure 8 This is a set of pictures of outdoor temperature test, Figure 8 It can be seen that this material has excellent refrigeration performance. The temperature of the group covered with the super-amphiphobic radiation refrigeration film under direct sunlight is 5±3℃ lower than that of the group covered with commercial cloth, and 10±5℃ lower than that of the exposed group.
[0064] Fig. 9 The effect of different amounts of B liquid added on CA (contact angle) and SA (sliding angle); Fig. 9 It can be seen that with the increase of the content of liquid B, CA (contact angle) and SA (sliding angle) do not change much at the beginning, and then CA (contact angle) gradually decreases and SA (sliding angle) gradually increases.
[0065] Fig.10 The effect of different amounts of B liquid added on the mechanical properties is shown in Figure 2. Fig.10 It can be seen that when the addition amount of B liquid is 3g, it has the best mechanical strength and can withstand 60g of gravel impact without losing the super amphiphobic property.
[0066] Example 2
[0067] This example explores the effect of the content of aluminum oxide nanoparticles on reflectivity.
[0068] The preparation process of super-amphiphobic radiation cooling material includes the following steps:
[0069] (1) Add 2 g of vinylidene fluoride-hexafluoropropylene to 7 g of acetone, stir evenly, and then ultrasonicate for 30 min to form a uniform dispersion.
[0070] (2) Add a non-solvent containing a series of mass concentrations of 300 nm alumina dispersion to the above dispersion, wherein the non-solvent consists of 50% ethanol and 50% ultrapure water, and the mass ratio of vinylidene fluoride-hexafluoropropylene: acetone: non-solvent is 2:7:4. After stirring evenly, ultrasonic dispersion is performed for 1 hour to obtain a stable white dispersion, i.e., the base liquid of the radiation refrigeration material.
[0071] (3) Take 2 g of isopropyl alcohol, 5 g of ultrapure water, and 0.3 g of silicon dioxide, stir them evenly, and then ultrasonicate for 1 h to form a uniform dispersion liquid A. Take 3 g of tetraethyl silicate, 1 g of 0.1 mol / L dilute hydrochloric acid, and 1.5 g of ethanol, stir them evenly, and then ultrasonicate for 1 h to obtain a stably dispersed liquid B. Add 3 g of liquid B to liquid A to prepare a super-amphiphobic spray liquid.
[0072] (4) using a scraping method to obtain a radiative cooling substrate using a base liquid of the radiative cooling material, the scraping parameters of the scraping machine are set to 30 cm / min, and the scraping distance is 20 cm; spraying the super-amphiphobic spray liquid onto the radiative cooling base film by a spraying method to obtain a super-amphiphobic radiative cooling material, wherein the spraying is as follows: placing the super-amphiphobic spray liquid under a pressure of 0.3-0.5 MPa, first placing the radiative cooling substrate on a hot plate at 65°C and heating it for 5 minutes, then adjusting the spray brush to a distance of 15 cm from the surface of the radiative cooling substrate, the spray brush angle is 60° with the surface of the radiative cooling substrate, and spraying the solution on the surface of the substrate.
[0073] (5) Surface fluorosilane modification by vapor deposition: first, the sprayed super-amphiphobic radiation cooling material and an open container are placed in a sealed environment, and then a drop of 1H,1H,2H,2H-perfluorodecyltrichlorosilane is dripped into the container, and the super-amphiphobic radiation cooling material is allowed to stand at room temperature in a vacuum-sealed environment for 15 minutes, and finally washed and dried to obtain the super-amphiphobic radiation cooling material.
[0074] According to the above preparation process, 300nm alumina particles with a percentage content of 0%, 1%, 2%, 3%, 4%, 5%, and 6% are added respectively for preparation. The preparation process is the same as that of the above embodiment 1. The different percentage contents of 300nm alumina particles will lead to different reflectivities of the super-amphiphobic radiation cooling material. The reflectivities corresponding to different percentage contents of 300nm alumina are shown in Table 2 below:
[0075] Table 2
[0076] Alumina content (%) Reflectivity(%) 0 96.3347 1 96.4708 2 97.5315 3 98.3992 4 98.7501 5 99.2795 6 99.2747
[0077] It can be seen from the above table that with the increase of the percentage of aluminum oxide particles, the reflectivity performance is greatly improved, reaching the optimal value at 5%, so the aluminum oxide percentage content is 5% is the optimal value.
[0078] Example 3
[0079] This example explores the effect of silicon dioxide content on the contact angle.
[0080] (1) Add 2 g of vinylidene fluoride-hexafluoropropylene to 7 g of acetone, stir evenly, and then ultrasonicate for 30 min to form a uniform dispersion.
[0081] (2) Add a non-solvent containing 5 wt% of 300 nm aluminum oxide dispersion to the above dispersion, the non-solvent consists of 50% ethanol and 50% ultrapure water, and the mass ratio of vinylidene fluoride-hexafluoropropylene: acetone: non-solvent is 2:7:4. After stirring evenly, ultrasonic dispersion is performed for 1 hour to obtain a stable white dispersion, i.e., the base liquid of the radiation refrigeration material.
[0082] (3) 2 g of isopropanol, 4 g of ultrapure water, and different contents of silicon dioxide were mixed and then ultrasonicated for 1 h to form a uniform dispersion A liquid. 3 g of tetraethyl silicate, 1 g of 0.1 mol / L dilute hydrochloric acid, and 1.5 g of ethanol were mixed and then ultrasonicated for 1 h to obtain a stably dispersed B liquid. 3 g of B liquid was added to A liquid to prepare a super-amphiphobic spray liquid.
[0083] (4) using a scraping method to obtain a radiative cooling substrate using a base liquid of the radiative cooling material, the scraping parameters of the scraping machine are set to 30 cm / min, and the scraping distance is 20 cm; spraying the super-amphiphobic spray liquid onto the radiative cooling base film by a spraying method to obtain a super-amphiphobic radiative cooling material, wherein the spraying is as follows: placing the super-amphiphobic spray liquid under a pressure of 0.3-0.5 MPa, first placing the radiative cooling substrate on a hot plate at 65°C and heating it for 5 minutes, then adjusting the spray brush to a distance of 15 cm from the surface of the radiative cooling substrate, the spray brush angle is 60° with the surface of the radiative cooling substrate, and spraying the solution on the surface of the substrate.
[0084] (5) Surface fluorosilane modification by vapor deposition: first, the sprayed super-amphiphobic radiation cooling material and an open container are placed in a sealed environment, and then a drop of 1H,1H,2H,2H-perfluorodecyltrichlorosilane is dripped into the container, and the super-amphiphobic radiation cooling material is allowed to stand at room temperature in a vacuum-sealed environment for 15 minutes, and finally washed and dried to obtain the super-amphiphobic radiation cooling material.
[0085] According to the above preparation process, 0.6wt%, 1.2wt%, 1.8wt%, 2.4wt%, and 3.0wt% of silica were added to the A liquid respectively. The preparation process was the same as that of Example 1. The contact angle and sliding angle of different silica contents were measured. The results are as follows Fig.11 As shown by Fig.11 It can be seen that with the increase of the mass fraction of silicon oxide, the CA (contact angle) and SA (sliding angle) performance data of oil droplets are significantly improved, with the CA (contact angle) improving by more than 40° and the SA (sliding angle) improving by more than 10°.
[0086] The embodiments of the present invention are described in detail above, but the present invention is not limited to the described embodiments. For those skilled in the art, various changes, modifications, substitutions and variations of these embodiments are made without departing from the principles and spirit of the present invention, and still fall within the protection scope of the present invention.
Claims
1. A method for preparing a super-amphiphobic radiation refrigeration material, characterized in that: The following steps are involved: (1) dissolving polyvinylidene fluoride-hexafluoropropylene in acetone and then adding alumina dispersion to prepare a radiation refrigeration material base liquid; (2) mixing isopropyl alcohol, water and silicon dioxide to prepare liquid A, and mixing tetraethyl silicate, hydrochloric acid and ethanol to prepare liquid B. Liquid A and liquid B are mixed to prepare a super-amphiphobic spray liquid; (3) After the radiation cooling material base liquid is obtained by a doctor blade method, the super-amphiphobic spray liquid is sprayed onto the radiation cooling substrate by a spraying method to obtain the super-amphiphobic radiation cooling material.
2. The method for preparing the super-amphiphobic radiation refrigeration material according to claim 1, characterized in that: The mass fraction of aluminum oxide in the aluminum oxide dispersion is 4-6wt%, and the dispersion medium is ethanol and ultrapure water in a mass ratio of 1: (0.5-1.5).
3. The method for preparing the super-amphiphobic radiation refrigeration material according to claim 2, characterized in that: The mass ratio of the dispersion medium of the polyvinylidene fluoride-hexafluoropropylene, acetone and aluminum oxide dispersion is 2:7:(3-5).
4. The method for preparing the super-amphiphobic radiation refrigeration material according to claim 1, characterized in that: The particle size of the aluminum oxide particles in the aluminum oxide dispersion is 250-350 nm; the particle size of the silicon dioxide is 25-35 nm.
5. The method for preparing the super-amphiphobic radiation refrigeration material according to claim 1, characterized in that: The content of silicon dioxide in the liquid A is 1-10wt%, the content of tetraethyl silicate in the liquid B is 50-60wt%, and the mass ratio of the liquid A to the liquid B is 1:(0.3-0.7).
6. The method for preparing the super-amphiphobic radiation refrigeration material according to claim 1, characterized in that: In step (3), the spraying amount of the super-amphiphobic spraying liquid on each square centimeter of the radiation cooling substrate is 0.1-0.2 g.
7. The method for preparing the super-amphiphobic radiation refrigeration material according to claim 1, characterized in that: After the super-amphiphobic radiation refrigeration material is prepared in step (3), the surface is modified with fluorosilane by vapor deposition, and finally washed and dried.
8. The method for preparing the super-amphiphobic radiation refrigeration material according to claim 7, characterized in that: The fluorosilane material used for the surface fluorosilane modification includes 1H, 1H, 2H, 2H-perfluorodecyltrichlorosilane.
9. The method for preparing the super-amphiphobic radiation refrigeration material according to claim 8, characterized in that: The surface fluorosilane modification is as follows: firstly, the sprayed super-amphiphobic radiation cooling material and an open container are placed in a sealed environment, then 1H, 1H, 2H, 2H-perfluorodecyltrichlorosilane is dripped into the container, and vacuum is drawn to allow the super-amphiphobic radiation cooling material to stand at room temperature in a vacuum sealed environment for 10-20 minutes.
10. A super-amphiphobic radiation refrigeration material, characterized in that: The super-amphiphobic radiation refrigeration material is prepared by the preparation method of the super-amphiphobic radiation refrigeration material according to any one of claims 1 to 9.
Citation Information
Patent Citations
Super-hydrophobic self-cleaning radiation self-cooling material and preparation method thereof
CN112852079A
Preparation method of antifouling self-cleaning type organic silicon radiation refrigeration coating
CN117025096A
Pervaporation separation membrane and method of manufacturing this membrane
JP2010149002A
Superhydrophobic surface and method for forming same
US20090011222A1